Organic molecule modified gold nanocluster as well as preparation method and application thereof
The gold nanoclusters modified by organic molecules have good inhibitory effects on DAAO, solving the complex problem of DAAO inhibitor synthesis in the prior art, and providing a simple preparation method and a solution with wide application prospects.
Patent Information
- Application Number
- CN202411097951.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
Nanomaterials with DAAO inhibitory effect are rare in the prior art, and the synthesis and purification methods of DAAO inhibitors are complex, making it difficult to meet the needs of biomedical applications.
Gold nanoclusters modified by organic molecules are prepared by reducing chloroatric acid, organic molecules and reducing agent in water to obtain gold nanoclusters with good DAAO inhibition effect, including L-penicillamine and D-cyanium. Gold nanoclusters modified by mycamine, racemic penicillamine, L-cysteine, D-cysteine, etc.
Effective inhibition of DAAO activity is achieved, the preparation method is simple, and it has broad application prospects, especially in analgesics and improving morphine tolerance.
Smart Images

Figure CN118987270A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanomaterials, and in particular to an organic molecule-modified gold nanocluster and a preparation method and application thereof. Background Art
[0002] Chirality refers to the phenomenon that a molecule cannot overlap with its mirror image. Molecules with chirality are called chiral molecules. Chiral molecules have two structures, which can be recorded as D-type and L-type. Amino acids, glucose, and many drug molecules have chirality. Although D-type and L-type molecules have the same molecular formula, their physiological activities or efficacy are different. The amino acids in the human body are mainly L-type amino acids, but a small amount of D-type amino acids also have unique physiological effects.
[0003] D-Amino acid oxidase (DAAO) can specifically catalyze the degradation of D-amino acids (D-alanine, D-proline, D-serine, etc.), causing them to undergo oxidative deamination and produce α-keto acid, ammonia, and hydrogen peroxide. D-serine is an N-methyl-D-aspartate (NMDA) receptor agonist that can improve negative symptoms and cognitive impairment in schizophrenia. However, DAAO can degrade D-serine in the body, resulting in a decrease in D-serine concentration, and the hydrogen peroxide produced during the degradation process can also cause neurotoxicity, nephrotoxicity, and other side effects.
[0004] DAAO inhibitors can reduce DAAO activity, alleviate the degradation of D-serine, and maintain the D-serine content in the body at an appropriate level. In addition, with the gradual deepening of research on DAAO inhibitors in analgesia in recent years, it has been found that DAAO inhibitors can not only effectively inhibit chronic pain, but also improve the tolerance of morphine. Therefore, DAAO inhibitors have a very broad application prospect.
[0005] At present, DAAO inhibitors can be divided into three categories according to their structures, namely aromatic carboxylic acids, benzisoxazoles and α-hydroxyketones. For example, Chinese patent CN1922157A provides a benzo[d]isoxazole-3-ol DAAO inhibitor, and Chinese patent CN103748079A discloses a pyridazinone mixture and its use as a DAAO inhibitor. The above DAAO inhibitors are all organic molecules, and the synthesis and purification methods are relatively complicated.
[0006] With the development of science and technology, materials science and biomedicine are becoming more and more closely integrated. Nanomaterials have made great achievements in biological applications and have shown good development momentum and huge development potential. However, nanomaterials with DAAO inhibitory effects are very rare in this field. Summary of the invention
[0007] In view of this, the present invention provides an organic molecule-modified gold nanocluster and a preparation method and application thereof. The organic molecule-modified gold nanocluster provided by the present invention has a good inhibitory effect on the activity of DAAO, and the preparation method is simple and has broad application prospects.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] An organic molecule-modified gold nanocluster comprises a gold nanocluster and an organic molecule modified on the gold nanocluster; the organic molecule is one or more of L-penicillamine, D-penicillamine, racemic penicillamine, L-cysteine, D-cysteine and racemic cysteine.
[0010] Preferably, the average particle size of the gold nanoclusters modified by organic molecules is 2.0 to 2.5 nm.
[0011] The present invention also provides a method for preparing the gold nanoclusters modified by organic molecules described in the above scheme, comprising the following steps:
[0012] Chloroauric acid, organic molecules, a reducing agent and water are mixed to carry out a reduction reaction, thereby obtaining gold nanoclusters modified with the organic molecules.
[0013] Preferably, the molar ratio of chloroauric acid to organic molecules is 1:(1.5-4).
[0014] Preferably, the reducing agent is borane tert-butylamine complex or sodium borohydride.
[0015] Preferably, when the organic molecule is one or more of L-penicillamine, D-penicillamine and racemic penicillamine, the reducing agent is a borane tert-butylamine complex; the molar ratio of the chloroauric acid to the borane tert-butylamine complex is 1:(1-2);
[0016] When the reducing agent is borane tert-butylamine complex, the reduction reaction time is 10 to 120 minutes.
[0017] Preferably, when the organic molecule is one or more of L-cysteine, D-cysteine and racemic cysteine, the reducing agent is sodium borohydride; and the molar ratio of chloroauric acid to sodium borohydride is 1:(150-450).
[0018] Preferably, when the reducing agent is sodium borohydride, sodium hydroxide is also added during the mixing; the molar ratio of chloroauric acid to sodium hydroxide is 1:(15-65);
[0019] When the reducing agent is sodium borohydride, the reduction reaction time is 10 to 180 minutes.
[0020] Preferably, after the reduction reaction is completed, the process further comprises freeze-drying the obtained reaction solution to obtain gold nanocluster powder modified with organic molecules.
[0021] The present invention also provides the use of the gold nanoclusters modified with organic molecules described in the above scheme or the gold nanoclusters modified with organic molecules prepared by the preparation method described in the above scheme in the preparation of D-amino acid oxidase inhibitors.
[0022] The present invention provides a gold nanocluster modified with an organic molecule, comprising a gold nanocluster and an organic molecule modified on the gold nanocluster; the organic molecule is one or more of L-penicillamine (L-Pen), D-penicillamine (D-Pen), racemic penicillamine (DL-Pen), L-cysteine (L-Cys), D-cysteine (D-Cys) and racemic cysteine (DL-Cys). The present invention uses organic molecules to modify the gold nanocluster, and the modified gold nanocluster has a good inhibitory effect on DAAO. The results of the embodiment show that the inhibitory effect of the gold nanoclusters modified by organic molecules on DAAO is related to the concentration and volume. When the amount of the gold nanoclusters modified by organic molecules is 500 μL (the concentration of the gold nanoclusters modified by organic molecules in the dispersion is 0.83 mg / mL), the DAAO inhibition rate of the gold nanoclusters modified by L-Pen (Au@L-Pen) is 92.3%, the DAAO inhibition rate of the gold nanoclusters modified by DL-Pen (Au@DL-Pen) is 92.1%, and the DAAO inhibition rate of the gold nanoclusters modified by D-Pen (Au@D-Pen) is 92.1%. The inhibition rate is 75.6%; when the dosage of the organic molecule modified gold nanocluster dispersion is 500 μL (the molar concentration of the gold element in the dispersion is 0.1 mmol / L), the inhibition rate of L-Cys modified gold nanocluster (Au@L-Cys) on DAAO is 65.6%, and the inhibition rate of D-Cys modified gold nanocluster (Au@D-Cys) on DAAO is 22.9%; and, among them, the gold nanoclusters modified with L-Pen and L-Cys have the best inhibitory effect on DAAO, indicating that the inhibitory effect of gold nanoclusters on DAAO is related to the chiral structure of organic molecules.
[0023] The present invention also provides a method for preparing the gold nanoclusters modified by organic molecules described in the above scheme. The preparation method provided by the present invention has simple steps and is easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the transmission electron microscopy (TEM) image of the Au@D-Pen prepared in Example 1;
[0025] Figure 2This is an X-ray photoelectron spectroscopy (XPS) graph of the Au@D-Pen cluster prepared in Example 1;
[0026] Figure 3 Circular dichroism (CD) spectra of Au@D-Pen, Au@L-Pen and Au@DL-Pen prepared in Example 1;
[0027] Figure 4 This is a schematic diagram of the principle of evaluating the DAAO inhibitory effect of the present invention;
[0028] Figure 5 The UV-visible absorption spectra of the products without adding gold nanoclusters (purple line), adding Au@L-Pen (black line), adding Au@D-Pen (red line) and adding Au@DL-Pen (blue line);
[0029] Figure 6 This is the transmission electron microscopy (TEM) image of Au@D-Cys prepared in Example 2;
[0030] Figure 7 Circular dichroism (CD) spectra of Au@D-Cys and Au@L-Cys samples prepared in Example 2. DETAILED DESCRIPTION
[0031] The present invention provides a gold nanocluster modified with an organic molecule, comprising a gold nanocluster and an organic molecule modified on the gold nanocluster; the organic molecule is one or more of L-penicillamine, D-penicillamine, racemic penicillamine, L-cysteine, D-cysteine and racemic cysteine.
[0032] In the present invention, the average particle size of the gold nanoclusters modified by organic molecules is preferably 2.0 to 2.5 nm.
[0033] The present invention also provides a method for preparing the gold nanoclusters modified by organic molecules described in the above scheme, comprising the following steps:
[0034] Chloroauric acid, organic molecules, a reducing agent and water are mixed to carry out a reduction reaction, thereby obtaining gold nanoclusters modified with the organic molecules.
[0035] In the present invention, the molar ratio of the chloroauric acid to the organic molecule is preferably 1:(1.5-4), more preferably 1:(2-3); the reducing agent is preferably borane tert-butylamine complex or sodium borohydride.
[0036] In the present invention, when the organic molecule is one or more of L-penicillamine, D-penicillamine and racemic penicillamine, the reducing agent is preferably a borane tert-butylamine complex; the molar ratio of chloroauric acid to the borane tert-butylamine complex is preferably 1:(1-2), more preferably 1:(1-1.5).
[0037] In the present invention, when the reducing agent is a borane tert-butylamine complex, the mixing preferably includes: first mixing chloroauric acid, an organic molecule and a borane tert-butylamine complex with water respectively to obtain an aqueous solution of chloroauric acid, an aqueous solution of an organic molecule and an aqueous solution of a borane tert-butylamine complex, and then mixing the aqueous solution of chloroauric acid, the aqueous solution of an organic molecule and the aqueous solution of a borane tert-butylamine complex; the concentration of the aqueous solution of chloroauric acid is preferably 4 mmol / L, the solubility of the aqueous solution of an organic molecule is preferably 100 mmol / L, and the concentration of the aqueous solution of a borane tert-butylamine complex is preferably 100 mmol / L.
[0038] In the present invention, when the reducing agent is borane tert-butylamine complex, the time of the reduction reaction is preferably 10 to 120 min, more preferably 30 to 60 min; the temperature of the reduction reaction is preferably room temperature.
[0039] In the present invention, when the organic molecule is one or more of L-cysteine, D-cysteine and racemic cysteine, the reducing agent is preferably sodium borohydride; the molar ratio of chloroauric acid to sodium borohydride is preferably 1:(150-450), more preferably 1:(200-300); in a specific embodiment of the present invention, the sodium borohydride is preferably used in the form of a sodium borohydride solution, and the preparation method of the sodium borohydride solution is preferably: dissolving sodium borohydride powder in a sodium hydroxide solution to obtain a sodium borohydride solution; the concentration of the sodium hydroxide solution used to dissolve the sodium borohydride powder is preferably 0.2 mol / L, and the amount ratio of the sodium borohydride powder to the sodium hydroxide solution is preferably 40-50 mg:10 mL; when calculating the molar ratio of chloroauric acid to sodium hydroxide, the sodium hydroxide used to prepare the sodium borohydride solution is not counted.
[0040] In the present invention, when the reducing agent is sodium borohydride, sodium hydroxide is preferably added during the mixing; the molar ratio of chloroauric acid to sodium hydroxide is preferably 1:(15-65), more preferably 1:(20-50).
[0041] In the present invention, when the reducing agent is sodium borohydride, the mixing preferably includes: first mixing chloroauric acid, organic molecules, sodium hydroxide and water respectively to obtain chloroauric acid aqueous solution, organic molecule aqueous solution and sodium hydroxide aqueous solution; mixing the chloroauric acid aqueous solution and the organic molecule aqueous solution, then adding sodium hydroxide aqueous solution, and then adding sodium borohydride solution dropwise.
[0042] In the present invention, when the reducing agent is sodium borohydride, the time of the reduction reaction is preferably 10 to 180 min, more preferably 30 to 120 min; the temperature of the reduction reaction is preferably room temperature.
[0043] In the present invention, after the reduction reaction is completed, the obtained reaction solution is a dispersion of gold nanoclusters modified by organic molecules, wherein the concentration of gold nanoclusters modified by organic molecules is preferably 0.5 to 4 mmol / L (calculated as the molar concentration of gold element).
[0044] In the present invention, after the reduction reaction is completed, it is preferred to further include freeze-drying the obtained reaction solution to obtain organic molecule-modified gold nanocluster powder; the present invention has no special requirements for the freeze-drying conditions, and the conditions familiar to those skilled in the art can be used. In a specific embodiment of the present invention, when used, the organic molecule-modified gold nanocluster powder is preferably dispersed in a PBS solution to prepare a high-concentration organic molecule-modified gold nanocluster solution; the concentration of the high-concentration organic molecule-modified gold nanocluster solution is preferably 0.8-0.9 mg / mL, more preferably 0.83 mg / mL.
[0045] The present invention also provides the use of the gold nanoclusters modified with organic molecules described in the above scheme or the gold nanoclusters modified with organic molecules prepared by the preparation method described in the above scheme in the preparation of D-amino acid oxidase inhibitors (DAAO inhibitors); the present invention has no special requirements for the application, and methods familiar to those skilled in the art can be used.
[0046] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Example 1
[0048] A chloroauric acid aqueous solution (concentration of 4 mmol / L), an L-penicillamine (L-Pen) aqueous solution (concentration of 100 mmol / L) and a borane tert-butylamine complex aqueous solution (concentration of 100 mmol / L) were mixed, wherein the amount of the chloroauric acid aqueous solution was 2.6 mL, the molar ratio of chloroauric acid to L-penicillamine was 1:2, and the molar ratio of chloroauric acid to borane tert-butylamine complex was 1:1.5; the mixture was reacted at room temperature for 30 min to obtain a dispersion of L-penicillamine-modified gold nanoclusters (denoted as Au@L-Pen) with a concentration of 3.3 mmol / L (calculated as the molar concentration of the gold element).
[0049] L-penicillamine was replaced by D-penicillamine (D-Pen), and a dispersion of D-penicillamine-modified gold nanoclusters was prepared using the same method. The sample was denoted as Au@D-Pen, and the concentration was 3.3 mmol / L (calculated as the molar concentration of the gold element).
[0050] Equal amounts of L-penicillamine and D-penicillamine were mixed to prepare a racemic penicillamine (DL-Pen) solution. L-penicillamine was replaced with DL-penicillamine (DL-Pen), and a dispersion of DL-penicillamine-modified gold nanoclusters was prepared in the same manner. The sample was recorded as Au@DL-Pen, and the concentration was 3.3 mmol / L (calculated as the molar concentration of the gold element).
[0051] Sample characterization:
[0052] Figure 1 This is a transmission electron microscope (TEM) image of the Au@D-Pen prepared in Example 1. Figure 1 It can be seen that the average particle size of Au@D-Pen is about 2.1 nm.
[0053] Figure 2 This is the X-ray photoelectron spectroscopy (XPS) diagram of the Au@D-Pen cluster prepared in Example 1. Figure 2 It can be seen that the sample contains Au, S, C, O, and N elements, indicating that D-Pen has been modified on the surface of gold nanoclusters.
[0054] Figure 3 Circular dichroism (CD) spectra of Au@D-Pen, Au@L-Pen and Au@DL-Pen prepared in Example 1. Figure 3 It can be seen that Au@D-Pen exhibits negative, positive, and negative CD signals in the wavelength ranges of 200-250nm, 250-300nm, and 300-400nm, respectively. Au@L-Pen also exhibits CD signals in the above wavelength ranges, but the signal values are opposite to those of Au@D-Pen, indicating that Au@D-Pen and Au@L-Pen clusters have chiral characteristics. The Au@DL-Pen sample does not exhibit a CD signal.
[0055] Test Example 1
[0056] The DAAO inhibitory effect of the gold nanoclusters modified with organic molecules prepared in Example 1 was evaluated. The inhibitory effect evaluation principle is as follows: DAAO oxidizes D-alanine (D-Ala) to D-pyruvic acid. After adding 2,4-dinitrophenylhydrazine (DNP) and NaOH, D-pyruvic acid is converted into phenylhydrazone products, which have a characteristic absorption peak at a wavelength of 530 nm. The absorbance value (A530) of the absorption peak is used to evaluate the DAAO activity; after adding the gold nanoclusters modified with organic molecules in the present invention, the DAAO activity is inhibited and the A530 value is reduced; in the present invention, the A530 value of adding Au@L-Pen is less than the A530 value of adding Au@D-Pen; Figure 4 Schematic diagram of the principle of evaluating the DAAO inhibitory effect of the present invention.
[0057] The test method for the inhibitory effect of DAAO is as follows:
[0058] The organic molecule modified gold nanocluster dispersion prepared in Example 1 was diluted 10 times with PBS buffer solution (pH = 7.4), and a certain volume (500 μL or 50 μL) of the diluted dispersion was mixed with 20 μL DAAO solution (10 U / mL), and incubated at 37°C for 30 minutes. Then 2 mL of D-alanine (D-Ala) solution (1 mmol / L) was added to the above solution and incubated at 37°C for 30 minutes. Then 2,4-dinitrophenylhydrazine (DNP) solution (1 mmol / L) and sodium hydroxide solution (1.5 mol / L) were added in sequence, and after incubation in a constant temperature water bath at 37°C for 10 minutes, the UV-visible absorption spectrum of the final product was measured, and the absorbance value A at 530 nm was recorded.
[0059] The calculation method of DAAO inhibition efficiency is shown in Formula I:
[0060]
[0061] In formula I: I x represents the DAAO inhibition rate;
[0062] x represents a chiral configuration identifier of an organic molecule (e.g., x=D represents D-penicillamine, x=L represents L-penicillamine, and x=DL represents DL-penicillamine);
[0063] A o is the absorbance value of the final product at 530 nm when no gold nanoclusters are added;
[0064] A x is the absorbance value of the product obtained after adding gold nanoclusters modified with organic molecules at 530 nm.
[0065] Figure 5 The UV-visible absorption spectra of the products obtained without adding gold nanoclusters (purple line), adding Au@L-Pen (black line), adding Au@D-Pen (red line) and adding Au@DL-Pen (blue line) (the addition amount is 500μL). The test results show that when the volume of the diluted organic molecule-modified gold nanocluster dispersion is 500μL, the DAAO inhibition efficiency of Au@L-Pen, Au@DL-Pen and Au@D-Pen is 51.8%, 29.7% and 14.6%, respectively. When the volume of the diluted organic molecule-modified gold nanocluster dispersion is 50μL, the DAAO inhibition efficiency of Au@L-Pen, Au@DL-Pen and Au@D-Pen is 10.6%, 5.6% and 1.6%, respectively.
[0066] In addition, the three organic molecule-modified gold nanocluster dispersions prepared in Example 1 were freeze-dried respectively to obtain powders of Au@L-Pen, Au@DL-Pen and Au@D-Pen, and the powders were dispersed in PBS solution to prepare a high-concentration organic molecule-modified gold nanocluster dispersion (the concentration of organic molecule-modified gold nanoclusters in the dispersion was 0.83 mg / mL). 500 μL of the high-concentration organic molecule-modified gold nanocluster dispersion was taken and the DAAO inhibition efficiency was tested according to the above method. The results showed that the inhibition efficiencies of Au@L-Pen, Au@DL-Pen and Au@D-Pen were 92.3%, 92.1% and 75.6%, respectively.
[0067] Based on the above results, it can be seen that the inhibitory effect of DAAO is related to the volume and concentration of the gold nanoclusters modified with organic molecules and the chiral structure of penicillamine. Under the same experimental conditions, the inhibitory efficiency of the three clusters is in the following order: Au@L-Pen>Au@DL-Pen>Au@D-Pen.
[0068] Example 2
[0069] A chloroauric acid aqueous solution (concentration of 20 mmol / L) and an L-cysteine (L-Cys) aqueous solution (concentration of 5 mmol / L) were mixed, and then a NaOH aqueous solution (concentration of 1 mol / L) was added, followed by dropwise addition of a freshly prepared NaBH4 solution (prepared by dissolving 43 mg of NaBH4 powder in 10 mL of 0.2 mol / L NaOH solution), wherein the amount of the chloroauric acid aqueous solution was 250 μL, the molar ratio of chloroauric acid to L-cysteine was 1:3, the molar ratio of chloroauric acid to NaBH4 was 1:300, and the molar ratio of chloroauric acid to NaOH was 1:30; after the addition of the NaBH4 solution was completed, the reaction was continued for 30 min to obtain a dispersion of L-Cys-modified gold nanoclusters (denoted as Au@L-Cys) with a concentration of 1.0 mmol / L (calculated as the molar concentration of the gold element).
[0070] L-Cys was replaced by D-Cys, and a dispersion of D-cysteine-modified gold nanoclusters was prepared by the same method. The sample was denoted as Au@L-Cys, and the concentration was 1.0 mmol / L (calculated as the molar concentration of the gold element).
[0071] Sample characterization:
[0072] Figure 6 This is a transmission electron microscope (TEM) image of Au@D-Cys prepared in Example 2. Figure 6 It can be seen that the average particle size of Au@D-Cys is about 2.3 nm.
[0073] Figure 7 Circular dichroism (CD) spectra of Au@D-Cys and Au@L-Cys samples prepared in Example 2. Figure 7 It can be seen that in the wavelength range of 300 to 600 nm, the CD signal values of Au@D-Cys and Au@L-Cys are opposite, indicating that the samples have chiral characteristics.
[0074] Test Example 2
[0075] The organic molecule modified gold nanocluster dispersion prepared in Example 2 was diluted 10 times with PBS buffer solution (pH = 7.4), 500 μL of the diluted dispersion was mixed with 20 μL of DAAO solution (10 U / mL), and the DAAO inhibition effect test was performed according to the method in Test Example 1. The test results show that when the volume of the diluted organic molecule modified gold nanocluster dispersion is 500 μL, the DAAO inhibition efficiency of Au@L-Cys and Au@D-Cys is 65.6% and 22.9%, respectively.
[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A gold nanocluster modified with organic molecules, characterized in that: It comprises gold nanoclusters and organic molecules modified on the gold nanoclusters; the organic molecules are one or more of L-penicillamine, D-penicillamine, racemic penicillamine, L-cysteine, D-cysteine and racemic cysteine.
2. The organic molecule-modified gold nanoclusters according to claim 1, characterized in that: The average particle size of the gold nanoclusters modified by organic molecules is 2.0-2.5 nm.
3. The method for preparing the gold nanoclusters modified with organic molecules according to claim 1 or 2, characterized in that: The following steps are involved: Chloroauric acid, organic molecules, a reducing agent and water are mixed to carry out a reduction reaction, thereby obtaining gold nanoclusters modified with the organic molecules.
4. The preparation method according to claim 3, characterized in that: The molar ratio of the chloroauric acid to the organic molecule is 1:(1.5-4).
5. The preparation method according to claim 3, characterized in that: The reducing agent is borane tert-butylamine complex or sodium borohydride.
6. The preparation method according to claim 5, characterized in that: When the organic molecule is one or more of L-penicillamine, D-penicillamine and racemic penicillamine, the reducing agent is a borane tert-butylamine complex; the molar ratio of the chloroauric acid to the borane tert-butylamine complex is 1:(1-2); When the reducing agent is borane tert-butylamine complex, the reduction reaction time is 10 to 120 minutes.
7. The preparation method according to claim 5, characterized in that: When the organic molecule is one or more of L-cysteine, D-cysteine and racemic cysteine, the reducing agent is sodium borohydride; the molar ratio of chloroauric acid to sodium borohydride is 1:(150-450).
8. The preparation method according to claim 7, characterized in that: When the reducing agent is sodium borohydride, sodium hydroxide is also added during the mixing; the molar ratio of chloroauric acid to sodium hydroxide is 1:(15-65); When the reducing agent is sodium borohydride, the reduction reaction time is 10 to 180 minutes.
9. The preparation method according to claim 3, characterized in that: After the reduction reaction is completed, the obtained reaction solution is freeze-dried to obtain gold nanocluster powder modified with organic molecules.
10. Use of the gold nanoclusters modified with organic molecules according to claim 1 or 2 or the gold nanoclusters modified with organic molecules prepared by the preparation method according to any one of claims 3 to 9 in the preparation of D-amino acid oxidase inhibitors.
Citation Information
Cited By
Hypoxia response type gold-copper cluster nano-enzyme microgel as well as preparation method and application of hypoxia response type gold-copper cluster nano-enzyme microgel
CN120022231A
Hypoxia-responsive gold-copper cluster nanoszyme microgel, preparation method and application thereof
CN120022231B