High-strength integrally-formed anti-fingerprint plate and preparation method thereof

By using anti-fingerprint polymer film and modified resin layer on the decorative panel, combined with the hot pressing process, the fingerprint problem caused by uneven surfaces of the steel template is solved, and a high-strength integrated anti-fingerprint board is realized, which improves the board's Wet resistance and bonding strength.

CN118952782AInactive Publication Date: 2024-11-15GUANGDONG G&P NEW COMPOSITE MATERIAL CO LTD

Patent Information

Application Number
CN202411014714.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The steel formwork surface of existing decorative panels is difficult to achieve microscopic flatness, resulting in easy residual fingerprints, affecting the touch and appearance of high-end decorative panels.

Method used

Anti-fingerprint polymer film and modified resin layer are used to form anti-fingerprint sheets by pressing by a hot press, and fluorine-containing plating layer of PET film and modified phenolic resin are used to improve surface smoothness and bonding strength.

Benefits of technology

It effectively prevents fingerprints from being generated during touch, improves the moisture, heat resistance and service life of the board, and enhances bonding strength and toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118952782A_ABST
    Figure CN118952782A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength integrally-formed anti-fingerprint plate and a preparation method thereof, and relates to the technical field of building materials. The preparation method of the anti-fingerprint plate comprises the following steps: sequentially arranging an anti-fingerprint polymeric membrane, a steel plate, a base plate, a base plate and an anti-fingerprint polymeric membrane, and performing compression molding through a hot press to obtain the anti-fingerprint plate, the base plate comprises kraft paper subjected to resin dipping treatment and colored paper layers which are arranged on the two sides of the kraft paper and subjected to resin dipping treatment; the steel plate is arranged on the side face of the base plate, so that the strength of the plate is effectively improved, and the anti-fingerprint polymeric membrane is arranged on the surface of the plate, so that fingerprints or stains are effectively prevented from being left after people touch the plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a high-strength integrally formed anti-fingerprint plate and a preparation method thereof. Background Art

[0002] Existing decorative panels are generally made of surface materials and substrates. Steel templates are composited on the surface of the substrate and surface treated to form a variety of patterns and textures to meet the diverse needs of customers. Decorative panels with steel template veneer have excellent decorative, waterproof and moisture-proof, wear-resistant and crack-resistant, heat-insulating and flame-retardant properties, and are widely used in high-end decorative materials for building decoration, furniture decoration and vehicle decoration.

[0003] In the prior art, it is difficult to achieve a microscopically flat surface for steel templates due to material reasons. Although the development of grinding and electroplating technology in recent years has achieved a super-sub skin-feel surface treatment, it is still difficult to avoid fingerprints or stains left after people touch the board due to the microscopic bumps, which greatly affects the touch and appearance of high-end decorative panels. Secondly, the base material of the decorative panel is made of plywood or kraft paper as the base material and impregnated film paper as the finishing material through hot pressing or cold pressing. Impregnated film paper is an impregnated paper with a certain resin content and volatile content obtained by impregnating resin on decorative base paper and drying and curing it to a certain degree. It can be pressed on the surface of the base material through a hot pressing process. The impregnated film paper is set as an intermediate layer between the kraft paper and the metal veneer material. The adhesive resin of the impregnated film paper needs to have not only bonding strength to the paper material, but also bonding strength to the metal veneer, and it also needs certain moisture resistance and temperature resistance. Summary of the invention

[0004] The purpose of the present invention is to provide a high-strength one-piece anti-fingerprint plate and a preparation method thereof, to solve the following technical problems:

[0005] The existing steel decorative panel surface has the problem of easy residual fingerprints.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a high-strength integrally formed anti-fingerprint plate comprises the following steps: arranging an anti-fingerprint polymer film, a steel plate, a base plate, a base plate, and an anti-fingerprint polymer film in sequence, and pressing and molding them by a hot press to obtain an anti-fingerprint plate;

[0008] The anti-fingerprint polymer film is a PET sheet decorative film, which is a composite film with a PET film as a substrate and a fluorine-containing coating coated on the surface. The fluorine-containing coating has a pure water contact angle of 115-120°, a hexadecane contact angle of 70-75°, a dynamic friction coefficient of less than 0.04, and a hardness of 8H-9H.

[0009] The base board includes a kraft paper layer and color paper layers arranged on both sides of the kraft paper layer;

[0010] The kraft paper layer is obtained by overlapping and hot-pressing three or more layers of pretreated kraft paper; the pretreated kraft paper is obtained by impregnating kraft paper in amino phenolic resin;

[0011] The color paper layer is obtained by dipping the color paper in melamine formaldehyde resin;

[0012] The preparation method of the melamine formaldehyde resin comprises the following steps:

[0013] Add 37% formaldehyde solution to a reaction bottle, add 30-40% sodium hydroxide solution under stirring to adjust the pH to 9-9.5, add 3-glycidyloxypropyltrimethoxysilane, control the temperature at 35-45°C, add melamine and urea, control the temperature at 90-95°C, keep warm for 20-30 minutes, control the temperature at 80-85°C, add 30-40% sodium hydroxide solution to adjust the pH to 8-8.5, keep warm for 1-1.5 hours, add 30-40% sodium hydroxide solution to adjust the pH to 8.5-9, and obtain melamine formaldehyde resin.

[0014] Preferably, the specific steps of hot press molding are: pressing temperature 150-170°C, pressure 5-15MPa, and heat preservation 10-60min.

[0015] Preferably, the specific steps of hot pressing and laminating are: first, hot pressing and curing the overlapped pre-treated kraft paper at a pressure of 1-2 MPa and a temperature of 110-130° C. for 15-25 minutes; and then hot pressing and curing at a pressure of 1-2 MPa and a temperature of 155-165° C. for 10-20 minutes.

[0016] Preferably, the preparation method of the amino phenolic resin comprises the following steps: adding phenol and sodium hydroxide solution into a reaction kettle and dispersing them evenly, adding the first batch of formaldehyde and γ-aminopropyltriethoxysilane, controlling the temperature at 80-85°C, and keeping the temperature for reaction for 30-60 minutes, controlling the temperature at 60-70°C, adding the second batch of formaldehyde, controlling the temperature at 90-95°C, and keeping the temperature for reaction for 3-5 hours to obtain a modified phenolic resin.

[0017] Preferably, the sodium hydroxide solution is a 30-40wt% sodium hydroxide aqueous solution, in which the sodium hydroxide accounts for 10-15% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1-1.1; the γ-aminopropyltriethoxysilane accounts for 4-6% of the total mass of phenol; and the molar ratio of formaldehyde: phenol is 1.2-1.5:1.

[0018] Preferably, the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.5-1.7:1.

[0019] Preferably, the melamine accounts for 5-7% of the total mass of the melamine formaldehyde resin.

[0020] Preferably, 3-glycidyloxypropyltrimethoxysilane accounts for 10-12% of the total mass of the melamine formaldehyde resin.

[0021] Preferably, the specific steps for preparing the base board are: color paper layers are arranged on both sides of the kraft paper layer, the temperature is controlled at 120-130° C., the pressure is 1-2 MPa, and the pressure is maintained for 1-2 minutes.

[0022] A high-strength one-piece anti-fingerprint plate is made by any one of the above preparation methods.

[0023] Beneficial effects of the present invention:

[0024] (1) This application uses a nano-polymer film with anti-fingerprint properties to be placed on the surface of the plate for pressing, which solves the problem of residual fingerprints caused by microscopic unevenness caused by traditional steel template pressing. After the polymer film is pressed on the surface of the plate, the unevenness of the plate surface is nanometer-level, which effectively prevents fingerprints from being generated by touch.

[0025] (2) The present application uses the residual polar phenolic hydroxyl groups in the curing reaction process of the prepared phenolic resin to undergo a polymerization reaction with the silanol of γ-aminopropyltriethoxysilane, thereby reducing the number of phenolic hydroxyl groups, reducing the water absorption of the phenolic resin in a high temperature and humid environment, improving the thermal properties and moisture resistance of the resin, solving the problem of poor durability of conventional phenolic resins, and increasing the service life of kraft paper.

[0026] (3) The present application utilizes melamine and formaldehyde to form a colorless aqueous solution of a resol resin by polycondensation under the action of a catalyst, and adds 3-glycidyloxypropyltrimethoxysilane for modification to form a resin protective film that is heat-resistant, wear-resistant, resistant to pollution and corrosion, and has a gloss. The present application uses the amino groups of the amino-phenolic resin on the surface of the kraft paper layer to react with the epoxy groups of the melamine formaldehyde resin on the surface to further improve the bonding strength and toughness of the board. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention will be further described below in conjunction with the accompanying drawings.

[0028] Figure 1 It is a schematic diagram of the structure of the anti-fingerprint plate prepared in this application;

[0029] In the figure: 1. base board; 101. kraft paper layer; 102. color paper layer; 2. steel plate; 3. anti-fingerprint polymer film. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1 Please refer to Figure 1 A method for preparing a high-strength one-piece anti-fingerprint plate comprises the following steps:

[0032] S1: The preparation method of melamine formaldehyde resin comprises the following steps: adding 37% formaldehyde solution into a reaction bottle, adding 40% sodium hydroxide solution under stirring to adjust the pH to 9, adding 3-glycidyloxypropyltrimethoxysilane, controlling the temperature at 35°C, adding melamine and urea, controlling the temperature at 90°C, keeping the temperature for 20 minutes, controlling the temperature at 80°C, adding 40% sodium hydroxide solution to adjust the pH to 8, keeping the temperature for 1 hour, adding 30% sodium hydroxide solution to adjust the pH to 8.5, and obtaining melamine formaldehyde resin; immersing color paper in melamine formaldehyde resin to obtain a color paper layer; the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.5:1; melamine accounts for 5% of the total mass of melamine formaldehyde resin; 3-glycidyloxypropyltrimethoxysilane accounts for 10% of the total mass of melamine formaldehyde resin;

[0033] S2: The preparation method of amino phenolic resin comprises the following steps: adding phenol and 40wt% sodium hydroxide aqueous solution into a reactor and dispersing them evenly, adding the first batch of formaldehyde and γ-aminopropyltriethoxysilane, controlling the temperature at 80°C, keeping the temperature for reaction for 30min, controlling the temperature at 60°C, adding the second batch of formaldehyde, controlling the temperature at 90°C, keeping the temperature for reaction for 3h, and obtaining modified phenolic resin; the sodium hydroxide in the sodium hydroxide solution accounts for 10% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1; γ-aminopropyltriethoxysilane accounts for 4% of the total mass of phenol; the molar ratio of formaldehyde: phenol is 1.2:1; kraft paper is impregnated in the amino phenolic resin to obtain pretreated kraft paper; three layers of pretreated kraft paper are heat-pressed and cured at a pressure of 1MPa and a temperature of 110°C for 15min on the overlapping pretreated kraft paper; and then heat-pressed and cured at a pressure of 1MPa and a temperature of 155°C for 10min to obtain a kraft paper layer;

[0034] S3: color paper layers are arranged on both sides of the kraft paper layer, the temperature is controlled at 120°C, the pressure is 1MPa, and the pressure is maintained for 1min to obtain a base board;

[0035] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 150°C, a pressure of 5MPa, and insulation for 10min to obtain an anti-fingerprint sheet.

[0036] Example 2 Please refer to Figure 1 A method for preparing a high-strength one-piece anti-fingerprint plate comprises the following steps:

[0037] S1: The preparation method of melamine formaldehyde resin comprises the following steps: adding 37% formaldehyde solution into a reaction bottle, adding 40% sodium hydroxide solution under stirring to adjust the pH to 9, adding 3-glycidyloxypropyltrimethoxysilane, controlling the temperature to 40°C, adding melamine and urea, controlling the temperature to 90°C, keeping the temperature for 30 minutes, controlling the temperature to 80°C, adding 40% sodium hydroxide solution to adjust the pH to 8.5, keeping the temperature for 1.5 hours, adding 40% sodium hydroxide solution to adjust the pH to 8.5, and obtaining melamine formaldehyde resin; immersing color paper in melamine formaldehyde resin to obtain a color paper layer; the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.6:1; melamine accounts for 6% of the total mass of melamine formaldehyde resin; 3-glycidyloxypropyltrimethoxysilane accounts for 11% of the total mass of melamine formaldehyde resin;

[0038] S2: The preparation method of amino phenolic resin comprises the following steps: adding phenol and 40wt% sodium hydroxide aqueous solution into a reaction kettle and dispersing them evenly, adding the first batch of formaldehyde and γ-aminopropyltriethoxysilane, controlling the temperature at 80°C, keeping the temperature for reaction for 60min, controlling the temperature at 60°C, adding the second batch of formaldehyde, controlling the temperature at 95°C, keeping the temperature for reaction for 3h, and obtaining a modified phenolic resin; the sodium hydroxide in the sodium hydroxide solution accounts for 12% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1; γ-aminopropyltriethoxysilane accounts for 5% of the total mass of phenol; the molar ratio of formaldehyde: phenol is 1.3:1; immersing kraft paper in the amino phenolic resin to obtain pretreated kraft paper; hot-pressing and curing the three layers of pretreated kraft paper at a pressure of 1.5MPa and a temperature of 120°C for 20min; hot-pressing and curing at a pressure of 1.5MPa and a temperature of 160°C for 15min to obtain a kraft paper layer;

[0039] S3: color paper layers are placed on both sides of the kraft paper layer, the temperature is controlled at 125°C, the pressure is 1.5 MPa, and the pressure is maintained for 1 minute to obtain a base board;

[0040] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 160°C, a pressure of 10MPa, and heat preservation for 30min to obtain an anti-fingerprint sheet.

[0041] Example 3, please refer to Figure 1 A method for preparing a high-strength one-piece anti-fingerprint plate comprises the following steps:

[0042] S1: The preparation method of melamine formaldehyde resin comprises the following steps: adding 37% formaldehyde solution to a reaction bottle, adding 40% sodium hydroxide solution under stirring to adjust the pH to 9.5, adding 3-glycidyloxypropyltrimethoxysilane, controlling the temperature to 45°C, adding melamine and urea, controlling the temperature to 95°C, keeping the temperature for 30 minutes, controlling the temperature to 85°C, adding 40% sodium hydroxide solution to adjust the pH to 8.5, keeping the temperature for 1.5 hours, adding 40% sodium hydroxide solution to adjust the pH to 9, and obtaining melamine formaldehyde resin; immersing color paper in melamine formaldehyde resin to obtain a color paper layer; the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.7:1; melamine accounts for 7% of the total mass of melamine formaldehyde resin; 3-glycidyloxypropyltrimethoxysilane accounts for 12% of the total mass of melamine formaldehyde resin;

[0043] S2: The preparation method of amino phenolic resin comprises the following steps: adding phenol and 40wt% sodium hydroxide aqueous solution into a reaction kettle and dispersing them evenly, adding the first batch of formaldehyde and γ-aminopropyltriethoxysilane, controlling the temperature at 85°C, keeping the temperature for reaction for 60min, controlling the temperature at 70°C, adding the second batch of formaldehyde, controlling the temperature at 95°C, keeping the temperature for reaction for 5h, and obtaining modified phenolic resin; sodium hydroxide in the sodium hydroxide solution accounts for 15% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1.1; γ-aminopropyltriethoxysilane accounts for 6% of the total mass of phenol; the molar ratio of formaldehyde: phenol is 1.5:1; kraft paper is impregnated in amino phenolic resin to obtain pretreated kraft paper; three layers of pretreated kraft paper are heat-pressed and cured at a pressure of 2MPa and a temperature of 130°C for 25min for overlapping pretreated kraft paper; and then heat-pressed and cured at a pressure of 2MPa and a temperature of 165°C for 20min to obtain a kraft paper layer;

[0044] S3: color paper layers are arranged on both sides of the kraft paper layer, the temperature is controlled at 130°C, the pressure is 2MPa, and the pressure is maintained for 2 minutes to obtain a base board;

[0045] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 170°C, a pressure of 15MPa, and heat preservation for 60min to obtain an anti-fingerprint sheet.

[0046] Comparative Example 1 A method for preparing a high-strength integrally formed anti-fingerprint plate comprises the following steps:

[0047] S1: The preparation method of melamine formaldehyde resin comprises the following steps: adding 37% formaldehyde solution to a reaction bottle, adding 40% sodium hydroxide solution under stirring to adjust the pH to 9, controlling the temperature to 40°C, adding melamine and urea, controlling the temperature to 90°C, keeping the temperature for 30 minutes, controlling the temperature to 80°C, adding 40% sodium hydroxide solution to adjust the pH to 8.5, keeping the temperature for 1.5 hours, adding 40% sodium hydroxide solution to adjust the pH to 8.5, and obtaining melamine formaldehyde resin; immersing color paper in melamine formaldehyde resin to obtain a color paper layer; the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.6:1; melamine accounts for 6% of the total mass of the melamine formaldehyde resin;

[0048] S2: The preparation method of amino phenolic resin comprises the following steps: adding phenol and 40wt% sodium hydroxide aqueous solution into a reaction kettle and dispersing them evenly, adding the first batch of formaldehyde and γ-aminopropyltriethoxysilane, controlling the temperature at 80°C, keeping the temperature for reaction for 60min, controlling the temperature at 60°C, adding the second batch of formaldehyde, controlling the temperature at 95°C, keeping the temperature for reaction for 3h, and obtaining a modified phenolic resin; the sodium hydroxide in the sodium hydroxide solution accounts for 12% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1; γ-aminopropyltriethoxysilane accounts for 5% of the total mass of phenol; the molar ratio of formaldehyde: phenol is 1.3:1; immersing kraft paper in the amino phenolic resin to obtain pretreated kraft paper; hot-pressing and curing the three layers of pretreated kraft paper at a pressure of 1.5MPa and a temperature of 120°C for 20min; hot-pressing and curing at a pressure of 1.5MPa and a temperature of 160°C for 15min to obtain a kraft paper layer;

[0049] S3: color paper layers are placed on both sides of the kraft paper layer, the temperature is controlled at 125°C, the pressure is 1.5 MPa, and the pressure is maintained for 1 minute to obtain a base board;

[0050] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 160°C, a pressure of 10MPa, and heat preservation for 30min to obtain an anti-fingerprint sheet.

[0051] Comparative Example 2 A method for preparing a high-strength integrally formed anti-fingerprint plate comprises the following steps:

[0052] S1: The preparation method of melamine formaldehyde resin comprises the following steps: adding 37% formaldehyde solution into a reaction bottle, adding 40% sodium hydroxide solution under stirring to adjust the pH to 9, adding 3-glycidyloxypropyltrimethoxysilane, controlling the temperature to 40°C, adding melamine and urea, controlling the temperature to 90°C, keeping the temperature for 30 minutes, controlling the temperature to 80°C, adding 40% sodium hydroxide solution to adjust the pH to 8.5, keeping the temperature for 1.5 hours, adding 40% sodium hydroxide solution to adjust the pH to 8.5, and obtaining melamine formaldehyde resin; immersing color paper in melamine formaldehyde resin to obtain a color paper layer; the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.6:1; melamine accounts for 6% of the total mass of melamine formaldehyde resin; 3-glycidyloxypropyltrimethoxysilane accounts for 11% of the total mass of melamine formaldehyde resin;

[0053] S2: The preparation method of amino phenolic resin comprises the following steps: adding phenol and 40wt% sodium hydroxide aqueous solution into a reaction kettle and dispersing them evenly, adding the first batch of formaldehyde, controlling the temperature at 80°C, keeping the temperature for reaction for 60min, controlling the temperature at 60°C, adding the second batch of formaldehyde, controlling the temperature at 95°C, keeping the temperature for reaction for 3h, and obtaining a modified phenolic resin; the sodium hydroxide in the sodium hydroxide solution accounts for 12% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1; the molar ratio of formaldehyde: phenol is 1.3:1; kraft paper is impregnated in the amino phenolic resin to obtain pretreated kraft paper; three layers of pretreated kraft paper are heat-pressed and cured at a pressure of 1.5MPa and a temperature of 120°C for 20min on the overlapping pretreated kraft paper; and then heat-pressed and cured at a pressure of 1.5MPa and a temperature of 160°C for 15min to obtain a kraft paper layer;

[0054] S3: color paper layers are placed on both sides of the kraft paper layer, the temperature is controlled at 125°C, the pressure is 1.5 MPa, and the pressure is maintained for 1 minute to obtain a base board;

[0055] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 160°C, a pressure of 10MPa, and heat preservation for 30min to obtain an anti-fingerprint sheet.

[0056] Comparative Example 3 A method for preparing a high-strength integrally formed anti-fingerprint plate comprises the following steps:

[0057] S1: The preparation method of melamine formaldehyde resin comprises the following steps: adding 37% formaldehyde solution to a reaction bottle, adding 40% sodium hydroxide solution under stirring to adjust the pH to 9, controlling the temperature to 40°C, adding melamine and urea, controlling the temperature to 90°C, keeping the temperature for 30 minutes, controlling the temperature to 80°C, adding 40% sodium hydroxide solution to adjust the pH to 8.5, keeping the temperature for 1.5 hours, adding 40% sodium hydroxide solution to adjust the pH to 8.5, and obtaining melamine formaldehyde resin; immersing color paper in melamine formaldehyde resin to obtain a color paper layer; the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.6:1; melamine accounts for 6% of the total mass of the melamine formaldehyde resin;

[0058] S2: The preparation method of amino phenolic resin comprises the following steps: adding phenol and 40wt% sodium hydroxide aqueous solution into a reaction kettle and dispersing them evenly, adding the first batch of formaldehyde, controlling the temperature at 80°C, keeping the temperature for reaction for 60min, controlling the temperature at 60°C, adding the second batch of formaldehyde, controlling the temperature at 95°C, keeping the temperature for reaction for 3h, and obtaining a modified phenolic resin; the sodium hydroxide in the sodium hydroxide solution accounts for 12% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1; the molar ratio of formaldehyde: phenol is 1.3:1; kraft paper is impregnated in the amino phenolic resin to obtain pretreated kraft paper; three layers of pretreated kraft paper are heat-pressed and cured at a pressure of 1.5MPa and a temperature of 120°C for 20min on the overlapping pretreated kraft paper; and then heat-pressed and cured at a pressure of 1.5MPa and a temperature of 160°C for 15min to obtain a kraft paper layer;

[0059] S3: color paper layers are placed on both sides of the kraft paper layer, the temperature is controlled at 125°C, the pressure is 1.5 MPa, and the pressure is maintained for 1 minute to obtain a base board;

[0060] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 160°C, a pressure of 10MPa, and heat preservation for 30min to obtain an anti-fingerprint sheet.

[0061] Comparative Example 4 A method for preparing a high-strength integrally formed anti-fingerprint plate comprises the following steps:

[0062] S1: The preparation method of melamine formaldehyde resin comprises the following steps: adding 37% formaldehyde solution into a reaction bottle, adding 40% sodium hydroxide solution under stirring to adjust the pH to 9, adding 3-glycidyloxypropyltrimethoxysilane, controlling the temperature to 40°C, adding melamine and urea, controlling the temperature to 90°C, keeping the temperature for 30 minutes, controlling the temperature to 80°C, adding 40% sodium hydroxide solution to adjust the pH to 8.5, keeping the temperature for 1.5 hours, adding 40% sodium hydroxide solution to adjust the pH to 8.5, and obtaining melamine formaldehyde resin; immersing color paper in melamine formaldehyde resin to obtain a color paper layer; the molar ratio of formaldehyde to urea in the 37% formaldehyde solution is 1.6:1; melamine accounts for 6% of the total mass of melamine formaldehyde resin; 3-glycidyloxypropyltrimethoxysilane accounts for 11% of the total mass of melamine formaldehyde resin;

[0063] S2: impregnating kraft paper in melamine formaldehyde resin to obtain pretreated kraft paper; hot pressing and curing the three layers of pretreated kraft paper at a pressure of 1.5 MPa and a temperature of 120° C. for 20 minutes; and hot pressing and curing at a pressure of 1.5 MPa and a temperature of 160° C. for 15 minutes to obtain a kraft paper layer;

[0064] S3: color paper layers are placed on both sides of the kraft paper layer, the temperature is controlled at 125°C, the pressure is 1.5 MPa, and the pressure is maintained for 1 minute to obtain a base board;

[0065] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 160°C, a pressure of 10MPa, and heat preservation for 30min to obtain an anti-fingerprint sheet.

[0066] Comparative Example 5 A method for preparing a high-strength integrally formed anti-fingerprint plate comprises the following steps:

[0067] S1: The preparation method of amino phenolic resin comprises the following steps: adding phenol and 40wt% sodium hydroxide aqueous solution into a reaction kettle and dispersing them evenly, adding the first batch of formaldehyde and γ-aminopropyltriethoxysilane, controlling the temperature to 80°C, keeping the temperature for reaction for 60min, controlling the temperature to 60°C, adding the second batch of formaldehyde, controlling the temperature to 95°C, keeping the temperature for reaction for 3h, and obtaining modified phenolic resin; the sodium hydroxide in the sodium hydroxide solution accounts for 12% of the total mass of phenol; the mass ratio of the first batch of formaldehyde: the second batch of formaldehyde is 1:1; γ-aminopropyltriethoxysilane accounts for 5% of the total mass of phenol; the molar ratio of formaldehyde: phenol is 1.3:1; immersing kraft paper in the amino phenolic resin to obtain pretreated kraft paper; hot-pressing and curing the overlapping pretreated kraft paper at a pressure of 1.5MPa and a temperature of 120°C for 20min; and hot-pressing and curing at a pressure of 1.5MPa and a temperature of 160°C for 15min to obtain a kraft paper layer;

[0068] S2: impregnating the color paper in an amino phenolic resin to obtain a color paper layer;

[0069] S3: color paper layers are placed on both sides of the kraft paper layer, the temperature is controlled at 125°C, the pressure is 1.5 MPa, and the pressure is maintained for 1 minute to obtain a base board;

[0070] S4: The anti-fingerprint polymer film (PET film with a fluorine-containing coating on the surface, pure water contact angle of 120°, hexadecane contact angle of 72°, dynamic friction coefficient of 0.03, hardness of 9H), steel plate, base plate, base plate, and anti-fingerprint polymer film are arranged in sequence, and pressed by a hot press at a temperature of 160°C, a pressure of 10MPa, and heat preservation for 30min to obtain an anti-fingerprint sheet.

[0071] Performance Testing

[0072] (1) Gluing strength: The test was conducted according to 4.1 Surface bonding strength determination method 1 in GB / T 17657-2013 “Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels”. The test results are shown in Table 1.

[0073] (2) Static bending strength: tested according to the three-point bending method in GB / T 17657-2013 “Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels”. The test results are shown in Table 1.

[0074] (3) Elastic modulus: tested according to the three-point bending method in GB / T 17657-2013 “Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels”. The test results are shown in Table 1.

[0075] (4) Water absorption thickness expansion rate: The test was conducted according to 4.4 Water absorption thickness expansion rate determination method 1 in GB / T 17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels". The test results are shown in Table 1.

[0076] Table 1: Statistical table of performance test data of Examples 1-3 and Comparative Examples 1-5

[0077]

[0078]

[0079] As can be seen from Table 1, the phenolic resin prepared in the present application is used in combination with the melamine formaldehyde resin to prepare a board having the advantages of high bonding strength and good waterproof performance.

[0080] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a high-strength integrally formed anti-fingerprint plate, characterized in that: The method comprises the following steps: arranging an anti-fingerprint polymer film (3), a steel plate (2), a base plate (1), a base plate (1), and an anti-fingerprint polymer film (3) in sequence, and pressing and molding them by a hot press to obtain an anti-fingerprint plate; The base board (1) comprises a kraft paper layer (101) and color paper layers (102) arranged on both sides of the kraft paper layer (101); The kraft paper layer (101) is obtained by overlapping and hot-pressing three or more layers of pretreated kraft paper; the pretreated kraft paper is obtained by impregnating kraft paper in an amino phenolic resin; The color paper layer (102) is obtained by impregnating color paper in melamine formaldehyde resin; The preparation method of the melamine formaldehyde resin comprises the following steps: Add 37% formaldehyde solution to a reaction bottle, add 30-40% sodium hydroxide solution under stirring to adjust the pH to 9-9.5, add 3-glycidyloxypropyltrimethoxysilane, control the temperature at 35-45°C, add melamine and urea, control the temperature at 90-95°C, keep warm for 20-30 minutes, control the temperature at 80-85°C, add 30-40% sodium hydroxide solution to adjust the pH to 8-8.5, keep warm for 1-1.5 hours, add 30-40% sodium hydroxide solution to adjust the pH to 8.5-9, and obtain melamine formaldehyde resin.

2. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 1, characterized in that: The specific steps of hot press molding are: pressing temperature 150-170°C, pressure 5-15MPa, and heat preservation 10-60min.

3. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 1, characterized in that: The specific steps of hot pressing and laminating are: first, hot pressing and curing the overlapped pre-treated kraft paper for 15-25 minutes at a pressure of 1-2 MPa and a temperature of 110-130° C.; and then hot pressing and curing for 10-20 minutes at a pressure of 1-2 MPa and a temperature of 155-165° C.

4. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 1, characterized in that: The preparation method of the amino phenolic resin comprises the following steps: adding phenol and sodium hydroxide solution into a reaction kettle and dispersing them uniformly, adding the first batch of formaldehyde and γ-aminopropyltriethoxysilane, controlling the temperature at 80-85°C, and keeping the temperature for reaction for 30-60 minutes, controlling the temperature at 60-70°C, adding the second batch of formaldehyde, controlling the temperature at 90-95°C, and keeping the temperature for reaction for 3-5 hours to obtain the modified phenolic resin.

5. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 4, characterized in that: The sodium hydroxide solution is a 30-40wt% sodium hydroxide aqueous solution, in which the sodium hydroxide accounts for 10-15% of the total mass of phenol; the mass ratio of the first batch of formaldehyde to the second batch of formaldehyde is 1:1-1.1; the gamma-aminopropyltriethoxysilane accounts for 4-6% of the total mass of phenol; and the molar ratio of formaldehyde to phenol is 1.2-1.5:

1.

6. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 1, characterized in that: The molar ratio of formaldehyde to urea in 37% formaldehyde solution is 1.5-1.7:

1.

7. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 1, characterized in that: The melamine accounts for 5-7% of the total mass of the melamine formaldehyde resin.

8. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 1, characterized in that: 3-Glycidyloxypropyltrimethoxysilane accounts for 10-12% of the total mass of the melamine formaldehyde resin.

9. The method for preparing a high-strength integrally formed anti-fingerprint plate according to claim 1, characterized in that: The specific steps of preparing the base board (1) are as follows: color paper layers (102) are arranged on both sides of the kraft paper layer (101), the temperature is controlled at 120-130°C, the pressure is 1-2MPa, and the pressure is maintained for 1-2min.

10. A high-strength one-piece anti-fingerprint plate, characterized in that: Prepared by the preparation method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Low-hydroscopicity phenolic resin insulating gel and preparation method thereof

    CN105754062A

  • Scratch-resistant fingerprint-resistant touch feel decorative film and preparation process thereof

    CN111777936A

  • Melamine decorative sheet and method for manufacturing melamine decorative sheet

    CN114945466A

  • Thermosetting resin decorative material having metal gloss

    JP2002067219A

  • Decorative laminated sheet

    JP2002192657A

Cited By

  • High-strength waterproof board and preparation method thereof

    CN120396494A

  • High-strength waterproof sheet and preparation method thereof

    CN120396494B