Anion exchange chromatography medium and preparation method thereof
By synthesizing cationic block copolymers and adsorbing and chemical bonding of the matrix, the problems of low loading and complex preparation of anion exchange chromatography media are solved, and a high loading and high resolution anion exchange chromatography media is achieved, which is suitable for large-scale protein purification.
Patent Information
- Application Number
- CN202411836414.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-13
- Publication Date
- 2025-03-21
AI Technical Summary
In the prior art, the anion exchange chromatography medium has a low ion load, which is difficult to meet the requirements of large-scale protein purification, and the preparation method is cumbersome and the post-processing steps are many.
By synthesizing a cationic block copolymer, the matrix is first adsorbed and then chemically bonded, a high load and high resolution anion exchange chromatography medium was obtained. The process is simple in steps and has a high product load.
The high ion load and high resolution of anion exchange chromatography medium are achieved, and the loading of bovine serum albumin can reach more than 60.0 mg/mL. The preparation steps are simple, easy to industrially produce, good product stability, and the ligands are not easy to fall off.
Smart Images

Figure CN119657237A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biological separation and polymer materials, and in particular to a high-performance anion exchange chromatography medium and a preparation method thereof. Background Art
[0002] Chromatography is an important biological separation technology, which is widely used in biopharmaceuticals, medical treatment, environmental testing and food. Biomolecules can use different chromatography techniques according to their own special properties, such as ion exchange chromatography, hydrophobic chromatography, reverse phase chromatography and affinity chromatography.
[0003] Among them, ion exchange chromatography (IEC) has been applied to the separation of biomolecules since the 1960s and has always played an important role in the separation and purification of biomolecules. As one of the most widely used chromatographic techniques, ion chromatography is used for the separation and purification of proteins, peptides, nucleic acids and other charged biomolecules. This technology can separate different molecules with only slight differences in charge, such as two proteins with only one charged amino acid difference. In the ion exchange chromatography separation process, the binding and elution of specific molecules are achieved by controlling the reversible interaction between the charged molecules and the ion exchange fillers with opposite charges, thereby achieving the separation effect. The net surface charge of proteins in an environment with the same pH value as the isoelectric point is zero, and they will not interact with the charged fillers. However, when the pH value of the environment is higher than its isoelectric point, the protein will bind to the filler with a positive charge, that is, the anion exchange medium; and when the pH value of the environment is lower than its isoelectric point, the protein will bind to the filler with a negative charge, that is, the cation exchange medium. Therefore, ion exchange chromatography is divided into cation exchange chromatography and anion exchange chromatography.
[0004] The commonly used carrier coupling ligand for anion exchange chromatography media is ammonium ion. CN106824307A discloses a mixed anion exchange medium and a preparation method thereof. The mixed anion exchange medium uses agarose as a medium, and phenyl glycidyl ether and 2,3-epoxypropyltrimethylammonium chloride are bonded to the surface, thereby obtaining a mixed anion exchange medium having both hydrophobic interaction and a strong anion exchange mode. However, the anion exchange medium prepared by the invention has a low ion load and is difficult to meet the requirements of large-scale protein purification. CN109806916A discloses a high-performance anion exchange medium and a preparation method thereof. The invention uses agarose as a medium, first activates the matrix with allyl glycidyl ether, then brominates and grafts dextran, and then couples with anion exchange ligands to obtain the final product. The preparation method of the invention is relatively cumbersome, and there are many post-processing steps. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a high-load and high-resolution anion exchange chromatography medium. Compared with the traditional preparation process, the method has the advantages of simple steps and high product loading, and obtains the target product by synthesizing a cationic block copolymer, first adsorbing the matrix and then chemically bonding it; the anion exchange chromatography medium prepared by the method can have a loading capacity of more than 60.0 mg / mL for bovine serum albumin (BSA).
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] A method for preparing an anion exchange chromatography medium comprises the following steps:
[0008] S1. Preparation of cationic block copolymer:
[0009] In a polar solvent, an allyl epoxy compound, an ammonium chloride salt monomer and an initiator are added to initiate a polymerization reaction to obtain a cationic block copolymer, an organic solvent is added to precipitate the copolymer, and the product is obtained after washing and drying; wherein the cationic block copolymer has the following structure:
[0010]
[0011] n = 35-80;
[0012] S2. Coating of cationic block copolymer on the substrate surface:
[0013] The cationic block copolymer prepared in step S1 is dissolved in water, and a matrix is added. After the mixture is dispersed, it is stirred and swelled so that the cationic block covers the surface of the matrix and the inside of the pores;
[0014] S3. Bonding of cationic block copolymers on the substrate surface
[0015] Add an alkaline substance to the reaction system of step S2 for reaction, and obtain an anion exchange chromatography medium after washing.
[0016] Preferably, the polar solvent in step S1 is selected from one or more of dioxane, dimethyl sulfoxide, N,N-dimethylformamide and methanol. The monomers include allyl epoxy compounds and ammonium chloride salt monomers, and the polar solvent is 10-30 times the mass of the monomers.
[0017] Preferably, the allyl epoxy compound in the above step S1 includes glycidyl methacrylate and allyl glycidyl ether, etc. The allyl epoxy compound of the present invention is not limited to the above two types, and any monomer with double bonds and epoxy can be used.
[0018] Preferably, the ammonium chloride salt monomer in the above step S1 includes allyltrimethylammonium chloride, (3-acrylamidopropyl)trimethylammonium chloride, dimethyldiallylammonium chloride, acryloyloxyethyltrimethylammonium chloride, methacryloyloxyethyltrimethylammonium chloride and the like.
[0019] Preferably, the mass ratio of the allyl epoxy compound to the ammonium chloride salt monomer is (1-10):(10-1), for example, it can be 1:10, 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc.; preferably, the mass ratio of the allyl epoxy compound to the ammonium chloride salt monomer is 1:0.5-1.5.
[0020] Preferably, the initiator in the above step S1 is preferably an organic initiator, including but not limited to azobisisobutyronitrile (AIBN), benzoyl peroxide (BPO), tert-butyl perbenzoate (TBPB), etc., and the mass fraction of the initiator to the monomer is 1%-10%, preferably 4%.
[0021] Preferably, the free radical initiation temperature in the above step S1 is 40-100°C, for example, it can be 40°C, 60°C, 70°C, 90°C, 100°C, preferably 70°C; the reaction time is 4-24h, for example, it can be 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 24h, preferably 20h.
[0022] Preferably, the organic solvent in the above step S1 is selected from one or more of toluene, n-hexane and n-heptane.
[0023] The volume (ml) of the organic solvent used is 5-10 times the mass (g) of the final copolymer.
[0024] Furthermore, in the above step S2, the concentration of the cationic block copolymer aqueous solution is 5%-20%, preferably 10%, and the mass ratio of the substrate to the cationic block copolymer is 6:1-1:2, preferably 1-2:1.
[0025] Furthermore, in the above step S2, the matrix includes agarose microspheres, dextran microspheres and polystyrene microspheres, preferably hydrophilically modified polystyrene microspheres, with a particle size of 15-100 μm, a pore size of 50 nm-150 nm, and a cross-linking degree of 10%-80%.
[0026] Furthermore, in the above step S2, the stirring speed is 100 rpm-500 rpm, and the swelling time is 8 h-24 h.
[0027] Preferably, the alkaline substance in the above step S3 is sodium hydroxide or potassium hydroxide, preferably sodium hydroxide, and its concentration is 5%-50%.
[0028] Preferably, in the above step S3, the reaction temperature is 40°C-70°C, and the reaction time is 10h-24h.
[0029] The second object of the present invention is to provide an anion exchange chromatography medium obtained by the preparation method.
[0030] In the present invention, a cationic block copolymer is first synthesized by free radical initiated polymerization, and the polymer is characterized by high ion density and good hydrophilicity; the cationic block copolymer is coated on the surface of the filler matrix by physical adsorption, and further a high-load and high-resolution anion exchange chromatography medium is obtained by chemical bonding under alkaline conditions.
[0031] The beneficial effects of the present invention are as follows: the method bonds a cationic block copolymer with high ion density on the surface of a filler matrix, which can significantly improve the ion loading capacity; secondly, bonding the polymer on the surface of the matrix can form a long-chain hydrophilic spacer arm, which can effectively reduce the spatial position and thus improve the protein loading capacity. The anion exchange chromatography medium prepared by the method can have a loading capacity of bovine serum albumin (BSA) of more than 60.0 mg / mL; thirdly, the method has simple preparation steps and is easy to industrialize, and the prepared anion exchange chromatography medium has the characteristics of good stability and the ligand is not easy to fall off. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is an electron micrograph of a 15 μm anion exchange chromatography medium of Example 5;
[0033] Figure 2 This is a chromatogram of the functional test of the anion exchange chromatography medium prepared in Example 5. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below with reference to the embodiments, but is not limited thereto.
[0035] Example 1: Preparation of cationic block copolymer
[0036] Weigh 10.5g of glycidyl methacrylate and 12.0g of allyltrimethylammonium chloride, transfer them to a 1000mL three-necked flask, add 400mL of dioxane solvent, mix the reactants thoroughly at 200rpm, then add 0.67g of AIBN, pass nitrogen for 30min, raise the temperature to 70°C, react for 20h, remove the high temperature after the reaction and allow the reaction system to cool naturally to room temperature, add 10mL of n-hexane to precipitate the product, filter and wash with 100mL of n-hexane, and finally vacuum dry at 60°C to obtain the dried product, 14.5g, yield 64.4%, purity 82.5%.
[0037] Example 2: Preparation of cationic block copolymer
[0038] Weigh 10.0g of allyl glycidyl ether and 8.0g of dimethyldiallylammonium chloride, transfer them to a 1000mL three-necked flask, add 400mL of dimethyl sulfoxide solvent, mix the reactants thoroughly at 200rpm, then add 0.55g of BPO, pass nitrogen for 30min, raise the temperature to 80°C, react for 20h, remove the high temperature after the reaction and allow the reaction system to cool naturally to room temperature, add 10mL of n-hexane to precipitate the product, filter and wash with 100mL of n-hexane, and finally vacuum dry at 60°C to obtain the dried product, 13.6g, yield 75.6%, purity 80%.
[0039] Example 3: Preparation of cationic block copolymer
[0040] Weigh 15.0g of glycidyl methacrylate and 10.0g of (3-acrylamidopropyl)trimethylammonium chloride, transfer to a 1000mL three-necked flask, add 350mL of dioxane solvent, mix the reactants thoroughly at 200rpm, then add 1.0g of TBPB, pass nitrogen for 30min, heat to 80°C, react for 20h, remove the high temperature after the reaction is completed, let the reaction system cool naturally to room temperature, add 10mL of toluene to precipitate the product, filter and wash with 150mL of toluene, and finally vacuum dry at 60°C to obtain the dried product, 16.7g, yield 66.8%, purity 77.8%.
[0041] Example 4: Preparation of cationic block copolymer
[0042] Weigh 12.0g of allyl glycidyl ether and 10.0g of acryloyloxyethyl trimethylammonium chloride, transfer them to a 1000mL three-necked flask, add 350mL of N,N-dimethylformamide solvent, mix the reactants thoroughly at 200rpm, then add 0.88g of TBPB, raise the temperature to 70°C, react for 24h, remove the high temperature after the reaction and allow the reaction system to cool naturally to room temperature, add 10mL of toluene to precipitate the product, filter and wash with 100mL of toluene, and finally vacuum dry at 60°C to obtain the dried product, 15.2g, yield 69.1%, purity 79.0%.
[0043] Example 5: Cationic block copolymer grafted onto substrate surface
[0044] Weigh 10.0g of the block copolymer of glycidyl methacrylate and allyl trimethyl ammonium chloride into a 500mL flask, add 200mL of water to fully dissolve the polymer, then add 15.0g of hydrophilically modified polystyrene microspheres (particle size 15μm, pore size 50nm), ultrasonically disperse, and allow the polymer solution to fully infiltrate the surface of the polystyrene microspheres and the inside of the pores. The suspension was stirred at 25°C and 200rpm for 24h. 10.0g of NaOH was added to the suspension, the temperature was raised to 60°C, and the reaction was carried out for 18h. After the reaction, the product was filtered and washed alternately with 100mL of water and 100mL of ethanol to obtain an anion exchange chromatography medium with a BSA loading of 62.0mg / mL and an ion loading of 0.3645mmol / mL.
[0045] Example 6: Grafting of cationic block copolymers on substrate surfaces
[0046] Weigh 15.0g of the block copolymer of allyl glycidyl ether and dimethyl diallyl ammonium chloride into a 500mL flask, add 300mL of water to fully dissolve the polymer, then add 25.0g of hydrophilically modified polystyrene microspheres (particle size 30μm, pore size 70nm), ultrasonically disperse, and allow the polymer solution to fully infiltrate the surface of the polystyrene microspheres and the inside of the pores. The suspension was stirred at 25°C and 200rpm for 24h. 30.0g of NaOH was added to the suspension, the temperature was raised to 60°C, and the reaction was carried out for 18h. After the reaction, the product was filtered and washed alternately with 150mL of water and 150mL of ethanol to obtain an anion exchange chromatography medium with a BSA loading of 65.0mg / mL and an ion loading of 0.3428mmol / mL.
[0047] Example 7: Cationic block copolymer grafted onto substrate surface
[0048] Weigh 10.0g of the block copolymer of glycidyl methacrylate and (3-acrylamidopropyl) trimethylammonium chloride into a 500mL flask, add 200mL of water to fully dissolve the polymer, then add 20.0g of hydrophilically modified polystyrene microspheres (particle size 50μm, pore size 100nm), ultrasonically disperse, and allow the polymer solution to fully infiltrate the surface of the polystyrene microspheres and the inside of the pores. The suspension was stirred at 25°C and 200rpm for 24h. Add 25.0g of NaOH to the suspension, heat to 60°C, react for 18h, and filter the product after the reaction. Wash it alternately with 150mL of water and 150mL of ethanol to obtain an anion exchange chromatography medium with a BSA loading of 75.0mg / mL and an ion loading of 0.3276mmol / mL.
[0049] Example 8: Cationic block copolymer grafted onto substrate surface
[0050] Weigh 18.0g of the block copolymer of allyl glycidyl ether and acryloyloxyethyl trimethylammonium chloride into a 500mL flask, add 300mL of water to fully dissolve the polymer, then add 30.0g of hydrophilically modified polystyrene microspheres (particle size 50μm, pore size 100nm), ultrasonically disperse, and allow the polymer solution to fully infiltrate the surface of the polystyrene microspheres and the inside of the pores. The suspension was stirred at 25°C and 200rpm for 24h. 30.0g of NaOH was added to the suspension, the temperature was raised to 70°C, and the reaction was carried out for 24h. After the reaction, the product was filtered and washed alternately with 200mL of water and 200mL of ethanol to obtain an anion exchange chromatography medium with a BSA loading of 70.0mg / mL and an ion loading of 0.3905mmol / mL.
[0051] Example 9: Anion exchange chromatography medium stability experiment
[0052] 4 g of the anion exchange chromatography medium prepared in Example 5 was dispersed in a 1 M NaOH solution and shaken in a constant temperature shaker at 40° C. for 24 h, and its ion loading and BSA loading were measured.
[0053] Ion loading test conditions
[0054] 1. Load the pretreated chromatographic medium into a column (column specification: 4.7 mL preloaded column);
[0055] 2. Rinse the pre-packed column with 50 mL of ultrapure water;
[0056] 3. Use 65mL of 0.1mol / L hydrochloric acid solution containing 5% sodium chloride for the first balance;
[0057] 4. Continue to balance with 65mL of 0.001mol / L hydrochloric acid solution, and rinse the pre-packed column with ultrapure water after balance;
[0058] 5. Load: 25mL of 0.1mol / L sodium hydroxide standard solution and collect;
[0059] 6. After loading, rinse the pre-packed column with 50 mL of ultrapure water and collect;
[0060] 7. Calculate the loading by acid titration: Q = (C sodium hydroxide * 25-C hydrochloric acid * V) / 4.7.
[0061] BSA loading test conditions
[0062] Balance solution: 20 mM Bis-Tris, pH 7.0;
[0063] Elution buffer: 20 mM Bis-Tris, 1 M NaCl, pH 7.0;
[0064]
[0065] After alkali treatment, the ion load of the anion exchange chromatography medium was measured to be 0.3565 mmol / mL, a decrease of about 2.2%, and the BSA load was 60.7 mg / mL, a decrease of about 2.1%; therefore, it can be seen that the anion exchange chromatography medium synthesized by this method has obvious advantages in alkali tolerance, has good stability, and the ligand is not easy to fall off, which can extend the service life of the chromatography medium.
[0066] Example 10: Functional Test
[0067] Materials: Anion exchange chromatography medium prepared in Example 5
[0068] Sample: GammaBind G type 2, 5.33 mg / mL
[0069] β-Lactoglobulin A, 11 mg / mL
[0070] β-Lactoglobulin B, 11 mg / mL
[0071] Balance solution: 20 mM piperazine hexahydrate, pH 6.2
[0072] Eluent: 20 mM piperazine hexahydrate, 0.3 M NaCl, pH 6.2
[0073]
[0074] Functional chromatograms such as Figure 2As shown in the figure, the anion exchange chromatography medium prepared in Example 5 can effectively separate three different types of proteins, GammaBind G type 2, β-Lactoglobulin A, and β-Lactoglobulin B. The degree of separation of the different peaks eluted is high, and the peaks are narrow and symmetrical, indicating that the chromatography medium has good selectivity for the three proteins and high resolution.
[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing an anion exchange chromatography medium, characterized in that: The following steps are involved: S1. Preparation of cationic block copolymer: In a polar solvent, an allyl epoxy compound, an ammonium chloride salt monomer and an initiator are added to initiate a polymerization reaction to obtain a cationic block copolymer, an organic solvent is added to precipitate the copolymer, and the product is obtained after washing and drying; The cationic block copolymer has the following structure: n=35-80; S2. Coating of cationic block copolymer on the substrate surface: The cationic block copolymer prepared in step S1 is dissolved in water, and a matrix is added. After the mixture is dispersed, it is stirred and swelled so that the cationic block covers the surface of the matrix and the inside of the pores; S3. Bonding of cationic block copolymers on the substrate surface Add an alkaline substance to the reaction system of step S2 for reaction, and obtain an anion exchange chromatography medium after washing.
2. The preparation method according to claim 1, characterized in that: The allyl epoxy compound in step S1 includes glycidyl methacrylate and allyl glycidyl ether.
3. The preparation method according to claim 1, characterized in that: The ammonium chloride salt monomers in step S1 include allyl trimethyl ammonium chloride, (3-acrylamidopropyl) trimethyl ammonium chloride, dimethyl diallyl ammonium chloride, acryloyloxyethyl trimethyl ammonium chloride, and methacryloyloxyethyl trimethyl ammonium chloride.
4. The preparation method according to claim 1, characterized in that: In the step S1, the mass ratio of the allyl epoxy compound to the ammonium chloride salt monomer is 1-10:10-1.
5. The preparation method according to claim 1, characterized in that: In the step S1, the initiator is selected from azobisisobutyronitrile, benzoyl peroxide, and tert-butyl perbenzoate; the ratio of the mass of the initiator to the mass of the allyl epoxy compound and the ammonium chloride salt monomer is 1%-10%.
6. The preparation method according to claim 1, characterized in that: In the step S1, the polar solvent is selected from one or more of dioxane, dimethyl sulfoxide, N,N-dimethylformamide and methanol; the organic solvent in the step S1 is selected from one or more of toluene, n-hexane and n-heptane.
7. The preparation method according to claim 1, characterized in that: In the step S1, the initiation temperature of the initiator is 40-100° C., and the reaction time is 4-24 hours.
8. The preparation method according to claim 1, characterized in that: In the step S2, the concentration of the cationic block copolymer aqueous solution is 5%-20%, and the mass ratio of the matrix to the cationic block copolymer is 6:1-1:2; in the step S2, the matrix includes agarose microspheres, dextran microspheres and polystyrene microspheres, the stirring speed is 100rpm-500rpm, and the swelling time is 8h-24h.
9. The preparation method according to claim 1, characterized in that: In step S3, the alkaline substance is sodium hydroxide or potassium hydroxide, and the concentration thereof is 5%-50%; the reaction temperature is 40° C.-70° C., and the reaction time is 10h-24h.
10. An anion exchange chromatography medium obtained according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Mixed type anion exchange medium and preparation method thereof
CN106824307A
High-property anion exchange medium and preparation method thereof
CN109806916A