Sodium ion electrolyte, preparation method and sodium ion battery
By using additive A with a fluorine structure and additive B with specific functional groups in sodium-ion batteries, a stable SEI is formed, which solves the problem of low cycle performance of sodium-ion batteries and significantly improves the cycle life of the battery.
Patent Information
- Application Number
- CN202411483306.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2025-01-24
AI Technical Summary
The cycling performance of sodium ion batteries is low, mainly due to the uneven structure of the SEI layer and easy to break, resulting in a short battery cycle life.
Add agent A with fluoride-containing structures and additives B and sulfurllinl, phosphorhin, or tritenal silicon oxygen structure B, combined with non-water solvents and conductive sodium salts to form a stable SEI and improve the electrolyte-electrode interface.
Through the combined use of additives A and B, the uniform deposition of sodium ions is promoted, the growth of dendrites is inhibited, a uniform and stable SEI is formed, and the cycle life of the sodium ion battery is improved.
Smart Images

Figure BDA0005098049620000031 
Figure BDA0005098049620000051 
Figure BDA0005098049620000061
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium ion electrolyte, a preparation method thereof, and a sodium ion battery. Background Art
[0002] Compared with the limited reserves and price fluctuations of lithium resources, sodium resources are abundant in the earth's crust and are cheap, and are attracting more and more attention. In particular, they have broad application prospects in the fields of stationary energy storage and low-speed vehicles, and are expected to promote the upgrading of lithium-ion batteries. The working principle of sodium-ion batteries is similar to that of lithium-ion batteries, both of which are "rocking chair batteries." As an ion transport medium, the electrolyte is one of the key components of sodium-ion batteries and plays a decisive role in the electrical performance of the battery. The solvent of the electrolyte of sodium-ion batteries is basically the same as that of lithium-ion batteries. Carbonate solvents are usually used, and the conductive salt is changed to sodium hexafluorophosphate. The solid electrolyte interface (SEI) of sodium-ion batteries is mainly composed of sodium carbonate and sodium fluoride.
[0003] In the free state, the radius of sodium ions is about 1.02 angstroms, and the radius of lithium ions is about 0.76 angstroms. Compared with lithium ions, the larger volume of sodium ions and their interaction with electrolytes easily lead to a more sparse and uneven structure of the SEI layer. In addition, compared with lithium salts, sodium salts such as sodium carbonate, sodium fluoride, and sodium sulfate have higher solubility in solvents, which causes the SEI to be easily damaged and reorganized during the cycle, continuously consuming solvents and active sodium, accompanied by gas production, which reduces the cycle life of the battery. Therefore, selecting suitable film-forming additives to induce the formation of a uniform and stable SEI is one of the most effective ways to improve the cycle life of sodium-ion batteries. Summary of the invention
[0004] The first object of the present invention is to provide a sodium ion electrolyte to solve the technical problem of low cycle performance of existing sodium ion batteries.
[0005] A second object of the present invention is to provide a method for preparing a sodium ion electrolyte.
[0006] The third object of the present invention is to provide a sodium ion battery.
[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0008] A sodium ion electrolyte comprises an additive A and an additive B, wherein the additive A is a fluoride, and the additive B contains a sulfonyl group, a carbonyl group, a phosphazene group or a trimethylsiloxy group.
[0009] Furthermore, the additive A is one or more of pentafluorophenyl methacrylate, 2,3,5,6-tetrafluorophenyl methacrylate, 3-(2,5-difluorophenyl)ethyl acrylate, pentafluorophenyl acrylate, 1-(allyloxy)-2,3,4,5,6-pentafluorobenzene, and olefinic pentafluorobenzene.
[0010] Further, the additive B is one or more of bisvinylsulfonemethane, propylene sulfite, vinyl sulfate, vinyl sulfite, propylene-1,3-sultone, vinylene carbonate, vinyl ethylene carbonate, methylene disulfonate, 1,4-butane sultone, methylene disulfonate, pentafluoro(phenoxy)cyclotriphosphazene, pentafluoro(ethoxy)cyclotriphosphazene, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)borate.
[0011] Furthermore, it also includes a non-aqueous solvent and a conductive sodium salt; the additive A accounts for 0.1-1.5wt% of the sodium ion electrolyte, the additive B accounts for 0.1-5wt% of the sodium ion electrolyte, and the conductive sodium salt accounts for 5-15wt% of the sodium ion electrolyte.
[0012] Furthermore, the non-aqueous solvent is one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, fluoroethylene carbonate, dimethyl carbonate, ethylene carbonate, diethyl carbonate, ethyl propionate, propionic acid ester, 1,3-dioxolane, and ethylene glycol dimethyl ether.
[0013] Furthermore, the conductive sodium salt is one or more of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium bis(fluorooxalyl)borate, sodium bis(fluorosulfonyl)imide, and sodium bis(trifluoromethyl)sulfonyl imide.
[0014] A method for preparing a sodium ion electrolyte comprises the following steps: adding a conductive sodium salt into a non-aqueous solvent to obtain a precursor solution, mixing an additive A and an additive B with the precursor solution, and then shaking the mixture under a sealed condition to obtain the electrolyte.
[0015] A sodium ion battery comprises the sodium ion electrolyte mentioned above.
[0016] Beneficial effects of the present invention:
[0017] Fluorine has high bonding strength, extremely strong electronegativity and high free energy of fluoride formation. The additive A of the present invention has a fluorine-containing structure, which can promote the uniform deposition of sodium ions on the negative electrode side, inhibit dendrite growth, and improve cycle life. Additive B contains a carbonyl (-C=O), sulfacyl (-S=O), phosphazene (-P=N-) or trimethylsilyl ((CH3)3Si-O-) structure, which can participate in the formation of a uniform SEI / CEI with good mechanical properties, and the oxygen atoms can form a stable complex with sodium ions, which can enhance the migration ability of ions, optimize ion transport during charging and discharging, and reduce battery polarization. The -P=N- structure increases the highest occupied molecular orbital (HOMO) of additive B, which can achieve preferential oxidation at the cathode and inhibit the side reaction between the cathode and the electrolyte. The (CH3)3Si-O- structure can participate in the film formation of the positive and negative electrodes, generate silicate components with high ionic conductivity, reduce the internal resistance of the battery, and prevent further reaction between the electrode and the electrolyte. By using additive A and additive B together, the electrolyte-electrode interface can be synergistically improved, a stable SEI can be obtained, and the loss of active substances in the sodium-ion battery during the cycle process can be reduced, thereby improving the cycle life of the sodium-ion battery. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the embodiments of the present invention.
[0019] The non-aqueous solvent of Examples 1-12 and Comparative Examples 1-5 is a mixture of polycarbonate (PC): diethyl carbonate (DEC): ethyl methyl carbonate (EMC) in a volume ratio of 3:2:5.
[0020] The structure of pentafluorophenyl methacrylate is shown in formula (1), the structure of 2,3,5,6-tetrafluorophenyl methacrylate is shown in formula (2), the structure of 3-(2,5-difluorophenyl)ethyl acrylate is shown in formula (3), the structure of pentafluorophenyl acrylate is shown in formula (4), 1-(allyloxy)-2,3,4,5,6-pentafluorobenzene is shown in formula (5), and the structure of olefinic pentafluorobenzene is shown in formula (6);
[0021]
[0022] Example 1
[0023] The preparation method of the sodium ion electrolyte of Example 1 comprises the following steps: adding 13wt% of a conductive sodium salt to 85.8wt% of a non-aqueous solvent to obtain a precursor solution, mixing 1wt% of an additive A and 0.2wt% of an additive B with the precursor solution, and shaking the mixture under sealing conditions to obtain the result.
[0024] The structure of additive A is shown in formula (1), additive B is bisvinylsulfonemethane, and the conductive sodium salt is sodium hexafluorophosphate.
[0025] Example 2
[0026] The preparation method of the sodium ion electrolyte of Example 2 is substantially the same as that of Example 1. The difference between the preparation method of the sodium ion electrolyte of Example 2 and Example 1 is that the structure of the additive A of Example 2 is shown as (4).
[0027] Example 3
[0028] The preparation method of the sodium ion electrolyte of Example 3 is substantially the same as that of Example 1. The difference between the preparation method of the sodium ion electrolyte of Example 3 and that of Example 1 is that the structure of the additive A of Example 3 is as shown in (2).
[0029] Example 4
[0030] The preparation method of the sodium ion electrolyte of Example 4 is substantially the same as that of Example 1. The difference between the preparation method of the sodium ion electrolyte of Example 4 and that of Example 1 is that the additive B of Example 4 is propylene sulfite, the added amount is 1 wt%, and the added amount of the non-aqueous solvent is 85 wt%.
[0031] Example 5
[0032] The preparation method of the sodium ion electrolyte of Example 5 is substantially the same as that of Example 4. The difference between the preparation method of the sodium ion electrolyte of Example 5 and Example 4 is that the additive B of Example 5 is vinyl sulfate.
[0033] Example 6
[0034] The preparation method of the sodium ion electrolyte of Example 6 is substantially the same as that of Example 4. The difference between the preparation method of the sodium ion electrolyte of Example 6 and Example 4 is that the additive B of Example 6 is pentafluoro(ethoxy)cyclotriphosphazene.
[0035] Example 7
[0036] The preparation method of the sodium ion electrolyte of Example 7 is substantially the same as that of Example 4. The difference between the preparation method of the sodium ion electrolyte of Example 7 and Example 4 is that the additive B of Example 7 is vinylene carbonate.
[0037] Example 8
[0038] The preparation method of the sodium ion electrolyte of Example 8 is substantially the same as that of Example 4. The difference between the preparation method of the sodium ion electrolyte of Example 8 and Example 4 is that the additive B of Example 8 is propenyl-1,3-sultone.
[0039] Example 9
[0040] The preparation method of the sodium ion electrolyte of Example 9 is substantially the same as that of Example 4. The difference between the preparation method of the sodium ion electrolyte of Example 9 and Example 4 is that the additive B of Example 9 is tris(trimethylsilyl) phosphate.
[0041] Example 10
[0042] The preparation method of the sodium ion electrolyte of Example 10 is substantially the same as that of Example 1. The difference between the preparation method of the sodium ion electrolyte of Example 10 and Example 1 is that the additive B of Example 10 is propylene sulfite, the addition amount is 3wt%, and the addition amount of the non-aqueous solvent is 83%.
[0043] Embodiment 11
[0044] The preparation method of the sodium ion electrolyte of Example 11 is substantially the same as that of Example 10. The difference between the preparation method of the sodium ion electrolyte of Example 11 and Example 10 is that the additive B of Example 11 is vinylene carbonate.
[0045] Example 12
[0046] The preparation method of the sodium ion electrolyte of Example 12 is substantially the same as that of Example 10. The difference between the preparation method of the sodium ion electrolyte of Example 12 and Example 10 is that the additive B of Example 12 is tri(trimethylsilyl) phosphate.
[0047] Comparative Example 1
[0048] The preparation method of the sodium ion electrolyte of Comparative Example 1 comprises the following steps: 13 wt% of a conductive sodium salt and 87 wt% of a non-aqueous solvent are mixed and shaken in a sealed condition to obtain the conductive sodium salt. The conductive sodium salt is sodium hexafluorophosphate.
[0049] Comparative Example 2
[0050] The preparation method of the sodium ion electrolyte of Comparative Example 2 is substantially the same as that of Example 1. The difference between the preparation method of the sodium ion electrolyte of Comparative Example 2 and Example 1 is that additive B is not added in Comparative Example 2, and the addition amount of the non-aqueous solvent is 86 wt %.
[0051] Comparative Example 3
[0052] The preparation method of the sodium ion electrolyte of Comparative Example 3 is substantially the same as that of Example 1, and the difference between the preparation method of the sodium ion electrolyte of Comparative Example 3 and Example 1 is that the addition amount of the additive A of Comparative Example 3 is 2 wt % and the addition amount of the non-aqueous solvent is 84.8 wt %.
[0053] Comparative Example 4
[0054] The preparation method of the sodium ion electrolyte of Comparative Example 4 is substantially the same as that of Example 2. The difference between the preparation method of the sodium ion electrolyte of Comparative Example 4 and Example 2 is that additive B is not added in Comparative Example 4, and the addition amount of the non-aqueous solvent is 86 wt %.
[0055] Comparative Example 5
[0056] The preparation method of the sodium ion electrolyte of Comparative Example 5 is to dissolve sodium hexafluorophosphate in a non-aqueous solvent to obtain a mixed solution, add bisvinyl sulfone methane to the mixed solution, and shake well under a sealed condition to obtain the mixed solution. The addition amount of sodium hexafluorophosphate is 13wt%, the addition amount of bisvinyl sulfone methane is 1wt%, and the addition amount of the non-aqueous solvent is 86wt%.
[0057] The preparation method of the sodium ion battery of Examples 1-12 and Comparative Examples 1-5 is:
[0058] Preparation of positive electrode: weigh 1000g of sodium nickel iron manganese oxide (NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2), 10g of conductive carbon black, 10g of conductive carbon tube, 18g of polyvinylidene fluoride, and 3g of oxalic acid are added to 400g of N-methylpyrrolidone (NMP), mixed evenly to obtain positive electrode slurry, and the slurry is coated on both sides of aluminum foil by a coating machine, and the positive electrode sheet is obtained after baking, rolling, slitting, and ear welding.
[0059] Preparation of negative electrode sheet: 600g of hard carbon, 6g of conductive carbon black, 6g of conductive carbon tube, 12g of styrene-butadiene rubber and 24g of carboxymethyl cellulose were weighed according to the mass ratio of 100:1:2:4, added into 550g of deionized water, stirred evenly to obtain negative electrode slurry, coated the slurry on both sides of aluminum foil by a coating machine, and obtained the negative electrode sheet after baking, rolling, slitting and tab welding.
[0060] Sodium ion battery assembly: The separator, positive electrode sheet and negative electrode sheet are wound into a soft-pack battery cell.
[0061] Liquid injection: The sodium ion electrolyte of Examples 1-12 and Comparative Examples 1-5 was injected, sealed, and aged for 48 hours.
[0062] Formation: High-voltage fixture is used for formation, the pressure is 0.6MPa, the formation standard is: charge and discharge for 5 cycles at 0.1C, the cut-off voltage range is 1.5V-3.95V, the constant voltage cut-off current ratio is 0.01C, and then the airbag is cut off, and the sodium ion battery is obtained after secondary sealing and ironing.
[0063] The sodium ion batteries of Examples 1-12 and Comparative Examples 1-5 and the cycle test results are shown in Table 1. Test conditions for the internal resistance of the sodium ion battery: Use an internal resistance meter to test the internal resistance of the sodium ion battery in a fully charged state. Cycle test conditions: (1) 25°C cycle: In a constant temperature environment of 25°C, the cycle test is carried out in a 0.5C charge / 1C discharge mode, and the constant voltage cut-off current ratio is 0.02C; (2) 45°C cycle: In a constant temperature environment of 45°C, the cycle test is carried out in a 0.5C charge / 1C discharge mode, and the constant voltage cut-off current ratio is 0.02C. Calculation of cycle retention rate: Cycle retention rate = 1000th cycle capacity / maximum capacity*100%.
[0064] Table 1 Sodium ion batteries and cycle test results of Examples 1-12 and Comparative Examples 1-5
[0065]
[0066]
[0067] As can be seen from Table 1, the compounding of additive A and additive B forms a stable SEI. Compared with comparative example 1, the cycle life of the sodium ion battery of Example 1 is greatly improved, and the cycle retention rate of 1000 cycles at room temperature is 91.8%, and the cycle retention rate of 1000 cycles at 45°C is 85.74%. Additive B in Examples 4 and 5 can be reduced to generate a stable SEI at the negative electrode, reduce the side reactions of the electrode at high temperature, and improve the cycle life of the sodium ion battery at high temperature. The fluorine substituent and π-π conjugated-P=N-structure in pentafluoro(ethoxy)cyclotriphosphazene in Example 6 respectively reduce the lowest unoccupied molecular orbital (LUMO) and increase the highest occupied molecular orbital (HOMO), which can be reduced to generate a stable SEI at the negative electrode, and oxidized on the positive electrode side to form a positive electrode electrolyte interface (CEI), reduce the interface side reactions, and improve the cycle life of the sodium ion battery at high temperature. The vinylene carbonate in Example 7 can be reduced to generate sodium carbonate and polymer components at the negative electrode during the first cycle of charging, forming a stable SEI, reducing the interface side reactions, and improving the cycle life of the battery at high temperature. The decomposition products of tris(trimethylsilyl)phosphate in Example 9 can participate in the film formation of positive and negative electrodes, generate silicate and carbonate components with high stability and high conductivity, reduce the transmission resistance of sodium ions, and improve the cycle performance. The proportion of additive B in Examples 10-12 is increased to 3wt%. A higher additive B is conducive to maintaining the stability of the electrode interface, so the cycle life is better than the addition ratio of 1wt%, but there is a marginal effect of the addition ratio, so the improvement is limited.
[0068] Comparative Example 2 contains only 1wt% of pentafluorophenyl methacrylate, and the retention rate of 1000 cycles at 25°C is 90.8%, but the retention rate at 45°C is only 63%, and it is accompanied by a certain amount of gas production. The SEI formed by pentafluorophenyl methacrylate is not stable enough under high temperature conditions. Comparative Example 3 increases the amount of additive A to 2wt%. Pentafluorophenyl methacrylate contains pentafluorophenyl. Too high a ratio leads to greater impedance, affecting the migration rate of sodium ions, so the cycle retention rate of Comparative Example 3 deteriorates. Comparative Example 5 does not contain additive A, and the proportion of bisvinylsulfone methane is increased to 1wt%. The decrease in cycle performance is attributed to the excessively high content of organic components in SEI, which causes SEI to tend to form a disordered structure and reduce its ion conductivity.
[0069] In summary, additive A can improve the negative electrode interface and stabilize the room temperature cycle performance of sodium-ion batteries, but has little effect on the high temperature cycle performance. The combination of additive A and additive B can synergistically passivate the negative electrode interface to form a stable SEI, thereby improving the cycle performance of sodium-ion batteries.
Claims
1. A sodium ion electrolyte, characterized in that The invention comprises an additive A and an additive B, wherein the additive A is a fluoride, and the additive B contains a sulfonyl group, a carbonyl group, a phosphazene group or a trimethylsilyloxy group.
2. The sodium ion electrolyte according to claim 1, characterized in that The additive A is one or more of pentafluorophenyl methacrylate, 2,3,5,6-tetrafluorophenyl methacrylate, 3-(2,5-difluorophenyl)ethyl acrylate, pentafluorophenyl acrylate, 1-(allyloxy)-2,3,4,5,6-pentafluorobenzene, and olefinic pentafluorobenzene.
3. The sodium ion electrolyte according to claim 1, characterized in that The additive B is one or more of bisvinylsulfonemethane, propylene sulfite, vinyl sulfate, vinyl sulfite, propylene-1,3-sultone, vinylene carbonate, vinylethylene carbonate, methylene disulfonate, 1,4-butane sultone, methylene disulfonate, pentafluoro(phenoxy)cyclotriphosphazene, pentafluoro(ethoxy)cyclotriphosphazene, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)borate.
4. The sodium ion electrolyte according to claim 1, characterized in that It also includes a non-aqueous solvent and a conductive sodium salt; the additive A accounts for 0.1-1.5wt% of the sodium ion electrolyte, the additive B accounts for 0.1-5wt% of the sodium ion electrolyte, and the conductive sodium salt accounts for 5-15wt% of the sodium ion electrolyte.
5. The sodium ion electrolyte according to claim 4, characterized in that The non-aqueous solvent is one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, fluoroethylene carbonate, dimethyl carbonate, ethylene carbonate, diethyl carbonate, ethyl propionate, propionic acid ester, 1,3-dioxolane, and ethylene glycol dimethyl ether.
6. The sodium ion electrolyte according to claim 4, characterized in that The conductive sodium salt is one or more of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium bis(fluorooxalyl)borate, sodium bis(fluorosulfonyl)imide, and sodium bis(trifluoromethyl)sulfonyl imide.
7. A method for preparing a sodium ion electrolyte as claimed in claim 1, characterized in that: The following steps are involved: A conductive sodium salt is added to a non-aqueous solvent to obtain a precursor solution, and additives A and B are mixed with the precursor solution and then shaken under a sealed condition to obtain the product.
8. A sodium ion battery, characterized in that: Comprising the sodium ion electrolyte according to claim 1.
Citation Information
Patent Citations
Non-aqueous Electrolytic Solution, And Non-aqueous Electrolyte Battery Comprising Same
CN104112870A
Lithium ion battery non-aqueous electrolyte and lithium ion battery
CN104979588A
Additive for nonaqueous electrolyte solutions, nonaqueous electrolyte solution, and electricity storage device
CN110383565A
Sodium-ion battery electrolyte additive, electrolyte and battery
CN116826169A
Cited By
Preparation method and device of sodium ion electrolyte
CN122441329A