Ultrahigh impurity copper electrolysis process
Through the ultra-high impurity copper electrolysis process, using fire roughing and electrolysis treatment, recycling the electrolyte and recovering copper and nickel sulfate, the problem of high impurity electrolysis and high cost in the anode plate is solved, and efficient copper recovery and process cost are achieved. reduce.
Patent Information
- Application Number
- CN202411062409.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-11
AI Technical Summary
In the existing copper smelting process, the impurity content in the copper anode plate increases, and the copper grade fluctuates greatly, resulting in an increase in the complexity of the electrolysis process, and the raw material grade is low. It is difficult for the existing process to effectively handle high-impurity copper electrolysis, resulting in frequent passivation, and the process The cost is high.
Using ultra-high impurity copper electrolysis process, the anode plate is poured after rough refining by fire method, and electrolysis treatment is performed. Direct current is used to deposit copper ions under the action of electric field to deposit pure copper. The composition of the electrolyte is maintained through circulation pumps and heaters, and electrolysis is recycled. liquid, recover copper sulfate and nickel sulfate, and reduce process costs.
Effectively adapt to the electrolysis of high impurities in the anode plate, reduce passivation, realize recycling of electrolyte, reduce process costs, extend the use time of electrolyte, and improve copper recovery efficiency.
Smart Images

Figure CN118756248A_ABST
Abstract
Description
Technical Field
[0001] The invention specifically relates to a process for electrolysis of ultra-high impurity copper, and belongs to the technical field of copper electrolysis. Background Art
[0002] The existing copper smelting process mainly includes side-blown furnace smelting, converter blowing, anode furnace refining, and electrolytic refining. With the competition among the copper smelting industry and the deterioration of raw material procurement, the copper grade of existing copper raw materials is lower and the impurity composition is more complex. Therefore, the content of impurities such as arsenic, antimony, and bismuth in the copper anode plate treated by the copper electrolysis process has doubled, while the content of main grade copper has dropped below 98%. In order to cope with the more complex situation of copper raw materials, the large fluctuation of anode plate copper grade, and the increase in the types of recovered metals, we propose a process for high-impurity copper electrolysis. Summary of the invention
[0003] The purpose of the present invention is to provide a process for the electrolysis of ultra-high impurity copper in view of the deficiencies of the prior art, which can adapt to the electrolysis of anode plates with relatively high impurities and reduce the occurrence of passivation. A certain amount of electrolyte is discharged into a liquid purification system every day, and the electrolyte is subjected to copper sulfate recovery, electrolytic impurity removal, and nickel sulfate extraction. The remaining acid is returned to the electrolysis for continued use, thereby directly recovering nickel sulfate and reducing process costs.
[0004] The present invention achieves the above-mentioned purpose through the following technical scheme, a process for electrolysis of ultra-high impurity copper, comprising the following steps:
[0005] Step 1: Placing anode plates: After high-impurity copper is roughly smelted by fire, it is cast into anode plates. Then workers arrange the anode plates as a whole and place them together with the starting electrode in the electrolytic cell for electrolysis;
[0006] Step 2, electrolysis: direct current is passed into the electrolytic cell, so that the copper ions in the electrolyte move to the cathode under the action of the electric field. At the cathode, the copper ions gain electrons and are reduced to pure copper and deposited on the cathode plate, while the copper on the anode loses electrons and becomes copper ions and enters the electrolyte, and anode mud is generated in the electrolytic cell at the same time;
[0007] Step 3: Maintain the composition of the electrolyte: During electrolysis, workers tear up the copper foil and add it to the copper melter. The electrolyte and air have a certain oxidizing property after mixing, which can dissolve the copper foil into the electrolyte to achieve the effect of replenishing copper ions. At the same time, when the electrolyte is pumped from the low-level tank to the high-level tank through the circulation pump, the heater can use steam to exchange heat with the electrolyte, thereby achieving the effect of heating the electrolyte;
[0008] Step 4: Cleaning the electrolytic cell: After the electrolysis is completed, stop supplying direct current to the electrolytic cell, then peel off the deposited pure copper from the cathode plate, and then take out the electrolyte and anode mud in the electrolytic cell for treatment;
[0009] Step 5: Treatment of impurities and filtrate: The mixed liquid of electrolyte and anode mud is separated by filter pressing, and the filtrate enters the clarification tank, and then is treated by filter pressing again, and then filled into the low-level tank for repeated use;
[0010] Step 6. Recovery of waste electrolyte: After the electrolysis is completed, the waste electrolyte in the low-level tank is decoppered, and the decoppered solution is passed into a nickel sulfate solution for reaction, followed by freezing and crystallization. After filtration, it is separated into crude nickel sulfate and black acid, and the black acid can be reused in the electrolysis process.
[0011] Furthermore, in order to improve the efficiency of electrolysis, the weight of the anode plate in step one is 210 kg, the spacing between the same poles is 95 mm, the size of the starting electrode plate is 0.74*1 m, the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
[0012] Furthermore, in order to electrolyze the anode plate, the direct current introduced in the step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte, and anode mud is generated in the electrolytic cell.
[0013] Furthermore, in order to complete the circulation of the electrolyte and heat the electrolyte to improve the efficiency of electrolysis, the circulation speed of the electrolyte in step three is 35L / min. The circulation speed of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after heating by the heater is 60-100°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions.
[0014] Furthermore, in order to complete the collection of pure copper and electrolyte, in the step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is peeled off, and then the peeled pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
[0015] Furthermore, in order to facilitate the processing of the electrolytic cell and thus enable it to be reused, the solution in the electrolytic cell collected in the step 4 is a mixed solution of anode mud and the electrolyte after the reaction, and the mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud, and then the filtrate is filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
[0016] Furthermore, in order to process part of the waste electrolyte and precipitate copper sulfate at the same time, the waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses, and the workers draw electrolyte from the low-level tank every day as waste electrolyte for treatment, thereby extending the use time of the electrolyte, and the waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, and then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, so that copper sulfate can be precipitated, and then the solution is subjected to primary and secondary decopperization, so that black copper mud can be precipitated, thereby obtaining a secondary decopperization solution.
[0017] Furthermore, in order to directly recover nickel sulfate and thus reduce process costs, the secondary decopperizing solution in step six is passed into a nickel sulfate solution for freeze crystallization, and then filtered to obtain a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be re-used in the electrolysis process.
[0018] The technical effects and advantages of the present invention are as follows: the present invention can adapt to electrolysis with a high level of impurities in the anode plate, and can reduce the occurrence of passivation. A certain amount of electrolyte is discharged into the liquid purification system every day, and the electrolyte is subjected to copper sulfate recovery, electrolytic impurity removal, and nickel sulfate extraction. The remaining acid is returned to the electrolysis for continued use, thereby directly recovering nickel sulfate and reducing process costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The electrolysis flow chart of the present invention;
[0020] Figure 2 is a processing flow chart of the waste electrolyte of the present invention;
[0021] Figure 3 The following is a detailed list of embodiments and comparative examples of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] See also Figure 1-Figure 2 As shown, a process for ultra-high impurity copper electrolysis comprises the following steps:
[0024] Step 1: Placing anode plates: After high-impurity copper is roughly smelted by fire, it is cast into anode plates. Then workers arrange the anode plates as a whole and place them together with the starting electrode in the electrolytic cell for electrolysis;
[0025] Step 2, electrolysis: direct current is passed into the electrolytic cell, so that the copper ions in the electrolyte move to the cathode under the action of the electric field. At the cathode, the copper ions gain electrons and are reduced to pure copper and deposited on the cathode plate, while the copper on the anode loses electrons and becomes copper ions and enters the electrolyte, and anode mud is generated in the electrolytic cell at the same time;
[0026] Step 3: Maintain the composition of the electrolyte: During electrolysis, workers tear up the copper foil and add it to the copper melter. The electrolyte and air have a certain oxidizing property after mixing, which can dissolve the copper foil into the electrolyte to achieve the effect of replenishing copper ions. At the same time, when the electrolyte is pumped from the low-level tank to the high-level tank through the circulation pump, the heater can use steam to exchange heat with the electrolyte, thereby achieving the effect of heating the electrolyte;
[0027] Step 4: Cleaning the electrolytic cell: After the electrolysis is completed, stop supplying direct current to the electrolytic cell, then peel off the deposited pure copper from the cathode plate, and then take out the electrolyte and anode mud in the electrolytic cell for treatment;
[0028] Step 5: Treatment of impurities and filtrate: The mixed liquid of electrolyte and anode mud is separated by filter pressing, and the filtrate enters the clarification tank, and then is treated by filter pressing again, and then filled into the low-level tank for repeated use;
[0029] Step 6. Recovery of waste electrolyte: After the electrolysis is completed, the waste electrolyte in the low-level tank is decoppered, and the decoppered solution is passed into a nickel sulfate solution for reaction, followed by freezing and crystallization. After filtration, it is separated into crude nickel sulfate and black acid, and the black acid can be reused in the electrolysis process.
[0030] Embodiment 1
[0031] The weight of the anode plate in step one is 210 kg, the spacing between the same poles is 95 mm, the size of the starting pole piece is 0.74*1 m, the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
[0032] The direct current introduced in step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte. At the same time, anode mud is generated in the electrolytic cell.
[0033] In step three, the circulation rate of the electrolyte is 35L / min. The circulation rate of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after heating by the heater is 65°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions. At this time, the time required for electrolysis is 330min, and the number of short circuits is 0.
[0034] In step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is stripped off, and then the stripped pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
[0035] The solution in the electrolytic cell collected in step 4 is a mixed solution of anode mud and the electrolyte after the reaction. The mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud. The filtrate is then filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
[0036] The waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses. Workers draw electrolyte from the low-level tank every day as waste electrolyte for treatment, thereby extending the service life of the electrolyte. The waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, thereby precipitating copper sulfate. The solution is then subjected to primary and secondary decoppering, thereby precipitating black copper mud, thereby obtaining a secondary decoppering solution. The secondary decoppering solution in step six is passed into a nickel sulfate solution for freeze crystallization, and then filtered, thereby obtaining a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be re-entered into the electrolysis process for use.
[0037] Embodiment 2
[0038] The weight of the anode plate in step one is 210 kg, the spacing between the same poles is 95 mm, the size of the starting pole piece is 0.74*1 m, the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
[0039] The direct current introduced in step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte. At the same time, anode mud is generated in the electrolytic cell.
[0040] In step three, the circulation rate of the electrolyte is 35L / min. The circulation rate of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after heating by the heater is 75°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions. At this time, the total time required to complete the electrolysis is 332min, the electrolysis time is 312min, and the number of short circuits is 1.
[0041] In step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is stripped off, and then the stripped pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
[0042] The solution in the electrolytic cell collected in step 4 is a mixed solution of anode mud and the electrolyte after the reaction. The mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud. The filtrate is then filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
[0043] The waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses. Workers draw electrolyte from the low-level tank every day as waste electrolyte for treatment, thereby extending the service life of the electrolyte. The waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, thereby precipitating copper sulfate. The solution is then subjected to primary and secondary decoppering, thereby precipitating black copper mud, thereby obtaining a secondary decoppering solution. The secondary decoppering solution in step six is passed into a nickel sulfate solution for freeze crystallization, and then filtered, thereby obtaining a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be re-entered into the electrolysis process for use.
[0044] Embodiment 3
[0045] The weight of the anode plate in step one is 210 kg, the spacing between the same poles is 95 mm, the size of the starting pole piece is 0.74*1 m, the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
[0046] The direct current introduced in step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte. At the same time, anode mud is generated in the electrolytic cell.
[0047] In step three, the circulation rate of the electrolyte is 35L / min. The circulation rate of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after heating by the heater is 85°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions. At this time, the total time required to complete the electrolysis is 344min, the electrolysis time is 304min, and the number of short circuits is 2 times.
[0048] In step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is stripped off, and then the stripped pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
[0049] The solution in the electrolytic cell collected in step 4 is a mixed solution of anode mud and the electrolyte after the reaction. The mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud. The filtrate is then filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
[0050] The waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses. Workers draw electrolyte from the low-level tank every day as waste electrolyte for treatment, thereby extending the service life of the electrolyte. The waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, thereby precipitating copper sulfate. The solution is then subjected to primary and secondary decoppering, thereby precipitating black copper mud, thereby obtaining a secondary decoppering solution. The secondary decoppering solution in step six is passed into a nickel sulfate solution for freeze crystallization, and then filtered, thereby obtaining a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be re-entered into the electrolysis process for use.
[0051] Embodiment 4
[0052] The weight of the anode plate in step one is 210 kg, the spacing between the same poles is 95 mm, the size of the starting pole piece is 0.74*1 m, the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
[0053] The direct current introduced in step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte. At the same time, anode mud is generated in the electrolytic cell.
[0054] In step three, the circulation rate of the electrolyte is 35L / min. The circulation rate of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after heating by the heater is 95°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions. At this time, the total time required to complete the electrolysis is 359min, the electrolysis time is 299min, and the number of short circuits is 3 times.
[0055] In step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is stripped off, and then the stripped pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
[0056] The solution in the electrolytic cell collected in step 4 is a mixed solution of anode mud and the electrolyte after the reaction. The mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud. The filtrate is then filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
[0057] The waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses. Workers draw electrolyte from the low-level tank every day as waste electrolyte for treatment, thereby extending the service life of the electrolyte. The waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, thereby precipitating copper sulfate. The solution is then subjected to primary and secondary decoppering, thereby precipitating black copper mud, thereby obtaining a secondary decoppering solution. The secondary decoppering solution in step six is passed into a nickel sulfate solution for freeze crystallization, and then filtered, thereby obtaining a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be re-entered into the electrolysis process for use.
[0058] Comparative Example 5
[0059] The weight of the anode plate in step one is 210 kg, the spacing between the same poles is 95 mm, the size of the starting pole piece is 0.74*1 m, the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
[0060] The direct current introduced in step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte. At the same time, anode mud is generated in the electrolytic cell.
[0061] In step three, the circulation rate of the electrolyte is 35L / min. The circulation rate of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after heating by the heater is 105°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions. At this time, the total time required to complete the electrolysis is 404min, the electrolysis time is 284min, and the number of short circuits is 6 times.
[0062] In step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is stripped off, and then the stripped pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
[0063] The solution in the electrolytic cell collected in step 4 is a mixed solution of anode mud and the electrolyte after the reaction. The mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud. The filtrate is then filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
[0064] The waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses. Workers draw electrolyte from the low-level tank every day as waste electrolyte for treatment, thereby extending the service life of the electrolyte. The waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, thereby precipitating copper sulfate. The solution is then subjected to primary and secondary decoppering, thereby precipitating black copper mud, thereby obtaining a secondary decoppering solution. The secondary decoppering solution in step six is passed into a nickel sulfate solution for freeze crystallization, and then filtered, thereby obtaining a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be re-entered into the electrolysis process for use.
[0065] Comparative Example 2
[0066] The weight of the anode plate in step one is 210 kg, the spacing between the same poles is 95 mm, the size of the starting pole piece is 0.74*1 m, the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
[0067] The direct current introduced in step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte. At the same time, anode mud is generated in the electrolytic cell.
[0068] In step three, the circulation rate of the electrolyte is 35L / min. The circulation rate of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after heating by the heater is 50°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions. At this time, the time required for electrolysis is 416min, and the number of short circuits is 0.
[0069] In step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is stripped off, and then the stripped pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
[0070] The solution in the electrolytic cell collected in step 4 is a mixed solution of anode mud and the electrolyte after the reaction. The mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud. The filtrate is then filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
[0071] The waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses. Workers draw electrolyte from the low-level tank every day as waste electrolyte for treatment, thereby extending the service life of the electrolyte. The waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, thereby precipitating copper sulfate. The solution is then subjected to primary and secondary decoppering, thereby precipitating black copper mud, thereby obtaining a secondary decoppering solution. The secondary decoppering solution in step six is passed into a nickel sulfate solution for freeze crystallization, and then filtered, thereby obtaining a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be re-entered into the electrolysis process for use.
[0072] In summary, the higher the temperature of the electrolyte, the faster the electrolysis efficiency, but the higher the temperature, the more times short circuits occur. Therefore, the total time required at 65°C is the shortest, and there is no need to eliminate the short circuit fault.
[0073] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0074] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A process for electrolysis of ultra-high impurity copper, Features: The following steps are involved: Step 1: Placing anode plates: After high-impurity copper is roughly smelted by fire, it is cast into anode plates. Then workers arrange the anode plates as a whole and place them together with the starting electrode in the electrolytic cell for electrolysis; Step 2, electrolysis: direct current is passed into the electrolytic cell, so that the copper ions in the electrolyte move to the cathode under the action of the electric field. At the cathode, the copper ions gain electrons and are reduced to pure copper and deposited on the cathode plate, while the copper on the anode loses electrons and becomes copper ions and enters the electrolyte, and anode mud is generated in the electrolytic cell at the same time; Step 3: Maintain the composition of the electrolyte: During electrolysis, workers tear up the copper foil and add it to the copper melter. The electrolyte and air have a certain oxidizing property after mixing, which can dissolve the copper foil into the electrolyte to achieve the effect of replenishing copper ions. At the same time, when the electrolyte is pumped from the low-level tank to the high-level tank through the circulation pump, the heater can use steam to exchange heat with the electrolyte, thereby achieving the effect of heating the electrolyte; Step 4: Cleaning the electrolytic cell: After the electrolysis is completed, stop supplying direct current to the electrolytic cell, then peel off the deposited pure copper from the cathode plate, and then take out the electrolyte and anode mud in the electrolytic cell for treatment; Step 5: Treatment of impurities and filtrate: The mixed liquid of electrolyte and anode mud is separated by filter pressing, and the filtrate enters the clarification tank, and then is treated by filter pressing again, and then filled into the low-level tank for repeated use; Step 6. Recovery of waste electrolyte: After the electrolysis is completed, the waste electrolyte in the low-level tank is decoppered, and the decoppered solution is passed into a nickel sulfate solution for reaction, followed by freezing and crystallization. After filtration, it is separated into crude nickel sulfate and black acid, and the black acid can be reused in the electrolysis process.
2. The process for electrolysis of ultra-high impurity copper as claimed in claim 1, Features: The weight of the anode plate in step 1 is 210 kg, the spacing between the same poles is 95 mm, the size of the starting pole piece is 0.74*1 m, wherein the number of cathodes in each electrolytic cell is 45, the number of anodes is 46, and the cathodes and anodes are placed at the two ends of the electrolytic cell respectively.
3. The process for electrolysis of ultra-high impurity copper as claimed in claim 1, Features: The direct current introduced in the step 2 is 7000A. Under the action of direct current, the copper ions in the electrolyte move toward the cathode under the action of the electric field. At the cathode, the copper ions obtain electrons and are reduced to pure copper and deposited on the cathode plate. The copper on the anode loses electrons and becomes copper ions and enters the electrolyte, and anode mud is generated in the electrolytic cell.
4. The process for electrolysis of ultra-high impurity copper as claimed in claim 1, Features: The circulation speed of the electrolyte in step three is 35L / min, and the circulation speed of the electrolyte is related to the power of the circulation pump. The electrolyte composition is about 170g / L sulfuric acid, 40g / L copper, and 15g / L arsenic. The temperature of the electrolyte after being heated by the heater is 60-100°C. At the same time, during electrolysis, the workers tear the copper foil into pieces and add it to the copper melter. The electrolyte and air are mixed with a certain oxidizing property, and then the copper foil can be dissolved into the electrolyte, thereby achieving the effect of replenishing copper ions.
5. The process for electrolysis of ultra-high impurity copper as claimed in claim 1, Features: In the step 4, the cathode plate is taken out and rinsed, and then the pure copper deposited on the cathode plate is stripped off, and then the stripped pure copper is post-processed, and the post-processed copper is packaged for storage or sale, and then the solution in the electrolytic cell is collected.
6. The process for electrolysis of ultra-high impurity copper as claimed in claim 1, Features: The solution in the electrolytic cell collected in the step 4 is a mixed solution of anode mud and the electrolyte after the reaction. The mixed solution is passed into a filter press device for filter press treatment, so that the solution can be separated into filtrate and anode mud. The filtrate is then filter pressed again, and the filtrate after filter pressing is passed into a low-level tank for reuse.
7. The process for electrolysis of ultra-high impurity copper as claimed in claim 1, Features: The waste electrolyte in step six comes from the electrolyte in the low-level tank, wherein the waste electrolyte is the electrolyte after multiple uses. Workers draw electrolyte from the low-level tank every day for treatment as waste electrolyte, thereby extending the use time of the electrolyte. The waste electrolyte is evaporated by a copper sulfate plate vacuum evaporator, then crystallized by a copper sulfate water-cooled crystallization reactor, and then filtered by a copper sulfate vacuum belt filter, thereby precipitating copper sulfate, and then the solution is subjected to primary and secondary decoppering, thereby precipitating black copper mud, thereby obtaining a secondary decoppering solution.
8. The process for electrolysis of ultra-high impurity copper as claimed in claim 7, Features: The secondary decopperizing solution in step six is introduced into a nickel sulfate solution for freeze crystallization, and then filtered to obtain a crude nickel sulfate product and black acid. The crude nickel sulfate product can be packaged and sold after subsequent treatment, and the black acid can be reused in the electrolysis process.
Citation Information
Cited By
Electrolyte for copper refining and electrolytic refining method for high-gold-silver complex copper anode plate
CN119615288A
Electrolyte for copper refining and electrolytic refining method of high-gold-silver complex copper anode plate