Method for preparing gold-based catalyst by taking alluvial gold as gold source and application of gold-based catalyst in acetylene hydrochlorination reaction
By using sand gold as the gold source, combining acid treatment and eutectic solvents to prepare gold-based catalysts, the problem of high cost of gold-based catalysts is solved, and an efficient and low-cost acetylene hydrochlorination reaction is achieved, and a green chemical process is promoted.
Patent Information
- Application Number
- CN202510708923.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-29
- Publication Date
- 2025-09-02
AI Technical Summary
The preparation cost of existing gold-based catalysts is high, and it is difficult to recover gold resources. Traditional gold sources such as chloroatric acid are expensive, resulting in high cost of acetylene hydrochlorination reaction and high environmental risks.
Sand gold is used as the gold source, and combined with activated carbon through acid treatment and water regia to control the active site by introducing a low eutectic solvent to prepare a gold-based catalyst for acetylene hydrochlorination reaction.
It reduces the cost of catalyst preparation, maintains high activity and selectivity, reduces the dependence of precious metals, promotes the industrialization of green catalytic technology, reduces energy consumption and improves reaction efficiency.
Smart Images

Figure BDA0005426571000000181 
Figure BDA0005426571000000182 
Figure BDA0005426571000000183
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and particularly relates to a method for preparing a gold-based catalyst using gold sand as a gold source and an application of the method in acetylene hydrochlorination reaction. Background Art
[0002] Polyvinyl chloride (PVC) is an important organic synthetic material, one of the five most common synthetic resins, and currently one of the most widely used plastics in the world. The demand for PVC is increasing year by year. Due to its excellent physical, chemical, and mechanical properties, PVC is widely used in industry, agriculture, construction, and other fields. Vinyl chloride monomer (VCM), a key monomer in the synthesis of PVC, currently accounts for 90% of VCM production in the production of PVC.
[0003] Gold-based catalysts exhibit high activity in acetylene hydrochlorination, achieving acetylene conversion rates exceeding 90%. Currently, the most commonly used gold sources are chloroauric acid and gold-organic complexes. However, gold is a precious metal, making catalyst preparation expensive, with the international gold price exceeding $3,050 per ounce. Recycling is also difficult; while gold can be recovered, the process is complex and costly. Summary of the Invention
[0004] In order to reduce the cost of preparing gold-based catalysts, the purpose of the present invention is to provide a method for preparing a gold-based catalyst using gold sand as a gold source and its application in acetylene hydrochlorination reaction, which reduces the cost while maintaining high activity and high selectivity of the catalyst.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a gold-based catalyst using gold sand as a gold source comprises the following steps:
[0007] Treating the gold sand with acid and then with aqua regia to obtain a gold-containing solution;
[0008] The carrier is added into the gold-containing solution and reacted under reflux to obtain a gold-based catalyst.
[0009] Furthermore, the gold-containing solution also includes a low eutectic solvent, which is prepared by the following process: mixing tetrabutylammonium chloride and acetamide, or mixing tetrabutylammonium chloride and propionamide, or mixing tetrabutylammonium chloride and urea, or mixing tetrabutylammonium chloride and 4-chlorobenzamide, or mixing tetrabutylammonium chloride and benzamide, or mixing tetrabutylammonium chloride and 4-methylbenzamide, and then stirring at 70-90° C. for 1-3 hours and drying to obtain a low eutectic solvent.
[0010] Furthermore, the molar ratio of tetrabutylammonium chloride to acetamide, the molar ratio of tetrabutylammonium chloride to urea, the molar ratio of tetrabutylammonium chloride to 4-chlorobenzamide, and the molar ratio of tetrabutylammonium chloride to propionamide are 1:2, and the molar ratio of tetrabutylammonium chloride to benzamide and the molar ratio of tetrabutylammonium chloride to 4-methylbenzamide are 1:1.
[0011] Furthermore, the mass ratio of the low eutectic solvent to the carrier in the gold-containing solution is 1:10; when the gold-containing solution includes a low eutectic solvent, the carrier is added to the gold-containing solution, and the reaction time under reflux is 4-8 hours.
[0012] Furthermore, the reaction temperature is 60-80° C. and the reaction time is 12-24 hours.
[0013] Furthermore, the carrier is activated carbon.
[0014] Furthermore, the gold sand is treated with acid and then with aqua regia to obtain a gold-containing solution, which includes the following steps:
[0015] Place the gold sand in nitric acid, react at 50-80°C for 12-30 hours, and separate to obtain the remaining solid;
[0016] Add the remaining solid aqua regia and let it stand to obtain a gold-containing solution.
[0017] Furthermore, the mass concentration of nitric acid is 5%-15%; and the standing time is 24-48 hours.
[0018] A gold-based catalyst.
[0019] Application of a gold-based catalyst in acetylene hydrochlorination.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] This invention utilizes relatively inexpensive gold dust as a new gold source in the acetylene hydrochlorination reaction, replacing previously expensive chloroauric acid and other alternatives. This significantly reduces production costs, while also lowering the costs and environmental risks of the acetylene hydrochlorination process, laying the technical foundation for its large-scale industrial application. This invention not only maintains the high activity and selectivity of the catalytic system, but also effectively alleviates the problem of precious metal resource constraints by using gold dust as a gold source, thereby simultaneously advancing the industrialization of green catalytic technology.
[0022] Furthermore, the present invention uses gold dust to replace the traditional gold source, pre-treats the gold dust, dissolves it with aqua regia, and finally adopts an impregnation method to prepare a gold-based catalyst. The gold dust is decomposed into Au during the impregnation or reduction process. 3+ and form stable active sites by combining with oxygen-containing functional groups on the surface of activated carbon. 3+By adsorbing HCl and activating its Cl-, the electrophilic addition reaction of acetylene is promoted to produce vinyl chloride. The present invention reduces energy consumption while also successfully achieving a significant optimization of the preparation cost of the gold-based catalytic material.
[0023] Furthermore, while reducing the preparation cost of the gold-based catalyst, the introduction of a deep eutectic solvent can modulate the electronic structure of the active sites, further facilitating the adsorption and reaction of acetylene and hydrogen chloride, thereby increasing the reactivity and selectivity and further improving the catalyst's performance. The deep eutectic solvent can evenly disperse the gold species in the system, preventing gold species aggregation. This allows acetylene and hydrogen chloride to more fully contact the active sites during the acetylene hydrochlorination reaction, improving the reaction conversion rate and selectivity for vinyl chloride. Furthermore, the low volatility, low toxicity, and biodegradability of the deep eutectic solvent further align with the development requirements of green chemistry.
[0024] The present invention utilizes gold sand as a novel gold source, enabling gold-based catalysts to maintain high activity and selectivity in acetylene hydrochlorination reactions at low temperatures, thereby accelerating their promotion and application in industrial production. Implementation of the present invention will help reduce reliance on expensive gold resources, promote the development of green chemical processes, and bring significant economic and environmental benefits to related industries. DETAILED DESCRIPTION
[0025] In order to facilitate understanding of the present invention, the present invention will be described in more detail below through specific embodiments.
[0026] The following examples are provided to facilitate a better understanding of the present invention, but are not intended to limit the present invention. The experimental methods in the following examples, unless otherwise specified, are conventional methods. The experimental materials used in the following examples, unless otherwise specified, were purchased from conventional biochemical reagent companies.
[0027] In the present invention, there are two methods for preparing gold-based catalysts using gold sand as a gold source. One method is to add a low eutectic solvent, and the other method is to add a non-low eutectic solvent.
[0028] Method 1: The method of preparing a gold-based catalyst using gold sand as a gold source in the present invention comprises the following steps:
[0029] Step 1: Use activated carbon as a carrier. After purchase, pre-treat it before use. First, grind it with a ball mill and screen out activated carbon with a mesh size of 40-60. Weigh the activated carbon and pour the prepared hydrochloric acid solution (mass concentration is 1 mol / L) into the weighed activated carbon to ensure that the activated carbon is completely immersed. At 70°C, use a magnetic stirrer to continuously stir and reflux for 6-12 hours. Subsequently, the gold-containing solution is vacuum filtered through a Buchner funnel to separate the solid activated carbon and rinse with deionized water. The washed activated carbon is dried at 120°C for 12-24 hours, and after naturally cooling to room temperature, a structurally stable carrier, namely the pre-treated activated carbon, is obtained.
[0030] Step 2: 4-20 g of gold dust is placed in excess dilute nitric acid with a mass concentration of 5%-15%, and the mixture is allowed to react in a water bath at a constant temperature of 50-80° C. for 12-30 hours. After the reaction is complete, the mixture is vacuum filtered using a Buchner funnel to obtain a residual solid. In the present invention, the dilute nitric acid soaking method is used to remove interference from other metals in the gold dust with the prepared gold-based catalyst.
[0031] Step 3: Measure concentrated hydrochloric acid (mass concentration of 37%) and concentrated nitric acid (mass concentration of 69%) in a volume ratio of 3:1, slowly add the concentrated nitric acid to the concentrated hydrochloric acid while gently stirring with a stirring rod to obtain aqua regia.
[0032] Step 4: Slowly add the remaining solid obtained after filtration in step 2 into the prepared aqua regia in batches, stirring while adding. After the addition is completed, let it stand for 24-48 hours until the gold sand is completely dissolved to obtain a gold-containing solution.
[0033] Step 5: Add the pretreated activated carbon to the gold-containing solution under continuous stirring, stir continuously for 12-24 hours, reflux at 60-80°C for 12-24 hours, and finally dry in a vacuum oven at 70-80°C for 24-48 hours to obtain a gold-based catalyst.
[0034] Method 2: The method of preparing a gold-based catalyst by using sand gold as a gold source and further introducing a deep eutectic solvent in the present invention comprises the following steps:
[0035] Step 1: Use activated carbon as a carrier. After purchase, pre-treat it before use. First, grind it with a ball mill and screen out activated carbon with a mesh size of 40-60. Weigh the activated carbon and pour the prepared hydrochloric acid solution (mass concentration is 1 mol / L) into the weighed activated carbon to ensure that the activated carbon is completely immersed. At 70°C, use a magnetic stirrer to continuously stir and reflux for 6-12 hours. Subsequently, the gold-containing solution is vacuum filtered through a Buchner funnel to separate the solid activated carbon and rinse with deionized water. The washed activated carbon is dried at 120°C for 12-24 hours, and after naturally cooling to room temperature, a structurally stable carrier, namely the pre-treated activated carbon, is obtained.
[0036] Step 2: 4-20 g of gold dust is placed in excess dilute nitric acid with a mass concentration of 5%-15%, and the mixture is allowed to react in a water bath at a constant temperature of 50-80° C. for 12-30 hours. After the reaction is complete, the mixture is vacuum filtered using a Buchner funnel to obtain a residual solid. In the present invention, the dilute nitric acid soaking method is used to remove interference from other metals in the gold dust with the prepared gold-based catalyst.
[0037] Step 3: Measure concentrated hydrochloric acid (mass concentration of 37%) and concentrated nitric acid (mass concentration of 69%) in a volume ratio of 3:1, slowly add the concentrated nitric acid to the concentrated hydrochloric acid while gently stirring with a stirring rod to obtain aqua regia.
[0038] Step 4: Slowly add the remaining solid obtained after filtration in step 2 into the prepared aqua regia in batches, stirring while adding. After the addition is completed, let it stand for 24-48 hours until the gold sand is completely dissolved to obtain a gold-containing solution.
[0039] Step 5: Place the gold-containing solution obtained in step 4 in a constant temperature oil bath at 70-90°C and gently stir the solution with a stirring rod to remove excess hydrochloric acid and nitric acid. The entire operation is performed in a fume hood to obtain a gold-containing solution after removing the hydrochloric acid and nitric acid.
[0040] Step 6. Preparing a low eutectic solvent: mixing tetrabutylammonium chloride and acetamide in a molar ratio of 1:2, or mixing tetrabutylammonium chloride and propionamide in a molar ratio of 1:2, or mixing tetrabutylammonium chloride and urea in a molar ratio of 1:2, or mixing tetrabutylammonium chloride and 4-chlorobenzamide in a molar ratio of 1:2, or mixing tetrabutylammonium chloride and benzamide in a molar ratio of 1:1, or mixing tetrabutylammonium chloride and 4-methylbenzamide in a molar ratio of 1:1, and then adding the mixture to a 50 ml beaker, stirring and refluxing continuously at 70-90° C. and 500 rpm for 1-3 hours, and then drying in a vacuum oven at 60-80° C. for 20-26 hours to obtain a low eutectic solvent.
[0041] 0.5 g of a deep eutectic solvent is added to 10-15 ml of deionized water, and the mixture is stirred at 70-80° C. for 0.5-1 hour to obtain a deep eutectic solvent solution.
[0042] Step 7: Add the low eutectic solvent solution to the gold-containing solution obtained in step 5 after removing hydrochloric acid and nitric acid, stir at 70-80°C for 2-3 hours, then add the pretreated activated carbon under continuous stirring, stir continuously for 12-24 hours, and then reflux at 60-80°C for 4-8 hours. Finally, dry in a blast oven at 100-120°C for 10-14 hours to obtain a gold-based catalyst.
[0043] The gold-based catalyst of the present invention comprises a carrier and a stable metal precursor; the stable metal precursor is the gold element in gold sand, and the carrier is activated carbon. This invention significantly reduces the cost of the gold-based catalyst while maintaining high catalyst activity and selectivity.
[0044] When preparing the gold-based catalyst in the present invention, a low reaction temperature is adopted, which reduces energy consumption and saves costs while being beneficial to improving the stability, selectivity and safety of the catalyst, and is suitable for a green and efficient acetylene hydrochlorination process.
[0045] The present invention uses gold sand as a gold source to maintain high activity and high selectivity of the catalyst, and introduces a deep eutectic solvent to optimize the adsorption strength of acetylene and hydrogen chloride on the catalyst surface, further improving the selectivity of vinyl chloride and also helping to extend the service life of the catalyst.
[0046] The gold-based catalyst of the present invention can be used in acetylene hydrochlorination reaction. The acetylene hydrochlorination reaction is a gas phase reaction in which acetylene and hydrogen chloride react to generate vinyl chloride.
[0047] The main reactions involved in acetylene hydrochlorination include:
[0048] Main reaction:
[0049] C2H2+HCl→CH2=CHCl
[0050] Non-polymerization side reactions:
[0051] CH2=CHCl+HCl→CH3CHCl2
[0052] CH2=CHCl+HCl→CH2ClCH2Cl
[0053] Polymerization side reactions:
[0054] 2CH2=CHCl→CH2Cl-CH=CCI-CH3
[0055] 2CH2=CHCl→CH2Cl-CH=CCI-CH3
[0056] Existing thermodynamic studies have shown that the above-mentioned main reaction is greatly affected by the polymerization side reaction, and the non-polymerization side reaction has little effect on the main reaction. The above-mentioned main and side reactions are all exothermic reactions, but the thermal effect of the polymerization side reaction is larger than that of the main reaction. Higher temperatures are more conducive to suppressing the polymerization side reaction (polymerization products may be deposited on the catalyst surface to form carbon deposits), improving the selectivity of the main reaction and reducing carbon deposits. However, at high temperatures, the metal catalyst has the problem of valence deactivation. After comprehensively considering the effect of temperature on the polymerization side reaction and catalyst reduction deactivation, the reaction temperature is controlled at 110-300 ° C. The volume ratio of acetylene to hydrogen chloride adopts a commonly used volume ratio in this area, specifically 1: 1-2, and more preferably, the volume ratio of acetylene to hydrogen chloride is 1: 1.02-1.2.
[0057] The gold-based catalyst of the present invention is used in the acetylene hydrochlorination reaction, specifically: the gold-based catalyst is loaded into a fixed bed reactor, and acetylene and hydrogen chloride are introduced into the fixed bed reactor, and the acetylene space velocity is controlled within the range commonly used in the art, specifically within the range of 30-2000h -1 Preferably, the acetylene space velocity is controlled at 30-180h -1 , react at 140-180℃ to produce vinyl chloride.
[0058] Example 1
[0059] Step 1: When using activated carbon (AC) as a catalyst carrier, it needs to be systematically pretreated to optimize its physical and chemical properties. The specific process is as follows: First, the original activated carbon is subjected to particle size standardization, mechanical grinding is performed using a ball mill, and uniform particles of 40-60 mesh are screened out through a standard sieve. Subsequently, the quantitatively weighed activated carbon is placed in an acid-resistant container and injected with a pre-prepared hydrochloric acid solution (concentration of 1 mol / L) to ensure that the carbon material is completely immersed in the solution. The mixed system is transferred to a constant temperature magnetic stirring reaction device, and under precise temperature control at 70°C, it is continuously stirred and refluxed at a speed of 500 rpm for 12 hours. After the reaction is completed, a Buchner funnel is connected to a vacuum filtration system for solid-liquid separation, and the filtrate is repeatedly washed with deionized water until the filtrate is neutral (pH≈6.5-7.5) to eliminate the interference of residual chloride ions on subsequent applications. The washed activated carbon was transferred to a forced air drying oven and heat treated at a constant temperature of 120°C for 24 hours to finally obtain a modified carrier with high mechanical strength, low impurity content and controllable surface properties, namely the pretreated activated carbon.
[0060] Step 2: Place 4g of gold sand in 5% dilute nitric acid and allow to react in a 60°C water bath for 20 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0061] Step 3: In a 500mL glass beaker, measure 30mL of concentrated hydrochloric acid (37% by mass) and 90mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring with a glass rod to avoid localized heat release that could cause splashing. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0062] The remaining solid obtained after filtration in step 2 is slowly added to aqua regia in portions. The dissolution process needs to continue for 24 hours until the solution is clear and no solid remains, thereby obtaining a solution.
[0063] Step 4: Add 3 g of pretreated activated carbon to the above solution and stir for 12 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the solution at 70°C for 12 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 70°C for 24 hours to obtain the gold-based catalyst, designated Au / AC-1.
[0064] Example 2
[0065] Step 1: Same as Example 1.
[0066] Step 2: Place 8g of gold sand in 9% dilute nitric acid and allow to react in a 60°C water bath for 30 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0067] Step 3: In a 500mL glass beaker, measure 40mL of concentrated hydrochloric acid (37% by mass) and 120mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring at a constant speed with a glass rod to avoid localized heat release that could cause splashing of the solution. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0068] The remaining solid obtained after filtration in step 2 was slowly added to aqua regia in portions. The dissolution process was continued for 28 hours until the solution was clear and no solid remained, thereby obtaining a solution.
[0069] Step 4: Add 3 g of pretreated activated carbon to the solution and stir for 14 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the mixture at 70°C for 20 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 70°C for 36 hours to obtain the gold-based catalyst, designated Au / AC-2.
[0070] Example 3
[0071] Step 1: Same as Example 1.
[0072] Step 2: Place 12g of gold sand in 12% dilute nitric acid and allow to react in a 70°C water bath for 20 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0073] Step 3: In a 500mL glass beaker, measure 50mL of concentrated hydrochloric acid (37% by mass) and 150mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring at a constant speed with a glass rod to avoid localized heat release that could cause splashing of the solution. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0074] The remaining solid obtained after filtration in step 2 was slowly added to aqua regia in portions. The dissolution process was continued for 36 hours until the solution was clear and no solid remained, thereby obtaining a solution.
[0075] Step 4: Add 3 g of pretreated activated carbon to the above solution and stir for 18 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the solution at 80°C for 12 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 80°C for 24 hours to obtain the gold-based catalyst, designated Au / AC-3.
[0076] Example 4
[0077] Step 1: Same as Example 1.
[0078] Step 2: Place 16g of gold sand in 14% dilute nitric acid and allow to react in an 80°C water bath for 12 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0079] Step 3: In a 500mL glass beaker, measure 60mL of concentrated hydrochloric acid (37% by mass) and 180mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring at a constant speed with a glass rod to avoid localized heat release that could cause splashing of the solution. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0080] The remaining solid obtained after filtration in step 2 was slowly added to aqua regia in portions. The dissolution process was continued for 44 hours until the solution was clear and no solid remained, thereby obtaining a solution.
[0081] Step 4: Add 3 g of pretreated activated carbon to the above solution and stir for 22 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the solution at 80°C for 20 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 80°C for 36 hours to obtain the gold-based catalyst, designated Au / AC-4.
[0082] Example 5
[0083] Step 1: Same as Example 1.
[0084] Step 2: Place 20g of gold sand in 15% dilute nitric acid and allow to react in an 80°C water bath for 16 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0085] Step 3: In a 500mL glass beaker, measure 65mL of concentrated hydrochloric acid (37% by mass) and 195mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring with a glass rod to avoid localized heat release that could cause splashing. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0086] The remaining solid obtained after filtration in step 2 was slowly added to the aqua regia in portions while stirring. After the addition was completed, it was allowed to stand for 48 hours until the gold was completely dissolved to obtain a solution.
[0087] Step 4: Add 3 g of pretreated activated carbon to the above solution and stir for 24 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the solution at 80°C for 24 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 80°C for 48 hours to obtain the gold-based catalyst, designated Au / AC-5.
[0088] Example 6
[0089] Step 1: Prepare a deep eutectic solvent of tetrabutylammonium chloride and acetamide at a molar ratio of 1:2. Place 2.9889 g of tetrabutylammonium chloride and 1.1814 g of acetamide in a 50 ml beaker. Stir continuously at 500 rpm for 2 hours under precise temperature control at 80°C. Then, dry in a vacuum oven at 70°C for 24 hours to obtain a deep eutectic solvent.
[0090] Step 2, 4g of gold dust is put into the dilute nitric acid with a mass concentration of 5%, and the reaction is allowed to stand in a water bath at 60°C for 20h. After the reaction is complete, vacuum filtration is carried out using a Buchner funnel to separate, and the solid is rinsed with deionized water to obtain residual solid. In a 500mL glass beaker, 30ml of concentrated hydrochloric acid (mass concentration 37%) and 90ml of concentrated nitric acid (mass concentration 69%) are measured in strict accordance with a volume ratio of 1:3. In a fume hood, nitric acid is slowly poured into the hydrochloric acid along the wall of the beaker, and the solution is stirred at a uniform speed with a glass rod to avoid local intense heat release and causing the solution to splash. After mixing is complete, aqua regia is an orange-red transparent liquid, and is left to cool to room temperature for standby use. The residual solid obtained after suction filtration in step 2 is slowly added to aqua regia in portions, and the dissolution process needs to continue for 24 hours until the solution is clarified without solid residue, to obtain a solution.
[0091] Step 3: Place the solution from Step 2 into a 500ml beaker. Place the beaker in a constant-temperature oil bath at 80°C. Gently stir the solution with a stirring rod to allow excess hydrochloric acid and nitric acid to evaporate slowly. Stop heating when the solution volume is approximately 40ml. Add 30ml of deionized water to the beaker and heat again to evaporate the solution to approximately 40ml. Repeat this process three times. Perform all operations in a fume hood.
[0092] Step 4: Weigh 0.5 g of the deep eutectic solvent prepared in Step 1, add 10 ml of deionized water, and stir at 80°C for 0.5 hours to obtain a deep eutectic solvent solution. Add the solution obtained in Step 3 to the deep eutectic solvent solution and stir at 80°C for 2 hours. Then, add 5 g of activated carbon, stir continuously for 12 hours, and then incubate in a 70°C water bath for 6 hours. Finally, dry in a forced air oven at 120°C for 12 hours to obtain the gold-based catalyst, designated Au / AC-6.
[0093] Example 7
[0094] Step 1: Prepare a deep eutectic solvent of tetrabutylammonium chloride and propionamide at a molar ratio of 1:2. Place 2.9889 g of tetrabutylammonium chloride and 1.4618 g of propionamide in a 50 ml beaker. Stir continuously at 500 rpm and reflux for 2 hours at 80°C under precise temperature control. Dry the resulting deep eutectic solvent in a vacuum oven at 70°C for 24 hours.
[0095] Step 2: Same as Example 6;
[0096] Step 3: Same as Example 6;
[0097] Step 4: Same as Example 6; the obtained gold-based catalyst is recorded as Au / AC-7.
[0098] Example 8
[0099] Step 1: Prepare a tetrabutylammonium chloride-urea deep eutectic solvent by combining tetrabutylammonium chloride and urea in a 1:2 molar ratio. Place 2.9889 g of tetrabutylammonium chloride and 1.2012 g of urea in a 50 ml beaker and reflux at 80°C with continuous stirring at 500 rpm for 2 hours. Dry the resulting deep eutectic solvent in a vacuum oven at 70°C for 24 hours.
[0100] Step 2: Same as Example 6;
[0101] Step 3: Same as Example 6;
[0102] Step 4: Same as Example 6;
[0103] Example 9
[0104] Step 1: Prepare a tetrabutylammonium chloride-benzamide deep eutectic solvent by combining tetrabutylammonium chloride and benzamide in a 1:1 molar ratio. Place 2.9889 g of tetrabutylammonium chloride and 1.2114 g of benzamide in a 50 ml beaker and reflux at 500 rpm under precise temperature control at 80°C for 2 hours. Dry the resulting deep eutectic solvent in a vacuum oven at 70°C for 24 hours.
[0105] Step 2: Same as Example 6;
[0106] Step 3: Same as Example 6;
[0107] Step 4: Same as Example 6;
[0108] Example 10
[0109] Step 1: Prepare a deep eutectic solvent of tetrabutylammonium chloride and 4-methylbenzamide by combining tetrabutylammonium chloride and 4-methylbenzamide in a 1:1 molar ratio. Place 2.9889 g of tetrabutylammonium chloride and 1.3516 g of 4-methylbenzamide in a 50 ml beaker and reflux at 500 rpm under precise temperature control at 80°C for 2 hours. Dry the resulting deep eutectic solvent in a vacuum oven at 70°C for 24 hours.
[0110] Step 2: Same as Example 6;
[0111] Step 3: Same as Example 6;
[0112] Step 4: Same as Example 6;
[0113] Example 11
[0114] Step 1: Prepare a deep eutectic solvent of tetrabutylammonium chloride and 4-chlorobenzamide by mixing tetrabutylammonium chloride and 4-chlorobenzamide in a molar ratio of 1:2. Place 2.9889 g of tetrabutylammonium chloride and 3.1116 g of 4-chlorobenzamide in a 50 ml beaker and reflux at 500 rpm under precise temperature control at 80°C for 2 hours. Dry the resulting deep eutectic solvent in a vacuum oven at 70°C for 24 hours.
[0115] Step 2: Same as Example 6;
[0116] Step 3: Same as Example 6;
[0117] Step 4: Same as Example 6;
[0118] Example 12
[0119] Step 1: When using activated carbon (AC) as a catalyst carrier, it needs to be systematically pretreated to optimize its physical and chemical properties. The specific process is as follows: First, the original activated carbon is subjected to particle size standardization, mechanical grinding is performed using a ball mill, and uniform particles of 40-60 mesh are screened out through a standard sieve. Subsequently, the quantitatively weighed activated carbon is placed in an acid-resistant container and injected with a pre-prepared hydrochloric acid solution (concentration of 1 mol / L) to ensure that the carbon material is completely immersed in the solution. The mixed system is transferred to a constant temperature magnetic stirring reaction device, and under precise temperature control at 70°C, it is continuously stirred and refluxed at a speed of 500 rpm for 6 hours. After the reaction is completed, a Buchner funnel is connected to a vacuum filtration system for solid-liquid separation, and the filtrate is repeatedly washed with deionized water until the filtrate is neutral (pH≈6.5-7.5) to eliminate the interference of residual chloride ions with subsequent applications. The washed activated carbon was transferred to a forced air drying oven and heat treated at a constant temperature of 120°C for 12 hours to finally obtain a modified carrier with high mechanical strength, low impurity content and controllable surface properties, namely the pretreated activated carbon.
[0120] Step 2: Place 15g of gold sand in 13% dilute nitric acid and allow to react in a 50°C water bath for 30 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0121] Step 3: In a 500mL glass beaker, measure 55mL of concentrated hydrochloric acid (37% by mass) and 165mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring at a constant speed with a glass rod to avoid localized heat release that could cause splashing of the solution. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0122] The remaining solid obtained after filtration in step 2 was slowly added to aqua regia in portions. The dissolution process was continued for 40 hours until the solution was clear and no solid remained, thereby obtaining a solution.
[0123] Step 4: Add 3g of pretreated activated carbon to the solution and stir for 20 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the solution at 80°C for 16 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 80°C for 30 hours to obtain the gold-based catalyst.
[0124] Example 13
[0125] Step 1: When using activated carbon (AC) as a catalyst carrier, it needs to be systematically pretreated to optimize its physical and chemical properties. The specific process is as follows: First, the original activated carbon is subjected to particle size standardization, mechanical grinding is performed using a ball mill, and uniform particles of 40-60 mesh are screened out through a standard sieve. Subsequently, the quantitatively weighed activated carbon is placed in an acid-resistant container and injected with a pre-prepared hydrochloric acid solution (concentration of 1 mol / L) to ensure that the carbon material is completely immersed in the solution. The mixed system is transferred to a constant temperature magnetic stirring reaction device, and under precise temperature control at 70°C, it is continuously stirred and refluxed at a speed of 500 rpm for 12 hours. After the reaction is completed, a Buchner funnel is connected to a vacuum filtration system for solid-liquid separation, and the filtrate is repeatedly washed with deionized water until the filtrate is neutral (pH≈6.5-7.5) to eliminate the interference of residual chloride ions on subsequent applications. The washed activated carbon was transferred to a forced air drying oven and heat treated at a constant temperature of 120°C for 24 hours to finally obtain a modified carrier with high mechanical strength, low impurity content and controllable surface properties, namely the pretreated activated carbon.
[0126] Step 2: Place 10g of gold sand in 10% dilute nitric acid and allow to react in a 70°C water bath for 16 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0127] Step 3: In a 500mL glass beaker, measure 45mL of concentrated hydrochloric acid (37% by mass) and 135mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring at a constant speed with a glass rod to avoid localized heat release that could cause splashing of the solution. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0128] The remaining solid obtained after filtration in step 2 was slowly added to aqua regia in portions. The dissolution process was continued for 32 hours until the solution was clear and no solid remained, thereby obtaining a solution.
[0129] Step 4: Add 3g of pretreated activated carbon to the solution and stir for 16 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the solution at 70°C for 24 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 70°C for 42 hours to obtain the gold-based catalyst.
[0130] Example 14
[0131] Step 1: When using activated carbon (AC) as a catalyst carrier, it needs to be systematically pretreated to optimize its physical and chemical properties. The specific process is as follows: First, the original activated carbon is subjected to particle size standardization, mechanical grinding is performed using a ball mill, and uniform particles of 40-60 mesh are screened out through a standard sieve. Subsequently, the quantitatively weighed activated carbon is placed in an acid-resistant container and injected with a pre-prepared hydrochloric acid solution (concentration of 1 mol / L) to ensure that the carbon material is completely immersed in the solution. The mixed system is transferred to a constant temperature magnetic stirring reaction device, and under precise temperature control at 70°C, it is continuously stirred and refluxed at a speed of 500 rpm for 8 hours. After the reaction is completed, a Buchner funnel is connected to a vacuum filtration system for solid-liquid separation, and the filtrate is repeatedly washed with deionized water until the filtrate is neutral (pH≈6.5-7.5) to eliminate the interference of residual chloride ions on subsequent applications. The washed activated carbon was transferred to a forced air drying oven and heat treated at a constant temperature of 120°C for 15 hours to finally obtain a modified carrier with high mechanical strength, low impurity content and controllable surface properties, namely the pretreated activated carbon.
[0132] Step 2: Place 7g of gold sand in 7% dilute nitric acid and allow to react in a 60°C water bath for 24 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0133] Step 3: In a 500mL glass beaker, measure 35mL of concentrated hydrochloric acid (37% by mass) and 105mL of concentrated nitric acid (69% by mass) in a strict volume ratio of 1:3. In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker while stirring at a constant speed with a glass rod to avoid localized heat release that could cause splashing of the solution. After mixing, the aqua regia will be an orange-red, transparent liquid. Allow to cool to room temperature before use.
[0134] The remaining solid obtained after filtration in step 2 is slowly added to aqua regia in portions. The dissolution process needs to continue for 24 hours until the solution is clear and no solid remains, thereby obtaining a solution.
[0135] Step 4: Add 3g of pretreated activated carbon to the solution and stir for 12 hours to ensure that the activated carbon particles are evenly dispersed in the solution. Reflux the solution at 70°C for 16 hours. After reflux, transfer the filter cake to a vacuum drying oven and dry it at 70°C for 30 hours to obtain the gold-based catalyst.
[0136] Example 15
[0137] Step 1: Prepare a deep eutectic solvent of tetrabutylammonium chloride and acetamide at a molar ratio of 1:2. Place 2.9889 g of tetrabutylammonium chloride and 1.1814 g of acetamide in a 50 ml beaker. Stir and reflux continuously at 500 rpm for 3 hours at 70°C under precise temperature control. Then, dry in a vacuum oven at 70°C for 22 hours to obtain a deep eutectic solvent.
[0138] Step 2: Place 4g of gold sand in 5% dilute nitric acid and allow to react in a 70°C water bath for 20 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0139] Step 3: In a 500mL glass beaker, strictly follow the volume ratio of 1:3 to measure 30ml of concentrated hydrochloric acid (mass concentration 37%) and 90ml of concentrated nitric acid (mass concentration 69%). In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker, and stir synchronously with a glass rod at a uniform speed to avoid local intense heat release and splashing of the solution. After mixing, the aqua regia is an orange-red transparent liquid, which is allowed to cool to room temperature for use. The remaining solid obtained after filtration in step 2 is slowly added to the aqua regia in batches, and the dissolution process needs to continue for 24 hours until the solution is clear and no solid residues remain to obtain a solution.
[0140] Step 4: Weigh 0.5 g of the deep eutectic solvent prepared in Step 1, add 15 ml of deionized water, and stir at 70°C for 0.5 hours to obtain a deep eutectic solvent solution. Add the solution obtained in Step 3 to the deep eutectic solvent solution and stir at 70°C for 3 hours. Then, add 5 g of pretreated activated carbon, continue stirring for 15 hours, and then incubate in a 60°C water bath for 8 hours. Finally, dry in a forced air oven at 100°C for 14 hours to obtain the gold-based catalyst.
[0141] Example 16
[0142] Step 1: Prepare a deep eutectic solvent of tetrabutylammonium chloride and acetamide at a molar ratio of 1:2. Place 2.9889 g of tetrabutylammonium chloride and 1.1814 g of acetamide in a 50 ml beaker. Reflux at 500 rpm with continuous stirring at 80°C for 2 hours. Dry in a vacuum oven at 80°C for 20 hours to obtain a deep eutectic solvent.
[0143] Step 2: Place 4g of gold sand in 5% dilute nitric acid and allow to react in a 50°C water bath for 30 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0144] Step 3: In a 500mL glass beaker, strictly follow the volume ratio of 1:3 to measure 30ml of concentrated hydrochloric acid (mass concentration 37%) and 90ml of concentrated nitric acid (mass concentration 69%). In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker, and stir synchronously with a glass rod at a uniform speed to avoid local intense heat release and splashing of the solution. After mixing, the aqua regia is an orange-red transparent liquid, which is allowed to cool to room temperature for use. The remaining solid obtained after filtration in step 2 is slowly added to the aqua regia in batches, and the dissolution process needs to continue for 48 hours until the solution is clear and no solid residues remain to obtain a solution.
[0145] Step 4: Place the solution from Step 3 into a 500ml beaker. Place the beaker in a constant-temperature oil bath at 80°C. Gently stir the solution with a stirring rod to allow excess hydrochloric acid and nitric acid to evaporate slowly. Stop heating when the solution volume is approximately 40ml. Add 30ml of deionized water to the beaker and heat again to evaporate the solution to approximately 40ml. Repeat this process three times. Perform all operations in a fume hood.
[0146] Step 5: Weigh 0.5 g of the deep eutectic solvent prepared in Step 1, add 12 ml of deionized water, and stir at 80°C for 0.5 hours to obtain a deep eutectic solvent solution. Add the solution obtained in Step 3 to the deep eutectic solvent solution and stir at 80°C for 2 hours. Then, add 5 g of pretreated activated carbon, stir continuously for 24 hours, and then in an 80°C water bath for 4 hours. Finally, dry in a forced air oven at 110°C for 12 hours to obtain the gold-based catalyst.
[0147] Example 17
[0148] Step 1: Prepare a deep eutectic solvent of tetrabutylammonium chloride and acetamide at a molar ratio of 1:2. Place 2.9889 g of tetrabutylammonium chloride and 1.1814 g of acetamide in a 50 ml beaker. Reflux at 500 rpm with continuous stirring at 90°C for 1 hour. Dry in a vacuum oven at 60°C for 26 hours to obtain a deep eutectic solvent.
[0149] Step 2: Place 4 g of gold sand in 15% dilute nitric acid and allow to react in a 50°C water bath for 30 hours. After the reaction is complete, vacuum filter the mixture using a Buchner funnel and rinse the solid with deionized water to obtain the remaining solid.
[0150] Step 3: In a 500mL glass beaker, strictly follow the volume ratio of 1:3 to measure 30ml of concentrated hydrochloric acid (mass concentration 37%) and 90ml of concentrated nitric acid (mass concentration 69%). In a fume hood, slowly pour the nitric acid into the hydrochloric acid along the wall of the beaker, and stir synchronously with a glass rod at a uniform speed to avoid local intense heat release and splashing of the solution. After mixing, the aqua regia is an orange-red transparent liquid, which is allowed to cool to room temperature for use. The remaining solid obtained after filtration in step 2 is slowly added to the aqua regia in batches, and the dissolution process needs to continue for 30 hours until the solution is clear and no solid residues remain to obtain a solution.
[0151] Step 4: Place the solution from Step 3 into a 500ml beaker. Place the beaker in a constant-temperature oil bath at 80°C. Gently stir the solution with a stirring rod to allow excess hydrochloric acid and nitric acid to evaporate slowly. Stop heating when the solution volume is approximately 40ml. Add 30ml of deionized water to the beaker and heat again to evaporate the solution to approximately 40ml. Repeat this process three times. Perform all operations in a fume hood.
[0152] Step 5: Weigh 0.5 g of the deep eutectic solvent prepared in Step 1, add 10 ml of deionized water, and stir at 75°C for 0.5 hours to obtain a deep eutectic solvent solution. Add the solution obtained in Step 3 to the deep eutectic solvent solution and stir at 75°C for 2.5 hours. Then, add 5 g of pretreated activated carbon, stir continuously for 12 hours, and then incubate in a 70°C water bath for 6 hours. Finally, dry in a forced air oven at 120°C for 10 hours to obtain the gold-based catalyst.
[0153] The gold-based catalysts prepared in Examples 1-7 were respectively subjected to acetylene hydrochlorination reaction: 2 ml of the gold-based catalysts prepared in Examples 1-7 were respectively used as catalysts to load into a fixed bed reactor, acetylene and hydrogen chloride reaction gases were introduced, and the reaction temperature was 140° C., the acetylene space velocity was 180 h -1 The reaction was carried out under the reaction conditions of a volume ratio of acetylene to hydrogen chloride of 1:1.15. The calculation results of acetylene conversion rate and vinyl chloride selectivity are shown in Table 1.
[0154] The calculation method of acetylene conversion rate is:
[0155]
[0156] The calculation method of vinyl chloride selectivity is:
[0157]
[0158] Where: φ A0 Indicates the volume fraction of acetylene in the reactants; φ A Represents the volume fraction of residual acetylene in the reaction; φ VCIndicates the volume fraction of vinyl chloride produced.
[0159] Table 1 Acetylene conversion and vinyl chloride selectivity of Examples 1-7 at low temperature 140°C
[0160]
[0161] As can be seen from Table 1, when only the gold sand is used as a new gold source, the corresponding gold-based catalyst can show superior performance under low temperature conditions. Taking the Au / AC-1 catalyst of Example 5 as an example, at a reaction temperature of 140°C and an acetylene space velocity of 180h -1 After 24 hours of reaction at a volume ratio of acetylene to hydrogen chloride of 1:1.15, the catalyst still achieved an acetylene conversion of 73.37%, while the selectivity for vinyl chloride remained above 99% throughout the reaction. To further improve the catalyst's performance, the introduction of a deep eutectic solvent significantly improved the performance of the Au / AC-1 gold-based catalyst compared to the same mass of gold sand prepared alone. The Au / AC-6 catalyst, which incorporated the deep eutectic solvent of tetrabutylammonium chloride-acetamide, achieved an acetylene conversion of 94.18% after 24 hours of reaction, while the Au / AC-7 catalyst, which incorporated tetrabutylammonium chloride-propionamide, achieved an acetylene conversion of 94.18%.
[0162] The gold-based catalyst of Example 5 was selected and heated at an acetylene space velocity of 180 h -1 The reactions were carried out at a volume ratio of acetylene to hydrogen chloride of 1:1.15 and reaction temperatures of 160°C and 180°C, respectively. The acetylene conversion and vinyl chloride selectivity are shown in Table 2.
[0163] Table 2 Acetylene conversion and vinyl chloride selectivity of Example 5 at different reaction temperatures
[0164]
[0165] It can be seen from Table 2 that as the temperature increases, the acetylene conversion rate of Example 5 gradually increases, achieving higher acetylene hydrochlorination activity and vinyl chloride selectivity.
[0166] The present invention uses gold sand as a gold source to prepare a gold-based catalyst for low-temperature acetylene hydrochlorination. The low-temperature reaction can delay catalyst deactivation, improve catalyst stability (the ability of the catalyst to maintain properties such as activity, selectivity, and thermal stability, as well as its structure), inhibit side reactions, reduce energy consumption, and improve safety. This significantly optimizes the economic efficiency and sustainability of the acetylene hydrochlorination process, achieving efficient and green vinyl chloride production. Furthermore, the introduction of a deep eutectic solvent improves catalyst performance, resists sintering and agglomeration, and is environmentally friendly.
[0167] The above description is merely a description of the preferred embodiment of the present invention and is not to be construed as limiting the claims. The present invention is not limited to the above embodiment, and variations in the specific structure are permitted. Any variations made within the scope of the independent claims of the present invention are also within the scope of protection of the present invention.
[0168] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention pertains. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
Claims
1. A method for preparing a gold-based catalyst using gold sand as a gold source, characterized in that: The following steps are involved: Treating the gold sand with acid and then with aqua regia to obtain a gold-containing solution; The carrier is added into the gold-containing solution and reacted under reflux to obtain a gold-based catalyst.
2. The method for preparing a gold-based catalyst using alluvial gold as a gold source according to claim 1, wherein: The gold-containing solution also includes a low eutectic solvent, which is prepared by the following process: mixing tetrabutylammonium chloride and acetamide, or mixing tetrabutylammonium chloride and propionamide, or mixing tetrabutylammonium chloride and urea, or mixing tetrabutylammonium chloride and 4-chlorobenzamide, or mixing tetrabutylammonium chloride and benzamide, or mixing tetrabutylammonium chloride and 4-methylbenzamide, and then stirring at 70-90° C. for 1-3 hours and drying to obtain a low eutectic solvent.
3. The method for preparing a gold-based catalyst using alluvial gold as a gold source according to claim 2, wherein: The molar ratio of tetrabutylammonium chloride to acetamide, the molar ratio of tetrabutylammonium chloride to urea, the molar ratio of tetrabutylammonium chloride to 4-chlorobenzamide, and the molar ratio of tetrabutylammonium chloride to propionamide are 1:2, and the molar ratio of tetrabutylammonium chloride to benzamide and the molar ratio of tetrabutylammonium chloride to 4-methylbenzamide are 1:
1.
4. The method for preparing a gold-based catalyst using alluvial gold as a gold source according to claim 2, wherein: The mass ratio of the deep eutectic solvent to the carrier in the gold-containing solution is 1:10; When the gold-containing solution includes a low eutectic solvent, the carrier is added to the gold-containing solution and the reaction is carried out under reflux for 4-8 hours.
5. The method for preparing a gold-based catalyst using alluvial gold as a gold source according to claim 1, wherein: The reaction temperature is 60-80°C and the reaction time is 12-24 hours.
6. The method for preparing a gold-based catalyst using alluvial gold as a gold source according to claim 1, wherein: The carrier is activated carbon.
7. The method for preparing a gold-based catalyst using alluvial gold as a gold source according to claim 1, wherein: The gold sand is treated with acid and then with aqua regia to obtain a gold-containing solution, comprising the following steps: Place the gold sand in nitric acid, react at 50-80°C for 12-30 hours, and separate to obtain the remaining solid; Add the remaining solid aqua regia and let it stand to obtain a gold-containing solution.
8. The method for preparing a gold-based catalyst using alluvial gold as a gold source according to claim 7, wherein: The mass concentration of nitric acid is 5%-15%, and the standing time is 24-48h.
9. A gold-based catalyst prepared according to the method according to any one of claims 1 to 8.
10. Use of a gold-based catalyst prepared according to the method according to any one of claims 1 to 8 in acetylene hydrochlorination.