Polyvinylidene fluoride film with high infrared reflectivity and preparation method thereof
By the modification of nano -titanium dioxide and the co -concentration of the modified monomer of nanolytic titanium dioxide film in a polyticonythyls, solve the problem of improving infrared reflectance and weather resistance of the film, and achieve higher infrared reflectances and longer Trends.
Patent Information
- Application Number
- CN202411720138.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-28
- Publication Date
- 2025-01-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When existing polyvinylidene fluoride films are applied to PVDF film coating, there is still room for improvement in infrared reflectivity and weather resistance, and the addition of nano titanium dioxide will affect the thermal stability of polymethyl methacrylate, resulting in weather resistance. decline.
By introducing sodium silicate to a specific solvent and decentralized additives, the titanium-oxygen-silicon key is generated, and silicon dioxide is evenly covered with titanium dioxide surfaces to increase the infrared reflectance of a polyticonythylene film. At the same time, the introduction of the modified monomer of acrylics and methamphetamine of methamphetamine and methyl acrylic.
It significantly improves the infrared reflection rate and weather resistance of polyticonylinylinylene film, ensure the tightness and average one of the film, and avoid the negative effects of nano -titanium dioxide on thermal stability.
Smart Images

Figure BDA0005157821680000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of polyvinylidene fluoride materials, and particularly relates to a polyvinylidene fluoride film with high infrared reflectivity and a preparation method thereof. Background Art
[0002] Polyvinylidene fluoride is a semi-crystalline polymer obtained by the polymerization of the monomer 1,1-difluoroethylene. It is a highly non-reactive thermoplastic fluorinated polymer with a fluorine content of 59%. It has excellent mechanical properties, heat resistance, chemical corrosion resistance and weather resistance. It is hydrophobic and easily soluble in organic solvents.
[0003] Polyvinylidene fluoride film is made of polyvinylidene fluoride resin through biaxial stretching process. It has excellent performance, including excellent weather resistance, excellent mechanical properties, and chemical corrosion resistance. It is one of the commonly used coating materials in aerospace, crystalline silicon solar cells, construction and other fields. In the existing technology, polyvinylidene fluoride resin is often mixed with pigments, fillers and various additives to make composite materials to give polyvinylidene fluoride film higher performance.
[0004] The invention patent with application number 202010204067.2 discloses a high and low temperature resistant polyvinylidene fluoride film for photovoltaics, including polyvinylidene fluoride, antioxidant, toughening agent, stabilizer, surface lubricant PTFE wax powder, polymethyl methacrylate, titanium dioxide, and processing aid. The weight ratio is: 50-80 parts of polyvinylidene fluoride, 0.1-5 parts of antioxidant, 2-30 parts of acrylic toughening agent, 0.5-5 parts of stabilizer, 0.1-5 parts of surface lubricant PTFE wax powder, 2-30 parts of polymethyl methacrylate, 5-20 parts of titanium dioxide, and 0.1-3 parts of processing aid. The polyvinylidene fluoride film of the invention is resistant to high and low temperatures, anti-oxidation, high strength, good thermal insulation performance, anti-static, high safety performance, waterproof and fireproof, environmentally friendly and non-toxic, low cost, long service life, durable, simple manufacturing process, and easy to implement.
[0005] However, when the polyvinylidene fluoride film is used for PVDF film coating, its infrared reflectivity and weather resistance still have room for improvement, and in the prior art, the amount of pigments and fillers such as nano-titanium dioxide is often increased to achieve higher infrared reflectivity, and the weather-resistant toughening component polymethyl methacrylate is added to increase the mechanical properties and weather resistance of the polyvinylidene fluoride film. However, nano-titanium dioxide often affects the thermal stability of polymethyl methacrylate, resulting in a decrease in the weather resistance of the polyvinylidene fluoride film and a shortened weathering time.
[0006] In view of this, it is particularly important to disclose a polyvinylidene fluoride film with high infrared reflectivity. Summary of the invention
[0007] In view of the defects of the prior art, the present invention provides a polyvinylidene fluoride film with high infrared reflectivity and a preparation method thereof. The polyvinylidene fluoride film disclosed in the present invention has high infrared reflectivity, good compatibility and dispersibility between components, greatly improved density and uniformity of the film material, and compensates for the adverse effects of nano titanium dioxide on the thermal stability of the film, so that the polyvinylidene fluoride film has longer weather resistance.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] On one hand, the present invention provides a polyvinylidene fluoride film with high infrared reflectivity. The preparation of the polyvinylidene fluoride film comprises the following raw materials in parts by weight: 30 to 40 parts of polyvinylidene fluoride, 10 to 15 parts of modified polymethyl methacrylate, 5 to 10 parts of modified nano titanium dioxide, 1 to 5 parts of plasticizer and 5 to 10 parts of solvent.
[0010] In some embodiments of the present invention, the preparation steps of the modified nano titanium dioxide are as follows:
[0011] The nano titanium dioxide and butyl acetate are stirred and mixed, and then a dispersing aid is added, and ultrasonic dispersion is performed for 10 to 30 minutes. The temperature is raised to 80 to 100° C., sodium silicate is added, and then an inorganic acid is added to adjust the pH value to 8 to 10. The mixture is kept warm and allowed to stand for 2 to 3 hours, and then a modifier is added. The mixture is stirred and mixed, and then high-temperature drying and grinding are performed to obtain the modified nano titanium dioxide.
[0012] In some embodiments of the present invention, the particle size of the nano titanium dioxide is 30 to 100 nm.
[0013] Preferably, the particle size of the nano titanium dioxide is 80 nm.
[0014] In some embodiments of the present invention, the modifier is at least one of stearic acid and a silane coupling agent.
[0015] Preferably, the modifier is a silane coupling agent.
[0016] More preferably, the silane coupling agent is 3-(methacryloyloxy)propyltrimethoxysilane.
[0017] Preferably, the amount of the modifier added is 0.5-1.5% of the total mass of nano-titanium dioxide and sodium silicate.
[0018] Further preferably, the amount of the modifier added is 1% of the total mass of nano titanium dioxide and sodium silicate.
[0019] Preferably, the dispersing aid is fatty acid methyl ester (CAS: 627-91-8).
[0020] In some embodiments of the present invention, the mass ratio of the nano titanium dioxide to sodium silicate is 1:(1-3).
[0021] Preferably, the mass ratio of the nano titanium dioxide to sodium silicate is 1:2.
[0022] In the prior art, higher infrared reflectivity is often achieved by increasing the amount of pigments and fillers such as nano-titanium dioxide. However, a larger amount added will inevitably lead to compatibility mismatch problems. Agglomerated nano-titanium dioxide cannot be effectively dispersed in the system. Even if the nano-titanium dioxide is modified for compatibility by common means, the problem of insufficient compatibility of the modified nano-titanium dioxide will still occur when a larger amount of modified nano-titanium dioxide is added. This not only causes the infrared reflectivity to fail to meet expectations, but also affects the uniformity of the polyvinylidene fluoride film system, and affects its basic performance and the durability of its performance.
[0023] The present invention introduces sodium silicate, performs a modification in a specific solvent of ethyl acetate and a dispersing aid of fatty acid methyl ester, and after adding an inorganic acid, the sodium silicate is acidified to generate a titanium-oxygen-silicon bond on the surface of the nano titanium dioxide, and while occupying the surface active sites that cause the nano titanium dioxide to be easily agglomerated, the silicon dioxide is uniformly coated on the surface in the form of chemical bonding, so that the infrared reflectivity of the polyvinylidene fluoride film is greatly improved. This may be because, under a specific solvent and a dispersing aid, the nano titanium dioxide has a wide particle size distribution, a high degree of particle dispersion, is conducive to the bonding and coating of silicon dioxide, and the coating amount is significantly improved, and silicon dioxide also helps to improve the infrared reflectivity.
[0024] Furthermore, the present invention continues to add specific 3-(methacryloyloxy)propyltrimethoxysilane to further replace the active hydroxyl groups on the surface of nano-titanium dioxide that are not bonded to silicon dioxide, and the polarity brought by the methacryloxy group on the specific silane coupling agent chain segment can further assist the dispersion and compatibility of the modified nano-titanium dioxide in the solvent ethyl acetate of the polyvinylidene fluoride film of the present invention, which is conducive to ensuring the density and uniformity of the film after film formation and ensuring the high performance of the film.
[0025] In some embodiments of the present invention, the preparation steps of the modified polymethyl methacrylate are as follows:
[0026] Add ethyl acetate into the reactor and heat it to 70-80° C., then add the modified monomer, methyl methacrylate and the first weight portion of initiator in sequence, stir and mix, continue to heat to 80-90° C., react for 0.5-1h, then add the second weight portion of initiator, react for 4-7h, precipitate and dry to obtain the modified polymethyl methacrylate.
[0027] In some embodiments of the present invention, the modifying monomer is hexafluorobutyl acrylate.
[0028] In some embodiments of the present invention, the mass ratio of the modified monomer to methyl methacrylate is (1-3):10.
[0029] Preferably, the mass ratio of the modified monomer to methyl methacrylate is 2:10.
[0030] In the present invention, the applicant first performs secondary modification on nano-titanium dioxide, which significantly improves the infrared reflectivity of the polyvinylidene fluoride film. However, even if the composite modification of silicon dioxide and the modifier reduces the amount of nano-titanium dioxide added to a certain extent, when a weather-resistant toughening component such as polymethyl methacrylate is added to the system in order to increase the mechanical properties and weather resistance of the polyvinylidene fluoride film, the nano-titanium dioxide will still have a certain effect on the thermal stability of the polymethyl methacrylate.
[0031] The applicant introduced the modified monomer hexafluorobutyl acrylate and copolymerized it with methyl methacrylate. The introduction of hexafluorobutyl acrylate increased the steric hindrance and high heat resistance of polymethyl methacrylate. When it was added to the polyvinylidene fluoride film system, it compensated for the adverse effects of nano-titanium dioxide on the thermal stability of the film. The possible reason is that the special properties of fluorine atoms make the modified polymethyl methacrylate still have stable performance under high temperature environment, which to a certain extent hinders the ester exchange reaction that may occur between the residual hydroxyl groups of the modified nano-titanium dioxide and polymethyl methacrylate, and improves the segment stability of polymethyl methacrylate, which is conducive to the polyvinylidene fluoride film to maintain longer weather resistance.
[0032] In some embodiments of the present invention, the plasticizer is diisononyl phthalate.
[0033] In some embodiments of the present invention, the solvent is ethyl acetate.
[0034] Another aspect of the present invention further provides a method for preparing a polyvinylidene fluoride film with high infrared reflectivity, comprising the following steps:
[0035] Polyvinylidene fluoride, modified polymethyl methacrylate, modified nano titanium dioxide, a plasticizer and a solvent are blended in a high-speed mixer, and then transferred to a vacuum oven for drying to constant weight to obtain a dried material, the dried material is added to a twin-screw blending extruder for granulation, and then subjected to a flat-plate vulcanizer for film pressing to obtain the polyvinylidene fluoride film.
[0036] In some embodiments of the present invention, the polyvinylidene fluoride film has a thickness of 10 to 100 μm.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) The polyvinylidene fluoride film disclosed in the present invention has a high infrared reflectivity, good compatibility and dispersibility between the components, greatly improved density and uniformity of the film material, and compensates for the adverse effects of nano-titanium dioxide on the thermal stability of the film, so that the polyvinylidene fluoride film has longer weather resistance.
[0039] (2) The present invention improves the compatibility and dispersion uniformity of the system by performing secondary modification on nano-titanium dioxide, and while significantly improving the infrared reflectivity of the polyvinylidene fluoride film, ensures the density and uniformity of the polyvinylidene fluoride film during film formation, thereby ensuring the high performance of the film.
[0040] (3) The present invention increases the steric hindrance and high heat resistance of polymethyl methacrylate by introducing modified monomers hexafluorobutyl acrylate and copolymerizing with methyl methacrylate, thereby compensating for the adverse effects of nano-titanium dioxide on the thermal stability of the film and making the polyvinylidene fluoride film have longer weather resistance. DETAILED DESCRIPTION
[0041] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0042] If not otherwise specified, the reagents used below can be easily obtained from commercial companies, among which polymethyl methacrylate was purchased from Dongguan Baojia Plastic Co., Ltd., polyvinylidene fluoride was purchased from Dongguan Xinfengyi Plastic Co., Ltd., and nano titanium dioxide (particle size 80 nm) was purchased from Shanghai Yantai E-Commerce Co., Ltd.
[0043] Preparation Example 1
[0044] The preparation steps of modified nano titanium dioxide are as follows:
[0045] 2g of nano-titanium dioxide and 50mL of butyl acetate were stirred and mixed, and then 0.6×10 -4 g fatty acid methyl ester, dispersed by ultrasound for 20 min, heated to 90 ° C, added with 4 g sodium silicate, and then added with 2 mol / L dilute sulfuric acid to adjust the pH to 9, kept warm and allowed to stand for 2.5 h, and then added with 0.06 g 3-(methacryloyloxy)propyltrimethoxysilane, stirred and mixed, and then dried and ground at 105 ° C to obtain modified nano titanium dioxide.
[0046] Preparation Example 2
[0047] The preparation steps of modified nano titanium dioxide are the same as those of Preparation Example 1, except that 0.12 g of 3-(methacryloyloxy)propyltrimethoxysilane is added.
[0048] Preparation Example 3
[0049] The preparation steps of modified nano titanium dioxide are the same as those in Preparation Example 1, except that 8 g of sodium silicate is added.
[0050] Preparation Example 4
[0051] The preparation steps of modified polymethyl methacrylate are as follows:
[0052] Add 100 mL of ethyl acetate to the reactor and heat it to 75°C. Then add 10 g of hexafluorobutyl acrylate, 50 g of methyl methacrylate and 0.3 g of azobisisobutyronitrile in sequence, stir and mix, continue to heat to 85°C, react for 0.75 h, then add 0.025 g of azobisisobutyronitrile, react for 5.5 h, precipitate with methanol and dry to obtain modified polymethyl methacrylate.
[0053] Preparation Example 5
[0054] The preparation steps of modified polymethyl methacrylate are the same as those of Preparation Example 6, except that 20 g of hexafluorobutyl acrylate is added.
[0055] Unless otherwise specified, the plasticizer used in the following examples and comparative examples is diisononyl phthalate, and the solvent is ethyl acetate.
[0056] Example 1
[0057] A polyvinylidene fluoride film with high infrared reflectivity comprises the following raw materials in parts by weight: 35 parts of polyvinylidene fluoride, 12.5 parts of modified polymethyl methacrylate, 7.5 parts of modified nano titanium dioxide, 3 parts of plasticizer and 7.5 parts of solvent.
[0058] The modified polymethyl methacrylate used in this example is prepared by Preparation Example 4, and the modified nano titanium dioxide used is prepared by Preparation Example 1.
[0059] The method for preparing a polyvinylidene fluoride film having high infrared reflectivity comprises the following steps:
[0060] Polyvinylidene fluoride, modified polymethyl methacrylate, modified nano titanium dioxide, a plasticizer and a solvent are blended in a high-speed mixer, and then transferred to a vacuum oven and dried to constant weight to obtain a dried material. The dried material is added to a twin-screw blending extruder for granulation. The extrusion temperature is controlled at 215°C, and then the film is pressed on a flat vulcanizer to obtain a polyvinylidene fluoride film with a thickness of 55 μm.
[0061] Example 2
[0062] A polyvinylidene fluoride film with high infrared reflectivity comprises the following raw materials in parts by weight: 40 parts of polyvinylidene fluoride, 15 parts of modified polymethyl methacrylate, 10 parts of modified nano titanium dioxide, 5 parts of plasticizer and 10 parts of solvent.
[0063] The modified polymethyl methacrylate used in this example is prepared by Preparation Example 4, and the modified nano titanium dioxide used is prepared by Preparation Example 1.
[0064] The method for preparing a polyvinylidene fluoride film having high infrared reflectivity comprises the following steps:
[0065] Polyvinylidene fluoride, modified polymethyl methacrylate, modified nano titanium dioxide, a plasticizer and a solvent are blended in a high-speed mixer, and then transferred to a vacuum oven and dried to constant weight to obtain a dried material. The dried material is added to a twin-screw blending extruder for granulation. The extrusion temperature is controlled at 210°C, and then the film is pressed on a flat vulcanizer to obtain a polyvinylidene fluoride film with a thickness of 100 μm.
[0066] Example 3
[0067] A polyvinylidene fluoride film with high infrared reflectivity comprises the following raw materials in parts by weight: 30 parts of polyvinylidene fluoride, 10 parts of modified polymethyl methacrylate, 5 parts of modified nano titanium dioxide, 1 part of plasticizer and 5 parts of solvent.
[0068] The modified polymethyl methacrylate used in this example is prepared by Preparation Example 4, and the modified nano titanium dioxide used is prepared by Preparation Example 1.
[0069] The method for preparing a polyvinylidene fluoride film having high infrared reflectivity comprises the following steps:
[0070] Polyvinylidene fluoride, modified polymethyl methacrylate, modified nano titanium dioxide, a plasticizer and a solvent are blended in a high-speed mixer, and then transferred to a vacuum oven and dried to constant weight to obtain a dried material. The dried material is added to a twin-screw blending extruder for granulation. The extrusion temperature is controlled at 220°C, and then the film is pressed on a flat vulcanizer to obtain a polyvinylidene fluoride film with a thickness of 10 μm.
[0071] Example 4
[0072] A polyvinylidene fluoride film with high infrared reflectivity and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified nano titanium dioxide used is prepared by Preparation Example 2.
[0073] Example 5
[0074] A polyvinylidene fluoride film with high infrared reflectivity and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified nano titanium dioxide used is prepared by Preparation Example 3.
[0075] Example 6
[0076] A polyvinylidene fluoride film with high infrared reflectivity and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified polymethyl methacrylate used is prepared by Preparation Example 5.
[0077] Comparative Example 1
[0078] A polyvinylidene fluoride film with high infrared reflectivity and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of nano titanium dioxide is used to replace the modified nano titanium dioxide.
[0079] Comparative Example 2
[0080] A polyvinylidene fluoride film with high infrared reflectivity and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of polymethyl methacrylate is used to replace the modified polymethyl methacrylate.
[0081] Performance Test:
[0082] The following performance tests were performed on the polyvinylidene fluoride films prepared in the above Examples 1-6 and Comparative Examples 1-2. The specific test results are shown in Table 1:
[0083] (1) Infrared reflection performance: The infrared reflectivity of the polyvinylidene fluoride film was tested using a Shimadzu UV-3600i Plus ultraviolet-visible-near-infrared spectrophotometer. The higher the infrared reflectivity, the better the performance.
[0084] (2) Mechanical properties: The weather resistance of polyvinylidene fluoride film is expressed by mechanical properties. The more stable the mechanical properties, the better the weather resistance of polyvinylidene fluoride film. The polyvinylidene fluoride film was cut into rectangles with a length of 150 mm, a width of 20 mm, and a thickness of 1 mm using a blade. The film was subjected to a simulated 480-hour natural light aging test, specifically, it was placed in an atmospheric light weather aging test chamber with a set temperature of 40°C, a humidity of 38°C, and an irradiation intensity of 230 w / m 2 , distance 26cm, the polyvinylidene fluoride film samples obtained before and after the aging test were tested for tensile strength and elongation at break using a WDW3020 micro-controlled electronic universal testing machine.
[0085] Table 1
[0086]
[0087] It can be seen from Table 1 that the polyvinylidene fluoride films provided in Examples 1 to 3 of the present invention have higher infrared reflectivity and better weather resistance, and the loss of mechanical properties before and after the 480h natural light aging test is small.
[0088] By comparing Example 4 with Example 1, it can be seen that when the amount of 3-(methacryloyloxy)propyltrimethoxysilane added to prepare modified nano-titanium dioxide is changed, the infrared reflectivity of the polyvinylidene fluoride film decreases, and the changes in tensile strength and elongation at break are relatively insignificant, which may be caused by the poor compatibility of nano-titanium dioxide.
[0089] By comparing Example 5 with Example 1, it can be seen that when the amount of sodium silicate added to prepare modified nano-titanium dioxide changes, the infrared reflectivity of the polyvinylidene fluoride film will decrease. This is because the coating amount of silicon dioxide coated on the nano-titanium dioxide changes, but it has little effect on the weather resistance of the polyvinylidene fluoride film, and the tensile strength and elongation at break of the polyvinylidene fluoride film change little.
[0090] By comparing Example 6 with Example 1, it can be seen that when the amount of hexafluorobutyl acrylate added to the modified polymethyl methacrylate is changed, the weather resistance of the polyvinylidene fluoride film will deteriorate, and both the tensile strength and the elongation at break will decrease significantly. This may be due to the decrease in the thermal stability of the polymethyl methacrylate in the polyvinylidene fluoride film due to the influence of the modified nano-titanium dioxide.
[0091] It can be seen from the comparison between Comparative Example 1 and Example 1 that when an equal amount of unmodified nano-titanium dioxide is added to replace the modified nano-titanium dioxide, the infrared reflectivity of the polyvinylidene fluoride film will be significantly deteriorated.
[0092] By comparing Comparative Example 2 with Example 1, it can be seen that when an equal amount of unmodified polymethyl methacrylate is added to replace the modified polymethyl methacrylate, the tensile strength and elongation at break of the polyvinylidene fluoride film will be significantly deteriorated, especially the elongation at break will decrease significantly. This may be because the thermal stability of polymethyl methacrylate is greatly affected by the system, and it is very easy to fracture brittlely after the aging test, resulting in a decrease in the mechanical properties of the polyvinylidene fluoride film and poor weather resistance.
[0093] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A polyvinylidene fluoride film with high infrared reflectivity, characterized in that: The polyvinylidene fluoride film comprises the following raw materials in parts by weight: 30 to 40 parts of polyvinylidene fluoride, 10 to 15 parts of modified polymethyl methacrylate, 5 to 10 parts of modified nano titanium dioxide, 1 to 5 parts of plasticizer and 5 to 10 parts of solvent.
2. A polyvinylidene fluoride film with high infrared reflectivity according to claim 1, characterized in that: The preparation steps of the modified nano titanium dioxide are as follows: The nano titanium dioxide and butyl acetate are stirred and mixed, and then a dispersing aid is added, and ultrasonic dispersion is performed for 10 to 30 minutes. The temperature is raised to 80 to 100° C., sodium silicate is added, and then an inorganic acid is added to adjust the pH value to 8 to 10. The mixture is kept warm and allowed to stand for 2 to 3 hours, and then a modifier is added. The mixture is stirred and mixed, and then high-temperature drying and grinding are performed to obtain the modified nano titanium dioxide.
3. A polyvinylidene fluoride film with high infrared reflectivity according to claim 2, characterized in that: The particle size of the nano titanium dioxide is 30-100 nm.
4. The polyvinylidene fluoride film with high infrared reflectivity according to claim 2, characterized in that: The modifier is at least one of stearic acid and a silane coupling agent.
5. The polyvinylidene fluoride film with high infrared reflectivity according to claim 2, characterized in that: The mass ratio of the nano titanium dioxide to the sodium silicate is 1:(1-3).
6. The polyvinylidene fluoride film with high infrared reflectivity according to claim 1, characterized in that: The preparation steps of the modified polymethyl methacrylate are as follows: Add ethyl acetate into the reactor and heat it to 70-80° C., then add the modified monomer, methyl methacrylate and the first weight portion of initiator in sequence, stir and mix, continue to heat to 80-90° C., react for 0.5-1h, then add the second weight portion of initiator, react for 4-7h, precipitate and dry to obtain the modified polymethyl methacrylate.
7. The polyvinylidene fluoride film with high infrared reflectivity according to claim 6, characterized in that: The modified monomer is hexafluorobutyl acrylate.
8. The polyvinylidene fluoride film with high infrared reflectivity according to claim 6, characterized in that: The mass ratio of the modified monomer to methyl methacrylate is (1-3):
10.
9. A method for preparing a polyvinylidene fluoride film with high infrared reflectivity according to any one of claims 1 to 8, characterized in that: The following steps are involved: Polyvinylidene fluoride, modified polymethyl methacrylate, modified nano titanium dioxide, a plasticizer and a solvent are blended in a high-speed mixer, and then transferred to a vacuum oven for drying to constant weight to obtain a dried material, the dried material is added to a twin-screw blending extruder for granulation, and then subjected to a flat-plate vulcanizer for film pressing to obtain the polyvinylidene fluoride film.
10. The method for preparing a polyvinylidene fluoride film with high infrared reflectivity according to claim 9, characterized in that: The thickness of the polyvinylidene fluoride film is 10-100 μm.
Citation Information
Patent Citations
Photovoltaic high and low temperature resistant polyvinylidene fluoride film and preparation method thereof
CN111234425A