Hydrophobic and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining and preparation method of hydrophobic and maintenance-free cement-based wear-resistant material
By using water-repellent, curing-free cement-based wear-resistant materials in the lining of reinforced concrete silos, combined with components such as silicate cement, sulfoaluminate cement and gypsum, fiber cellulose and water-absorbing resin, wear resistance is solved The problems of cracking, high water absorption and poor crack resistance after material construction have been achieved, which have achieved high early strength, no shrinkage in the later stage and strong water repellency, extending the service life and reducing safety hazards.
Patent Information
- Application Number
- CN202411011646.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The wear-resistant materials of existing reinforced concrete silo linings are prone to cracking, falling off, high water absorption and poor crack resistance after construction, resulting in a shortened service life and safety hazards, and require maintenance, which limits its application scope.
Use water-repellent and curing-free cement-based wear-resistant materials, and use modified components such as silicate cement, sulfur aluminate cement, gypsum, etc. to form early-stage high-strength and wear-resistant Materials with strong properties and good crack resistance avoid cracking problems after moisture adsorption and coagulation hardening.
The reinforced concrete silo lining has high early strength and no shrinkage in the later stage. The construction surface layer is free of maintenance, strong water repellency and good crack resistance. It extends the service life and reduces the risk of blockage of coal outlets. , improves the safety and reliability of the structure.
Smart Images

Figure CN118955073A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and relates to wear-resistant materials for reinforced concrete silo structures, in particular to a water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo linings and a preparation method thereof. Background Art
[0002] Reinforced concrete coal silos play an important role in coal storage, transportation and environmental protection, especially as the country's environmental protection requirements are increasingly strengthened. Compared with open-air storage, the advantages of silo structures in dust suppression and environmental protection are becoming more obvious. At present, the lining structures of coal silos that have been built are mostly in the form of microcrystalline cement adhered to the rolled microcrystalline plate. Affected by the frequent impact loads and friction of loading and unloading coal, and the failure of microcrystalline cement to reduce the bonding force, the rolled microcrystalline plate in the lining structure has fallen off to varying degrees. The falling off of the rolled microcrystalline plate accelerates the wear of the coal silo lining concrete, further causing local damage to the coal silo structure, and then reducing the overall safety of the coal silo structure, seriously reducing the service life of the silo structure. Strengthening the maintenance of the in-service coal silo structure and ensuring the reliability of the structure are of great significance to the efficiency of the port.
[0003] For the silo lining rolled microcrystalline plate shedding disease, the more effective repair solution is to coat the area where the rolled microcrystalline plate has fallen off with high-strength wear-resistant material, reduce the wear of the silo lining structure caused by loading and unloading coal during service, and thus ensure the overall stability of the silo structure. With the in-depth application of high-strength wear-resistant materials in engineering and material research, the following problems have emerged during the construction of high-strength wear-resistant materials: (1) The surface layer of the coated high-strength wear-resistant material cracks. When the temperature and humidity change greatly during the construction process, the surface layer is prone to small cracks. As the frequency of loading and unloading coal in the silo increases, the diffusion of small cracks further deepens, causing the repaired wear-resistant surface layer to cause regional shedding, exposed tendons and other deterioration phenomena, seriously affecting the service life of the repaired wear-resistant surface layer; (2) The feed port of the coal silo structure is blocked. Factors such as temperature, moisture, mineral composition and additives make the coal more viscous during storage, causing the feed port to be blocked. The moisture content in coal is the key to the change in viscosity. High-strength wear-resistant materials belong to the water-soluble minerals. The rough interface of the mud-based material after repair is prone to the accumulation of fly ash with a high moisture content. As the amount of fly ash accumulated increases, the feed port is blocked, which affects normal operation and easily causes a series of safety problems; (3) "White spots" appear on the surface of the wear-resistant layer after repair. The main reason is the precipitation of Ca(OH)2 during the coagulation and hardening of cement-based materials. In order to improve construction efficiency and ensure the hydration degree of cement-based materials during construction, the amount of water used in the mixing process of cement-based wear-resistant materials is increased. The Ca(OH)2 produced by the hydration of cement-based materials moves along the free water to the surface of the wear-resistant layer, showing the "white spots" phenomenon. Accompanied by the large amount of precipitation of the hydration product Ca(OH)2, the gelling property of the wear-resistant material is seriously reduced, resulting in a decrease in the service life of the wear-resistant layer.
[0004] The wear-resistant materials currently on the market all have the above problems, and the main reasons are as follows: (1) the wear-resistant layer is not properly maintained after construction; (2) the wear-resistant layer has a high water absorption rate after solidification; (3) the wear-resistant layer has poor crack resistance after hardening. Chinese patent CN101353243A discloses a cement-based wear-resistant material that can be used for the lining of industrial storage structures. It is compounded with cement, sand, water reducer, toughening agent, water retention agent, microcapsule quicklime and other components, and uses high-grade silicate cement or fast-hardening sulphoaluminate cement as a binder to bind aggregates with good wear resistance to form a wear-resistant layer; the microcapsule quicklime and toughening agent work synergistically to compensate for the chemical shrinkage and drying shrinkage of the cement-based material during the curing process, and prevent cracks, hollowing and peeling. However, the wear-resistant layer of the cement-based wear-resistant material needs to be maintained after construction, and the wear-resistant layer has a high water absorption rate after hardening. Chinese patent CN101921085A discloses a cement-based wear-resistant material prepared with steel slag, and its components are proportioned as follows by mass: 25-40 parts of cement, 10-35 parts of steel slag powder, 40-90 parts of steel slag particles, 0.5-10 parts of activator, 0.1-2.0 parts of water reducer, 0.15-1.5 parts of toughening agent, 0.3-3.0 parts of water retaining agent, and 0.5-6.0 parts of expansion agent. Although the cement-based wear-resistant material uses steel slag to replace sand, improves the wear resistance of the cement-based wear-resistant material and prolongs the service life of the material, the wear-resistant layer still needs to be maintained after construction, and the wear-resistant layer after hardening has poor crack resistance.
[0005] In order to overcome various problems in the construction process of high-strength wear-resistant materials, the concept of water-repellent and maintenance-free is introduced. Based on the special environment of silo loading and unloading coal, a water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining is developed, which has broad prospects. Summary of the invention
[0006] In view of the defects of existing wear-resistant materials such as inadequate maintenance of the wear-resistant layer after construction, strong water absorption, poor crack resistance and being limited by the construction environment below 5°C, the present invention provides a hydrophobic and maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos and a preparation method thereof, on the premise of meeting the requirements of high strength and wear resistance. The cement-based wear-resistant material has the characteristics of high early strength, strong wear resistance, maintenance-free construction surface layer, strong hydrophobicity of the layer after hardening, good crack resistance of the construction surface layer, and is not limited to low-temperature construction environment. The preparation process of the invention is simple, energy-saving and environmentally friendly.
[0007] The present invention is achieved through the following technical solutions:
[0008] On one hand, the present invention provides a water-repellent, maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos, which contains the following components and mass percentages:
[0009] Cement-based cementitious powder 43-53wt%,
[0010] Aggregate 45~55wt%
[0011] Modified component 0.3~0.6wt%,
[0012] Fiber component 0.3~0.8wt%,
[0013] Water reducing agent 0.2~0.9wt%,
[0014] The sum of the mass percentages of the above components is 100wt%;
[0015] The components and mass percentages of the cement-based cementitious powder are as follows:
[0016] Portland cement 70~85wt%,
[0017] Sulphoaluminate cement 10~25wt%
[0018] Gypsum 4~8wt%
[0019] The sum of the mass percentages of the above components is 100wt%;
[0020] The components and mass percentages of the aggregate are as follows:
[0021] Diamond 45~60wt%
[0022] Quartz sand 15~28wt%
[0023] White corundum 12~20wt%
[0024] Spinel 6~15wt%
[0025] The sum of the mass percentages of the above components is 100wt%;
[0026] The modified components and mass percentages are as follows:
[0027] Hydroxypropyl methylcellulose 22-35wt%,
[0028] Rigid rubber powder 15~28wt%
[0029] Silane-based powder 25-40wt%,
[0030] Water-absorbing resin 18~26wt%
[0031] The sum of the mass percentages of the above components is 100wt%;
[0032] The fiber components and mass percentages are as follows:
[0033] Polyvinyl alcohol fiber 22~35wt%,
[0034] Polypropylene fiber 32~45wt%,
[0035] Polyester fiber 30~40wt%,
[0036] The sum of the mass percentages of the above components is 100wt%;
[0037] The water reducing agent is a polycarboxylic acid high performance water reducing agent.
[0038] The hydrophobic, maintenance-free cement-based wear-resistant material is obtained by mixing cement-based cementitious powder, aggregate, modified component, fiber component and water reducer in proportion and then stirring them evenly. Its hydration mechanism is that the aggregate and fiber component are bonded by hydration of cement-based cementitious powder, while the modified component and water reducer assist the hydration process, and work together to form a material with high early strength and good wear resistance.
[0039] Cement-based cementitious powder includes silicate cement, sulphoaluminate cement and gypsum. The hydration of sulphoaluminate cement is the key to the high early strength of wear-resistant materials and the construction is not limited to low-temperature environments. The addition of gypsum mainly adjusts the hydration rate of sulphoaluminate cement, ensuring the development of early strength while controlling the occurrence of later strength shrinkage. The early hydration rate of silicate cement is lower than that of sulphoaluminate cement. As the hydration process of sulphoaluminate slows down, silicate cement begins to hydrate, and the generated hydrated crystalline phase fills the original hydration interface, effectively ensuring the later strength. The hydration process is not limited to low-temperature environments and has high early strength and no later strength shrinkage.
[0040] Aggregates include corundum, quartz sand, white corundum and spinel. Corundum is the key to ensure the strength development of wear-resistant materials. Quartz sand and white corundum are used in wear-resistant materials to increase the wear resistance and corrosion resistance of the back layer after repair. Spinel can reduce the problem of large friction of the repair surface layer.
[0041] The modified components include hydroxypropyl methylcellulose, rigid rubber powder, silane-based powder, and water-absorbent resin. The main functions of the modified components are to adjust the workability of the mortar during construction, the curing properties after construction, and the hydrophobicity of the layer after coagulation and hardening. Hydroxypropyl methylcellulose added to mortar can improve the dispersion of cement-sand, improve the plasticity and water retention of mortar, effectively prevent the occurrence of cracks in the surface layer of coagulation and hardening, and thus enhance the strength of the hardened slurry; rigid rubber powder has high solubility at low temperatures, and can be added to repair materials to improve adhesion and bonding, and reduce the risk of shrinkage and cracking of the back layer after coagulation and hardening; silane-based powder has excellent weather resistance and durability, and can be added to cement-based materials to enhance additional protection and waterproofing capabilities. At the same time, the addition of silane-based powder can enhance adhesion and wear resistance, and improve the stability and durability of the repaired structure; water-absorbent resin can absorb free water in the mixing process, and form a highly swollen state after absorbing water. The straight chains, branches, and cross-links in its structure overlap with each other to form a network structure, forming a "water reservoir" inside. The absorbed water will be slowly released under dry conditions, causing the unhydrated cement particles to hydrate, increasing the density of the coagulation and hardening section and improving the strength.
[0042] The fiber components include polyvinyl alcohol fiber, polypropylene fiber, and polyester fiber. The three fibers interact with each other to absorb the energy released in the hydration process of cement-based cementitious powder, and play an anti-cracking and crack-blocking role in wear-resistant mortar, reducing the risk of cracking in the back layer after repair and reducing the development of cracks. Among them, polyvinyl alcohol fiber has the characteristics of high strength, high modulus, wear resistance, acid and alkali resistance, and good weather resistance. It has strong bonding and combining properties with base materials such as cement and gypsum, and is friendly to the environment and construction workers; polypropylene fiber has the characteristics of high strength, acid resistance, alkali resistance, and anti-microbial resistance. As a filling material, it is added to mortar and concrete to improve impact resistance, waterproof and heat insulation properties; polyester fiber has the characteristics of easy dispersion, high breaking strength, high elastic modulus, wear resistance, acid resistance, alkali resistance, microbial resistance, high temperature resistance, etc., and can be used in high-strength mortar and high-strength concrete to play an anti-cracking role.
[0043] Another aspect of the present invention provides a method for preparing a water-repellent, maintenance-free cement-based wear-resistant material suitable for the lining of a reinforced concrete silo, comprising the following steps:
[0044] According to the mass percentage, the aggregate and fiber components are put into an adjustable-speed mortar mixer, stirred evenly at a speed of 40 to 70 r / min, and the stirring is stopped after stirring for 1 to 2 minutes. The cement-based cementitious powder is added and stirred evenly at a speed of 40 to 70 r / min. During this period, an appropriate amount of water is added, and the stirring is stopped after stirring for 1 to 2 minutes. The modified component is added and stirred at a speed of 80 to 100 r / min for 2 minutes. During this period, water is added to increase the fluidity of the wear-resistant material until it meets the fluidity requirements of on-site coating. The fluidity of the wear-resistant material is adjusted to 140 to 160 mm to obtain a hydrophobic and maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos.
[0045] Furthermore, the specific surface area of the silicate cement is 300 to 350 m 2 / kg; the sulphoaluminate cement adopts 42.5 strength grade and specific surface area of 400-500m 2 / g. When the above specific surface area is selected for silicate cement or sulphoaluminate cement, the hydration rate and setting and hardening rate are both excellent, and the strength value after setting and hardening is optimal. When the specific surface area is lower than the lower limit, the hydration rate decreases, and the early setting and hardening strength value is low. When the specific surface area is higher than the upper limit, the hydration rate accelerates. The excessively fast hydration rate reduces the number of crystallization points of the hydration products overlapping each other, and shortens the time for the crystal phases to overlap and arrange each other. Although the early strength is improved, the later strength is seriously reduced.
[0046] Furthermore, the sum of β-CaSO4·1 / 2H2O and soluble anhydrous calcium sulfate (CaSO4) in the gypsum material is 70%. The main function of CaSO4 in gypsum is to regulate the hydration of sulphoaluminate cement. Controlling the sum of CaSO4 to 70% can effectively regulate the setting and hardening time of the wear-resistant material.
[0047] Furthermore, the specific gravity of the diamond is 3.1 g / cm 3 The average particle size is 0.3-0.6mm; the selection of diamond abrasive particle size of 0.3-0.6mm can effectively ensure the strength development of wear-resistant materials. If it is lower than 0.3mm, the aggregate particle size is too small and the spatial skeleton effect of the hardened slurry is small, which is not conducive to strength development. If the particle size is greater than 0.6mm, the coarse particles overlap each other to form a large void ratio, which is not conducive to strength development.
[0048] Furthermore, the quartz sand SiO2≥90%, the average particle size is 0.5-1.0mm; the white corundum Al2O3≥90wt%, the particle size specification is 20-60 mesh; the spinel particle size is 0.2-0.6mm. The main purpose of selecting the above particle size is to facilitate the adjustment of the hardening slurry porosity and ensure the strength development. If it is lower than the lower limit, the skeleton function of the aggregate in the strength development process of the wear-resistant mortar is lost. If it is higher than the upper limit, the aggregate particle size is too large, the porosity of the hardened slurry is too large, and the strength development is affected.
[0049] Further, the hydroxypropyl methylcellulose has a viscosity grade of 200,000 and a particle size of 20 to 60 meshes. The addition of hydroxypropyl methylcellulose will improve the dispersibility of cementitious materials-aggregates, improve the plasticity and water retention of wear-resistant mortar, but as the viscosity grade of hydroxypropyl methylcellulose increases, the strength decreases accordingly. The comprehensive analysis of different viscosity grades on strength development shows that the cement-based wear-resistant material that meets the hydrophobic and maintenance-free type of the present invention has a viscosity grade of 200,000. The dissolution rates of different particle sizes show a large difference, which is beneficial to the wear-resistant material strength development. The optimal particle size is 20 to 60 meshes. Further, the rigid rubber powder has a viscosity grade of 600,000 and a particle size of 40 to 80 meshes. The addition of rigid rubber powder mainly improves the bonding ability of wear-resistant mortar and repair interface. The larger the viscosity grade, the stronger the bonding ability, but the compressive strength shows a downward trend. The optimal viscosity grade for the development of comprehensive bonding performance and strength performance is 600,000. The selection of a dissolution rate of 40 to 80 meshes is beneficial to the development of viscosity strength and compressive strength of wear-resistant materials.
[0050] Furthermore, the silane-based powder has a pH value of 7.0-8.5 and a particle size of 80-120 meshes. The addition of the silane-based powder effectively enhances the hydrophobicity of the wear-resistant material and isolates the penetration of liquid water through the capillary. When the particle size is 80-120 meshes, the silane-based powder has the best solubility in the wear-resistant material, and the hydrophobicity of the wear-resistant material can be maximized.
[0051] Furthermore, the water-absorbing resin has a water absorption multiple of 200 and a particle size of 60 to 100 meshes. The addition of the water-absorbing resin can absorb free water in the hydration process of the wear-resistant material. If the particle size is too large, the resin particles formed after absorbing water are large. With the increase of the hydration process, large particles of water-absorbing resin will leave large gaps after releasing internal water, causing the strength to decrease in the later stage. If the particle size is too small, the resin particles are small after absorbing water, and the amount of internal free water released in the later stage of the hydration reaction is low, which is not conducive to the later strength development of the wear-resistant material.
[0052] Furthermore, the polyvinyl alcohol fiber has an average molecular weight of 60,000 to 150,000 and a length of 6 mm to 19 mm; the polypropylene fiber has a diameter of 10 to 95 μm and a length of 3 to 20 mm; and the polyester fiber has a density of 1.2 to 1.37 g / cm 3 , length 3 ~ 9mm. The thickness of the wear-resistant repair layer is 40mm ~ 50mm. The use of longer fibers is not conducive to the workability of the wear-resistant mortar, and the longer fibers are easily pulled out, resulting in defects in the hardened wear-resistant mortar. The shorter fiber diameter will reduce the mechanical properties of the wear-resistant mortar, that is, the strength, and ultimately affect the service life of the wear-resistant layer.
[0053] The advantages and positive effects of the present invention are:
[0054] (1) The gelling property of the water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining prepared by the present invention is derived from the hydration of silicate cement, sulphoaluminate cement and gypsum in the cement-based powder. Among them, sulphoaluminate cement undergoes hydration reaction first. The addition of gypsum slows down the hydration rate of sulphoaluminate cement to ensure the network density of the early microstructure hydrated crystal phase, thereby improving the early strength. In addition, the hydration process of sulphoaluminate cement is not limited to a low temperature environment, that is, coagulation and hardening in a low temperature environment ensures strength development. As the hydration process proceeds, the hydration rate of sulphoaluminate slows down and the hydration rate of silicate cement increases. Unlike the shrinkage of the strength of sulphoaluminate cement at 28 days of age, the strength of silicate cement shows an increasing trend. The crystalline phase formed by the hydration of silicate cement is effectively filled in the interface formed by the original hydration of sulphoaluminate cement. The synergistic effect of the three not only ensures the later strength of the wear-resistant material, but also makes the hydration process not limited to a low temperature environment, and the early strength is high and the later strength does not shrink.
[0055] (2) The hydrophobic, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining prepared by the present invention has the characteristics of high strength, wear resistance and reduced interface friction. Corundum is the key to ensuring the strength development of wear-resistant materials. Corundum has a hard texture and a crushing index value much higher than river sand and machine-made sand, which lays a foundation for the high strength of wear-resistant mortar. Quartz sand and white corundum are used in wear-resistant materials to increase the wear resistance and corrosion resistance of the back layer after repair. The main oxide SiO2 in quartz sand and the main oxide Al2O3 in white corundum have a unique structural arrangement that greatly improves the wear resistance and corrosion resistance of the material. Spinel is mainly composed of magnesium aluminum oxide, which has a hard texture and a smooth surface. Adding it to wear-resistant materials can reduce the problem of large friction of the repair surface layer.
[0056] (3) The hydrophobic and maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos prepared by the present invention has the characteristics of being hydrophobic and maintenance-free. The silane-based powder in the modified component has the characteristics of being waterproof, wear-resistant, and improving bonding adhesion. When added to the wear-resistant material, it can reduce the adsorption capacity of the hardened slurry to water, thereby achieving waterproofing. The main reason for the blockage of the discharge port of the reinforced concrete silo is that the lining wear-resistant layer is adsorbed together with the water-containing agglomerated coal particles, which hinders the coal from falling. The hydrophobic wear-resistant layer can effectively reduce the adsorption of coal particles with a higher water content and the wear-resistant layer, thereby reducing the coal The risk of blockage during the falling process; the addition of water-absorbent resin can form a "water reservoir" inside the slurry. When the surface is dry, the absorbed water will be slowly released, increasing the hydration of the internal cementitious material and improving the strength. At the same time, the hydroxypropyl methylcellulose and rigid rubber powder in the modified components have a certain water retention capacity. After the construction is completed, the evaporation rate of the rear layer of water is reduced, reducing the occurrence of early plastic cracks. The synergistic effect of water-absorbent resin, hydroxypropyl methylcellulose and rigid rubber powder ensures the strength development while reducing the investment in maintenance measures for the entire process of coagulation and hardening of wear-resistant materials.
[0057] (4) The surface layer prepared by the present invention, which is suitable for the construction of water-repellent, maintenance-free cement-based wear-resistant materials for reinforced concrete silo linings, has crack resistance. The polyvinyl alcohol fiber, polypropylene fiber, and polyester fiber in the fiber components have the characteristics of high strength, high modulus, wear resistance, acid and alkali resistance, and good weather resistance. When added to high-strength mortar, they synergistically enhance the impact resistance, waterproofing, heat insulation, and crack prevention effects. The randomly distributed fiber structure can absorb the energy released during the hydration process of the cementitious material, thereby reducing the development of cracks in the later layer after repair.
[0058] In summary, the hydrophobic and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining prepared by the present invention has the characteristics of high early strength, strong wear resistance, maintenance-free construction surface layer, strong hydrophobicity after hardening, good crack resistance of the construction surface layer, and is not limited to low-temperature construction environment. In addition, the preparation process is simple, easy to use, energy-saving and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 This is a process diagram of the preparation of a water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo linings according to the present invention. DETAILED DESCRIPTION
[0060] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0061] according to Figure 1 The process of preparing the water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining can be divided into four stages: the first stage is the preparation of aggregate, the second stage is the preparation of fiber component, the third stage is the preparation of cement-based gelling powder filler, the fourth stage is the preparation of modified component, and the fifth stage is the preparation of water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining.
[0062] The above scheme is further described below in conjunction with specific examples. It should be understood that these examples are used to illustrate the present invention but not to limit the scope of the present invention. The implementation conditions adopted in the examples can be further adjusted according to specific construction conditions, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0063] Example 1
[0064] A water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining, containing the following components and mass percentages:
[0065] Cement-based cementitious powder 44.0wt%, aggregate 55.0wt%, modified component 0.4wt%, fiber component 0.4wt%, high-performance polycarboxylate water-reducing agent 0.2wt%.
[0066] The cement-based cementitious powder contains the following components and mass percentages: 71.0wt% of silicate cement, 22.0wt% of sulphoaluminate cement, and 7.0wt% of gypsum. The strength grade of the silicate cement is 42.5, and the specific surface area is 300-350m 2 / kg, purchased from Hebei Zanhuang Jinyu Cement Co., Ltd., P.O42.5; the strength grade of the sulphoaluminate cement is 42.5, and the specific surface area is 400-500m 2 / kg, purchased from Hebei Zanhuang Jinyu Cement Co., Ltd. and R·SAC; the sum of β-CaSO4·1 / 2H2O and soluble anhydrous calcium sulfate (CaSO4) in the gypsum is 70%, purchased from Hebei Shengyun Mining, β-type gypsum powder.
[0067] The components and mass percentages of the aggregate are: 55.0wt% corundum, 22.0t% quartz sand, 15.0wt% white corundum, and 8.0wt% spinel. The average particle size of the corundum is 0.3-0.6mm, purchased from Lingshou County Zhan Teng Mineral Products Processing Plant, with a product model of 0.3-0.6mm; the average particle size of the quartz sand is 0.5-1.0mm, purchased from Lingshou County Zhan Teng Mineral Products Processing Plant, with a product model of 0.5-1.0mm; the particle size of the white corundum is 20-60 mesh, purchased from Lingshou County Zhan Teng Mineral Products Processing Plant, with a product model of 20-60 mesh; the particle size of the spinel is 0.2-0.6mm, purchased from Lingshou County Zhan Teng Mineral Products Processing Plant, with a product model of 0.2-0.6mm.
[0068] The modified component contains the following components and mass percentages: 28.0wt% hydroxypropyl methylcellulose, 22.0wt% rigid rubber powder, 30.0wt% silane-based powder, and 20.0wt% water-absorbent resin. The hydroxypropyl methylcellulose is purchased from Langfang Feicheng New Materials Technology Co., Ltd., with a viscosity grade of 200,000 and a particle size of 20-60 meshes; the rigid rubber powder is purchased from German Wacker Group, Wacker 8 series latex powder, with a viscosity grade of 600,000 and a particle size of 40-80 meshes; the silane-based powder has a pH value of 7.0-8.5 and a particle size of 80-120 meshes, and is purchased from Shanghai Chenqi Chemical Technology Co., Ltd., Yilaitai SEAL81; the water-absorbent resin has a water absorption multiple of 200 and a particle size of 60-120 meshes, and the water-absorbent resin is specifically a polymer water-absorbent resin, which is purchased from Renqiu Yibang Environmental Protection Technology Co., Ltd., with a particle size of 60-120 meshes.
[0069] The fiber components contain the following components and their mass percentages: 33.0wt% polyvinyl alcohol fiber, 35.0wt% polypropylene fiber, and 32.0wt% polyester fiber. The polyvinyl alcohol fiber has an average molecular weight of 60,000 to 150,000 and a length of 6 to 19 mm, which is purchased from Shandong Hongyao Ecological and Environmental Protection Materials Co., Ltd., 6 to 19 mm; the polypropylene fiber has a diameter of 10 to 95 μm and a length of 3 to 20 mm, which is purchased from Shandong Hongyao Ecological and Environmental Protection Materials Co., Ltd., 3 to 20 mm; the polyester fiber has a density of 1.20 to 1.37 g / cm 3 , length 3~9mm, purchased from Shandong Hongyao Ecological and Environmental Protection Materials Co., Ltd., 3~9mm.
[0070] A method for preparing a water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining is as follows:
[0071] (1) Preparation of aggregate components: According to 55.0wt% of corundum, 22.0t% of quartz sand, 15.0wt% of white corundum, and 8.0wt% of spinel, corundum, quartz sand, white corundum, and spinel were weighed and then uniformly mixed to obtain aggregate;
[0072] (2) Preparation of fiber component: According to 33.0 wt% of polyvinyl alcohol fiber, 35.0 wt% of polypropylene fiber and 32.0 wt% of polyester fiber, polyvinyl alcohol fiber, polypropylene fiber and polyester fiber were weighed and then uniformly mixed to obtain a fiber component;
[0073] (3) Preparation of cement-based cementitious powder: According to 71.0 wt% of silicate cement, 22.0 wt% of sulphoaluminate cement and 7.0 wt% of gypsum, silicate cement, sulphoaluminate cement and gypsum are weighed and then uniformly mixed to obtain cement-based cementitious powder;
[0074] (4) Preparation of modified component: According to 28.0 wt% of hydroxypropyl methylcellulose, 22.0 wt% of rigid rubber powder, 30.0 wt% of silane-based powder and 20.0 wt% of water-absorbent resin, hydroxypropyl methylcellulose, rigid rubber powder, silane-based powder and water-absorbent resin were weighed and then uniformly mixed to obtain a modified component;
[0075] (5) Preparation of water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining: According to 55.0wt% of aggregate and 0.4wt% of fiber component, the aggregate and fiber component are put into an adjustable-speed mortar mixer, and stirred evenly at a speed of 42r / min. After stirring for 1min, the stirring is stopped, and the cement-based cementitious powder is added, and the stirring is evenly stirred at a speed of 42r / min. After stirring for 1min, the stirring is stopped, and the modified component is added. An appropriate amount of water is added, and the stirring is evenly stirred at a speed of 90r / min for 2min. The fluidity of the wear-resistant material is adjusted to 140-160mm to obtain a water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining with a fluidity that meets the construction requirements.
[0076] Directions:
[0077] An old concrete component was used as a test piece substrate. After cleaning the surface layer, the water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining prepared in Example 1 was evenly applied to the surface of the old concrete component and cured for more than 28 days under natural conditions. According to "Industrial Structure Cement-Based Wear-Resistant Materials" JG / T270-2010, the basic properties of the water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining in Example 1 were tested, and the results are shown in Table 1.
[0078] Table 1 Example 1 Performance of water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining
[0079]
[0080] Example 2
[0081] A water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining, containing the following components and mass percentages:
[0082] 52.0wt% cementitious powder, 47.0wt% aggregate, 0.3wt% modified component, 0.3wt% fiber component, and 0.4wt% high-performance polycarboxylate water-reducing agent.
[0083] The components and mass percentages of the cement-based cementitious powder are: 80.0wt% of Portland cement, 15.0wt% of sulphoaluminate cement, and 5.0wt% of gypsum.
[0084] The components and mass percentages of the aggregate are: 50.0wt% corundum, 20.0t% quartz sand, 18.0wt% white corundum, and 12.0wt% spinel.
[0085] The modified component contains the following components and their mass percentages: 32.0 wt % of hydroxypropyl methylcellulose, 20.0 wt % of rigid rubber powder, 23.0 wt % of silane-based powder, and 25.0 wt % of water-absorbing resin.
[0086] The fiber component contains the following components and their mass percentages: 30.0 wt% of polyvinyl alcohol fiber, 40.0 wt% of polypropylene fiber, and 30.0 wt% of polyester fiber.
[0087] The raw materials used in Example 2 are the same as those in Example 1. The preparation method and use method of the water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining in Example 2 are the same as those in Example 1.
[0088] According to "Cement-based Wear-Resistant Materials for Industrial Structures" JG / T270-2010, the basic properties of the hydrophobic, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining in Example 2 were tested, and the results are shown in Table 2.
[0089] Table 2 Example 2 Performance of water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining
[0090]
[0091] Example 3
[0092] A water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining, containing the following components and mass percentages:
[0093] Cement-based cementitious powder 48.0wt%, aggregate 51.0wt%, modified component 0.4wt%, fiber component 0.3wt%, high-performance polycarboxylate water-reducing agent 0.3wt%.
[0094] The components and mass percentages of the cement-based cementitious powder are: 76.0wt% of Portland cement, 18.0wt% of sulphoaluminate cement, and 6.0wt% of gypsum.
[0095] The components and mass percentages of the aggregate are: 52.0wt% corundum, 24.0t% quartz sand, 17.0wt% white corundum, and 7.0wt% spinel.
[0096] The modified component contains the following components and their mass percentages: 30.0 wt % of hydroxypropyl methylcellulose, 21.0 wt % of rigid rubber powder, 27.0 wt % of silane-based powder, and 22.0 wt % of water-absorbing resin.
[0097] The fiber component contains the following components and their mass percentages: 32.0 wt% of polyvinyl alcohol fiber, 37.0 wt% of polypropylene fiber, and 31.0 wt% of polyester fiber.
[0098] The raw materials used in Example 3 are the same as those in Example 1. The preparation method and use method of the water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining in Example 3 are the same as those in Example 1.
[0099] According to "Cement-based Wear-Resistant Materials for Industrial Structures" JG / T270-2010, the basic properties of the hydrophobic, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining in Example 3 were tested, and the results are shown in Table 3.
[0100] Table 3 Example 3 Performance of water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining
[0101]
[0102]
[0103] Based on the test results of Examples 1-3, it can be seen that the technical indicators of the hydrophobic, maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos prepared by the preparation method of the present invention all meet the standards, and the fluidity, wear loss, compressive strength, impact strength, crack resistance and other aspects all meet the performance requirements of "Cement-based Wear-Resistant Materials for Industrial Structures" JG / T270-2010 for wear-resistant materials.
[0104] The water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining prepared by the present invention has high strength and wear-resistant properties. At present, cracks are generated in the surface layer of the wear-resistant material during construction and use due to inadequate maintenance. After the construction is completed, the repaired surface layer is rough and easy to cause blockage of the feed port. In the study, while meeting the high strength in the later stage, the type of cement-based gelling powder (adding sulphoaluminate cement + gypsum) is adjusted to improve the early strength of the wear-resistant material; secondly, corundum + quartz sand + white corundum + spinel are introduced to improve the wear resistance and reduce the friction of the back layer after the wear-resistant material is repaired; the addition of hydroxypropyl methylcellulose + rigid rubber powder + silane-based powder + water-absorbing resin is the key to the wear-resistant material showing water repellency and maintenance-free. The silane-based powder has the characteristics of waterproofness, wear resistance, and improved bonding adhesion, and can be added to the wear-resistant material to reduce the hardening The slurry's ability to adsorb water achieves waterproofing. The main reason for the blockage of the discharge port of the reinforced concrete silo is that the inner lining wear-resistant layer is adsorbed together with the water-containing agglomerated coal particles, which hinders the coal from falling. The hydrophobic wear-resistant layer can effectively reduce the adsorption of coal particles with higher moisture content and the wear-resistant layer, reducing the risk of clogging in the process of coal falling; the addition of water-absorbent resin can form a "water reservoir" inside the slurry. When the surface is dry, the absorbed water will be slowly released, increasing the hydration of the internal cementitious material and improving the strength. At the same time, the hydroxypropyl methylcellulose and rigid rubber powder in the modified components have a certain water retention capacity. After the construction is completed, the evaporation rate of the water in the back layer is reduced, reducing the occurrence of early plastic cracks. The water-absorbent resin, hydroxypropyl methylcellulose and rigid rubber powder work together to ensure the strength development while reducing the investment in maintenance measures for the entire process of wear-resistant material coagulation and hardening.
[0105] Comparative Example 1
[0106] The difference from Example 1 is that the cement-based powder only uses 74.0 wt% of Portland cement and 26.0 wt% of sulphoaluminate cement, and the other treatments and proportions are consistent with those in Example 1.
[0107] Comparative Example 2
[0108] The difference from Example 1 is that the cement-based powder only uses 90.0wt% of Portland cement and 10.0wt% of gypsum, and the other treatments and proportions are consistent with those in Example 1.
[0109] Comparative Example 3
[0110] The difference from Example 1 is that the cement-based powder only uses 70.0wt% sulphoaluminate cement and 30.0wt% gypsum, and the other treatments and proportions are consistent with those in Example 1.
[0111] Table 4 Performance of water-repellent and maintenance-free cement-based wear-resistant materials suitable for reinforced concrete silo linings prepared in Comparative Examples 1-3
[0112]
[0113] Comparative Example 4
[0114] The difference from Example 1 is that only quartz sand 42.0wt%, white corundum 35.0wt%, and spinel 23.0wt% are used as aggregates, and other treatments and proportions are consistent with those in Example 1.
[0115] Comparative Example 5
[0116] The difference from Example 1 is that the aggregate is 62.0wt% corundum, 25.0wt% white corundum, and 13.0wt% spinel, and the other treatments and proportions are consistent with those in Example 1.
[0117] Comparative Example 6
[0118] The difference from Example 1 is that the aggregate is 60.0wt% corundum, 27.0wt% quartz sand, and 13.0wt% spinel, and the other treatments and proportions are consistent with those in Example 1.
[0119] Comparative Example 7
[0120] The difference from Example 1 is that the aggregate is 58.0wt% corundum, 25.0wt% quartz sand, and 17.0wt% white corundum, and the other treatments and proportions are consistent with those in Example 1.
[0121] Table 5 Performance of water-repellent and maintenance-free cement-based wear-resistant materials suitable for reinforced concrete silo linings prepared in Comparative Examples 4-7
[0122]
[0123] Comparative Example 8
[0124] The difference from Example 1 is that the modified components are 32.0wt% of rigid rubber powder, 40.0wt% of silane-based powder, and 28.0wt% of water-absorbing resin. Other treatments and proportions are consistent with those in Example 1.
[0125] Comparative Example 9
[0126] The difference from Example 1 is that the modified component is 35.0wt% hydroxypropyl methylcellulose, 37.0wt% silane-based powder, and 28.0wt% water-absorbing resin. Other treatments and proportions are consistent with those in Example 1.
[0127] Comparative Example 10
[0128] The difference from Example 1 is that the modified component is 38.0wt% hydroxypropyl methylcellulose, 32.0wt% rigid rubber powder, and 30.0wt% water-absorbing resin. Other treatments and proportions are consistent with those in Example 1.
[0129] Comparative Example 11
[0130] The difference from Example 1 is that the modified component is 35.0wt% hydroxypropyl methylcellulose, 29.0wt% rigid rubber powder, and 36.0wt% silane-based powder. Other treatments and proportions are consistent with those in Example 1.
[0131] Table 6 Performance of water-repellent and maintenance-free cement-based wear-resistant materials suitable for reinforced concrete silo linings prepared in comparative examples 8-11
[0132]
[0133] Comparative Example 12
[0134] The difference from Example 1 is that the fiber components are 55.0wt% polypropylene fiber and 45.0wt% polyester fiber, and the other treatments and proportions are consistent with those in Example 1.
[0135] Comparative Example 13
[0136] The difference from Example 1 is that the fiber components are 58.0wt% polyvinyl alcohol fiber and 42.0wt% polyester fiber, and the other treatments and proportions are consistent with those in Example 1.
[0137] Comparative Example 14
[0138] The difference from Example 1 is that the fiber components are 49.0wt% polyvinyl alcohol fiber and 51.0wt% polypropylene fiber, and the other treatments and proportions are consistent with those in Example 1.
[0139] Table 7 Performance of water-repellent and maintenance-free cement-based wear-resistant materials suitable for reinforced concrete silo linings prepared in Comparative Examples 12-14
[0140]
[0141]
[0142] Comparative Example 15
[0143] The difference from Example 1 is that the modified component contains the following components and their mass percentages: 10.0 wt % hydroxypropyl methylcellulose, 28.0 wt % rigid rubber powder, 40.0 wt % silane-based powder, and 22.0 wt % water-absorbing resin.
[0144] Comparative Example 16
[0145] The difference from Example 1 is that the cement-based cementitious powder contains the following components and their mass percentages: 77.0 wt % of Portland cement, 22.0 wt % of sulphoaluminate cement, and 1.0 wt % of gypsum.
[0146] Comparative Example 17
[0147] The difference from Example 1 is that the modified component contains the following components and their mass percentages: 10.0 wt % hydroxypropyl methylcellulose, 28.0 wt % rigid rubber powder, 40.0 wt % silane-based powder, and 22.0 wt % water-absorbing resin.
[0148] The components and mass percentages of the cement-based cementitious powder are: 77.0wt% of Portland cement, 22.0wt% of sulphoaluminate cement, and 1.0wt% of gypsum.
[0149] Table 8 Performance of water-repellent and maintenance-free cement-based wear-resistant materials suitable for reinforced concrete silo linings prepared in Comparative Examples 15-17
[0150]
[0151]
[0152] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept, which all belong to the protection scope of the present invention.
Claims
1. A water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining. It is characterized in that The components and mass percentages are as follows: Cement-based cementitious powder 43-53wt%, Aggregate 45~55wt% Modified component 0.3~0.6wt%, Fiber component 0.3~0.8wt%, Water reducing agent 0.2~0.9wt%, The sum of the mass percentages of the above components is 100wt%; The components and mass percentages of the cement-based cementitious powder are as follows: Portland cement 70~85wt%, Sulphoaluminate cement 10~25wt% Gypsum 4~8wt% The sum of the mass percentages of the above components is 100wt%; The components and mass percentages of the aggregate are as follows: Diamond 45~60wt% Quartz sand 15~28wt% White corundum 12~20wt% Spinel 6~15wt% The sum of the mass percentages of the above components is 100wt%; The modified components and mass percentages are as follows: Hydroxypropyl methylcellulose 22-35wt%, Rigid rubber powder 15~28wt% Silane-based powder 25-40wt%, Water-absorbing resin 18~26wt% The sum of the mass percentages of the above components is 100wt%; The fiber components and mass percentages are as follows: Polyvinyl alcohol fiber 22~35wt%, Polypropylene fiber 32~45wt%, Polyester fiber 30~40wt%, The sum of the mass percentages of the above components is 100wt%; The water reducer is a high-performance polycarboxylate water reducer.
2. The method for preparing the water-repellent and maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining according to claim 1, It is characterized in that The following steps are involved: According to the mass percentage, the aggregate and fiber components are put into an adjustable-speed mortar mixer, stirred evenly at a speed of 40 to 70 r / min, and the stirring is stopped after stirring for 1 to 2 minutes. The cement-based cementitious powder is added and stirred evenly at a speed of 40 to 70 r / min. During this period, an appropriate amount of water is added, and the stirring is stopped after stirring for 1 to 2 minutes. The modified component is added and stirred at a speed of 80 to 100 r / min for 1 to 3 minutes. During this period, water is added to increase the fluidity of the wear-resistant material until it meets the fluidity requirements of on-site coating. The fluidity of the wear-resistant material is adjusted to 140 to 160 mm to obtain a hydrophobic and maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos.
3. The water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining obtained by the preparation method according to claim 1 or claim 2, It is characterized in that The specific surface area of the silicate cement is 300-350m 2 / kg; the sulphoaluminate cement adopts 42.5 strength grade and specific surface area of 400-500m 2 / g.
4. The water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining according to claim 3, It is characterized in that β-CaSO in the gypsum 4 1 / 2H 2 O and soluble anhydrous calcium sulfate (CaSO 4 ) is 70%.
5. The water-repellent, maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos according to claim 3, It is characterized in that The specific gravity of the diamond is 3.1 g / cm 3 , with an average particle size of 0.3 to 0.6 mm; the quartz sand SiO 2 ≥90%, with an average particle size of 0.5-1.0 mm; the white corundum Al 2 O 3 ≥90wt%, particle size specification 20-60 mesh; the spinel particle size 0.2-0.6mm.
6. The water-repellent, maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos according to claim 3, It is characterized in that The hydroxypropyl methylcellulose has a viscosity grade of 200,000 and a particle size of 20 to 60 meshes.
7. The water-repellent, maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos according to claim 3, Features: The rigid rubber powder has a viscosity grade of 600,000 and a particle size of 40 to 80 meshes.
8. The water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining according to claim 3, Features: The silane-based powder has a pH value of 7.0-8.5 and a particle size of 80-120 meshes.
9. The water-repellent, maintenance-free cement-based wear-resistant material suitable for the lining of reinforced concrete silos according to claim 3, Features: The water-absorbing resin has a water absorption multiple of 200 and a particle size of 60 to 100 meshes.
10. The water-repellent, maintenance-free cement-based wear-resistant material suitable for reinforced concrete silo lining according to claim 3, It is characterized in that The polyvinyl alcohol fiber has an average molecular weight of 60,000 to 150,000 and a length of 6 mm to 19 mm; the polypropylene fiber has a diameter of 10 to 95 μm and a length of 3 to 20 mm; the polyester fiber has a density of 1.2 to 1.37 g / cm 3 , length 3~9mm.
Citation Information
Patent Citations
Cement based wear resistant material for industry warehouse structure inner lining
CN101353243A
Cement-base wear-resistant material prepared from steel slag
CN101921085A
Wear-resistant cement mortar, wear-resistant floor and preparation method thereof
CN102910885A
Surface wear-resistant hydrophobic enhanced self-leveling mortar and preparation method thereof
CN112552000A
Wear-resistant ultra-high performance concrete and preparation method thereof
CN113372082A