Surface treatment composition and method for manufacturing wafer

By using surface treatment compositions of silicon compounds such as trialkylsilylamine and high-content hydrocarbon solvents, a water-repellent protective film is formed, which solves the problem of pattern collapse in semiconductor device manufacturing, and achieves higher water contact angle and stability sex.

CN118974894AInactive Publication Date: 2024-11-15CENT GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031774.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-12
Filing Date
2023-04-05
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the manufacturing process of semiconductor devices, as the circuit pattern is finer, the pattern is prone to collapse after cleaning or rinsing, resulting in a decrease in production yield, and it is difficult for the prior art to effectively prevent the pattern from collapse.

Method used

采用包含三烷基甲硅烷基胺等硅化合物作为甲硅烷基化剂和高含量烃溶剂的表面处理组合物,通过蒸气形式供给晶圆表面,形成拒水性保护膜以防止图案崩塌。

Benefits of technology

The water contact angle is effectively increased, pattern collapse is suppressed, and the stability of the wafer surface and the production efficiency of the manufacturing method are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005066641020000241
    Figure BDA0005066641020000241
  • Figure HDA0005066641030000011
    Figure HDA0005066641030000011
  • Figure HDA0005066641030000012
    Figure HDA0005066641030000012
Patent Text Reader

Abstract

The surface treatment composition according to the present invention is used for forming a water-repellent protective film on the surface by being supplied in the form of vapor to the surface of a wafer having a concave-convex pattern on the surface, the surface treatment composition comprising a silylating agent and a solvent, in which the silylating agent comprises (R1) 3Si-X (wherein R1 represents a hydrogen atom, and R2 represents a hydrogen atom; (In the formula, R1 each independently represents a group selected from the group consisting of a hydrocarbon group having 1-10 carbon atoms and a hydrocarbon group having 1-10 carbon atoms in which some or all of hydrogen atoms are substituted with fluorine atoms, and X represents an amino group), and the solvent contains 75 mass% or more of a hydrocarbon solvent based on 100 mass% of the total amount of the solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a surface treatment composition and a method for manufacturing a wafer. Background Art

[0002] Semiconductor devices used in networks or digital home appliances require higher performance / functionality and lower power consumption. Therefore, the circuit pattern has been miniaturized, and as the miniaturization progresses, the pattern collapse of the circuit pattern has become a problem. Cleaning processes are often used in the manufacture of semiconductor devices to remove particles and metal impurities. As a result, the cleaning process even occupies 30% to 40% of the entire semiconductor manufacturing process. In this cleaning process, as the semiconductor device becomes miniaturized, if the aspect ratio of the pattern becomes larger, the pattern will collapse when the gas-liquid interface passes through the pattern after cleaning or rinsing. This phenomenon is pattern collapse. In order to prevent the occurrence of pattern collapse, the pattern design has to be changed, which will also lead to a decrease in the yield during production. Therefore, a method for preventing pattern collapse in the cleaning process is desired.

[0003] As a method for preventing pattern collapse, it is known that forming a water-repellent protective film on the pattern surface is effective. The water repellency needs to be performed without drying the pattern surface, so a water-repellent protective film forming liquid that can make the pattern surface water-repellent is supplied to the pattern surface that is kept in a state of a cleaning liquid, etc., and the cleaning liquid is replaced with the above liquid to form a water-repellent protective film.

[0004] As such a technique, there is known a technique described in Patent Document 1. Patent Document 1 describes a surface treatment composition containing a silylating agent, diethyl carbonate, and propylene carbonate as a solvent (Example 5 of Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2019 / 193967 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] However, the present inventors have studied and found that the surface treatment composition described in Patent Document 1 has room for improvement in that it is easy to increase the water contact angle.

[0010] Solutions for solving problems

[0011] The present inventors conducted further research and found that by using a silicon compound such as trialkylsilylamine as a silylating agent and a hydrocarbon solvent having a content of 97% by mass or more in the solvent as a solvent, the surface treatment composition can easily increase the water contact angle. Subsequent research further found that if the content of the hydrocarbon solvent in the solvent is made to be 75% by mass or more, a practical and large contact angle can be maintained, thereby completing the present invention.

[0012] According to one aspect of the present invention, the following surface treatment composition and wafer manufacturing method are provided.

[0013] 1. A surface treatment composition for supplying in the form of vapor to the surface of a wafer having a concavo-convex pattern on the surface thereof and forming a water-repellent protective film on the surface thereof, the surface treatment composition comprising a silylating agent and a solvent,

[0014] The silylating agent comprises a silicon compound represented by formula (1),

[0015] (R 1 ) 3 Si-X(1)

[0016] (Among them, R 1 are each independently a group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, and a hydrocarbon group having 1 to 10 carbon atoms in which a part or all of the hydrogen atoms are substituted with fluorine atoms, and X is an amino group)

[0017] The solvent contains 75% by mass or more of a hydrocarbon solvent in 100% by mass of the total amount of the solvent.

[0018] 2. The surface treatment composition according to 1., wherein

[0019] The content of the hydrocarbon solvent is 97% by mass or more in 100% by mass of the total amount of the solvent.

[0020] 3. The surface treatment composition according to 1. or 2., wherein

[0021] The hydrocarbon solvent includes aromatic hydrocarbons.

[0022] 4. The surface treatment composition according to any one of 1. to 3., wherein

[0023] The content of the silylating agent is 0.3 mass % or more and 30 mass % or less in 100 mass % of the surface treatment composition.

[0024] 5. The surface treatment composition according to any one of 1. to 4., wherein

[0025] The boiling point difference between the boiling point of the solvent and the boiling point of the silylating agent (the boiling point of the solvent - the boiling point of the silylating agent) is 20° C. or more at 1 atmosphere.

[0026] 6. The surface treatment composition according to any one of 1. to 5., wherein

[0027] The aforementioned silicon compound includes one or more selected from the group consisting of trimethylsilyldimethylamine, trimethylsilyldiethylamine, N-(trimethylsilyl)-tert-butylamine, and hexamethyldisilazane, and compounds in which at least one trimethylsilyl group of these trimethylsilylamines is substituted by any one of ethyldimethylsilyl, propyldimethylsilyl, butyldimethylsilyl, hexyldimethylsilyl, octyldimethylsilyl, and decyldimethylsilyl.

[0028] 7. The surface treatment composition according to any one of 1. to 6., wherein

[0029] The water contact angle of the surface of the silicon wafer after surface treatment measured by the following steps exceeds 80°.

[0030] (step)

[0031] A smooth silicon wafer having a thermal oxide film on its surface was immersed in a 1 mass % hydrofluoric acid aqueous solution at 25°C for 10 minutes, immersed in pure water at 25°C for 1 minute, and immersed in 2-propanol (iPA) at 25°C for 1 minute for cleaning.

[0032] The cleaned silicon wafer is placed horizontally in a state where liquid iPA is contained, and the vapor of the surface treatment composition is supplied to the silicon wafer.

[0033] Next, on the surface of the silicon wafer, the vapor state is changed to liquid, and the iPA retained on the surface is replaced with the liquid.

[0034] Next, the silicon wafer was immersed in iPA at 25° C. for 1 minute.

[0035] Afterwards, air is blown onto the silicon wafer to remove the iPA on the surface.

[0036] The water contact angle was measured using 2 μl of pure water on the surface of the silicon wafer obtained through the above steps in accordance with JIS R 3257:1999 "Test methods for wettability of glass substrate surfaces".

[0037] 8. The surface treatment composition according to any one of 1. to 7., wherein

[0038] The surface treatment composition does not contain acyclic carbonate, or contains 2% by mass or less of acyclic carbonate in 100% by mass of the surface treatment composition.

[0039] 9. The surface treatment composition according to any one of 1. to 8., wherein

[0040] The surface treatment composition does not contain a catalyst, or contains a catalyst in an amount of 2% by mass or less in 100% by mass of the surface treatment composition.

[0041] 10. The surface treatment composition according to any one of 1. to 9., wherein

[0042] The number of particles larger than 0.2 μm measured by a light scattering liquid particle detector was 1.0×10 4 Less than .

[0043] 11. The surface treatment composition according to any one of 1. to 10., wherein

[0044] The total content of Na, Mg, Ca, Mn, Fe, Cu, Li, Al, Cr, Ni, Zn and Ag in the surface treatment composition measured using inductively coupled plasma mass spectrometry is 100 mass ppb or less.

[0045] 12. A method for manufacturing a wafer, comprising the following steps:

[0046] A process of preparing a wafer having a concavo-convex pattern on its surface;

[0047] A step of supplying a cleaning liquid to the surface of the wafer to clean the surface; and

[0048] The step of supplying the vapor of the surface treatment composition to the surface holding the cleaning liquid, changing the state of the vapor to liquid on the surface, replacing the cleaning liquid with the liquid, and forming a water-repellent protective film on at least a portion of the surface.

[0049] The surface treatment composition comprises a silylating agent and a solvent.

[0050] The silylating agent comprises a silicon compound represented by formula (1),

[0051] (R 1 ) 3 Si-X(1)

[0052] (Among them, R 1 are each independently a group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, and a hydrocarbon group having 1 to 10 carbon atoms in which a part or all of the hydrogen atoms are substituted with fluorine atoms, and X is an amino group)

[0053] The solvent contains 75% by mass or more of a hydrocarbon solvent in 100% by mass of the total amount of the solvent.

[0054] 13. The method for manufacturing a wafer according to 12., wherein:

[0055] The content of the hydrocarbon solvent is 97% by mass or more in 100% by mass of the total amount of the solvent.

[0056] 14. The method for manufacturing a wafer according to 12. or 13., wherein:

[0057] In the surface treatment composition, the hydrocarbon solvent contains an aromatic hydrocarbon.

[0058] 15. The method for manufacturing a wafer according to any one of 12. to 14., wherein:

[0059] In the surface treatment composition, the content of the silylating agent is 0.3% by mass or more and 30% by mass or less in 100% by mass of the surface treatment composition.

[0060] 16. The method for manufacturing a wafer according to any one of 12. to 15., wherein:

[0061] In the surface treatment composition, the boiling point difference between the boiling point of the solvent and the boiling point of the silylating agent (the boiling point of the solvent - the boiling point of the silylating agent) is 20° C. or more at 1 atmosphere.

[0062] 17. The method for manufacturing a wafer according to any one of 12. to 16., wherein:

[0063] In the surface treatment composition, the silicon compound comprises one or more selected from the group consisting of trimethylsilyldimethylamine, trimethylsilyldiethylamine, N-(trimethylsilyl)-tert-butylamine, and hexamethyldisilazane, and compounds in which at least one trimethylsilyl group of these trimethylsilylamines is substituted with any one of ethyldimethylsilyl, propyldimethylsilyl, butyldimethylsilyl, hexyldimethylsilyl, octyldimethylsilyl, and decyldimethylsilyl.

[0064] 18. The method for manufacturing a wafer according to any one of 12. to 17., wherein:

[0065] The surface treatment composition does not contain acyclic carbonate, or contains 2% by mass or less of acyclic carbonate in 100% by mass of the surface treatment composition.

[0066] 19. The method for manufacturing a wafer according to any one of 12. to 18., wherein:

[0067] The surface treatment composition does not contain a catalyst, or contains a catalyst in an amount of 2% by mass or less in 100% by mass of the surface treatment composition.

[0068] 20. The method for manufacturing a wafer according to any one of 12. to 19., wherein:

[0069] In the above-mentioned surface treatment composition, the number of particles larger than 0.2 μm measured by a light scattering liquid particle detector is 1.0×10 4 Less than .

[0070] 21. The method for manufacturing a wafer according to any one of 12. to 20., wherein:

[0071] In the aforementioned surface treatment composition, the total content of Na, Mg, Ca, Mn, Fe, Cu, Li, Al, Cr, Ni, Zn and Ag measured using inductively coupled plasma mass spectrometry is 100 mass ppb or less in the surface treatment composition.

[0072] 22. The method for manufacturing a wafer according to any one of 12. to 21., wherein:

[0073] The vapor of the surface treatment composition is supplied to the surface of the wafer while the iPA is maintained thereon.

[0074] 23. The method for manufacturing a wafer according to any one of 12. to 22., wherein:

[0075] The wafer manufacturing method includes a step of mixing materials of the respective components of the surface treatment composition, wherein the total amount of water in the materials is 2000 mass ppm or less relative to the total amount of the materials.

[0076] Effects of the Invention

[0077] According to the present invention, a surface treatment composition that can easily increase the water contact angle and a method for producing a wafer using the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1 A three-dimensional schematic diagram of a wafer having a fine concave-convex pattern on its surface.

[0079] Figure 2 To show Figure 1 A schematic cross-sectional view of a portion of the a-a' section.

[0080] Figure 3 This is a schematic cross-sectional view showing a state in which the vapor of the composition is supplied to the recessed portion retaining the liquid.

[0081] Figure 4 It is a schematic cross-sectional view of a wafer on which a water-repellent protective film is formed. DETAILED DESCRIPTION

[0082] Hereinafter, the embodiments of the present invention will be described using the accompanying drawings. It should be noted that in all the accompanying drawings, the same components are given the same symbols, and the description is appropriately omitted. In addition, the drawings are schematic diagrams and are not consistent with the actual size ratio.

[0083] The outline of the surface treatment composition according to the present embodiment will be described.

[0084] The surface treatment composition of the present embodiment is supplied in the form of vapor to the surface of a wafer having a concavo-convex pattern on the surface, and forms a water-repellent protective film on the surface.

[0085] The surface treatment composition comprises a silylating agent and a solvent, wherein the silylating agent comprises a silicon compound represented by the following formula (1), and the solvent comprises 75 mass % or more of a hydrocarbon solvent in 100 mass % of the total amount of the solvent.

[0086] (R 1 ) 3 Si-X(1)

[0087] (Among them, R 1 are each independently a group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, and a hydrocarbon group having 1 to 10 carbon atoms in which a part or all of the hydrogen atoms are substituted with fluorine atoms, and X is an amino group)

[0088] By using the surface treatment composition of the present embodiment for producing a wafer having a concavo-convex pattern on its surface, pattern collapse of the concavo-convex pattern can be suppressed.

[0089] Here, an example is given to illustrate the manufacture of semiconductor wafers.

[0090] In the manufacturing process of semiconductor wafers, a fine concave and convex pattern is formed on the surface of the substrate (wafer) through film formation, photolithography or etching. Afterwards, in order to clean the wafer surface, a wet treatment such as a cleaning process using water or an organic solvent is performed. A drying process is also performed to remove liquids such as cleaning liquid or rinse liquid that adhere to the wafer due to the wet treatment.

[0091] It is known that in such a drying step, a wafer having a fine concavo-convex pattern is prone to deformation or collapse of the concavo-convex pattern.

[0092] The water-repellent protective film is formed on the concavo-convex pattern using the vapor of the surface treatment composition, and the surface is modified to make the wafer surface water-repellent, thereby suppressing the deformation or collapse of the concavo-convex pattern in the drying process. Thus, a wafer manufacturing method with excellent manufacturing stability can be realized.

[0093] According to the present inventors' opinions, it has been found that the surface treatment composition is easy to increase the water contact angle by including the aforementioned specified silicon compound as a silylating agent and using a hydrocarbon solvent having a content of 97% by mass or more in the solvent in combination as a solvent. It has been further found that by using a hydrocarbon solvent having a content of 75% by mass or more in the solvent in combination, a practical and high contact angle can also be maintained. From the viewpoint of increasing the throughput of the manufacturing process, it is preferred to use a method that is easy to further increase the water contact angle even if the time is shorter.

[0094] Although the detailed mechanism is uncertain, it can be considered that by using a solvent that does not easily react with the aforementioned specified silicon compound of the silylating agent, i.e., a hydrocarbon, as the main component of the solvent, the reaction in the liquid can be suppressed, the storage stability can be improved, and the reaction in the gas (vapor) can also be suppressed, so the surface treatment composition is easy to increase the water contact angle.

[0095] It is also believed that since the solvent with a high boiling point (low volatility) preferentially accumulates on the wafer surface and replaces with the cleaning liquid, the silylating agent can be suppressed from reacting with the cleaning liquid and being consumed, thereby making it easier to increase the water contact angle.

[0096] Hereinafter, the configuration of the surface treatment composition according to the present embodiment will be described in detail.

[0097] (Silylating Agent)

[0098] The surface treatment composition contains one or two or more silicon compounds represented by the following formula (1) as silylating agents (hereinafter, the silicon compound represented by the formula (1) may also be simply referred to as a silicon compound).

[0099] However, the silylating agent may contain only the silicon compound of the following formula (1), or may contain a silylating agent other than the silicon compound of the following formula (1) unless the effects of the present invention are impaired.

[0100] (R 1 ) 3 Si-X(1)

[0101] (Among them, R 1 are each independently a group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, and a hydrocarbon group having 1 to 10 carbon atoms in which a part or all of the hydrogen atoms are substituted with fluorine atoms, and X is an amino group)

[0102] The amino group includes ammonia and a monovalent group obtained by removing hydrogen from a primary amine or a secondary amine. For example, -NH 2 , dialkylamino (-N(CH 3 ) 2 、-N(C 2 H 5 ) 2 etc.), tert-butylamino, allylamino, -NHSi(CH 3 ) 3 、-NH-C(=O)-Si(CH 3 ) 3 、-NHC(=O)CH 3 、-NHC(=O)CF 3 、-N(CH 3 )C(=O)CH 3 、-N(CH 3 )C(=O)CF 3 、-NHC(=O)-OSi(CH 3 ) 3 、-NHC(=O)-NH-Si(CH 3 ) 3 (e.g., N,N′-bis(trimethylsilyl)urea, etc.), a group having a nitrogen-containing ring (wherein the nitrogen atom constituting the ring is bonded to the aforementioned Si atom), etc. Examples of the nitrogen-containing ring include: a piperidine ring, an imidazole ring (e.g., N-trimethylsilylimidazole, etc.), a triazole ring (e.g., N-trimethylsilyltriazole, etc.), a tetrazole ring, an oxazolidinone ring, a morpholine ring, and other nitrogen-containing heterocyclic rings. From the viewpoint of further increasing the water contact angle, the amino group is preferably a dialkylamino group, more preferably a dialkylamino group having 1 to 4 carbon atoms in the alkyl group, and further preferably a dimethylamino group (-N(CH 3 ) 2 ).

[0103] From the perspective of further increasing the water contact angle, R 1 Preferably, each independently contains a hydrocarbon group having 1 to 10 carbon atoms, more preferably contains a hydrocarbon group having 1 to 6 carbon atoms, and further preferably contains a hydrocarbon group having 1 to 4 carbon atoms.

[0104] Furthermore, from the viewpoint of further increasing the water contact angle, it is preferred that at least one R 1 It contains a hydrocarbon group having 3 to 4 carbon atoms, and more preferably contains a propyl group or a butyl group.

[0105] The silicon compound has at least three of the R 1Silane compounds having a structure formed by bonding one amino group to the group shown in the figure. As specific examples, for example, trimethylsilyldimethylamine, trimethylsilyldiethylamine, N-(trimethylsilyl)-tert-butylamine, hexamethyldisilazane, trimethylsilylpiperidine and N-(trimethylsilyl)imidazole and other trimethylsilylamines; compounds in which at least one trimethylsilyl group of the above trimethylsilylamine is replaced by any one of ethyldimethylsilyl, propyldimethylsilyl, butyldimethylsilyl, hexyldimethylsilyl, octyldimethylsilyl and decyldimethylsilyl (specifically: ethyldimethylsilyldimethylamine, propyldimethylsilyldimethylamine, butyldimethylsilyldimethylamine, hexyldimethylsilyldimethylamine, octyldimethylsilyldimethylamine and decyldimethylsilyldimethylamine, etc.) can be mentioned. These can be used alone or in combination of two or more.

[0106] Among them, from the viewpoint of the difficulty of deactivation of the silylating agent during vaporization (vapor stability), preferably selected from the group consisting of trimethylsilyldimethylamine, trimethylsilyldiethylamine, N-(trimethylsilyl)-tert-butylamine, hexamethyldisilazane, a compound in which at least one trimethylsilyl group of the above trimethylsilylamines (trimethylsilyldimethylamine, trimethylsilyldiethylamine, N-(trimethylsilyl)-tert-butylamine and hexamethyldisilazane) is an ethyldimethylsilyl group, At least one of the group consisting of a propyldimethylsilyl compound, a butyldimethylsilyl compound, a hexyldimethylsilyl compound, an octyldimethylsilyl compound, and a decyldimethylsilyl compound (specifically: ethyldimethylsilyldimethylamine, propyldimethylsilyldimethylamine, butyldimethylsilyldimethylamine, hexyldimethylsilyldimethylamine, octyldimethylsilyldimethylamine and decyldimethylsilyldimethylamine, etc.).

[0107] Furthermore, from the viewpoint of silylation reactivity, at least one selected from the group consisting of trimethylsilyldimethylamine, trimethylsilyldiethylamine and N-(trimethylsilyl)-tert-butylamine is more preferred.

[0108] Furthermore, from the viewpoint of further increasing the water contact angle, at least one selected from the group consisting of trimethylsilyldimethylamine, propyldimethylsilyldimethylamine, and butyldimethylsilyldimethylamine is preferred.

[0109] The lower limit of the content of the silylating agent in 100 mass % of the surface treatment composition is, for example, 0.3 mass % or more, preferably 1 mass % or more, and more preferably 2 mass % or more. Thus, the surface treatment composition can easily increase the water contact angle.

[0110] On the other hand, the upper limit of the content of the silylating agent in 100% by mass of the surface treatment composition is, for example, 30% by mass or less, preferably 25% by mass or less, more preferably 20% by mass or less, and further preferably 15% by mass or less. This can improve storage stability.

[0111] The lower limit of the content of the silicon compound in 100% by mass of the silylating agent is, for example, 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, further preferably 90% by mass or more, and further preferably 95% by mass or more. Thus, the surface treatment composition is easy to increase the water contact angle.

[0112] On the other hand, the upper limit of the content of the silicon compound in 100 mass % of the silylating agent is not particularly limited and may be 100 mass % or less. When a plurality of silylating agents are used in combination, it may be 98 mass % or less.

[0113] (Solvent)

[0114] The surface treatment composition contains one or more hydrocarbon solvents as solvents.

[0115] The hydrocarbon solvent includes hydrocarbons having 5 to 24 carbon atoms and being liquid at 1 atmosphere, and may be not only straight-chain hydrocarbons but also branched hydrocarbons or cyclic hydrocarbons. Furthermore, the hydrocarbons may have double bonds, and may have some of the hydrogen atoms substituted by halogen atoms.

[0116] Specific examples of the hydrocarbon solvent include: straight-chain saturated aliphatic hydrocarbons such as n-hexane, n-heptane, n-octane, n-nonane, n-decane, n-undecane, n-dodecane, n-tridecane, n-tetradecane, n-hexadecane, n-octadecane, and n-eicosane, and branched saturated aliphatic hydrocarbons having a carbon number corresponding to these aliphatic hydrocarbons such as cyclohexane, methylcyclohexane, ethylcyclohexane, propylcyclohexane, isopropylcyclohexane, butylcyclohexane, pentylcyclohexane, 1,1,3-trimethylcyclohexane, 1,1,4-trimethylcyclohexane, 1,2,3-trimethylcyclohexane, 1,2,4-trimethylcyclohexane, 1,3,5-trimethylcyclohexane, and decalin; and menthane. Cyclic hydrocarbons such as benzene, phenylbenzene, benzophenone ...

[0117] Among them, from the viewpoint of the ease of increasing the water contact angle, the hydrocarbon solvent is preferably at least one selected from the group consisting of 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, tert-butylbenzene, ethylbenzene, 1,3-bis(trifluoromethyl)benzene, 1,4-bis(trifluoromethyl)benzene, p-xylene, n-nonane and isododecane; more preferably at least one selected from the group consisting of 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, tert-butylbenzene, ethylbenzene, 1,3-bis(trifluoromethyl)benzene, 1,4-bis(trifluoromethyl)benzene and p-xylene.

[0118] It should be noted that the easiness of increasing the water contact angle is evaluated in the following manner as described later in the examples, etc.: liquid iPA is placed on the surface of a silicon wafer with a smooth thermal oxide film, vapor of the surface treatment composition is supplied thereto under specified conditions for 40 seconds, the sample is cleaned with iPA and dried to obtain a sample, the water contact angle is measured at 5 locations of the obtained sample, and the average value is used for evaluation.

[0119] Furthermore, from the viewpoint of easily suppressing the deviation of the water contact angle, the hydrocarbon solvent preferably contains aromatic hydrocarbons. Among the aromatic hydrocarbons, it is more preferable to contain at least one selected from the group consisting of 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, tert-butylbenzene, ethylbenzene, 1,3-bis(trifluoromethyl)benzene, 1,4-bis(trifluoromethyl)benzene and p-xylene.

[0120] The variation in water contact angle was evaluated based on the standard deviation calculated from the measurement results of water contact angles at five locations of the sample.

[0121] The solvent is included in the total amount of 100 mass % of the solvent, which is 75 mass % or more, preferably 80 mass % or more, more preferably 85 mass % or more, further preferably 90 mass % or more, further preferably 97 mass % or more, and further preferably 99 mass % or more of the hydrocarbon solvent. Thus, the surface treatment composition is easy to increase the water contact angle. By making the content of the hydrocarbon solvent in the solvent 97 mass % or more and using the above-mentioned preferred types of hydrocarbon solvents in combination, a higher water contact angle can be achieved and the deviation of the water contact angle can be suppressed.

[0122] In addition, the solvent may substantially contain only hydrocarbon solvents. It should be noted that the content of the hydrocarbon solvent may be 100% by mass. In this case, it is permitted to contain other solvents to an extent that cannot be detected.

[0123] If the solvent is 25% by mass or less, preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, further preferably 5% by mass or less, further preferably 3% by mass or less, further preferably 1% by mass or less in the total amount of the solvent (100% by mass), other solvents other than the aforementioned hydrocarbon solvent may also be contained. As other solvents, aprotic solvents are preferred, for example, esters, ketones, halogen-containing solvents (except halogenated hydrocarbons in which at least a portion of the hydrogen atoms of the aforementioned hydrocarbon solvent are substituted by halogen atoms such as fluorine atoms), derivatives of polyols without OH groups, etc., and propylene glycol monoethyl ether acetate (PGMEA) is preferably used.

[0124] (Surface treatment composition)

[0125] As an example of this embodiment, the total content of the silicon compound and the hydrocarbon solvent in 100 mass % of the surface treatment composition is, for example, 60 mass % or more, preferably 80 mass % or more, and more preferably 95 mass % or more. This makes it easy to increase the water contact angle.

[0126] Furthermore, the surface treatment composition may contain only a silylating agent and a hydrocarbon solvent, but preferably contains only the aforementioned silicon compound and a hydrocarbon solvent.

[0127] Furthermore, the boiling point difference between the boiling point of the solvent and the boiling point of the silylating agent (the boiling point of the solvent - the boiling point of the silylating agent) of the surface treatment composition at 1 atmosphere is, for example, 10°C or more, preferably 20°C or more, more preferably 30°C or more, further preferably 40°C or more, further preferably 50°C or more, further preferably 55°C or more. Thus, since the solvent with a high boiling point will preferentially gather on the surface of the wafer and replace with the cleaning solution, the silylating agent can be inhibited from being inactivated by contact with the cleaning solution, and as a result, the surface treatment composition is easy to increase the water contact angle. Furthermore, as long as the boiling point of the solvent is such that the silylating agent does not thermally decompose when vaporized, the above-mentioned boiling point difference is not particularly limited. For example, it can be set to below 200°C, below 180°C, below 150°C, below 130°C, or below 110°C.

[0128] For boiling points of a plurality of solvents and silylating agents, the boiling point of the component with the highest content (mass %) among the components contained in the solvent and silylating agent is used (if there are two or more components with the highest content, the boiling point of the one with the highest temperature is used).

[0129] The surface treatment composition preferably contains a small amount of water, and particularly preferably contains substantially no water.

[0130] In the scope that does not hinder the purpose of the present invention, the surface treatment composition of the present embodiment may include other components other than the above components. As such other components, for example, other silylating agents other than the above silicon compounds, other solvents other than hydrocarbon solvents, surfactants, and antioxidants such as BHT (butylated hydroxytoluene) can be cited.

[0131] The above-mentioned surface treatment composition can be constituted in the following manner: the above-mentioned surface treatment composition does not contain non-cyclic carbonate or the above-mentioned surface treatment composition 100 mass % comprises the non-cyclic carbonate below 2 mass %.By being set within the above-mentioned scope, storage stability can be improved.And, the above-mentioned surface treatment composition also can not contain non-cyclic carbonate in fact.It should be noted that, not containing in fact refers to, as long as for the degree that can not affect the performance of the above-mentioned surface treatment composition, for example, can be set to below 1 mass % in the surface treatment composition.

[0132] The surface treatment composition can be constituted as follows: it does not contain a catalyst, or the surface treatment composition contains 2% or less of a catalyst in 100% by mass. The catalyst promotes the reaction between the wafer surface and the silylating agent (the silicon compound). In addition, for the purpose of further improving storage stability, it may be substantially free of a catalyst. It should be noted that substantially free means that it is sufficient to not affect the performance of the surface treatment composition, for example, it can be set to less than 1% by mass in the surface treatment composition.

[0133] Examples of the catalyst include trimethylsilyl trifluoroacetate, trimethylsilyl trifluoromethanesulfonate, dimethylsilyl trifluoroacetate, dimethylsilyl trifluoromethanesulfonate, butyldimethylsilyl trifluoroacetate, butyldimethylsilyl trifluoromethanesulfonate, hexyldimethylsilyl trifluoroacetate, hexyldimethylsilyl trifluoromethanesulfonate, octyldimethylsilyl trifluoroacetate, octyldimethylsilyl trifluoromethanesulfonate, decyldimethylsilyl trifluoroacetate, decyldimethylsilyl trifluoromethanesulfonate, sulfonic acid, anhydride of the sulfonic acid, salt of the sulfonic acid, sulfonic acid derivatives, sulfonic acid esters, sulfonimides, sulfonimide derivatives, sulfonyl methides, sulfonyl methide derivatives, carboxyimidates, nitrogen-containing heterocyclic compounds, and silylated heterocyclic compounds.

[0134] The surface treatment composition of the present embodiment can be obtained by mixing the above-mentioned components.

[0135] If necessary, the obtained mixed solution may be purified using an adsorbent, a filter, etc. Alternatively, each component may be purified by distillation in advance and purified using an adsorbent, a filter, etc.

[0136] The surface treatment composition is constituted in the following manner: the water contact angle of the surface of the silicon wafer after the surface treatment measured by the following steps is, for example, more than 80°, more preferably 81° or more, more preferably 83° or more, further preferably 85° or more, further preferably 87° or more, further preferably 89° or more. It can be said that the larger the water contact angle, the easier it is for the surface treatment composition to increase the water contact angle.

[0137] (step)

[0138] The silicon wafer having a thermal oxide film layer on the surface was immersed in 1 mass % hydrofluoric acid at 25° C. for 10 minutes, immersed in pure water at 25° C. for 1 minute, and immersed in 2-propanol (iPA) at 25° C. for 1 minute to be cleaned.

[0139] The cleaned silicon wafer is placed horizontally in a state where liquid iPA is contained, and the vapor of the surface treatment composition is supplied to the silicon wafer.

[0140] Next, the vapor is changed into a liquid state on the surface of the silicon wafer, and the iPA retained on the surface is replaced with the liquid.

[0141] Next, the silicon wafer was immersed in iPA at 25° C. for 1 minute.

[0142] Afterwards, air is blown onto the silicon wafer to remove the iPA on the surface.

[0143] The water contact angle was measured using 2 μl of pure water on the surface of the silicon wafer obtained by the above process in accordance with JIS R 3257:1999 "Wettability test method for substrate glass surface". The measurement was performed at 5 locations on the silicon wafer sample, and the average value was used as the "water contact angle". In addition, the standard deviation calculated based on the measurement results of the water contact angles at the 5 locations was used as the "deviation of the water contact angle".

[0144] The surface treatment composition is constituted in such a manner that the number of particles larger than 0.2 μm measured by a light scattering liquid particle detector is, for example, 1.0×10 4 Less than 1.0×10 3 less than 1.0×10 2 This can suppress the risk of contamination in the vapor treatment apparatus or in the vaporization chamber that vaporizes the surface treatment composition, other liquid delivery parts, etc., and the reduction in device yield and reliability.

[0145] On the other hand, the number of the particles larger than 0.2 μm is preferably as small as possible, and may be one or more per 1 mL of the composition as long as the content is within the above-mentioned range.

[0146] The measurement of particles in the liquid phase of the surface treatment composition is performed using a commercially available measuring device in a light scattering liquid particle measurement method using a laser as a light source. The particle size of the particles refers to the light scattering equivalent diameter based on PSL (polystyrene latex) standard particles.

[0147] Microparticles refer to particles of dust, dirt, organic solids, inorganic solids, etc. contained as impurities in the materials of the various components of the surface treatment composition; or particles of dust, dirt, organic solids, inorganic solids, etc. introduced as contaminants during the preparation of the composition, which are equivalent to substances that ultimately do not dissolve in the composition and exist in the form of particles.

[0148] The surface treatment composition is constituted as follows: in the surface treatment composition, the total content of Na, Mg, Ca, Mn, Fe, Cu, Li, Al, Cr, Ni, Zn and Ag measured by inductively coupled plasma mass spectrometry is, for example, 100 mass ppb or less, preferably 10 mass ppb or less, and more preferably 1 mass ppb or less. This can suppress the risk of contamination in the steam treatment device and reduction in device yield and reliability.

[0149] On the other hand, as long as the total content is within the above range, each element may be contained in an amount of 0.0001 ppb by mass or more relative to the total amount of the composition.

[0150] Hereinafter, a method for producing a wafer using the surface treatment composition will be described.

[0151] The wafer manufacturing method of the present embodiment includes: a process of preparing a wafer having a concave-convex pattern on its surface; a process of supplying a cleaning liquid to the surface of the wafer and cleaning it; and a process of supplying the vapor of the above-mentioned surface treatment composition to the surface maintaining the cleaning liquid, so that the state of the above-mentioned vapor on the surface changes to liquid, and using the liquid to replace the above-mentioned cleaning liquid to form a water-repellent protective film on at least a portion of the surface.

[0152] In addition to the above steps, one or more of a pre-rinsing (first rinsing) step, a post-rinsing (second rinsing) step, a drying step, and a water-repellent protective film removal step may be performed.

[0153] As the surface treatment composition used in the wafer manufacturing method of the present embodiment, the same surface treatment composition as described above can be used.

[0154] Figures 1 to 4 This is an example of a process for producing a wafer using a surface treatment composition.

[0155] Figure 1 It is a schematic perspective view of a wafer 1 having a fine concavo-convex pattern 2 on its surface. Figure 2 It is shown Figure 1 A schematic cross-sectional view of a portion of the wafer 1 taken along the line aa'. Figure 3 This is a diagram showing a step of supplying vapor 9 of a composition to the recess 4 holding the liquid 8 . Figure 4 This is a diagram showing a step of cleaning the recessed portion 4 on which the water-repellent protective film 11 is formed from the composition with the liquid 10 .

[0156] First, a wafer 1 having a concavo-convex pattern on its surface is prepared.

[0157] In the preparation step of the wafer 1 , the following method can be used: This method is an example of a method of forming the concavo-convex pattern 2 on the wafer surface.

[0158] First, a resist is applied to the surface of the wafer, and then the resist is exposed through a resist mask, and the exposed resist or the unexposed resist is removed to produce a resist having a desired concave-convex pattern. In addition, a resist having a concave-convex pattern can be obtained by pressing a mold having a pattern against the resist. Next, the wafer is etched. At this time, the substrate surface corresponding to the concave portion of the resist pattern is selectively etched. Finally, the resist is stripped off to obtain a wafer 1 having a concave-convex pattern 2 on the surface.

[0159] The wafer on which the concavo-convex pattern 2 is formed and the materials of the concavo-convex pattern 2 are not particularly limited.

[0160] As a material of the wafer 1 , various wafers such as a silicon wafer, a silicon carbide wafer, a wafer composed of a plurality of components including silicon element, a sapphire wafer, and various compound semiconductor wafers can be used.

[0161] The material of the concavo-convex pattern 2 may include one or more selected from the group consisting of Si, Ti, Ge, W and Ru, oxides, nitrides, oxynitrides, carbonitrides and oxycarbides including one or more of these. For example, the material of the concavo-convex pattern 2 may include: silicon-based materials such as silicon oxide, silicon nitride, polycrystalline silicon, single crystal silicon, silicon germanium; metal-based materials such as titanium nitride, tungsten, ruthenium, tantalum nitride, tin; and materials formed by combining the above materials, resist (photoresist) materials, etc.

[0162] The concave-convex pattern 2 may be composed of a three-dimensional structure, for example, and the three-dimensional structure has: one or more structures arranged along the vertical direction of the surface, and / or one or more structures arranged along the horizontal direction orthogonal to the vertical direction. As an example of such a three-dimensional structure, at least a part of a logic device or a memory device may be constituted, for example, FinFET, nanowire FET, nanosheet FET or other multi-gate FET, three-dimensional memory cell, etc.

[0163] Figure 2 It is a cross-sectional view showing an example of the concavo-convex pattern 2 .

[0164] In this embodiment, the pattern size of the concavo-convex pattern 2 may be defined as: at least one width dimension in the in-plane direction of the surface, and / or at least one height dimension in the vertical direction relative to the surface.

[0165] In the cross-sectional structure (in the direction of substrate thickness) in the pattern of the concave-convex pattern 2, the pattern size of at least one of its width and height, or in the three-dimensional structure (3D coordinates of XYZ) in the pattern of the concave-convex pattern 2, the pattern size of at least one of its width (length in the X-axis direction), height (length in the Y-axis direction) and depth (length in the Z-axis direction) can be, for example, less than 30nm, less than 20nm, or less than 10nm. It can also be the interval between patterns. In the case of using a wafer 1 having such a fine concave-convex pattern 2, the surface treatment composition of this embodiment can also be applied.

[0166] Such a surface treatment composition is suitably used for surface treatment of a wafer 1 having a concavo-convex pattern 2 having a pattern size of 30 nm or less, preferably 20 nm or less, for example.

[0167] The aspect ratio of the convex portion 3 may be, for example, not less than 3, not less than 5, or not less than 10. Even in the concavo-convex pattern 2 having the convex portion 3 having a fragile structure, pattern collapse can be suppressed.

[0168] On the other hand, the aspect ratio of the projection 3 is not particularly limited and may be 100 or less.

[0169] The aspect ratio of the convex portion 3 is represented by a value obtained by dividing the height 6 of the convex portion by the width 7 of the convex portion.

[0170] Furthermore, the width 5 of the recessed portion may be, for example, 70 nm or less, and preferably 45 nm or less.

[0171] exist Figure 2 In the cross-sectional view of , the width 5 of the recess is represented by the interval between adjacent protrusions 3 and 3 .

[0172] Next, the surface of the wafer 1 is cleaned with a cleaning liquid.

[0173] In the cleaning step, the surface of the wafer 1 may be brought into contact with an aqueous cleaning solution which is one of cleaning liquids.

[0174] Examples of the aqueous cleaning solution include water, alcohol, aqueous ammonium hydroxide solution, aqueous tetramethylammonium solution, aqueous hydrofluoric acid solution, aqueous hydrochloric acid solution, aqueous hydrogen peroxide solution, aqueous sulfuric acid solution, and organic solvents, etc. These may be used alone or in combination of two or more.

[0175] The cleaning step may be performed once or twice or more before the surface treatment step or before the first rinse step described below. Other steps may be included between the multiple cleaning steps or between the cleaning step and the surface treatment step.

[0176] Next, if necessary, the surface of the wafer 1 may be brought into contact with a first rinse solution which is one of the cleaning liquids (a first rinse step).

[0177] As the first rinse solution, a cleaning solution different from the aqueous cleaning solution may be used, and examples thereof include water, an organic solvent, a mixture thereof, or a mixture of these with at least one of an acid, an alkali, a surfactant, and an oxidizing agent.

[0178] Examples of the organic solvent used in the first rinse solution include hydrocarbons, esters, ethers, ketones, halogen-containing solvents, sulfoxide-based solvents, alcohols, polyol derivatives, nitrogen-containing solvents, etc. Among them, as the organic solvent, it is preferred to use at least one selected from alcohols having 3 or less carbon atoms, such as methanol, 1-propanol, and 2-propanol (isopropanol).

[0179] Furthermore, multiple types of first rinsing solutions may be used. For example, rinsing may be performed in the order of a solution containing an acidic aqueous solution or an alkaline aqueous solution, and an organic solvent. Furthermore, an aqueous cleaning solution may be further added, and the washing may be performed in the order of a solution containing an acidic aqueous solution or an alkaline aqueous solution, an aqueous cleaning solution, and an organic solvent.

[0180] The first rinsing step may be performed once or twice or more after the cleaning step or before the surface treatment step. Other steps may be included between the plurality of first rinsing steps or between the first rinsing step and the surface treatment step.

[0181] The cleaning liquid can be supplied by a known method, for example, a single wafer method, which is represented by a cleaning method using a rotary cleaning device that cleans wafers one by one while the wafers are rotated almost horizontally and the cleaning liquid is supplied near the center of rotation; a batch method, which uses a cleaning device that cleans multiple wafers by immersing them in a cleaning tank. In addition, the cleaning liquid can also be supplied in the form of vapor, as in the surface treatment composition described later.

[0182] Thereby, the cleaning liquid can be retained in at least the concave portions 4 of the concavo-convex pattern 2 of the wafer 1 .

[0183] Next, while at least the concave portion 4 of the concave-convex pattern 2 is maintained with a cleaning liquid (liquid 8), vapor 9 of the surface treatment composition of the present embodiment is supplied to the surface of the concave-convex pattern, so that the vapor 9 changes its state into liquid 10 on the wafer surface, and the liquid 8 maintained in at least the concave portion 4 is replaced with liquid 10 and maintained, thereby forming a water-repellent protective film (protective film 11) on at least a portion of the wafer surface, for example, the surface of the concave portion 4.

[0184] When the vapor 9 of the surface treatment composition is supplied, the cleaning liquid (liquid 8) maintained on the wafer surface can be the above-mentioned aqueous cleaning solution or the first rinsing solution. From the viewpoint of manufacturing stability, the first rinsing solution is preferred, which may also contain 2-propanol (iPA). That is, as one method of manufacturing the wafer, the vapor 9 of the surface treatment composition can be supplied while the wafer surface is maintained with iPA.

[0185] Furthermore, the manufacturing method of the wafer includes a step of mixing the materials of the various components of the surface treatment composition, and the total amount of water in the aforementioned materials can be, for example, 2000 mass ppm or less, preferably 500 mass ppm or less, more preferably 100 mass ppm or less, and further preferably 50 mass ppm or less relative to the total amount of the materials. The less the total amount of water in the material, the easier it is to obtain a surface treatment composition that is easy to increase the water contact angle, so it is preferred.

[0186] As a method for supplying the vapor 9 of the surface treatment composition, for example, there can be cited a method in which a wafer 1 having a liquid 8 retained in at least the concave portion 4 of the concave-convex pattern 2 is arranged in a chamber, the surface treatment composition is separately evaporated, and the obtained vapor is supplied to the concave-convex pattern surface via a pipeline or a nozzle, etc. A carrier gas such as nitrogen or dry air can also be used when supplying the vapor.

[0187] However, the method of vaporizing the surface treatment composition is not particularly limited to the above method.

[0188] For example, a batch vaporization method can be cited, which is to introduce a specified amount of liquid surface treatment composition into a vaporization chamber, heat it sufficiently to evaporate all the surface treatment composition, and after all the vapor is evaporated, send the vapor 9 to the pipeline and nozzle to supply it to the above-mentioned concave-convex pattern surface.

[0189] In addition, for example, a continuous vaporization method can be cited, which is to add liquid drops of the surface treatment composition to a pre-heated small-scale vaporization section (for example, a heating means is provided in a part of a pipeline, etc.), so that all the surface treatment composition dropped each time is evaporated, and the vapor 9 is sent to the pipeline and nozzle to be supplied to the above-mentioned concave-convex pattern surface.

[0190] It is to be noted that the vaporization temperature is preferably suppressed to a temperature that does not cause a risk of thermal decomposition of the silylation agent, which is a protective film-forming component.

[0191] Preferred conditions for the steam treatment include: introducing nitrogen gas, and supplying the mixed gas to the surface of the concavo-convex pattern after the composition of the mixed gas of the steam obtained as described above and the nitrogen gas becomes constant.

[0192] The ambient temperature near the substrate being processed, i.e., the temperature of the vapor, is preferably lower than the boiling point of the liquid 8 held in the recessed portion 4. If this is satisfied, the liquid 8 can be prevented from volatilizing before the liquid 8 held in the recessed portion is replaced by the surface treatment composition, thereby easily suppressing the pattern collapse of the concave-convex pattern 2.

[0193] Figure 3 A schematic diagram showing a state in which the vapor 9 is supplied to the recess 4 holding the liquid 8 . Figure 4 This is a schematic diagram showing a state in which the recessed portions 4 of the water-repellent protective film 11 are formed by the surface treatment composition. Figure 3 , Figure 4 The schematic diagram of wafer 1 is shown Figure 1 Part of the a-a' section.

[0194] like Figure 3 , 4 As shown, the supplied vapor 9 changes state into liquid 10 in the recess 4, and the liquid 10 replaces the liquid 8 held in the recess 4, so that the liquid 10 is held in the recess 4. In addition, in order to promote or stabilize the above-mentioned state change, temperature adjustment such as lowering or maintaining constant the temperature of the wafer 1 or the recess 4 may be performed.

[0195] On the wafer surface, the silylating agent in the liquid 10 reacts with the wafer surface, and the site having the water-repellent functional group is fixed to the wafer surface, thereby forming a water-repellent protective film (protective film 11 ).

[0196] The protective film 11 does not necessarily need to be formed continuously or uniformly, but is more preferably formed continuously and uniformly in order to impart more excellent water repellency.

[0197] By replacing the liquid 8 held on the wafer surface such as the first rinse solution or the aqueous cleaning solution with the liquid 10 obtained by liquefying the vapor 9 of the surface treatment composition, it is possible to perform surface modification treatment, i.e., form a protective film 11, before the surface of the concavo-convex pattern 2 on the surface of the wafer 1 becomes dry. Thus, pattern collapse of the concavo-convex pattern 2 can be suppressed.

[0198] If necessary, the liquid 10 retained on the wafer surface may be subjected to known means such as heating, decompression, and drying to promote the formation of the protective film 11 .

[0199] Next, if necessary, the wafer surface on which the protective film 11 is formed may be brought into contact with a second rinsing solution (a second rinsing step).

[0200] As the second rinse solution, those exemplified as the first rinse solution can be used.

[0201] Furthermore, multiple types of second rinse solutions may be used. For example, water and an organic solvent such as isopropyl alcohol may be sequentially contacted for rinsing.

[0202] The second rinsing step may be performed once or twice or more after the surface treatment step. Other steps may be included between the multiple second rinsing steps or between the second rinsing step and the surface treatment step.

[0203] Next, after the protective film 11 is formed, a drying step of drying the surface of the wafer 1 may be performed as necessary.

[0204] The drying step can remove the liquid on the surface of the wafer 1 .

[0205] The liquid may include liquid 10, a second flushing solution, or a mixture of these.

[0206] As the drying means, for example, known means such as a spin drying method, iPA (2-propanol) vapor drying, Marangoni drying, heating drying, warm air drying, vacuum drying, and reduced pressure drying can be used.

[0207] The drying step may be performed once or twice or more, for example, after the surface treatment step and after the second rinsing step. It should be noted that the drying step and the second rinsing step may be repeated alternately.

[0208] Next, the protective film 11 on the surface of the wafer 1 may be removed (removal step).

[0209] As removal means, heating, UV irradiation, ozone exposure, plasma irradiation, corona discharge, etc. can be cited. In addition, treatment with concentrated fluids such as supercritical fluids (which may contain acids, alkalis, oxidants), steam treatment can also be carried out. These can be used alone or in combination of two or more. These treatments can be carried out under atmospheric pressure or under reduced pressure.

[0210] As described above, the wafer 1 (semiconductor substrate) using the surface treatment composition of the present embodiment can be obtained.

[0211] Figures 1 to 4 The manufacturing method shown is for wafer patterns, but the present invention is not limited thereto. The manufacturing method of the substrate of the present embodiment can also be for resist patterns, and the surface treatment composition of the present invention can be used in the cleaning / drying steps to suppress the collapse of the resist pattern.

[0212] The above-mentioned supply process has been described as a manufacturing method in which the supply process is performed after the cleaning process, but the present invention is not limited thereto and the supply process may be performed after various treatments are performed on the concavo-convex pattern 2 .

[0213] In the method for manufacturing the substrate, in addition to the above steps, one or more known treatments may be used in combination. For example, a surface treatment such as plasma treatment may be performed after the above removal step.

[0214] The embodiments of the present invention are described above, but these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are also included in the present invention.

[0215] Example

[0216] Hereinafter, examples are shown to more specifically disclose the embodiments of the present invention. However, the present invention is not limited to these examples.

[0217] [Example 1]

[0218] (Preparation of surface treatment composition)

[0219] Trimethylsilyldimethylamine (CH 3 ) 3 Si-N(CH 3 ) 2 〕(hereinafter referred to as "TMSDMA") and 95 g of tert-butylbenzene as a solvent were mixed to obtain a surface treatment composition (hereinafter referred to as "composition").

[0220] The compositions immediately after preparation were evaluated according to the following criteria. The results are shown in Table 1.

[0221] (Evaluation of Ease of Increasing Water Contact Angle of Composition (Evaluation of Contact Angle of Water-Repellent Protective Film Formed on Wafer Surface))

[0222] Making the surface of a wafer have a concavo-convex pattern and replacing the cleaning liquid retained in at least the concave portion of the concavo-convex pattern with another cleaning liquid is a technique that has been established through various studies in other documents, etc. In the present invention, the effect of imparting water repellency when the surface of the wafer is treated with vapor of a composition is evaluated.

[0223] However, in the case of a wafer having a concavo-convex pattern on its surface, it is impossible to accurately evaluate the contact angle of the protective film 11 (water-repellent protective film) itself formed on the concavo-convex pattern surface.

[0224] The contact angle of a water droplet is evaluated by adding a few μl of water droplets to the surface of the sample (substrate) and measuring the angle formed by the water droplet and the surface of the substrate, as described in JIS R 3257:1999 "Test method for wettability of substrate glass surface". However, in the case of a wafer with a pattern, the contact angle of the water droplet becomes very large. This is because the Wenzel effect or Cassie effect occurs, and the contact angle is affected by the surface shape (roughness) of the substrate, and the apparent contact angle of the water droplet increases.

[0225] Therefore, in this embodiment, the vapor of the above composition is supplied to a wafer with a smooth surface to form a protective film on the surface of the wafer. The protective film is regarded as a protective film formed on the surface of a wafer with a concavo-convex pattern formed on the surface, and the evaluation is performed in the following steps. It should be noted that in this embodiment, as a wafer with a smooth surface, a silicon wafer with SiO 2 A silicon wafer with a thermal oxide film.

[0226] (1) Cleaning silicon wafers

[0227] A silicon wafer with a smooth thermal oxide film of 2 cm square (Si wafer with a thermal oxide film layer of 1 μm thickness on the surface; manufactured by KYODO INTERNATIONAL) was immersed in a 1 mass % hydrofluoric acid aqueous solution at 25°C for 10 minutes, immersed in pure water at 25°C for 1 minute, and then immersed in 2-propanol (hereinafter referred to as "iPA") at 25°C for 1 minute.

[0228] (2) Surface treatment of silicon wafers using steam

[0229] After the cleaning, the silicon wafer was horizontally placed in a vapor treatment chamber containing liquid iPA, and the solution composition prepared above was vaporized under the following vapor supply conditions, and the vapor was supplied to the vapor treatment chamber.

[0230] Then, the state of the vapor supplied to the wafer surface at 50° C. or lower is changed to liquid, and the iPA retained on the wafer surface is replaced with the liquid.

[0231] The vapor supply conditions of the above composition are: in a vaporization chamber heated to 165°C, at a rate of 2 dm 3 / min flow of nitrogen, while the above-prepared solution composition was added dropwise at a drop rate of 0.01 g / sec, and the entire amount added was vaporized. The vapor was immediately supplied to the steam treatment chamber in the form of a nitrogen gas stream. The treatment was performed for 40 seconds.

[0232] (3) Cleaning silicon wafer

[0233] After that, the silicon wafer was taken out from the vapor treatment chamber and immersed in iPA for 1 minute at 25° C. Finally, the silicon wafer was taken out from iPA and air was blown to remove the iPA on the surface.

[0234] Through the above, a silicon wafer having a protective film formed on the surface is obtained.

[0235] (4) Determination of water contact angle of protective film

[0236] 2 μl of pure water was placed on the surface of the wafer with a protective film formed thereon. In accordance with JIS R 3257:1999 "Wettability test method for glass substrate surfaces", the angle (water contact angle) formed by water droplets and the wafer surface at 5 locations was measured using a contact angle meter (manufactured by Kyowa Interface Science: CA-X model), and the average value and standard deviation (deviation of the water contact angle within the wafer surface) were calculated.

[0237] It should be noted that the contact angle of the surface of the silicon wafer subjected to the treatments (1) and (3) but without the above-mentioned (2) and without the protective film formed on the surface was less than 10°.

[0238] [Table 1]

[0239] Table 1

[0240]

[0241] [Example 2 to Example 31 and Comparative Example 1 to Comparative Example 2]

[0242] Except for using the solvents listed in Table 1, compositions were prepared in the same manner as in Example 1 and various evaluations were performed. The results are shown in Table 1. In Table 1, the boiling point difference between the silylating agent and the solvent was calculated using known literature values ​​or catalog values, and "-" indicates that there is no literature value and it is not calculated. In addition, "-" for the deviation of the water contact angle indicates that it was not measured.

[0243] It should be noted that the solvent of Example 24 is a mixed solvent of 60% by mass of 1,2,4-trimethylbenzene and 40% by mass of isododecane in the total amount of the solvent, the solvent of Example 25 is a mixed solvent of 60% by mass of 1,3,5-trimethylbenzene and 40% by mass of isododecane, the solvent of Example 26 is a mixed solvent of 60% by mass of tert-butylbenzene and 40% by mass of isododecane, the solvent of Example 27 is a mixed solvent of 98% by mass of 1,2,4-trimethylbenzene and 2% by mass of propylene glycol monoethyl ether acetate (PGMEA), the solvent of Example 28 is a mixed solvent of 80% by mass of 1,2,4-trimethylbenzene and 20% by mass of PGMEA, the solvent of Example 29 is a mixed solvent of 98% by mass of tert-butylbenzene and 2% by mass of PGMEA, and the solvent of Example 30 is a mixed solvent of 80% by mass of tert-butylbenzene and 20% by mass of PGMEA. The solvent of Comparative Example 1 is a mixed solvent of 47 mass % of propylene carbonate and 53 mass % of diethyl carbonate in the total amount of the solvent, and the solvent of Comparative Example 2 is a mixed solvent of 70 mass % of 1,2,4-trimethylbenzene and 30 mass % of PGMEA in the total amount of the solvent.

[0244] Furthermore, the silylating agent in Examples 4 and 6 is propyldimethylsilyldimethylamine "PDMSDMA:CH 3 CH 2 CH 2 )(CH 3 ) 2 Si-N(CH 3 ) 2 The silylating agent in Example 5 and Example 7 is butyldimethylsilyldimethylamine "BDMSDMA: (CH 3 CH 2 CH 2 CH 2 )(CH 3 ) 2 Si-N(CH 3 ) 2 ”.

[0245] Since the water contact angles (average value) of the surface treatment compositions of Examples 1 to 31 are larger than those of Comparative Examples 1 and 2, it can be said that the surface treatment compositions of the present invention are more likely to increase the water contact angle than conventional compositions.

[0246] Furthermore, in the above-mentioned embodiments, when 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, tert-butylbenzene, ethylbenzene, 1,3-bis(trifluoromethyl)benzene, 1,4-bis(trifluoromethyl)benzene, p-xylene, n-nonane or isododecane is used as the solvent, the water contact angle is more likely to be increased.

[0247] Furthermore, in the above embodiments, when 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, tert-butylbenzene, ethylbenzene, 1,3-bis(trifluoromethyl)benzene, 1,4-bis(trifluoromethyl)benzene or p-xylene is used as the solvent, not only a higher water contact angle is obtained, but also the deviation of the water contact angle is 2.0 less than the standard deviation.

[0248] This application claims the benefit of priority based on Japanese patent application No. 2022-065098 filed on April 11, 2022 and Japanese patent application No. 2022-128657 filed on August 12, 2022, the disclosures of which are incorporated herein in their entirety.

[0249] Description of Reference Numerals

[0250] 1 Wafer

[0251] 2 Concave and convex pattern

[0252] 3 convex part

[0253] 4 concavity

[0254] 5 Width of concave portion

[0255] 6 Height of convex part

[0256] 7 Width of convex part

[0257] 8 Liquid

[0258] 9 Steam

[0259] 10 Liquid

[0260] 11. Protective film

Claims

1. A surface treatment composition for supplying in the form of vapor to a surface of a wafer having a concavo-convex pattern on the surface and forming a water-repellent protective film on the surface, the surface treatment composition comprising a silylating agent and a solvent, The silylating agent comprises a silicon compound represented by formula (1), (R 1 )3Si-X(1) in, R 1 are each independently a group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, and a hydrocarbon group having 1 to 10 carbon atoms in which a part or all of the hydrogen atoms are substituted with fluorine atoms, X is an amino group, The solvent contains 75% by mass or more of a hydrocarbon solvent in 100% by mass of the total amount of the solvent.

2. The surface treatment composition according to claim 1, wherein The content of the hydrocarbon solvent is 97% by mass or more in 100% by mass of the total amount of the solvent.

3. The surface treatment composition according to claim 1 or 2, wherein: The hydrocarbon solvent includes an aromatic hydrocarbon.

4. The surface treatment composition according to any one of claims 1 to 3, wherein The content of the silylating agent is 0.3 mass % or more and 30 mass % or less in 100 mass % of the surface treatment composition.

5. The surface treatment composition according to any one of claims 1 to 4, wherein The boiling point difference between the boiling point of the solvent and the boiling point of the silylating agent (the boiling point of the solvent - the boiling point of the silylating agent) is 20° C. or more at 1 atmosphere.

6. The surface treatment composition according to any one of claims 1 to 5, wherein The silicon compound comprises one or more selected from the group consisting of trimethylsilyldimethylamine, trimethylsilyldiethylamine, N-(trimethylsilyl)-tert-butylamine, and hexamethyldisilazane, and compounds in which at least one trimethylsilyl group of these trimethylsilylamines is substituted by any one of ethyldimethylsilyl, propyldimethylsilyl, butyldimethylsilyl, hexyldimethylsilyl, octyldimethylsilyl, and decyldimethylsilyl.

7. The surface treatment composition according to any one of claims 1 to 6, wherein The water contact angle of the surface of the silicon wafer after surface treatment measured by the following steps exceeds 80°. (step) A smooth silicon wafer having a thermal oxide film on its surface was immersed in a 1 mass % hydrofluoric acid aqueous solution at 25°C for 10 minutes, immersed in pure water at 25°C for 1 minute, and immersed in 2-propanol (iPA) at 25°C for 1 minute, and cleaned. The cleaned silicon wafer is horizontally arranged in a state containing liquid iPA, and the vapor of the surface treatment composition is supplied to the silicon wafer. Next, the vapor is changed into a liquid state on the surface of the silicon wafer, and the iPA retained on the surface is replaced with the liquid. Next, the silicon wafer was immersed in iPA at 25° C. for 1 minute. Afterwards, air is blown to the silicon wafer to remove the iPA on the surface. 2 μl of pure water was applied to the surface of the silicon wafer obtained through the above steps, and the water contact angle was measured in accordance with JIS R 3257:1999 "Test methods for wettability of glass substrate surfaces".

8. The surface treatment composition according to any one of claims 1 to 7, wherein The surface treatment composition does not contain acyclic carbonate, or contains 2 mass % or less of acyclic carbonate in 100 mass % of the surface treatment composition.

9. The surface treatment composition according to any one of claims 1 to 8, wherein The surface treatment composition does not contain a catalyst, or contains a catalyst in an amount of 2 mass % or less in 100 mass % of the surface treatment composition.

10. The surface treatment composition according to any one of claims 1 to 9, wherein The number of particles larger than 0.2 μm measured by a light scattering liquid particle detector was 1.0×10 4 Less than .

11. The surface treatment composition according to any one of claims 1 to 10, wherein The total content of Na, Mg, Ca, Mn, Fe, Cu, Li, Al, Cr, Ni, Zn and Ag in the surface treatment composition measured using inductively coupled plasma mass spectrometry is 100 mass ppb or less.

12. A method for manufacturing a wafer, comprising the following steps: A process of preparing a wafer having a concavo-convex pattern on its surface; A step of supplying a cleaning liquid to the surface of the wafer to clean the surface; and supplying vapor of a surface treatment composition to the surface holding the cleaning liquid, changing the state of the vapor to liquid on the surface, replacing the cleaning liquid with the liquid, and forming a water-repellent protective film on at least a portion of the surface, The surface treatment composition comprises a silylating agent and a solvent, The silylating agent comprises a silicon compound represented by formula (1), (R 1 )3Si-X(1) in, R 1 are each independently a group selected from the group consisting of a hydrocarbon group having 1 to 10 carbon atoms, and a hydrocarbon group having 1 to 10 carbon atoms in which a part or all of the hydrogen atoms are substituted with fluorine atoms, X is an amino group, The solvent contains 75% by mass or more of a hydrocarbon solvent in 100% by mass of the total amount of the solvent.

13. The method for manufacturing a wafer according to claim 12, wherein: The content of the hydrocarbon solvent is 97% by mass or more in 100% by mass of the total amount of the solvent.

14. The method for manufacturing a wafer according to claim 12 or 13, wherein: In the surface treatment composition, the hydrocarbon solvent includes an aromatic hydrocarbon.

15. The method for manufacturing a wafer according to any one of claims 12 to 14, wherein: In the surface treatment composition, the content of the silylating agent is 0.3 mass % or more and 30 mass % or less based on 100 mass % of the surface treatment composition.

16. The method for manufacturing a wafer according to any one of claims 12 to 15, wherein: In the surface treatment composition, the boiling point difference between the boiling point of the solvent and the boiling point of the silylating agent (the boiling point of the solvent - the boiling point of the silylating agent) is 20° C. or more at 1 atmosphere.

17. The method for manufacturing a wafer according to any one of claims 12 to 16, wherein: In the surface treatment composition, the silicon compound includes one or more selected from the group consisting of trimethylsilyldimethylamine, trimethylsilyldiethylamine, N-(trimethylsilyl)-tert-butylamine, and hexamethyldisilazane, and compounds in which at least one trimethylsilyl group of these trimethylsilylamines is substituted with any one of ethyldimethylsilyl, propyldimethylsilyl, butyldimethylsilyl, hexyldimethylsilyl, octyldimethylsilyl, and decyldimethylsilyl.

18. The method for manufacturing a wafer according to any one of claims 12 to 17, wherein: The surface treatment composition does not contain acyclic carbonate, or contains 2 mass % or less of acyclic carbonate in 100 mass % of the surface treatment composition.

19. The method for manufacturing a wafer according to any one of claims 12 to 18, wherein: The surface treatment composition does not contain a catalyst, or contains a catalyst in an amount of 2 mass % or less in 100 mass % of the surface treatment composition.

20. The method for manufacturing a wafer according to any one of claims 12 to 19, wherein: In the surface treatment composition, the number of particles larger than 0.2 μm measured by a light scattering liquid particle detector is 1.0×10 4 Less than .

21. The method for manufacturing a wafer according to any one of claims 12 to 20, wherein: In the surface treatment composition, the total content of Na, Mg, Ca, Mn, Fe, Cu, Li, Al, Cr, Ni, Zn and Ag measured by inductively coupled plasma mass spectrometry is 100 mass ppb or less in the surface treatment composition.

22. The method for manufacturing a wafer according to any one of claims 12 to 21, wherein: The vapor of the surface treatment composition is supplied while the iPA is maintained on the surface of the wafer.

23. The method for manufacturing a wafer according to any one of claims 12 to 22, wherein: The wafer manufacturing method includes a step of mixing materials of the respective components of the surface treatment composition, wherein the total amount of water in the materials is 2000 mass ppm or less relative to the total amount of the materials.