Casting powder for high-pulling-speed slab low-carbon steel and application of casting powder
By using magnesium fluoride and barium fluoride instead of lithium carbonate in the protective slag, the quality defects in the continuous casting of high-pull slabs are solved, and the cost reduction and lubrication effect are improved. It is suitable for high-pull slabs and speed reduction, which is suitable for high-pull slabs. Continuous casting production.
Patent Information
- Application Number
- CN202411177487.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing technology lacks protective slag that does not contain lithium carbonate and has low melting point and good lubrication, which cannot effectively solve the problem of quality defects in the continuous casting of high-pull slabs, especially due to the surge in lithium carbonate prices, resulting in protection. The cost of slag increases.
Magnesium fluoride and/or barium fluoride replace lithium carbonate as raw material for protecting slag. By adjusting its usage and ratio, the melting point and viscosity are reduced, and the transparency and fluidity of the slag film are improved, thereby improving lubricating effect and reducing quality. defect.
The high-pull speed slab low-carbon steel protection slag without lithium carbonate is achieved, reducing costs, and improving lubrication effect, reducing quality defects such as rolling slag and inclusions, meeting the production needs of high-pull speed continuous casting.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of protective slag, and in particular to protective slag for low-carbon steel of high-drawing speed slab and application thereof. Background Art
[0002] Slab continuous casting achieves the advantage of reducing costs by increasing the drawing speed. However, the quality defects of the steel billets increase during the high-drawing-speed continuous casting production process, and a protective slag with low melting point, low crystallization rate and good lubrication is required. Generally, 2-4% lithium carbonate needs to be added to the raw materials of the protective slag. The protective slag film is glassy and stable, and has good lubrication with the surface of the steel billet to ensure smooth continuous casting production. However, due to the skyrocketing price of lithium carbonate, the cost of the protective slag has increased significantly. Therefore, it is urgent to develop a protective slag that does not contain lithium carbonate and has a low melting point and good lubrication for high-drawing-speed slab low-carbon steel.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] One of the objects of the present invention is to provide a protective slag for high-drawing speed slab low-carbon steel, so as to at least solve the technical problem in the prior art of lack of protective slag that does not contain lithium carbonate and has a low melting point and good lubrication for high-drawing speed slab low-carbon steel.
[0005] A second object of the present invention is to provide the application of the above-mentioned protective slag for high-speed drawing slab low-carbon steel in high-speed continuous casting of slab low-carbon steel.
[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0007] In a first aspect, the present invention provides a mold slag for low-carbon steel in a high-speed slab, using raw materials of magnesium fluoride and / or barium fluoride instead of raw material lithium carbonate;
[0008] The mass ratio of the amount of magnesium fluoride and / or barium fluoride used to the amount of lithium carbonate used in the replaced lithium carbonate-containing protective slag is 2.0-3.0:1.
[0009] Furthermore, the raw materials of the protective slag include 6 to 10 parts of magnesium fluoride and barium fluoride by weight.
[0010] Furthermore, the raw materials of the protective slag include 3 to 6 parts of magnesium fluoride or 3 to 6 parts of barium fluoride by weight.
[0011] Furthermore, the raw materials of the protective slag further include 1 to 2 parts of carbon black 1, 1 to 2 parts of carbon black 2 and 2 to 4 parts of earthy graphite, by weight.
[0012] The raw materials of the protective slag also include 6 to 9 parts of glass powder, 8 to 13 parts of fluorite, 5 to 7 parts of industrial soda ash, 38 to 46 parts of wollastonite, 2 to 4 parts of bentonite, 1 to 2 parts of magnesia, 4 to 8 parts of bauxite, 1 to 2 parts of dispersant, 2 to 4 parts of cryolite, 5 to 8 parts of slag powder and 1 to 1.5 parts of adhesive.
[0013] Furthermore, the mold slag contains the following chemical components in weight percentage: 25-28wt% CaO, 28-31wt% SiO2, 1-2.0wt% Fe2O3, 2-6wt% MgO, 4-8wt% Al2O3, 5-7wt% Na2O, 7-10wt% F - , 3-5wt% C and 2-4.5wt% BaO, and the balance are inevitable impurities.
[0014] Furthermore, the binary basicity of the protective slag is 0.85-0.95.
[0015] Furthermore, the melting point of the mold slag is 1060-1100°C.
[0016] Furthermore, at 1300° C., the viscosity of the mold slag is 0.16-0.26 Pa·s.
[0017] Furthermore, the melting time of the mold slag is 20 to 32 seconds;
[0018] Preferably, the crystallization rate of the mold slag is 5-15%.
[0019] In a second aspect, the present invention provides the use of the above-mentioned mold slag for high-speed slab low-carbon steel in high-speed continuous casting of slab low-carbon steel;
[0020] Preferably, the drawing speed of the slab low-carbon steel high-speed continuous casting is 1.6 to 2.2 m / min.
[0021] The present invention provides a protective slag for low-carbon steel in high-drawing speed slabs, which replaces lithium carbonate by introducing alkaline earth metal magnesium fluoride and barium fluoride into the raw materials. Magnesium fluoride and barium fluoride are used in the protective slag as co-solvents, wherein magnesium fluoride can improve the flowability of the protective slag film while lowering the melting point, and barium fluoride can improve the transparency of the slag film while lowering the melting point as a solvent. The two are used in combination according to the scheme design, which can significantly reduce the melting point and viscosity of the protective slag, and improve the transparency and fluidity of the slag film, play a role in promoting heat transfer and improving lubrication, and are conducive to obtaining high-viscosity protective slag with good lubrication effect, thereby reducing quality defects such as slag rolls and inclusions during high-drawing speed production of low-carbon steel. In addition, since alkaline earth metal magnesium fluoride and barium fluoride can replace materials such as white alkali and sodium fluoride in effect, the use of alkaline earth metal magnesium fluoride and barium fluoride can not only replace lithium carbonate but also reduce the amount of sodium-containing materials, reduce white spot-like precipitates on the surface of the ingot, and improve the surface appearance quality of the ingot after rolling. On the basis of ensuring the performance, from the perspective of the impact on melting point and viscosity, every addition of 2.0-3.0% magnesium fluoride or barium fluoride can achieve the effect of 1% lithium carbonate. The price of alkaline earth metal magnesium fluoride and barium fluoride is about 9,000 yuan / ton, which has a significant price advantage over 100,000 yuan / ton of lithium carbonate. Experimental verification shows that the crystallization rate of the protective slag after the replacement of ingredients is low, which is theoretically conducive to improving the lubrication effect, conforms to the design concept of high-drawing speed protective slag, and is suitable for high-drawing speed slab low-carbon steel continuous casting. DETAILED DESCRIPTION
[0022] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0023] The methods and techniques of the present invention are generally performed according to conventional methods well known in the art and as described in various general and more specific references that are cited and discussed throughout the present specification unless otherwise indicated.
[0024] On the one hand, the present invention provides a mold slag for low-carbon steel in a high-speed slab, using raw materials of magnesium fluoride and / or barium fluoride instead of raw material lithium carbonate;
[0025] The mass ratio of the amount of magnesium fluoride and / or barium fluoride used to the amount of lithium carbonate in the replaced lithium carbonate-containing protective slag is 2.5:1.
[0026] By introducing alkaline earth metal magnesium fluoride and barium fluoride into the raw materials, lithium carbonate is replaced. Magnesium fluoride and barium fluoride are used as co-solvents in protective slag, among which magnesium fluoride can improve the flowability of the protective slag film while reducing the melting point, and barium fluoride can improve the transparency of the slag film while reducing the melting point as a solvent. The two are used in combination according to the scheme design, which can significantly reduce the melting point and viscosity of the protective slag, and improve the transparency and fluidity of the slag film, play a role in promoting heat transfer and improving lubrication, and are conducive to obtaining high-viscosity protective slag with good lubrication effect, thereby reducing quality defects such as slag rolls and inclusions during high-speed production of low-carbon steel. In addition, since alkaline earth metal magnesium fluoride and barium fluoride can replace materials such as white alkali and sodium fluoride in effect, the use of alkaline earth metal magnesium fluoride and barium fluoride can not only replace lithium carbonate but also reduce the amount of sodium-containing materials, reduce white spot-like precipitates on the surface of the ingot, and improve the surface appearance quality of the ingot after rolling. On the basis of ensuring the performance, from the perspective of the impact on melting point and viscosity, the addition of about 2.0-3.0% of magnesium fluoride or barium fluoride can achieve the effect of 1% lithium carbonate. The price of alkaline earth metal magnesium fluoride and barium fluoride is about 9,000 yuan / ton, which has a significant price advantage over the 100,000 yuan / ton lithium carbonate. Experimental verification shows that the crystallization rate of the protective slag after the replacement of the ingredients is low, which is theoretically conducive to improving the lubrication effect, conforms to the design concept of high-speed protective slag, and is suitable for high-speed slab low-carbon steel continuous casting.
[0027] In some specific implementations, the raw materials of the mold slag include 6 to 10 parts by weight of magnesium fluoride and barium fluoride.
[0028] The proportion of magnesium fluoride and / or barium fluoride may be, but is not limited to, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5 or 10 parts, and may be any proportion between 6 and 10 parts.
[0029] In some specific embodiments, the raw materials of the mold slag include 3 to 6 parts of magnesium fluoride or 3 to 6 parts of barium fluoride by weight.
[0030] Specifically, the amount of magnesium fluoride may be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts or 6.0 parts, or any amount between 3 and 6 parts.
[0031] The amount of barium fluoride can be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts or 6.0 parts, or any amount between 3 and 6 parts.
[0032] According to the characteristics of high-speed continuous casting of low-carbon steel slabs, in order to avoid adhesion and steel leakage accidents and reduce quality defects such as slag curling and inclusions in rolling of castings, the lubrication performance should be considered first when designing the physical and chemical indicators of the protective slag. The alkalinity of the protective slag should be appropriately lower and the tendency of the slag film to vitrify should be larger to ensure good lubrication performance; in addition, the viscosity should be appropriately increased, because generally speaking, the viscosity of the protective slag is proportional to the surface tension, that is, the size of the surface tension increases with the increase of viscosity. The protective slag with large surface tension can effectively reduce the various shear forces caused by the molten steel flow field on the three-layer structure of the protective slag at high pulling speed in the crystallizer, avoid slag curling, thereby improving the surface quality of the casting and greatly reducing quality defects such as rolling black belts and inclusions.
[0033] In some specific embodiments, the raw materials of the mold slag further include 1 to 2 parts of carbon black 1, 1 to 2 parts of carbon black 2, and 2 to 4 parts of earthy graphite;
[0034] The carbon black 1 is required to have a carbon content greater than 98% and an oil absorption value greater than 100 g / cm 3 , iodine absorption value greater than 130g / kg. The carbon black 2 requires a carbon content greater than 98% and an oil absorption value greater than 35g / cm 3 , iodine absorption value is greater than 55g / kg.
[0035] Experiments have shown that the composite carbon formulation of 1 to 2 parts of carbon black 1, 1 to 2 parts of carbon black 2 and 2 to 4 parts of earthy graphite has a better skeleton effect, can control the melting time of the protective slag, is conducive to the uniform formation of slag, and makes the slag flow evenly into the gap between the billet shell and the crystallizer, thereby exerting a good lubrication effect; at the same time, this composite carbon formulation has a great influence on the three-layer structure of the protective slag, and can significantly improve the thermal insulation effect of the slag layer.
[0036] In some specific embodiments, the raw materials of the protective slag also include 6 to 9 parts of glass powder, 8 to 13 parts of fluorite, 5 to 7 parts of industrial soda ash, 38 to 46 parts of wollastonite, 2 to 4 parts of bentonite, 1 to 2 parts of magnesia, 4 to 8 parts of bauxite, 1 to 2 parts of dispersant, 2 to 4 parts of cryolite, 5 to 8 parts of slag powder and 1 to 1.5 parts of adhesive.
[0037] Wherein, the binder includes dextrin or sodium carboxymethyl cellulose. The dispersant includes sodium dodecylbenzene sulfonate, ethyl acetate or ethylene glycol.
[0038] The introduction of dispersants can make the carbonaceous materials dispersed more evenly, which can effectively solve the problems of rapid and developed slag rings, avoid blocking the liquid slag flow channel, and reduce the generation of slag roll defects.
[0039] In some specific embodiments, the mold slag contains the following chemical components in weight percentage: 25-28wt% CaO, 28-31wt% SiO2, 1-2.0wt% Fe2O3, 2-6wt% MgO, 4-8wt% Al2O3, 5-7wt% Na2O, 7-10wt% F - , 3-5wt% C and 2-4.5wt% BaO, and the balance are inevitable impurities.
[0040] In some specific embodiments, the binary basicity of the protective slag is 0.85-0.95, and a slag film with a high vitrification rate can be obtained.
[0041] The binary basicity of the protective slag may be, but is not limited to, 0.85, 0.86, 0.87, 0.88, 0.89, 0.90, 0.91, 0.92, 0.93, 0.94 or 0.95, or any value between 0.85 and 0.95.
[0042] In some specific embodiments, the melting point of the protective slag is 1060-1100°C, which can ensure that the slag film has a suitable surface tension, ensure the uniformity of the slag film inflow, take into account the requirements of lubrication and slag coiling, and can effectively solve the problems of adhesion leakage, slag coiling, inclusions, etc. during high-speed production, and meet the needs of smooth production on site.
[0043] The melting point of the slag protection may be, but is not limited to, 1060°C, 1065°C, 1070°C, 1075°C, 1080°C, 1085°C, 1090°C, 1095°C or 1100°C, and may also be any value between 1060 and 1100°C.
[0044] In some specific implementations, at 1300° C., the viscosity of the mold slag is 0.16-0.26 Pa·s.
[0045] Among them, the viscosity of the protective slag can be but not limited to 0.16Pa·s, 0.17Pa·s, 0.18Pa·s, 0.19Pa·s, 0.20Pa·s, 0.21Pa·s, 0.22Pa·s, 0.23Pa·s, 0.24Pa·s, 0.25Pa·s or 0.26Pa·s, and can also be any value between 0.16 and 0.26Pa·s.
[0046] In some specific implementations, the melting time of the mold slag is 20 to 32 seconds.
[0047] The melting time of the protective slag may be, but is not limited to, 20s, 21s, 22s, 23s, 24s, 25s, 26s, 27s, 28s, 29s, 30s, 31s or 32s, and may be any value between 20 and 32s.
[0048] In some specific implementations, the crystallization rate of the mold slag is 5-15%.
[0049] The crystallization rate of the protective slag may be, but is not limited to, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, or any value between 5 and 15%.
[0050] According to another aspect of the present invention, there is also provided the use of the above-mentioned mold slag for high-speed slab low-carbon steel in high-speed continuous casting of slab low-carbon steel;
[0051] In some specific implementations, the drawing speed of the slab low-carbon steel high-speed continuous casting is 1.6 to 2.2 m / min.
[0052] Among them, the pulling speed of the slab low-carbon steel high-speed continuous casting can be but not limited to 1.6m / min, 1.7m / min, 1.8m / min, 1.9m / min, 2.0m / min, 2.1m / min or 2.2m / min, and can also be any value between 1.6 and 2.2m / min.
[0053] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0054] Example 1
[0055] A protective slag for low-carbon steel of high-speed slab, the raw materials and weight parts of which are as follows: 8 parts of glass powder, 12 parts of fluorite powder, 6 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 40 parts of wollastonite, 3 parts of magnesium fluoride, 3 parts of barium fluoride, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 8 parts of water slag powder and 1 part of dextrin. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 27.3% CaO, 29.32% SiO2, 1.0% Fe2O3, 5.15% MgO, 6.6% Al2O3, 5.47% Na2O, 9.4% F - , 4.2% C, 2.57% BaO, and the balance are inevitable impurities.
[0056] The binary basicity of the above-mentioned protective slag is 0.93, the melting point is 1085° C., the viscosity at 1300° C. is 0.17 Pa·S, the melting time is 28 s, and the crystallization rate is 15%.
[0057] The test was conducted on the 1025*200 section, with the steel grade Q195L and the pulling speed of 2.1m / min. After tracking and observation, the protective slag reacted well in the crystallizer and could evenly cover the molten steel surface with the fluctuation of the molten steel level; the flame was moderate and the crystallizer was relatively active; the slag was evenly formed, and no irregular or obvious slag ring was generated. The average steel consumption per ton was 0.39Kg / t, and the thickness of the liquid slag layer was about 10mm. There were no defects such as cracks and slag rolls on the surface of the ingot, and the inclusion defect rate was much lower than the previous historical data. The qualified rate of quality inspection after rolling was above 99%, indicating that the protective slag can cast high-quality ingots and meet the customer's requirements for ingot quality.
[0058] Example 2
[0059] A protective slag containing magnesium fluoride and barium fluoride for high-speed slab low-carbon steel, the raw materials and weight composition of which are: 7 parts of glass powder, 11 parts of fluorite powder, 5 parts of industrial soda ash, 1 part of carbon black 1, 1.5 parts of carbon black 2, 2 parts of earthy graphite, 44 parts of wollastonite, 3 parts of magnesium fluoride, 5 parts of barium fluoride, 2 parts of bentonite, 1.5 parts of magnesia, 5 parts of bauxite, 1 part of sodium dodecylbenzene sulfonate, 2 parts of cryolite, 6 parts of water slag powder and 1 part of sodium carboxymethyl cellulose. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 27.33% CaO, 30.49% SiO2, 1.14% Fe2O3, 4.58% MgO, 6.3% Al2O3, 4.4% Na2O, 8.77% F - , 4.1% C, 4.28% BaO, and the balance are inevitable impurities.
[0060] The binary basicity of the above-mentioned protective slag is 0.90, the melting point is 1085° C., the viscosity at 1300° C. is 0.17 Pa·S, the melting time is 28 s, and the crystallization rate is 10%.
[0061] The test was conducted on the 1240*200 section, with steel grade SPHC and a pulling speed of 1.9m / min. After tracking and observation, the protective slag reacted well in the crystallizer and could evenly cover the molten steel surface with the fluctuation of the molten steel level; the flame was moderate and the crystallizer was relatively active; the slag was evenly formed, and no irregular or obvious slag ring was generated. The average steel consumption per ton was 0.38Kg / t, and the thickness of the liquid slag layer was about 10mm. There were no defects such as cracks and slag rolls on the surface of the ingot, and the inclusion defect rate was much lower than the previous historical data. The qualified rate of quality inspection after rolling was above 99%, indicating that the protective slag can cast high-quality ingots and meet the customer's requirements for ingot quality.
[0062] Example 3
[0063] A protective slag containing magnesium fluoride and barium fluoride for high-speed slab low-carbon steel, the raw materials and weight composition of which are: 7 parts of glass powder, 8 parts of fluorite powder, 7 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 3 parts of earthy graphite, 43.5 parts of wollastonite, 5 parts of magnesium fluoride, 3 parts of barium fluoride, 2 parts of bentonite, 1.5 parts of magnesia, 6 parts of bauxite, 2 parts of ethyl acetate, 2 parts of cryolite, 7 parts of water slag powder and 1 part of dextrin. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 25.57% CaO, 29.55% SiO2, 1.06% Fe2O3, 5.89% MgO, 6.95% Al2O3, 5.5% Na2O, 8.21% F - , 4.43% C, 2.57% BaO, and the balance are inevitable impurities.
[0064] The binary basicity of the protective slag is 0.86, the melting point is 1095° C., the viscosity at 1300° C. is 0.21 Pa·S, the melting time is 30 s, and the crystallization rate is 5%.
[0065] The test was conducted on the 1240*200 section, with steel grade SPHC and a pulling speed of 2.2m / min. After tracking and observation, the protective slag reacted well in the crystallizer and could evenly cover the molten steel surface with the fluctuation of the molten steel level; the flame was moderate and the crystallizer was relatively active; the slag was evenly formed, and no irregular or obvious slag ring was generated. The average steel consumption per ton was 0.37Kg / t, and the thickness of the liquid slag layer was about 12mm. There were no defects such as cracks and slag rolls on the surface of the ingot, and the inclusion defect rate was much lower than the previous historical data. The qualified rate of quality inspection after rolling was above 99%, indicating that the protective slag can cast high-quality ingots and meet the customer's requirements for ingot quality.
[0066] Example 4
[0067] Compared with Example 1, the difference is that barium fluoride is not added, and the amount of magnesium fluoride is 6 parts. The raw materials and weight parts are as follows: 8 parts of glass powder, 12 parts of fluorite powder, 6 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 40 parts of wollastonite, 6 parts of magnesium fluoride, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 8 parts of slag powder and 1 part of dextrin. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 27.3% CaO, 29.32% SiO2, 1.0% Fe2O3, 5.76% MgO, 6.6% Al2O3, 5.47% Na2O, 9.4% F - , 4.2% C, the balance being unavoidable impurities.
[0068] The binary basicity of the above-mentioned protective slag is 0.93, the melting point is 1082° C., the viscosity at 1300° C. is 0.16 Pa·S, the melting time is 27 s, and the crystallization rate is 15%.
[0069] Through the test under the same process conditions, the component design is suitable for on-site use.
[0070] Example 5
[0071] Compared with Example 1, the difference is that magnesium fluoride is not added, and the amount of barium fluoride is 6 parts. The raw materials and weight parts are as follows: 8 parts of glass powder, 12 parts of fluorite powder, 6 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 40 parts of wollastonite, 6 parts of barium fluoride, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 8 parts of slag powder and 1 part of dextrin. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 27.3% CaO, 29.32% SiO2, 1.0% Fe2O3, 2.65% MgO, 6.6% Al2O3, 5.47% Na2O, 9.4% F - , 4.2% C, 5.26% BaO, and the balance are inevitable impurities.
[0072] The binary basicity of the above-mentioned protective slag is 0.93, the melting point is 1087° C., the viscosity at 1300° C. is 0.18 Pa·S, the melting time is 29 s, and the crystallization rate is 15%.
[0073] Through the test under the same process conditions, the component design is suitable for on-site use.
[0074] Comparative Example 1
[0075] The difference between this comparative example and Example 1 is that its raw materials and weight parts are as follows: 7.4 parts of glass powder, 12 parts of fluorite powder, 13 parts of industrial soda ash, 0.8 parts of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 40 parts of wollastonite, 2 parts of bentonite, 2.3 parts of magnesia, 1 part of bauxite, 2 parts of ethyl acetate, 3.3 parts of cryolite, 2.5 parts of lithium carbonate, 7 parts of slag powder and 1 part of binder. The protective slag contains the following chemical components in mass percentage (wt%): 29.1% CaO, 32.33% SiO2, 1.0% Fe2O3, 2.52% MgO, 6.61% Al2O3, 5.45% Na2O, 1.0% Li2O 、 6.12% F - , 4.2% C, and the balance are inevitable impurities.
[0076] The binary basicity of the continuous casting mold protection slag is 0.9, the melting point is 1070°C, the viscosity at 1300°C is 0.16 Pa·S, the melting time is 32s, and the crystallization rate is 10%.
[0077] The same test method was used, and the results showed that compared with Example 1, the mold slag reacted well in the crystallizer and could evenly cover the steel liquid surface with the fluctuation of the steel liquid surface. The flame was moderate and the crystallizer was relatively active. The slag was uniform, and no irregular or obvious slag ring was generated. The average steel consumption per ton was 0.35 kg / t, and the thickness of the liquid slag layer was about 9 mm. There were no defects such as cracks and slag rolls on the surface of the ingot, and the inclusion defect rate was much lower than the previous historical data. The qualified rate of quality inspection after rolling was above 99%, indicating that the mold slag could cast high-quality ingots and meet the customer's requirements for ingot quality. However, the cost of the mold slag was 1,960 yuan higher than that of Example 1 per ton of steel.
[0078] Comparative Example 2
[0079] The difference between this comparative example and Example 1 is that: fluoride materials such as magnesium fluoride and barium fluoride are not used in the protective slag, but industrial soda ash is used instead, specifically: 8 parts of glass powder, 12 parts of fluorite powder, 12 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 40 parts of wollastonite, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 8 parts of slag powder and 1 part of dextrin. The protective slag contains the following chemical components in mass percentage (wt%): 29.3% CaO, 32.56% SiO2, 1.0% Fe2O3, 2.55% MgO, 6.6% Al2O3, 5.47% Na2O, 6.1% F - , 4.2% C, and the balance are inevitable impurities.
[0080] The binary basicity of the continuous casting mold protection slag is 0.9, the melting point is 1050°C, the viscosity at 1300°C is 0.14 Pa·S, the melting time is 21s, and the crystallization rate is 20%.
[0081] Using the same test method, the results show that the protective slag of Example 2 has a significant difference in the early trial effect compared with the protective slag of Example 1. The liquid level is not very stable at a pulling speed of 1.7m / min. With the increase of the pulling speed, when it exceeds 1.9m / min, the liquid level fluctuation increases due to the impact force of the molten steel. Since the surface tension of the protective slag of Example 2 is small, it is affected by the shear force of the flow field, resulting in an increased probability of slag rolling, and more black lines and inclusions after the ingot is rolled; the crystallization rate increases, the thermal conductivity becomes worse, and the number of steel leakage warnings increases; in addition, due to the large amount of industrial soda ash used, there are many white spot problems on the surface of the ingot, and the surface color of the steel plate after rolling is different.
[0082] Comparative Example 3
[0083] The difference between this comparative example and Example 1 is that the raw materials include 8 parts of glass powder, 12 parts of fluorite powder, 6 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 40 parts of wollastonite, 1.5 parts of magnesium fluoride, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 11 parts of slag powder and 1 part of dextrin. The carbon content of the first carbon black is 99.3%, and the oil absorption value is 116 g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 31.3% CaO, 33.62% SiO2, 1.0% Fe2O3, 1.78% MgO, 6.6% Al2O3, 2.87% Na2O, 6.4% F - , 4.2% C, and the balance being inevitable impurities.
[0084] The binary basicity of the above-mentioned protective slag is 0.93, the melting point is 1183° C., the viscosity at 1300° C. is 0.25 Pa·S, the melting time is 28 s, and the crystallization rate is 68%.
[0085] The same test method was used, and the results showed that when the protective slag was used in the crystallizer, the thickness of the liquid slag layer was about 15 mm, and the average steel consumption per ton was 0.30 kg / t, which was low. Large slag strips were produced, and the heat flow curve of the crystallizer alarm system was unstable, affecting smooth production. Large longitudinal cracks occurred in the ingot, which could not meet the requirements of continuous casting production.
[0086] Comparative Example 4
[0087] The difference between this comparative example and Example 1 is that the raw materials include 8 parts of glass powder, 12 parts of fluorite powder, 6 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 38.5 parts of wollastonite, 7.5 parts of magnesium fluoride, 6 parts of barium fluoride, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 8 parts of slag powder and 1 part of dextrin. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 27.3% CaO, 29.32% SiO2, 1.0% Fe2O3, 4.15% MgO, 6.6% Al2O3, 5.47% Na2O, 11.81% F- , 4.2% C, 4.69% BaO, and the balance are inevitable impurities.
[0088] The binary basicity of the above-mentioned protective slag is 0.93, the melting point is 985° C., the viscosity at 1300° C. is 0.12 Pa·S, the melting time is 22 s, and the crystallization rate is 0%.
[0089] Using the same test method, the results showed that when the protective slag was used in the crystallizer, the thickness of the liquid slag layer was about 8 mm, which was too thin. The average steel consumption per ton was 0.55 kg / t. The heat flow of the crystallizer expert system was too high, the consumption of protective slag was too large, the vibration marks of the ingot were deep, the corners of the ingot were missing, and the proportion of transverse cracks after rolling was as high as 45%, which could not meet the requirements of continuous casting production.
[0090] Comparative Example 5
[0091] The difference between this comparative example and Example 1 is that the raw materials include 8 parts of glass powder, 12 parts of fluorite powder, 9 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 40 parts of wollastonite, 1.5 parts of barium fluoride, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 8 parts of slag powder and 1 part of dextrin. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 27.3% CaO, 29.32% SiO2, 1.0% Fe2O3, 2.15% MgO, 6.6% Al2O3, 5.47% Na2O, 6.4% F - , 4.2% C, 0.87% BaO, and the balance are inevitable impurities.
[0092] The binary basicity of the above-mentioned protective slag is 0.93, the melting point is 1188° C., the viscosity at 1300° C. is 0.27 Pa·S, the melting time is 28 s, and the crystallization rate is 78%.
[0093] The same test method was used, and the results showed that when the protective slag was used in the crystallizer, the thickness of the liquid slag layer was about 17 mm, and the average steel consumption per ton was 0.28 kg / t, which was low. Large slag strips were produced, and the heat flow curve of the crystallizer alarm system was unstable, affecting smooth production. The ingot produced a large longitudinal depression problem and could not meet the requirements of continuous casting production.
[0094] Comparative Example 6
[0095] The difference between this comparative example and Example 1 is that the raw materials include 8 parts of glass powder, 12 parts of fluorite powder, 6 parts of industrial soda ash, 1 part of carbon black 1, 1 part of carbon black 2, 2.8 parts of earthy graphite, 37 parts of wollastonite, 3 parts of magnesium fluoride, 8.5 parts of barium fluoride, 3 parts of bentonite, 2 parts of magnesia, 5 parts of bauxite, 1 part of ethylene glycol, 3.2 parts of cryolite, 8 parts of slag powder and 1 part of dextrin. Among them, the carbon content of the first carbon black is 99.3%, and the oil absorption value is 116g / cm 3 , iodine absorption value is 137g / kg; the content of the second carbon black is 98.8%, and the oil absorption value is 38g / cm 3 The iodine absorption value is 58g / kg. The protective slag contains the following chemical components by weight percentage (wt%): 27.3% CaO, 29.32% SiO2, 1.0% Fe2O3, 5.65% MgO, 6.6% Al2O3, 3.25% Na2O, 9.4% F - , 4.2% C, 5.57% BaO, and the balance are inevitable impurities.
[0096] The binary basicity of the above-mentioned protective slag is 0.93, the melting point is 988° C., the viscosity at 1300° C. is 0.13 Pa·S, the melting time is 22 s, and the crystallization rate is 0%.
[0097] Using the same test method, the results showed that when the protective slag was used in the crystallizer, the thickness of the liquid slag layer was about 8 mm, which was too thin. The average steel consumption per ton was 0.54 kg / t. The heat flow of the crystallizer expert system was too high, the consumption of protective slag was too large, the vibration marks of the ingot were deep, the corners of the ingot were missing, and the proportion of transverse cracks after rolling was as high as 43%, which could not meet the requirements of continuous casting production.
[0098] In summary, the protective slag containing magnesium fluoride and barium fluoride provided in the preferred embodiment of the present invention is used for high-speed continuous casting of low-carbon steel slabs, which can effectively solve the surface defects such as slag curling and inclusions during high-speed production of low-carbon steel slabs, meet the smooth operation of on-site production, and reduce the cost of the protective slag.
[0099] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A mold slag for low-carbon steel with high-speed slab drawing, characterized in that: Using raw materials magnesium fluoride and / or barium fluoride instead of raw material lithium carbonate; The mass ratio of the amount of magnesium fluoride and / or barium fluoride used to the amount of lithium carbonate used in the replaced lithium carbonate-containing protective slag is 2.0-3.0:
1.
2. The mold slag for low carbon steel with high drawing speed slab according to claim 1, characterized in that: The raw materials of the protective slag include 6 to 10 parts of magnesium fluoride and barium fluoride by weight.
3. The mold slag for low carbon steel with high drawing speed slab according to claim 1, characterized in that: In terms of weight, the raw materials of the protective slag include 3 to 6 parts of magnesium fluoride or 3 to 6 parts of barium fluoride.
4. The mold slag for low carbon steel with high drawing speed slab according to any one of claims 1 to 3, characterized in that: The raw materials of the protective slag further include 1 to 2 parts of carbon black 1, 1 to 2 parts of carbon black 2 and 2 to 4 parts of earthy graphite by weight. The raw materials of the protective slag also include 6 to 9 parts of glass powder, 8 to 13 parts of fluorite, 5 to 7 parts of industrial soda ash, 38 to 46 parts of wollastonite, 2 to 4 parts of bentonite, 1 to 2 parts of magnesia, 4 to 8 parts of bauxite, 1 to 2 parts of dispersant, 2 to 4 parts of cryolite, 5 to 8 parts of slag powder and 1 to 1.5 parts of adhesive.
5. The mold slag for low carbon steel with high drawing speed slab according to claim 4, characterized in that: The protective slag contains the following chemical components in weight percentage: 25-28wt% CaO, 28-31wt% SiO2, 1-2.0wt% Fe2O3, 2-6wt% MgO, 4-8wt% Al2O3, 5-7wt% Na2O, 7-10wt% F - , 3-5wt% C and 2-4.5wt% BaO, and the balance are inevitable impurities.
6. The mold slag for low carbon steel with high drawing speed slab according to claim 5, characterized in that: The binary basicity of the protective slag is 0.85-0.
95.
7. The mold slag for low carbon steel with high drawing speed slab according to claim 6, characterized in that: The melting point of the protective slag is 1060-1100°C.
8. The mold slag for low carbon steel with high drawing speed slab according to claim 7, characterized in that: At 1300° C., the viscosity of the protective slag is 0.16-0.26 Pa·s.
9. The mold slag for low carbon steel with high drawing speed slab according to claim 8, characterized in that: The melting time of the protective slag is 20 to 32 seconds; Preferably, the crystallization rate of the mold slag is 5-15%.
10. Use of the mold slag for high-speed slab low-carbon steel according to any one of claims 1 to 9 in high-speed continuous casting of slab low-carbon steel; Preferably, the drawing speed of the slab low-carbon steel high-speed continuous casting is 1.6-2.2 m / min.