Preparation method and application of carbon-doped modified bentonite

Carbon-doped aluminum is deposited on bentonite by one-step hydrothermal method to form carbon-doped modified bentonite, which solves the problem of poor fluorine removal effect in the prior art, and achieves efficient fluorine ion adsorption and fluorine removal effects, which significantly improves the effect of significantly The adsorption capacity and fluorine removal rate of fluorine ions are obtained.

CN119056398AInactive Publication Date: 2024-12-03NANTONG UNIV

Patent Information

Application Number
CN202411298718.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing monometal modified bentonite and inorganic acid modified bentonite have no significant effect on fluorine removal, and it is difficult to meet the strict emission standards for fluoride in industrial wastewater.

Method used

A one-step hydrothermal method is used to deposit carbon-doped aluminum on bentonite, and a carbon-doped modified bentonite is formed by reacting low-molecular organic acids with alkaline aluminum. It uses its unique "sandwich" structure and negative surface charge to increase fluorine ions. Adsorption capacity.

Benefits of technology

The adsorption capacity and fluorine removal rate of fluorine ions are significantly improved, the theoretical maximum adsorption capacity reaches 85.51 mg/g, the actual fluorine removal rate can reach 95.3%, and it also exhibits high adsorption capacity under different pH conditions, reducing the cost of water treatment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method and application of carbon-doped modified bentonite, sodium bentonite dry powder and sodium metaaluminate dry powder are placed in a beaker, low-molecular organic acid is added, and after uniform stirring and mixing, the mixture is transferred to a reaction kettle for a hydrothermal reaction; after the reaction is finished, naturally cooling, taking out a sample in the reaction kettle, and centrifuging; washing and drying the centrifuged solid sample; placing the dried sample in a crucible, wrapping the sample with tinfoil, and calcining the sample in a muffle furnace to finally obtain carbon-doped modified bentonite; the composite material can be obtained through hydrothermal reaction and subsequent high-temperature calcination, hydrothermal synthesis of carbon-doped aluminum and loading of bentonite are completed at the same time, the adopted raw materials are small in amount and variety, the steps are simple, the synthesis reaction time is short, energy consumption is low, components of the adsorption material are adjustable, low toxicity and low carbon are achieved, and harm to the environment is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental protection water treatment, and in particular relates to a preparation method of carbon-doped modified bentonite and application thereof. Background Art

[0002] As the global population grows and industrialization and urbanization progress rapidly, ensuring water safety has become a top priority. However, fluoridated wastewater discharged from industries such as electroplating, metal processing and electronics manufacturing poses a significant risk to water quality, especially in less developed areas. Long-term exposure to high concentrations of fluoride can lead to fluorosis and stunt growth in children. Strict water fluoridation regulations set a maximum allowable limit of 10 mg / L in industrial wastewater. Therefore, the development of efficient fluoridation removal technologies has become a top priority.

[0003] Fluoride removal is commonly performed using several methods, including adsorption, precipitation, bioremediation, membrane filtration, ion exchange, and solvent extraction. Among these techniques, adsorption is highly valued due to its high fluoride removal efficiency, simple operation, cost-effectiveness, and availability of highly efficient adsorbents. Various materials have been studied for their effects on fluoride ion absorption, including clay minerals, activated carbon, zeolites, metal oxides, composites, functional polymers, and carbon nanotubes. Although activated carbon extracted from various biomass sources is commonly used as an adsorbent for fluoride removal, research exploring alternative adsorbents is urgently needed. Notably, clay minerals, which are naturally abundant, renewable, and environmentally sustainable, are respected for their durability as adsorbents due to their cost-effectiveness, excellent adsorption characteristics, and strong ion exchange capacity. Bentonite is a clay mineral composed primarily of montmorillonite, which has a unique structure consisting of tetrahedral (silicon / oxygen) and octahedral (aluminum / oxygen / hydroxyl) sheets. Its unique "sandwich" structure makes it easy to modify, thereby improving its adsorption performance.

[0004] Chemical modification is a common method to improve the defluorination performance of bentonites. For example, acid modification significantly increases the specific surface area but only achieves a modest adsorption capacity of 0.07 mg / g. In contrast, metal oxide modification has been shown to effectively improve the adsorption capacity in various studies. Kamble et al. demonstrated the efficiency of lanthanum-modified bentonite, while Thakre et al. showed that bentonite doped with magnesium chloride outperformed unmodified bentonite in fluoride removal. In addition, Gitari et al. highlighted that iron ion-modified bentonite can almost completely defluorinate, with a fluoride removal capacity of 2.91 mg / g. However, aluminum ion modification generally results in a lower adsorption capacity of approximately 0.7 mg / g at room temperature. In summary, single metal modification and acid-modified bentonite do not always universally produce significant improvements in the adsorption of fluoride. Summary of the invention

[0005] Technical issues solved:

[0006] The present application aims at the deficiencies of the prior art and solves the technical problems that the current single metal modified bentonite and inorganic acid modified bentonite are not effective in removing fluorine, and provides a preparation method and application of carbon-doped modified bentonite for removing fluoride in water, using a simple one-step hydrothermal method to deposit carbon-doped aluminum on bentonite.

[0007] Technical solution:

[0008] To achieve the above objectives, this application is implemented through the following technical solutions:

[0009] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0010] Step 1: Weigh 1.5-3g of sodium bentonite dry powder and 0.8-2.5g of sodium aluminate dry powder respectively according to the mass volume ratio and place them in a beaker, add 8-15ml of 10-100% (v / v) low molecular organic acid solution, and stir with a glass rod for 1min to mix evenly;

[0011] Step 2: transfer the stirred mixed solution obtained in the first step into a 50 ml reaction kettle and hydroheat at 100-200°C for 60-240 min;

[0012] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it;

[0013] Step 4: After centrifugation, remove the supernatant and wash the sample;

[0014] Step 5: Place the sample washed in step 4 into an oven for drying;

[0015] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 400-500°C for 1-3 hours to obtain carbon-doped modified bentonite.

[0016] Furthermore, the low molecular weight organic acid is formic acid, acetic acid or propionic acid.

[0017] Furthermore, in the third step, the centrifugation is performed at 4000-5000 r / min for 3-5 min.

[0018] Furthermore, the washing step in the fourth step is washing once with distilled water, then washing once with ethanol, and then washing once with distilled water.

[0019] Furthermore, in the fifth step, the drying temperature is 60° C. and the drying time is 12 hours.

[0020] Furthermore, in the sixth step, the calcination temperature is 450° C. and the calcination time is 1 hour.

[0021] The present application also discloses the use of the carbon-doped modified bentonite prepared by any of the above preparation methods in water treatment and fluorine removal.

[0022] Beneficial effects:

[0023] The present application provides a preparation method of carbon-doped modified bentonite and its application, which has the following beneficial effects compared with the prior art:

[0024] 1. Adopting innovative carbon doping process and one-step hydrothermal method, using alkaline aluminum and organic acid to react, the hydrothermal carbon doping and aluminum modification of bentonite are realized simultaneously. This is different from the traditional bentonite pillaring modification, which is to form high aluminum polymer by adding alkali to the general acidity of conventional aluminum salts, such as aluminum thirteen as a pillaring agent to carry out high-polymer aluminum pillaring modification on bentonite;

[0025] 2. The obtained material has a unique "sandwich" structure of bentonite, that is, an octahedral sheet is sandwiched between two tetrahedral sheets, and the isomorphic substitution within the octahedral sheet produces a net negative surface charge. Through a one-step hydrothermal method and calcination method, carbon-doped aluminum oxide is loaded on bentonite, making it have special fluorine-loving properties, which are mainly manifested in the rich -OH, Al-O structure and C-containing groups on the surface of the material. The main component of the material is bentonite. According to preliminary EDX analysis, the aluminum oxide loading accounts for about 7%;

[0026] 3. This method significantly increases the types and number of adsorption sites of the material, including the rarely reported carbon-fluorine binding sites, and strengthens the traditional aluminum-fluorine binding sites, which has a significant effect on improving the adsorption performance; calculated by the Langmuir model, its theoretical maximum adsorption capacity is as high as 85.51 mg / g, which is much higher than the general activated alumina, which is generally lower than 8 mg / g; under the adsorption conditions of fluoride ion initial concentration of 10 mg / L, adsorbent dosage of 1 g / L, and pH 6, the defluorination rate of the defluoridation agent can reach 95.3%, and the actual adsorption amount can reach 9.53 mg / g, which is a significant technical improvement over the adsorption capacity of 0.7 mg / g of the traditional activated alumina-loaded bentonite defluoridation agent;

[0027] 4. More importantly, the composite material has a significant coupling advantage, producing a "1+1>2" effect. First, under the same conditions of use, when the adsorption capacity of low-molecular organic acid modified bentonite is only 0.8-2 mg / g, the adsorption capacity of sodium aluminate modified bentonite with the same raw material dosage is 3.5-5 mg / g, and the sum of the two is 4.3-7 mg / g, while the adsorption capacity of the material obtained by the present invention is above 9, which is much greater than the sum of the two; secondly, the similar carbon-doped bentonite actually prepared by the direct mixing method has a fluorine removal effect of only 55.7% and an adsorption capacity of 5.64 mg / g, which is also far lower than the carbon-doped aluminum-loaded bentonite prepared by the one-step hydrothermal method, which has a fluorine removal effect of up to 95.3%; this also shows that the one-step hydrothermal method can effectively load carbon-doped aluminum on bentonite, so that it produces an unexpected effect of simply combining the two;

[0028] 5. It has a wide pH application range and is significantly better than traditional activated alumina in defluorination effect. It has a high adsorption capacity for fluoride ion solutions between pH 3 and 6. In practical applications, it can be used without adjusting the pH value of water, which further saves water treatment costs;

[0029] 6. Convenient preparation, low cost, easy process control. The present invention uses a small amount of raw materials, a small number of types, simple steps, can be obtained by hydrothermal method and subsequent high-temperature calcination, and simultaneously completes the hydrothermal synthesis of carbon-doped aluminum and the loading of bentonite. The synthesis reaction time is short, the energy consumption is low, the components of the adsorption material can be adjusted, low toxicity and low carbon, and will not cause harm to the environment; DETAILED DESCRIPTION

[0030] In order to further illustrate the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0031] Example 1

[0032] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0033] Step 1: Weigh 1.64g sodium bentonite dry powder and 0.82g sodium aluminate dry powder separately into a beaker, add 10ml acetic acid solution, and stir with a glass rod for 1min to mix evenly;

[0034] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 120 min;

[0035] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0036] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0037] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0038] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 450°C for 1 hour to obtain carbon-doped modified bentonite P01.

[0039] The invention discloses an application of carbon-doped modified bentonite in water treatment and fluoride removal. When the P01 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluoride removal rate of the sample can reach 90.1%, and the experimental adsorption amount is 8.85 mg / g.

[0040] Example 2

[0041] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0042] Step 1: Weigh 1.64g of sodium bentonite dry powder and 1.64g of sodium aluminate dry powder respectively into a beaker, add 10ml of acetic acid solution, and stir with a glass rod for 1min to mix evenly;

[0043] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 120 min;

[0044] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0045] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0046] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0047] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 450°C for 1 hour to obtain carbon-doped modified bentonite P02.

[0048] When the above P02 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample can reach 92.9%, and the experimental adsorption amount is 9.13 mg / g.

[0049] Example 3

[0050] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0051] Step 1: Weigh 2.45g of sodium bentonite dry powder and 2.45g of sodium aluminate dry powder respectively into a beaker, add 10ml of acetic acid solution, and stir with a glass rod for 1min to mix evenly;

[0052] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 120 min;

[0053] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0054] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0055] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0056] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 450°C for 1 hour to obtain carbon-doped modified bentonite P03.

[0057] The invention discloses an application of carbon-doped modified bentonite in water treatment and fluorine removal. When the above-mentioned P03 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample can reach 95.3%, and the experimental adsorption amount is 9.36 mg / g.

[0058] Example 4

[0059] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0060] Step 1: Weigh 2.45g of sodium bentonite dry powder and 2.45g of sodium aluminate dry powder into a beaker and add 10ml

[0061] Acetic acid solution, stir with glass rod for 1min to mix evenly;

[0062] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 60 min;

[0063] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0064] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0065] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0066] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 450°C for 1 hour to obtain carbon-doped modified bentonite P04.

[0067] The invention discloses an application of carbon-doped modified bentonite in water treatment and fluorine removal. When the above-mentioned P04 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample can reach 91.6%, and the experimental adsorption amount is 9.08 mg / g.

[0068] Example 5

[0069] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0070] Step 1: Weigh 2.45g of sodium bentonite dry powder and 2.45g of sodium aluminate dry powder respectively into a beaker, add 10ml of acetic acid solution, and stir with a glass rod for 1min to mix evenly;

[0071] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 240 min;

[0072] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0073] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0074] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0075] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 450°C for 1 hour to obtain carbon-doped modified bentonite P05.

[0076] The invention discloses an application of carbon-doped modified bentonite in water treatment and fluorine removal. When the P05 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample can reach 95.1%, and the experimental adsorption amount is 9.42 mg / g.

[0077] Example 6

[0078] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0079] Step 1: Weigh 2.45g of sodium bentonite dry powder and 2.45g of sodium aluminate dry powder respectively into a beaker, add 10ml of formic acid solution, and stir with a glass rod for 1min to mix evenly;

[0080] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 120 min;

[0081] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0082] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0083] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0084] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 450°C for 1 hour to obtain carbon-doped modified bentonite P06.

[0085] The invention discloses an application of carbon-doped modified bentonite in water treatment and fluorine removal. When the P06 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample can reach 81.5%, and the experimental adsorption amount is 8.08 mg / g.

[0086] Example 7

[0087] A method for preparing carbon-doped modified bentonite comprises the following steps:

[0088] Step 1: Weigh 2.45g of sodium bentonite dry powder and 2.45g of sodium aluminate dry powder respectively into a beaker, add 10ml of propionic acid solution, and stir with a glass rod for 1min to mix evenly;

[0089] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 120 min;

[0090] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0091] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0092] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0093] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 450°C for 1 hour to obtain carbon-doped modified bentonite P07.

[0094] The invention discloses an application of carbon-doped modified bentonite in water treatment and fluoride removal. When the P07 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluoride removal rate of the sample can reach 92.9%, and the experimental adsorption amount is 9.28 mg / g.

[0095] Comparative Example 1

[0096] A sodium bentonite defluoridation application effect: When the sodium bentonite is placed under adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6 (optimal pH conditions), the sodium bentonite in comparative example 1 has a fluoride removal rate of only 18.0% and an adsorption capacity of only 1.83 mg / g.

[0097] Comparative Example 2

[0098] A method for preparing sodium bentonite activated by low molecular weight organic acid: Sample D001 is prepared according to the preparation method of P01, except that sodium aluminate is not added to the raw materials. Other conditions are the same.

[0099] When the D001 sample was placed under the adsorption conditions of an initial fluoride ion concentration of 10 mg / L, an adsorbent dosage of 1 g / L, and a pH of 6, the fluorine removal rate of the sample was only 24.2%, and the experimental adsorption amount was 2.47 mg / g.

[0100] Comparative Example 3

[0101] A method for preparing sodium aluminate modified bentonite: According to the preparation method of P01, except that water is used in place of acetic acid in the raw material and other conditions are the same, a sodium aluminate modified bentonite sample D01 is prepared.

[0102] When the above D01 sample was placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample was only 30.1%, and the experimental adsorption amount was 3.0 mg / g.

[0103] Comparative Example 4

[0104] A method for preparing sodium aluminate modified bentonite: Sample D02 is prepared according to the preparation method of P02, except that water is used instead of acetic acid in the raw material, and other conditions are the same.

[0105] When the above D02 sample was placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample was only 26.1%, and the experimental adsorption amount was 2.61 mg / g.

[0106] Comparative Example 5

[0107] A method for preparing sodium aluminate modified bentonite: Sample D03 is prepared according to the preparation method of P03, except that water is used instead of acetic acid in the raw material, and other conditions are the same.

[0108] When the above D03 sample was placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6, the fluorine removal rate of the sample was only 28.6%, and the experimental adsorption amount was 2.86 mg / g.

[0109] Comparative Example 6

[0110] A method for preparing aluminum chloride modified bentonite, specifically comprising the following steps:

[0111] Step 1: Weigh 6.15g of anhydrous sodium acetate, 6.04g of aluminum chloride hexahydrate and 2.45g of bentonite into a beaker, add 25ml of deionized water, and stir with a glass rod for 1min;

[0112] Step 2: Transfer the stirred mixed solution obtained in the first step to a 50 ml reactor and heat at 200 °C for 120 min;

[0113] Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it at 4000-5000r / min for 3-5min;

[0114] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;

[0115] Step 5: Place the washed sample in step 4 in a 60°C oven and dry for 12 hours;

[0116] Step 6: Place the dried sample in a crucible, wrap it with tin foil, and calcine it in a muffle furnace at 450°C for 1 hour to obtain

[0117] Step 7: The sample from step 6 was placed under adsorption conditions of 10 mg / L initial fluoride ion concentration, 1 g / L adsorbent dosage, and pH 6. The fluoride removal rate of the sample was 81.9% and the experimental adsorption amount was 8.2 mg / g.

[0118] It can be seen from Comparative Examples 1 and 2 that the adsorption capacity of sodium bentonite is very low, only 1.8 mg / g; low molecular weight organic acid modification can increase the adsorption capacity of sodium bentonite to 2.4 mg / g, and the improvement is not obvious. Comparative Examples 3 to 5 are single sodium aluminate modified bentonites, and their adsorption capacity is between 2.6-3.0 mg / g, which is slightly improved compared to single organic acid modification. While Examples 1 to 3 are modified with organic acid and sodium aluminate at the same time, and their adsorption capacity is higher than 9.0 mg / g, the performance is significantly improved, and the technical effect of 1+1>>2 is achieved. In addition, the conventionally modified bentonite with aluminum chloride in Comparative Example 6 not only has a lower adsorption capacity than this application, but also the price of the raw material aluminum chloride hexahydrate used is about twice that of the sodium aluminate raw material of this application (500g price 95 yuan vs. 49 yuan), and this scheme significantly reduces the synthesis cost.

[0119] In summary, the innovative preparation process in this study, a one-step hydrothermal method, doped the carbon of the organic acid carbon source into aluminum-loaded bentonite. It achieved the technical effect of "1+1>>2", and also had better technical effects and cost advantages than conventional aluminum salt modification, so it has substantial and beneficial characteristics.

[0120] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A method for preparing carbon-doped modified bentonite, characterized in that: The specific steps include: Step 1: Weigh 1.5-3g of sodium bentonite dry powder and 0.8-2.5g of sodium aluminate dry powder respectively according to the mass volume ratio and place them in a beaker, add 8-15ml of 10-100% (v / v) low molecular organic acid solution, and stir with a glass rod for 1min to mix evenly; Step 2: transfer the stirred mixed solution obtained in the first step into a 50 ml reaction kettle and hydroheat at 100-200°C for 60-240 min; Step 3: After the hydrothermal treatment, wait for the reactor to cool naturally, take out the sample from the reactor and centrifuge it; Step 4: After centrifugation, remove the supernatant and wash the sample; Step 5: Place the sample washed in step 4 into an oven for drying; Step 6: Place the dried sample in a crucible, wrap it with tin foil, and place it in a muffle furnace and calcine at 400-500°C for 1-3 hours to obtain carbon-doped modified bentonite.

2. The method for preparing the carbon-doped modified bentonite according to claim 1, characterized in that: The low molecular weight organic acid is formic acid, acetic acid or propionic acid.

3. The method for preparing the carbon-doped modified bentonite according to claim 1, characterized in that: The centrifugation in the third step is specifically performed at 4000-5000 r / min for 3-5 min.

4. The method for preparing carbon-doped modified bentonite according to claim 1, characterized in that: The washing step in the fourth step is washing once with distilled water, then washing once with ethanol, and then washing once with distilled water.

5. The method for preparing carbon-doped modified bentonite according to claim 1, characterized in that: In the fifth step, the drying temperature is 60° C. and the drying time is 12 h.

6. The method for preparing carbon-doped modified bentonite according to claim 1, characterized in that: In the sixth step, the calcination temperature is 450° C. and the calcination time is 1 hour.

7. Use of the carbon-doped modified bentonite prepared by the preparation method according to any one of claims 1 to 6 in water treatment and fluorine removal.

Citation Information

Patent Citations

  • Carbon-doped aluminum-based adsorbent and preparation method thereof

    CN116474736A

  • Regeneration-free efficient fluorine removal agent containing carbon and aluminum and preparation method of regeneration-free efficient fluorine removal agent

    CN118002076A

  • Preparation method and application of fluorine-doped modified sludge defluorination adsorbent

    CN118002089A

  • Process for preparing aluminium modified montmorillonite as defluorinating material and its application

    CN1315293A

Cited By

  • Preparation method and application of bentonite-based adsorption material for sewage treatment

    CN121755179A

  • Preparation method and application of bentonite-based adsorption material for sewage treatment

    CN121755179B

  • Compound fluorine removal agent, preparation method thereof and application of compound fluorine removal agent in industrial wastewater

    CN122166913A

  • Compound defluorination agent, its preparation method and its application in industrial wastewater