Uv resistant bio-based thermoplastic polyurethane and method of making same

By using bio-based mucoacinol to synthesize bio-based polyester diol and reacting it with diisocyanate, a UV-resistant bio-based thermoplastic polyurethane with good UV absorption and transparency was prepared, which solved the problem of poor UV resistance of existing materials and is suitable for UV protection and building materials.

CN120463905BActive Publication Date: 2025-11-21HUADA CHEM GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510969045.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-15
Publication Date
2025-11-21
Estimated Expiration
2045-07-15

AI Technical Summary

Technical Problem

Existing bio-based thermoplastic polyurethane materials have poor UV resistance and complex preparation methods, which may affect transparency and compatibility.

Method used

Bio-based polyester diols were synthesized using bio-based mucoconic acid. Through the reaction with diisocyanate, chain extender and antioxidant, UV-resistant bio-based thermoplastic polyurethane with UV absorption function was prepared, while maintaining good transparency and tensile strength.

Benefits of technology

The prepared UV-resistant bio-based thermoplastic polyurethane maintains high tensile strength after UV aging and is suitable for UV protection coatings, building materials and sun protection fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application belongs to the technical field of thermoplastic polyurethane elastomer, and relates to a UV-resistant bio-based thermoplastic polyurethane and a preparation method thereof.The UV-resistant bio-based thermoplastic polyurethane comprises the following components in parts by weight: bio-based polyester diol 35-70 parts; diisocyanate 15-55 parts; chain extender 2-15 parts; antioxidant 0.2-1 part; catalyst 0.001-0.05 part; the bio-based polyester diol is obtained by polycondensation of dicarboxylic acid and dihydric alcohol; the dicarboxylic acid comprises biomass muconic acid.The present application uses bio-based muconic acid with ultraviolet absorption function to synthesize bio-based polyester diol, realizes the characteristics of bio-based and UV resistance, and the thermoplastic polyurethane obtained in this way has good ultraviolet light absorption function and good transparency, has a high tensile strength retention rate after ultraviolet aging, and can be used in the fields of ultraviolet protection coating, building materials and sunscreen fabric.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application belongs to the technical field of thermoplastic polyurethane elastomer, and relates to a UV-resistant bio-based thermoplastic polyurethane and a preparation method thereof. BACKGROUND

[0002] Most of the monomers used to synthesize polyurethane are fossil fuels, which are non-renewable resources. With the intensification of fossil fuel shortage and the aggravation of environmental pollution, the development and use of bio-based polyols to synthesize polyurethane have become a research hotspot at the present stage. The existing bio-based thermoplastic polyurethane and petrochemical-based thermoplastic polyurethane both have the disadvantage of poor UV resistance. Improving the UV resistance of thermoplastic polyurethane is mainly achieved by adding ultraviolet absorbers and inorganic fillers, which has the problems of complex preparation method, reduced transparency and poor compatibility.

[0003] Chinese patent application CN118755252A uses benzophenone to modify graphene, and then reacts with polyol and diisocyanate to obtain a UV-resistant thermoplastic polyurethane elastomer. However, its preparation method is complex, and it will have a certain impact on the light transmittance of the polyurethane product. Chinese patent CN115304737B discloses a low-temperature-resistant shoe material polyurethane elastomer and its preparation process. 2,2'-dihydroxy-4-methoxybenzophenone with UV resistance is used as a polyol, and wear-resistant agents, toughening agents, grafting agents and other additives are introduced to obtain a polyurethane elastomer with good UV aging resistance. However, its preparation method is complex. Chinese patent CN117757407B discloses an anti-UV garment fabric adhesive, its preparation method and application. Esterified modified silk fibroin and nano-silicon dioxide are used to synergistically enhance the anti-UV performance of the thermoplastic polyurethane elastomer hot melt adhesive. The above methods can improve the UV resistance of thermoplastic polyurethane, but may have the problems of poor compatibility and complex preparation method. Chinese patent application CN113861363A discloses a preparation method of an anti-UV transparent lignin-based polyurethane elastomer. Natural lignin polyol is directly used as a capping agent in the synthesis process, which has a certain absorption effect on ultraviolet light. However, the polyurethane elastomer prepared by this method has a deep color, which may reduce the visible light transmittance. SUMMARY

[0004] The present application provides a UV-resistant bio-based thermoplastic polyurethane and a preparation method thereof to solve the problems of the prior art.

[0005] The first object of the present application is to provide a UV-resistant bio-based thermoplastic polyurethane, which comprises the following components by weight:

[0006] Bio-based polyester diol: 35-70 parts; diisocyanate: 15-55 parts; chain extender: 2-15 parts; antioxidant: 0.2-1 part; catalyst: 0.001-0.05 parts;

[0007] The bio-based polyester diol is obtained by polycondensation of dicarboxylic acid and dihydric alcohol; the dicarboxylic acid includes biomass muconic acid.

[0008] The bio-based polyester diol is synthesized by using bio-based muconic acid with ultraviolet absorption function, realizing the characteristics of bio-based and UV resistance, and the thermoplastic polyurethane obtained by the method has good ultraviolet light absorption function and good transparency, and has a high tensile strength retention rate after ultraviolet aging.

[0009] Further, the molar ratio of the dicarboxylic acid to the dihydric alcohol is 1:1.01-1.5; the biomass muconic acid accounts for 5%-100% of the total mass of the dicarboxylic acid.

[0010] Further, the dicarboxylic acid further includes one or more of malonic acid, 1,4-succinic acid, 1,5-pentanedioic acid, 2-methyl-1,4-butanedioic acid, 2,2-dimethyl-1,3-propanedioic acid, 1,6-hexanedioic acid, alpha-methyl glutaric acid, beta-methyl glutaric acid, alpha-ethyl succinic acid, alpha-(dimethyl) succinic acid, n-propyl malonic acid, 1,7-heptanedioic acid, octanedioic acid, nonanedioic acid, decanedioic acid, dodecanedioic acid, dimer acid, terephthalic acid, isophthalic acid, and phthalic acid.

[0011] Further, the dihydric alcohol is one or more of ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,2-butanediol, 1,3-butanediol, 1,2-pentanediol, 1,5-pentanediol, 2,5-dimethyl-2,5-hexanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, dipropylene glycol, and diethylene glycol.

[0012] Further, the preparation method of the bio-based polyester diol includes the following steps:

[0013] The dicarboxylic acid and the dihydric alcohol are put into a reactor under nitrogen protection, stirred and heated, reacted at 140-180°C for 3-5h, then heated to 190-230°C at a heating rate of 20-30°C / h, reacted for 2-5h, 20-120ppm of a titanate catalyst or an organotin catalyst is added, reacted for 1-3h, then vacuum is opened to remove water and small molecule alcohol in the system, and the reaction is continued until the acid value and the hydroxyl value are qualified; the hydroxyl value is 20-200mg KOH / g, and the acid value is 0.15-0.35mg KOH / g.

[0014] Further, the diisocyanate is one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, xylylene diisocyanate, 1,5-naphthalene diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-cyclohexane diisocyanate, 1-methyl-2,4-cyclohexane diisocyanate, 1-methyl-2,6-cyclohexane diisocyanate, 2-methylpentamethylene-1,5-diisocyanate, 2-ethylbutylene-1,4-diisocyanate, pentamethylene-1,5-diisocyanate, butylene-1,4-diisocyanate.

[0015] Further, the isocyanate index of the diisocyanate is 0.95-1.05.

[0016] Further, the chain extender is one or more of ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,2-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,8-octanediol, 1,9-nonanediol, benzene glycol, dihydroxybenzene, trihydroxymethylpropane, glycerol, 3,3-dichloro-4,4'-diaminodiphenyl methane, isophorone diamine, 4,4'-diaminodiphenyl methane, 2-methyl-1,3-propanediol, neopentyl glycol, 1,1-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 2,4-toluene diamine, 2,6-toluene diamine, 3,5-diethyl-2,4-toluene diamine, 1,4-bis(β-hydroxyethyl)-hydroquinone, 1,4-bis(β-hydroxyethyl)-bisphenol A, ethylenediamine, 1,2-propanediamine, 1,3-propanediamine, N-methyl-propane-1,3-diamine, N,N'-dimethylethylenediamine, diethanolamine.

[0017] Further, the antioxidant is one or more of pentaerythritol tetrakis [3- (3, 5-di-tert-butyl-4-hydroxyphenyl) propionate] (Irganox 1010), 1, 3, 5-tris (3, 5-di-tert-butyl-4-hydroxybenzyl) -1, 3, 5-triazine-2, 4, 6 (1H, 3H, 5H) -trione (Irganox 3114), tris (2, 4-di-tert-butylphenyl) phosphite (Igrafos 168), bis (2, 4-bis (1, 1-dimethylethyl) -6-methylphenyl) ethyl phosphite (Igrafos 38); the catalyst is one of stannous octoate, dibutyltin dilaurate, dibutyltin diacetate, bis (dodecylthio) dibutyltin.

[0018] The second object of the present application is to provide a preparation method of the above-mentioned UV-resistant bio-based thermoplastic polyurethane, comprising the following steps:

[0019] The diisocyanate is heated and melted, the bio-based polyester diol, antioxidant and catalyst are added, and the mixture is reacted at 60-110 DEG C for 0.5-4 h to form a prepolymer; then a chain extender is added, the chain extender is mixed with the prepolymer uniformly, and the mixture is aged at 90-130 DEG C for 8-24 h to obtain the UV-resistant bio-based thermoplastic polyurethane.

[0020] The present application has the following advantages:

[0021] The UV-resistant bio-based thermoplastic polyurethane provided by the present application has good ultraviolet absorption function and transparency, has a high tensile strength retention rate after ultraviolet aging, and can be used in the fields of ultraviolet protection coating, building materials and sunscreen fabric. DETAILED DESCRIPTION

[0022] The principles and characteristics of the present application are described below in combination with examples, and the examples are only used to explain the present application and not to limit the scope of the present application.

[0023] Example 1:

[0024] A UV-resistant bio-based thermoplastic polyurethane comprises the following components by weight:

[0025] Bio-based polyester diol: 59.38 parts; diphenylmethane diisocyanate (MDI): 31.70 parts; chain extender 1, 4-butanediol: 8.60 parts; antioxidant pentaerythritol tetrakis [3- (3, 5-di-tert-butyl-4-hydroxyphenyl) propionate] (Irganox 1010): 0.30 parts; catalyst dibutyltin dilaurate: 0.02 parts;

[0026] The preparation method of the bio-based polyester diol comprises the following steps:

[0027] Under nitrogen protection, 100 parts of muconic acid and 1900 parts of 1,6-hexanedioic acid, 1296.35 parts of 1,4-butanediol were put into a reactor, heated and stirred, reacted at 160℃ for 4h, then heated to 210℃ at a heating rate of 25℃ / h for 3.5h, 70ppm of titanium isopropylate catalyst was added, reacted for 2h, then vacuum was opened to remove water and small molecule alcohol in the system, and the reaction continued until the acid value was 0.25mg KOH / g and the hydroxyl value was 56.0mg KOH / g, and the moisture was 72ppm.

[0028] The preparation method of the UV-resistant bio-based thermoplastic polyurethane comprises the following steps:

[0029] Diphenylmethane diisocyanate was heated and melted, bio-based polyester diol, antioxidant and catalyst were added, and the pre-polymer was generated after reaction at 80℃ for 2h; then chain extender was added to mix the chain extender with the pre-polymer uniformly, and the UV-resistant bio-based thermoplastic polyurethane was obtained after aging at 110℃ for 16h.

[0030] Example 2:

[0031] A UV-resistant bio-based thermoplastic polyurethane comprises the following components by weight:

[0032] Bio-based polyester diol: 59.27 parts; dicyclohexylmethane diisocyanate (HMDI): 31.67 parts; chain extender 2-methyl-1,3-propanediol: 8.73 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyltin dilaurate: 0.03 parts;

[0033] The preparation method of the bio-based polyester diol comprises the following steps:

[0034] Under nitrogen protection, 200 parts of muconic acid and 800 parts of 1,4-butanedioic acid, 773.07 parts of 1,4-butanediol were put into a reactor, heated and stirred, reacted at 160℃ for 4h, then heated to 210℃ at a heating rate of 25℃ / h for 3.5h, 70ppm of titanium isopropylate catalyst was added, reacted for 2h, then vacuum was opened to remove water and small molecule alcohol in the system, and the reaction continued until the acid value was 0.30mg KOH / g and the hydroxyl value was 56.2mg KOH / g, and the moisture was 106ppm.

[0035] The preparation method of the UV-resistant bio-based thermoplastic polyurethane is the same as that in Example 1, which will not be repeated here.

[0036] Example 3:

[0037] A UV resistant bio-based thermoplastic polyurethane, comprising the following components by weight:

[0038] Bio-based polyester diol: 57.27 parts; MDI: 33.69 parts; chain extender 1,4-butanediol: 8.72 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyl tin dilaurate: 0.02 parts;

[0039] The preparation method of the bio-based polyester diol comprises the following steps:

[0040] Under nitrogen protection, 500 parts of muconic acid and 750 parts of 1,6-hexanedioic acid, and 564.08 parts of ethylene glycol were put into a reactor, heated and stirred, reacted at 160°C for 4h, then heated to 210°C at a heating rate of 25°C / h, reacted for 3.5h, added titanium isopropyl titanate catalyst 70ppm, reacted for 2h, then opened the vacuum to remove water and small molecule alcohol in the system, and continued to react until the acid value was 0.23mg KOH / g and the hydroxyl value was 56.3mg KOH / g, and the moisture was 86ppm.

[0041] The preparation method of the UV resistant bio-based thermoplastic polyurethane is the same as that of Example 1, which is not repeated here.

[0042] Example 4:

[0043] A UV resistant bio-based thermoplastic polyurethane, comprising the following components by weight:

[0044] Bio-based polyester diol: 57.88 parts; MDI: 33.34 parts; chain extender 2-methyl-1,3-propanediol: 8.46 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyl tin dilaurate: 0.02 parts;

[0045] The preparation method of the bio-based polyester diol comprises the following steps:

[0046] Under nitrogen protection, 1000 parts of muconic acid and 666.67 parts of terephthalic acid, and 882.89 parts of 1,3-propanediol were put into a reactor, heated and stirred, reacted at 160°C for 4h, then heated to 210°C at a heating rate of 25°C / h, reacted for 3.5h, added titanium isopropyl titanate catalyst 70ppm, reacted for 2h, then opened the vacuum to remove water and small molecule alcohol in the system, and continued to react until the acid value was 0.28mg KOH / g and the hydroxyl value was 56.1mg KOH / g, and the moisture was 90ppm.

[0047] The method for preparing the UV-resistant bio-based thermoplastic polyurethane is the same as that in Embodiment 1, which is not repeated here.

[0048] Embodiment 5

[0049] A UV-resistant bio-based thermoplastic polyurethane comprises the following components in parts by weight:

[0050] Bio-based polyester diol: 59.34 parts; hexamethylene diisocyanate (HDI): 32.15 parts; chain extender 1,4-butanediol: 8.18 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyltin dilaurate: 0.03 parts;

[0051] The method for preparing the bio-based polyester diol comprises the following steps:

[0052] Under nitrogen protection, 1000 parts of muconic acid and 250 parts of 1,6-adipic acid and 1085.44 parts of dihydric alcohol 1,6-hexanediol are put into a reactor, heated and stirred, reacted at 160°C for 4h, then heated to 210°C at a heating rate of 25°C / h, reacted for 3.5h, 70ppm of titanium isopropyl titanate catalyst is added, reacted for 2h, then vacuum is opened to remove water and small molecule alcohol in the system, and continue to react until the acid value is 0.22mgKOH / g and the hydroxyl value is 55.9mgKOH / g, and the moisture is 110ppm.

[0053] The method for preparing the UV-resistant bio-based thermoplastic polyurethane is the same as that in Embodiment 1, which is not repeated here.

[0054] Embodiment 6

[0055] A UV-resistant bio-based thermoplastic polyurethane comprises the following components in parts by weight:

[0056] Bio-based polyester diol: 59.58 parts; MDI: 31.61 parts; chain extender 1,4-butanediol: 8.49 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyltin dilaurate: 0.02 parts;

[0057] The method for preparing the bio-based polyester diol comprises the following steps:

[0058] Under nitrogen protection, 1000 parts of oxalic acid and 640.50 parts of dihydric alcohol 1,4-butanediol were put into a reactor, heated and stirred, reacted at 160°C for 4h, then heated to 210°C at a heating rate of 25°C / h, reacted for 3.5h, 70ppm of titanium acid tetraisopropyl ester catalyst was added, reacted for 2h, then opened the vacuum to remove water and small molecule alcohol in the system, and the reaction was continued until the acid value was 0.27mg KOH / g and the hydroxyl value was 55.9mg KOH / g, and the moisture was 120ppm.

[0059] The preparation method of the UV-resistant bio-based thermoplastic polyurethane is the same as that of Example 1, which is not repeated here.

[0060] Example 7:

[0061] A UV-resistant bio-based thermoplastic polyurethane, comprising the following components by weight:

[0062] Bio-based polyester diol: 59.58 parts; MDI: 31.61 parts; chain extender 2-methyl-1,3-propanediol: 8.49 parts; antioxidant pentaerythritol tetra[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyltin dilaurate: 0.02 parts;

[0063] The preparation method of the bio-based polyester diol is the same as that of Example 6, which is not repeated here.

[0064] The preparation method of the UV-resistant bio-based thermoplastic polyurethane is the same as that of Example 1, which is not repeated here.

[0065] Example 8:

[0066] A UV-resistant bio-based thermoplastic polyurethane, comprising the following components by weight:

[0067] Bio-based polyester diol: 59.56 parts; HMDI: 31.82 parts; chain extender 1,4-butanediol: 8.30 parts; antioxidant pentaerythritol tetra[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyltin dilaurate: 0.02 parts;

[0068] The preparation method of the bio-based polyester diol is the same as that of Example 6, which is not repeated here.

[0069] The preparation method of the UV-resistant bio-based thermoplastic polyurethane is the same as that of Example 1, which is not repeated here.

[0070] Comparative Example 1:

[0071] A thermoplastic polyurethane, comprising the following components by weight:

[0072] Polybutylene adipate diol (PBA2000): 58.28 parts; MDI: 32.41 parts; chain extender 1,4-butanediol: 8.99 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyl tin dilaurate: 0.02 parts;

[0073] The method for preparing the thermoplastic polyurethane comprises the following steps:

[0074] The diisocyanate is heated and melted, polybutylene adipate diol PBA2000, a catalyst are added, and a prepolymer is generated at 135°C after 2h of reaction; then a chain extender is added, the chain extender is uniformly mixed with the prepolymer, and the thermoplastic polyurethane is obtained after 16h of curing at 110°C.

[0075] Comparative Example 2:

[0076] A thermoplastic polyurethane comprises the following components in parts by weight:

[0077] Polybutylene adipate diol (PBA2000): 59.47 parts; HMDI: 32.03 parts; chain extender 2-methyl-1,3-propanediol: 8.18 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyl tin dilaurate: 0.02 parts;

[0078] The method for preparing the thermoplastic polyurethane is the same as that in Comparative Example 1, which is not repeated here.

[0079] Comparative Example 3:

[0080] A thermoplastic polyurethane comprises the following components in parts by weight:

[0081] Polybutylene adipate diol (PBA2000): 55.28 parts; HDI: 30.61 parts; chain extender 1,4-butanediol: 13.79 parts; antioxidant pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010): 0.30 parts; catalyst dibutyl tin dilaurate: 0.02 parts;

[0082] The method for preparing the thermoplastic polyurethane is the same as that in Comparative Example 1, which is not repeated here.

[0083] Comparative Example 4:

[0084] A thermoplastic polyurethane comprises the following components in parts by weight:

[0085] Poly caprolactone (PCL2000): 58.34; MDI: 32.38 parts; chain extender 2-methyl-1, 3-propanediol: 8.96 parts; antioxidant pentaerythritol tetrakis [3- (3, 5-di-tert-butyl-4-hydroxyphenyl) propionate] (Irganox 1010): 0.30 parts; catalyst dibutyl tin dilaurate: 0.02 parts;

[0086] In the preparation method of the thermoplastic polyurethane, the polyol PCL2000 is used instead of the polyol PBA2000, and the other conditions are the same as those in the comparative example 1, which will not be repeated here.

[0087] The thermoplastic polyurethanes prepared in the examples and the comparative examples were tested after being crushed and injection molded, and the test results are shown in Table 1.

[0088] Performance test: the UV-3101 ultraviolet-visible spectrophotometer (Shimadzu) was used to obtain the absorption spectrum of the sample in the range of 200-800 nm.

[0089] Tensile strength retention rate: after 300h of ultraviolet irradiation, the tensile strength test was carried out, and the retention rate was obtained by comparing the tensile strength before aging.

[0090] Table 1 Test results table

[0091]

[0092] From the data in Table 1, the thermoplastic polyurethane prepared by the present application has a certain absorption function to ultraviolet rays, which can be used as ultraviolet protection, and does not affect the visible light transmittance, which can be used as transparent products; after 300h of ultraviolet aging, the thermoplastic polyurethane has a higher tensile strength retention rate compared with the unmodified thermoplastic polyurethane.

[0093] The above only describes the preferred embodiments of the present application, and is not intended to limit the present application. Any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A UV-resistant bio-based thermoplastic polyurethane, characterized in that, The components include the following parts by weight: Bio-based polyester diol: 35-70 parts; diisocyanate: 15-55 parts; Chain extender: 2-15 parts; antioxidant: 0.2-1 part; catalyst: 0.001-0.05 parts; The bio-based polyester diol is obtained by polycondensation of a dicarboxylic acid and a diol; the dicarboxylic acid is biomass mucoconic acid; the diol is 1,4-butanediol; the diisocyanate is dicyclohexylmethane diisocyanate; the chain extender is 1,4-butanediol; and the acid value of the bio-based polyester diol is 0.15–0.35 mg KOH / g.

2. The UV-resistant bio-based thermoplastic polyurethane according to claim 1, characterized in that, The method for preparing the bio-based polyester diol includes the following steps: Under nitrogen protection, dicarboxylic acids and diols are added to the reactor, heated and stirred, and reacted at 140–180°C for 3–5 hours. Then, the temperature is increased to 190–230°C at a rate of 20–30°C / h and reacted for 2–5 hours. 20–120 ppm of titanate catalyst or organotin catalyst is added, and the reaction is carried out for 1–3 hours. After that, a vacuum is turned on to remove water and small molecule alcohols from the system. The reaction continues until the acid value and hydroxyl value are qualified; the hydroxyl value is 20–200 mg KOH / g.

3. The UV-resistant bio-based thermoplastic polyurethane according to claim 1, characterized in that, The molar ratio of the dicarboxylic acid to the diol is 1:1.01 to 1.

5.

4. The UV-resistant bio-based thermoplastic polyurethane according to claim 3, characterized in that, The isocyanate index of the diisocyanate is 0.95 to 1.

05.

5. The UV-resistant bio-based thermoplastic polyurethane according to claim 1, characterized in that, The antioxidant is one or more of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, tris(2,4-di-tert-butylphenyl) phosphite, and bis(2,4-bis(1,1-dimethylethyl)-6-methylphenyl)ethyl phosphite; the catalyst is one of stannous octoate, dibutyltin dilaurate, dibutyltin diacetate, and di(dodecyl sulfide)dibutyltin.

6. A method for preparing the UV-resistant bio-based thermoplastic polyurethane as described in any one of claims 1-5, characterized in that, Includes the following steps: Diisocyanate is heated and melted, and bio-based polyester diol, antioxidant, and catalyst are added. The mixture is reacted at 60–110°C for 0.5–4 h to generate a prepolymer. Then, a chain extender is added to mix the chain extender with the prepolymer evenly. The mixture is then cured at 90–130°C for 8–24 h to obtain UV-resistant bio-based thermoplastic polyurethane.

Citation Information

Patent Citations

  • Preparation method of uvioresistant transparent lignin-based polyurethane elastomer

    CN113861363A

  • A low-temperature resistant polyurethane elastomer for footwear materials and its preparation process

    CN115304737B

  • Hot melt adhesive for laminating UV-resistant clothing fabrics and preparation method and application thereof

    CN117757407B

  • Preparation method of uvioresistant thermoplastic polyurethane elastomer

    CN118755252A

  • Unsaturated aliphatic dibasic acid-based polyester polyol

    CN114133543A