High-elastic wear-resistant sneaker material and preparation method thereof

By combining modified EVA with natural rubber, the elasticity and wear resistance of sports shoe materials are optimized, the contradiction between the elasticity and wear resistance of existing materials is resolved, and a coordinated improvement in high elasticity and wear resistance is achieved.

CN120590707AActive Publication Date: 2025-09-05FUJIAN GOOD BROTHER SPORTS GOODS CO LTD

Patent Information

Application Number
CN202511099403.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-07
Publication Date
2025-09-05
Estimated Expiration
2045-08-07

AI Technical Summary

Technical Problem

There is a contradiction between the elasticity and wear resistance of existing sports shoe materials. Although EVA foam material improves elasticity, it reduces wear resistance, affecting usage efficiency.

Method used

A modified EVA body is combined with natural rubber, nano-silver agent, reinforcing agent, etc. Through the preparation method of the nano-silver agent and the multi-step treatment of the modified EVA body, the antibacterial performance and interface properties of the material are optimized, and the elasticity and wear resistance are enhanced.

Benefits of technology

It improves the elasticity and wear resistance of sports shoe materials, inhibits bacterial growth, and improves the overall performance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of shoe materials, in particular to a high-elastic wear-resistant sports shoe material and a preparation method thereof, and the high-elastic wear-resistant sports shoe material comprises the following raw materials in parts by weight: 40-45 parts of a modified EVA body, 30-35 parts of natural rubber, 8-12 parts of a reinforcing agent, 8-12 parts of a nano-silver agent, 5-8 parts of zinc oxide, 3-5 parts of calcium stearate, 2-3 parts of an AC foaming agent, 2-3 parts of paraffin, 0.5-0.8 part of a cross-linking agent and 1-3 parts of an anti-aging agent. According to the sneaker material, the modified EVA body is matched with the natural rubber, and the zinc oxide, the calcium stearate, the AC foaming agent, the paraffin, the cross-linking agent and other raw materials are added to serve as functional auxiliaries, so that the prepared sneaker material can improve the elastic property and wear resistance of a product, can inhibit bacterium breeding and can improve the performance effect of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of shoe materials, and in particular to a high-elasticity and wear-resistant sports shoe material and a preparation method thereof. Background Art

[0002] Athletic shoes are footwear designed specifically for various athletic activities, providing foot protection, comfort, and enhanced athletic performance. The design and materials of athletic shoes vary depending on the type of sport and the user's needs, such as running shoes, basketball shoes, and soccer shoes, to provide optimal support and protection. Existing athletic shoes use EVA foam, which improves elasticity but can easily reduce wear resistance, negatively impacting performance. This present invention addresses this issue by further improving this material. Summary of the Invention

[0003] In view of the defects of the prior art, the purpose of the present invention is to provide a high-elasticity and wear-resistant sports shoe material and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0004] The present invention solves the technical problem by adopting the following technical solutions: The present invention provides a high-elasticity and wear-resistant sports shoe material, comprising the following raw materials in parts by weight: 40-45 parts of modified EVA body, 30-35 parts of natural rubber, 8-12 parts of reinforcing agent, 8-12 parts of nano silver agent, 5-8 parts of zinc oxide, 3-5 parts of calcium stearate, 2-3 parts of AC foaming agent, 2-3 parts of paraffin, 0.5-0.8 parts of crosslinking agent and 1-3 parts of antioxidant.

[0005] Preferably, the antioxidant is antioxidant RD; the cross-linking agent is sulfur and dicumyl peroxide prepared in a weight ratio of 2:1; The preparation method of the nano silver agent comprises the following steps: adding nano silver powder to a 15% sodium dodecylbenzene sulfonate solution having a mass fraction of 5-8 times the total weight of the nano silver powder, stirring and dispersing the mixture uniformly; then adding a silane solution having a mass fraction of 25-30% of the total weight of the nano silver powder and a triformaldehyde body having a mass fraction of 25-30% of the total weight of the nano silver powder; stirring the mixture at a stirring speed of 350-400 r / min for 1 hour at a stirring temperature of 48-52° C.; and finally filtering and drying the mixture to obtain the nano silver agent.

[0006] Preferably, the silane liquid is prepared by stirring silane coupling agent KH560, ethanol and water in a weight ratio of (3-5): (8-11): (5-6), at a stirring temperature of 50° C., a stirring speed of 300-350 r / min, and stirring for 1 hour; The preparation method of the tripolyformaldehyde body is as follows: melamine and paraformaldehyde are mixed in a weight ratio of 1:(3-5), and then distilled water is added in an amount of 5-8 times the total weight of the melamine. The pH is adjusted to 7.5 with sodium hydroxide. The temperature is raised to 76° C. under stirring conditions, and the reaction is carried out for 30 minutes. Then, a modifier terephthalaldehyde is added in an amount of 10-15% of the total weight of the melamine. The temperature is maintained and stirring is continued for 1 hour to obtain the melamine body.

[0007] Preferably, the preparation method of the modified EVA body is: S11: montmorillonite and silicon dioxide are compounded in a weight ratio of 3:2 to form a compound; the compound, 1-hydroxymethylpyrazole-3-carboxylic acid, polyethylene glycol 400, and phosphorous acid are subjected to an A-conditioning treatment in a weight ratio of (2-4):(4-6):(1-3):0.08, followed by suction filtration and drying to obtain a conditioning agent A; S12: Preparation of zeolite molecular sieve-organic composite B: S12a: soaking the zeolite molecular sieve in a sufficient amount of 8% by mass sodium hydroxide solution for 2 hours, washing, filtering, and drying to obtain a pretreated zeolite molecular sieve; S12b: Mix γ-aminopropyltriethoxysilane and 55-65% by mass ethanol solution in a weight ratio of 3:(8-11), and then add hydrochloric acid to adjust the pH to 4.5 to obtain organic solution B; The pretreated zeolite molecular sieve and the organic B solution were subjected to B grinding treatment in a weight ratio of 7:(3-5), and the treatment was completed to obtain a zeolite molecular sieve-organic composite B body; S13: adding EVA to tetrahydrofuran in a weight ratio of 5:(11-13) and stirring thoroughly to obtain an EVA liquid; mixing the modified A agent and the EVA liquid in a weight ratio of (3-5):11, and then filtering and drying to obtain the modified EVA agent; S14: The EVA agent prepared by A and the zeolite molecular sieve-organized composite B are subjected to a secondary stirring treatment in a weight ratio of (11-15):5. After the stirring is completed, the mixture is filtered and dried to obtain a modified EVA body.

[0008] The modified EVA body is prepared by treating EVA with tetrahydrofuran to form an EVA liquid, and montmorillonite and silica are compounded and then blended with raw materials such as 1-hydroxymethylpyrazole-3-carboxylic acid, polyethylene glycol 400 and phosphorous acid to form a conditioning agent A. The conditioning agent A and the EVA liquid are mutually improved and coordinated and optimized between the raw materials, and the lamellar montmorillonite is combined with a silica structure with a high specific surface area as a supporting structure and a supporting system interface to optimize the performance of the product. The zeolite molecular sieve is optimized and improved with a sodium hydroxide solution and then coordinated and improved with an organic B liquid prepared by blending γ-aminopropyltriethoxysilane, an ethanol solution with a mass fraction of 55-65% and hydrochloric acid. Through the coordination between the raw materials, the medium system of the zeolite molecular sieve is combined with the conditioning agent A and the zeolite molecular sieve-organic composite B body for primary and secondary improvements to prepare a modified EVA body that enhances the performance coordination of the product and the comprehensive performance effect of the product in the system.

[0009] Preferably, the A-adjustment treatment is carried out by stirring at a speed of 550-750 r / min for 2 h; and the B-milling treatment is carried out by ball milling at a speed of 1000-1500 r / min for 2 h.

[0010] Preferably, the stirring temperature of the first-stage stirring treatment is 50-55° C., the stirring speed is 450-500 r / min, and the stirring is carried out for 2 hours; the stirring temperature of the second-stage stirring treatment is 48-52° C., the stirring speed is 700-800 r / min, and the stirring is carried out for 1 hour; The vinyl acetate content of the EVA is 25%, and the melt index is 2 g / 10 min.

[0011] Preferably, the preparation method of the enhancer is: S101: Silica powder and an 8% by mass aqueous solution of ethyl cellulose are uniformly blended in a weight ratio of 5:(11-13), and then tannic acid (5-8% by weight of the total weight of the silica powder) and polyester fiber (15-20% by weight of the total weight of the silica powder) are added, and the mixture is thoroughly blended, and finally filtered and dried to obtain a silica powder-polyester fiber modified product; S102: 8-11 parts by weight of a polyvinyl alcohol solution, 3-5 parts by weight of a silane coupling agent KH550, and 2-4 parts by weight of soybean oleic acid are uniformly mixed to obtain a treatment solution; preheating the graphene at 55-60° C. for 1 hour to obtain preheated graphene; ultrasonically treating the preheated graphene and the treatment solution at a mass ratio of 3:7, and completing the ultrasonic treatment to obtain a treatment solution doped with graphene; S103: The silicon micropowder-polyester fiber modification and the graphene-doped treatment liquid are mixed and ball-milled in a weight ratio of 7:(3-4) at a ball-milling speed of 1000-1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a reinforcing agent.

[0012] The reinforcing agent is a blend of polyvinyl alcohol solution, silane coupling agent KH550 and soybean oleic acid, which are optimized and improved. The graphene is preheated and improved, and the graphene-doped treatment liquid prepared by combining with the treatment liquid enhances the organic interface of the graphene and fills the system structure in the system, thereby further improving the performance of the product. The silicon micropowder is combined with ethyl cellulose aqueous solution, tannic acid and polyester fiber raw materials. Through the co-matching improvement and mutual blending and optimization between the raw materials, the silicon micropowder-polyester fiber modified body is better matched with the graphene-doped treatment liquid, and the obtained reinforcing agent further improves the performance of the product in the system.

[0013] Preferably, the ultrasonic power of the ultrasonic treatment is 350-400W, the ultrasonic treatment is for 1 hour, and the mass fraction of the polyvinyl alcohol solution is 8-12%.

[0014] The present invention also provides a method for preparing a high-elasticity and wear-resistant sports shoe material, comprising the following steps: The raw materials of the high-elasticity and wear-resistant sports shoe material are weighed according to weight, and the raw materials are first mixed at a mixing temperature of 75-80° C. for 5 minutes, then vulcanized, and finally compression molded to obtain the high-elasticity and wear-resistant sports shoe material.

[0015] Preferably, the vulcanization temperature of the vulcanization treatment is 160-165° C., and the vulcanization time is 2 minutes; the pressure of the compression molding is 15-20 MPa, and the compression molding time is 20 minutes.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The sports shoe material of the present invention adopts modified EVA body and natural rubber, and adds raw materials such as zinc oxide, calcium stearate, AC foaming agent, paraffin and cross-linking agent as functional additives. The added nano silver agent optimizes the antibacterial performance of the product in the system. The nano silver agent adopts nano silver blended with sodium dodecylbenzene sulfonate solution to optimize its dispersion. The addition of trioxymethylene body provides multiple active groups for the nano silver agent, which facilitates better combination with the EVA and rubber product system and optimizes the dispersion and binding force of the nano silver. At the same time, the silane liquid adopts raw materials such as silane coupling agent to blend, further enhances the interface between the systems, thereby enhancing the antibacterial performance of the product. At the same time, the addition of the reinforcing agent can cooperate with the modified EVA body to achieve joint optimization and improvement. Thus, the sports shoe material prepared can improve the elasticity and wear resistance of the product, inhibit bacterial growth, and improve the performance effect of the product. DETAILED DESCRIPTION

[0017] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0018] The highly elastic and wear-resistant sports shoe material of this embodiment includes the following raw materials in parts by weight: 40-45 parts of modified EVA body, 30-35 parts of natural rubber, 8-12 parts of reinforcing agent, 8-12 parts of nano silver agent, 5-8 parts of zinc oxide, 3-5 parts of calcium stearate, 2-3 parts of AC foaming agent, 2-3 parts of paraffin, 0.5-0.8 parts of crosslinking agent and 1-3 parts of antioxidant.

[0019] The antioxidant in this embodiment is antioxidant RD; the cross-linking agent is sulfur and dicumyl peroxide prepared in a weight ratio of 2:1; The preparation method of the nano silver agent comprises the following steps: adding nano silver powder to a 15% sodium dodecylbenzene sulfonate solution having a mass fraction of 5-8 times the total weight of the nano silver powder, stirring and dispersing the mixture uniformly; then adding a silane solution having a mass fraction of 25-30% of the total weight of the nano silver powder and a triformaldehyde body having a mass fraction of 25-30% of the total weight of the nano silver powder; stirring the mixture at a stirring speed of 350-400 r / min for 1 hour at a stirring temperature of 48-52° C.; and finally filtering and drying the mixture to obtain the nano silver agent.

[0020] The preparation method of the silane liquid of this embodiment is as follows: silane coupling agent KH560, ethanol and water are stirred in a weight ratio of (3-5): (8-11): (5-6) at a stirring temperature of 50° C. and a stirring speed of 300-350 r / min for 1 hour; The preparation method of the tripolyformaldehyde body is as follows: melamine and paraformaldehyde are mixed in a weight ratio of 1:(3-5), and then distilled water is added in an amount of 5-8 times the total weight of the melamine. The pH is adjusted to 7.5 with sodium hydroxide. The temperature is raised to 76° C. under stirring conditions, and the reaction is carried out for 30 minutes. Then, a modifier terephthalaldehyde is added in an amount of 10-15% of the total weight of the melamine. The temperature is maintained and stirring is continued for 1 hour to obtain the melamine body.

[0021] The preparation method of the modified EVA body of this embodiment is: S11: montmorillonite and silicon dioxide are compounded in a weight ratio of 3:2 to form a compound; the compound, 1-hydroxymethylpyrazole-3-carboxylic acid, polyethylene glycol 400, and phosphorous acid are subjected to an A-conditioning treatment in a weight ratio of (2-4):(4-6):(1-3):0.08, followed by suction filtration and drying to obtain a conditioning agent A; S12: Preparation of zeolite molecular sieve-organic composite B: S12a: soaking the zeolite molecular sieve in a sufficient amount of 8% by mass sodium hydroxide solution for 2 hours, washing, filtering, and drying to obtain a pretreated zeolite molecular sieve; S12b: Mix γ-aminopropyltriethoxysilane and 55-65% by mass ethanol solution in a weight ratio of 3:(8-11), and then add hydrochloric acid to adjust the pH to 4.5 to obtain organic solution B; The pretreated zeolite molecular sieve and the organic B solution were subjected to B grinding treatment in a weight ratio of 7:(3-5), and the treatment was completed to obtain a zeolite molecular sieve-organic composite B body; S13: adding EVA to tetrahydrofuran in a weight ratio of 5:(11-13) and stirring thoroughly to obtain an EVA liquid; mixing the modified A agent and the EVA liquid in a weight ratio of (3-5):11, and then filtering and drying to obtain the modified EVA agent; S14: The EVA agent prepared by A and the zeolite molecular sieve-organized composite B are subjected to a secondary stirring treatment in a weight ratio of (11-15):5. After the stirring is completed, the mixture is filtered and dried to obtain a modified EVA body.

[0022] In this embodiment, the A-treatment is carried out by stirring at a speed of 550-750 r / min for 2 h; the B-milling treatment is carried out by ball milling at a speed of 1000-1500 r / min for 2 h.

[0023] The stirring temperature of the first-stage stirring treatment in this embodiment is 50-55°C, the stirring speed is 450-500 r / min, and the stirring is carried out for 2 hours; the stirring temperature of the second-stage stirring treatment is 48-52°C, the stirring speed is 700-800 r / min, and the stirring is carried out for 1 hour; The vinyl acetate content of the EVA is 25%, and the melt index is 2 g / 10 min.

[0024] The preparation method of the enhancer of this embodiment is: S101: Silica powder and an 8% by mass aqueous solution of ethyl cellulose are uniformly blended in a weight ratio of 5:(11-13), and then tannic acid (5-8% by weight of the total weight of the silica powder) and polyester fiber (15-20% by weight of the total weight of the silica powder) are added, and the mixture is thoroughly blended, and finally filtered and dried to obtain a silica powder-polyester fiber modified product; S102: 8-11 parts by weight of a polyvinyl alcohol solution, 3-5 parts by weight of a silane coupling agent KH550, and 2-4 parts by weight of soybean oleic acid are uniformly mixed to obtain a treatment solution; preheating the graphene at 55-60° C. for 1 hour to obtain preheated graphene; ultrasonically treating the preheated graphene and the treatment solution at a mass ratio of 3:7, and completing the ultrasonic treatment to obtain a treatment solution doped with graphene; S103: The silicon micropowder-polyester fiber modification and the graphene-doped treatment liquid are mixed and ball-milled in a weight ratio of 7:(3-4) at a ball-milling speed of 1000-1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a reinforcing agent.

[0025] The ultrasonic treatment in this embodiment has an ultrasonic power of 350-400 W and an ultrasonic treatment time of 1 hour; the mass fraction of the polyvinyl alcohol solution is 8-12%.

[0026] The method for preparing a highly elastic and wear-resistant sports shoe material of this embodiment includes the following steps: The raw materials of the high-elasticity and wear-resistant sports shoe material are weighed according to weight, and the raw materials are first mixed at a mixing temperature of 75-80° C. for 5 minutes, then vulcanized, and finally compression molded to obtain the high-elasticity and wear-resistant sports shoe material.

[0027] The vulcanization temperature of the vulcanization treatment in this embodiment is 160-165° C., and the vulcanization time is 2 minutes. The compression molding pressure is 15-20 MPa, and the compression molding time is 20 minutes.

[0028] Example 1: A highly elastic and wear-resistant sports shoe material, comprising the following raw materials in parts by weight: 40 parts of modified EVA body, 30 parts of natural rubber, 8 parts of reinforcing agent, 8 parts of nano silver agent, 5 parts of zinc oxide, 3 parts of calcium stearate, 2 parts of AC foaming agent, 2 parts of paraffin, 0.5 parts of crosslinking agent and 1 part of antioxidant.

[0029] The antioxidant in this embodiment is antioxidant RD; the cross-linking agent is sulfur and dicumyl peroxide prepared in a weight ratio of 2:1; The preparation method of the nano silver agent is as follows: adding the nano silver powder to a 15% sodium dodecylbenzene sulfonate solution with a mass fraction of 5 times the total weight of the nano silver powder, stirring and dispersing evenly, then adding a silane liquid with a mass fraction of 25% of the total weight of the nano silver powder and a triformaldehyde body with a mass fraction of 25% of the total weight of the nano silver powder, stirring at a stirring speed of 350 r / min, stirring for 1 hour, stirring at a stirring temperature of 48°C, and finally filtering and drying to obtain the nano silver agent.

[0030] The preparation method of the silane liquid of this embodiment is as follows: silane coupling agent KH560, ethanol and water are stirred in a weight ratio of 3:8:5 at a stirring temperature of 50° C. and a stirring speed of 300 r / min for 1 hour; The preparation method of the tripolyformaldehyde body is as follows: melamine and paraformaldehyde are mixed in a weight ratio of 1:3, and then distilled water is added in an amount of 5 times the total weight of the melamine. The pH is adjusted to 7.5 with sodium hydroxide. The temperature is raised to 76°C under stirring conditions and the reaction is carried out for 30 minutes. Then, a modifier terephthalaldehyde is added in an amount of 10% of the total weight of the melamine. The temperature is maintained and stirring is continued for 1 hour to obtain the melamine body.

[0031] The preparation method of the modified EVA body of this embodiment is: S11: montmorillonite and silicon dioxide are compounded in a weight ratio of 3:2 to form a compound; the compound, 1-hydroxymethylpyrazole-3-carboxylic acid, polyethylene glycol 400, and phosphorous acid are subjected to an A-conditioning treatment in a weight ratio of 2:4:1:0.08, followed by suction filtration and drying to obtain a conditioning agent A; S12: Preparation of zeolite molecular sieve-organic composite B: S12a: soaking the zeolite molecular sieve in a sufficient amount of 8% by mass sodium hydroxide solution for 2 hours, washing, filtering, and drying to obtain a pretreated zeolite molecular sieve; S12b: γ-aminopropyltriethoxysilane and 55% by mass ethanol solution were mixed in a weight ratio of 3:8, and then hydrochloric acid was added to adjust the pH to 4.5 to obtain an organic solution B; The pretreated zeolite molecular sieve and the organic B solution were subjected to B grinding treatment in a weight ratio of 7:3, and the treatment was completed to obtain a zeolite molecular sieve-organic composite B; S13: adding EVA to tetrahydrofuran at a weight ratio of 5:11 and stirring thoroughly to obtain EVA liquid; mixing the modified A agent and the EVA liquid at a weight ratio of 3:11, and then filtering and drying to obtain the modified A EVA agent; S14: The EVA agent prepared in A and the zeolite molecular sieve-organized composite B are subjected to a secondary stirring treatment in a weight ratio of 11:5. After the stirring is completed, the mixture is filtered and dried to obtain a modified EVA body.

[0032] In this embodiment, the A-treatment is carried out by stirring at a speed of 550 r / min for 2 h; the B-milling is carried out by ball milling at a speed of 1000 r / min for 2 h.

[0033] The stirring temperature of the first stirring process in this embodiment is 50°C, the stirring speed is 450r / min, and the stirring is carried out for 2h; the stirring temperature of the second stirring process is 48°C, the stirring speed is 700r / min, and the stirring is carried out for 1h; The vinyl acetate content of the EVA is 25%, and the melt index is 2 g / 10 min.

[0034] The preparation method of the enhancer of this embodiment is: S101: Silica powder and an 8% by mass ethyl cellulose aqueous solution are uniformly blended in a weight ratio of 5:11, and then tannic acid (5% by mass of the total weight of the silica powder) and polyester fiber (15% by mass of the total weight of the silica powder) are added and fully blended. Finally, the mixture is filtered and dried to obtain a silica powder-polyester fiber modified product. S102: 8 parts by weight of a polyvinyl alcohol solution, 3 parts by weight of a silane coupling agent KH550, and 2 parts by weight of soybean oleic acid are uniformly mixed to obtain a treatment solution; preheating the graphene at 55° C. for 1 hour to obtain preheated graphene; ultrasonically treating the preheated graphene and the treatment solution at a mass ratio of 3:7, and completing the ultrasonic treatment to obtain a treatment solution doped with graphene; S103: The silicon micropowder-polyester fiber modification and the graphene-doped treatment liquid are mixed and ball-milled in a weight ratio of 7:3 at a ball-milling speed of 1000 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a reinforcing agent.

[0035] The ultrasonic treatment in this embodiment was performed with an ultrasonic power of 350 W and for 1 h; the mass fraction of the polyvinyl alcohol solution was 8%.

[0036] The method for preparing a highly elastic and wear-resistant sports shoe material of this embodiment includes the following steps: The raw materials of the high-elasticity and wear-resistant sports shoe material are weighed according to weight, and the raw materials are first mixed at a mixing temperature of 75° C. for 5 minutes, then vulcanized, and finally compression molded to obtain the high-elasticity and wear-resistant sports shoe material.

[0037] The vulcanization temperature of the vulcanization treatment in this embodiment is 160° C., and the vulcanization time is 2 minutes. The compression molding pressure is 15 MPa, and the compression molding time is 20 minutes.

[0038] Example 2: A highly elastic and wear-resistant sports shoe material, comprising the following raw materials in parts by weight: 45 parts of modified EVA body, 35 parts of natural rubber, 12 parts of reinforcing agent, 12 parts of nano silver agent, 8 parts of zinc oxide, 5 parts of calcium stearate, 3 parts of AC foaming agent, 3 parts of paraffin, 0.8 parts of crosslinking agent and 3 parts of antioxidant.

[0039] The antioxidant in this embodiment is antioxidant RD; the cross-linking agent is sulfur and dicumyl peroxide prepared in a weight ratio of 2:1; The preparation method of the nano silver agent is as follows: adding the nano silver powder to a 15% sodium dodecylbenzene sulfonate solution having a mass fraction of 8 times the total weight of the nano silver powder and stirring to disperse evenly, then adding a silane liquid having a mass fraction of 30% of the total weight of the nano silver powder and a triformaldehyde body having a mass fraction of 30% of the total weight of the nano silver powder, stirring at a stirring speed of 400 r / min for 1 hour and a stirring temperature of 52°C, and finally filtering and drying to obtain the nano silver agent.

[0040] The preparation method of the silane liquid of this embodiment is as follows: silane coupling agent KH560, ethanol and water are stirred in a weight ratio of 5:11:6 at a stirring temperature of 50° C. and a stirring speed of 350 r / min for 1 hour; The preparation method of the tripolyformaldehyde body is as follows: melamine and paraformaldehyde are mixed in a weight ratio of 1:5, and then distilled water in an amount of 8 times the total weight of the melamine is added, and the pH is adjusted to 7.5 with sodium hydroxide. The mixture is heated to 76°C under stirring conditions and reacted for 30 minutes. Then, a modifier, terephthalaldehyde, is added in an amount of 15% of the total weight of the melamine, the temperature is maintained, and stirring is continued for 1 hour to obtain the melamine body.

[0041] The preparation method of the modified EVA body of this embodiment is: S11: montmorillonite and silicon dioxide are compounded in a weight ratio of 3:2 to form a compound; the compound, 1-hydroxymethylpyrazole-3-carboxylic acid, polyethylene glycol 400, and phosphorous acid are subjected to an A-conditioning treatment in a weight ratio of 4:6:3:0.08, followed by suction filtration and drying to obtain a conditioning agent A; S12: Preparation of zeolite molecular sieve-organic composite B: S12a: soaking the zeolite molecular sieve in a sufficient amount of 8% by mass sodium hydroxide solution for 2 hours, washing, filtering, and drying to obtain a pretreated zeolite molecular sieve; S12b: γ-aminopropyltriethoxysilane and 65% ethanol solution were mixed in a weight ratio of 3:11, and then hydrochloric acid was added to adjust the pH to 4.5 to obtain an organic solution B; The pretreated zeolite molecular sieve and the organic B solution were subjected to B grinding treatment in a weight ratio of 7:5, and the treatment was completed to obtain a zeolite molecular sieve-organic composite B; S13: adding EVA to tetrahydrofuran at a weight ratio of 5:13 and stirring thoroughly to obtain EVA liquid; mixing the modified A agent and the EVA liquid at a weight ratio of 5:11, and then filtering and drying to obtain the modified A EVA agent; S14: The EVA agent prepared in A and the zeolite molecular sieve-organized composite B are subjected to a secondary stirring treatment in a weight ratio of 15:5. After the stirring is completed, the mixture is filtered and dried to obtain a modified EVA body.

[0042] In this embodiment, the A-treatment is carried out by stirring at a speed of 750 r / min for 2 h; the B-milling is carried out by ball milling at a speed of 1500 r / min for 2 h.

[0043] The stirring temperature of the first stirring process in this embodiment is 55°C, the stirring speed is 500 r / min, and the stirring is carried out for 2 hours; the stirring temperature of the second stirring process is 52°C, the stirring speed is 800 r / min, and the stirring is carried out for 1 hour; The vinyl acetate content of the EVA is 25%, and the melt index is 2 g / 10 min.

[0044] The preparation method of the enhancer of this embodiment is: S101: Silica powder and an 8% by mass ethyl cellulose aqueous solution are uniformly blended in a weight ratio of 5:13, and then tannic acid (8% by mass of the total weight of the silica powder) and polyester fiber (20% by mass of the total weight of the silica powder) are added, and the mixture is thoroughly blended. Finally, the mixture is filtered and dried to obtain a silica powder-polyester fiber modified product; S102: 11 parts by weight of a polyvinyl alcohol solution, 5 parts by weight of a silane coupling agent KH550, and 4 parts by weight of soybean oleic acid are uniformly mixed to obtain a treatment solution; preheating the graphene at 60° C. for 1 hour to obtain preheated graphene; ultrasonically treating the preheated graphene and the treatment solution at a mass ratio of 3:7, and completing the ultrasonic treatment to obtain a treatment solution doped with graphene; S103: The silicon micropowder-polyester fiber modification and the graphene-doped treatment liquid are mixed and ball-milled in a weight ratio of 7:4 at a ball-milling speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a reinforcing agent.

[0045] The ultrasonic treatment in this embodiment was performed with an ultrasonic power of 400 W and an ultrasonic treatment time of 1 h. The mass fraction of the polyvinyl alcohol solution was 12%.

[0046] The method for preparing a highly elastic and wear-resistant sports shoe material of this embodiment includes the following steps: The raw materials of the high-elasticity and wear-resistant sports shoe material are weighed according to weight, and the raw materials are first mixed at a mixing temperature of 80° C. for 5 minutes, then vulcanized, and finally compression molded to obtain the high-elasticity and wear-resistant sports shoe material.

[0047] The vulcanization temperature of the vulcanization treatment in this embodiment is 165° C., and the vulcanization time is 2 minutes. The compression molding pressure is 20 MPa, and the compression molding time is 20 minutes.

[0048] Example 3: A highly elastic and wear-resistant sports shoe material, comprising the following raw materials in parts by weight: 42.5 parts of modified EVA body, 32.5 parts of natural rubber, 10 parts of reinforcing agent, 10 parts of nano silver agent, 6.5 parts of zinc oxide, 4 parts of calcium stearate, 2.5 parts of AC foaming agent, 2.5 parts of paraffin, 0.65 parts of crosslinking agent and 2 parts of antioxidant.

[0049] The antioxidant in this embodiment is antioxidant RD; the cross-linking agent is sulfur and dicumyl peroxide prepared in a weight ratio of 2:1; The preparation method of the nano silver agent is as follows: adding the nano silver powder to a 15% sodium dodecylbenzene sulfonate solution with a mass fraction of 6.5 times the total weight of the nano silver powder, stirring and dispersing the solution uniformly, then adding a silane solution with a mass fraction of 27.5% of the total weight of the nano silver powder and a triformaldehyde body with a mass fraction of 27.5% of the total weight of the nano silver powder, stirring at a stirring speed of 375 r / min for 1 hour and a stirring temperature of 50°C, and finally filtering and drying to obtain the nano silver agent.

[0050] The preparation method of the silane liquid of this embodiment is as follows: silane coupling agent KH560, ethanol and water are stirred in a weight ratio of 4:10:5.5 at a stirring temperature of 50° C. and a stirring speed of 325 r / min for 1 hour; The preparation method of the tripolyformaldehyde body is as follows: melamine and paraformaldehyde are mixed in a weight ratio of 1:4, and then distilled water is added in an amount of 6.5 times the total weight of the melamine. The pH is adjusted to 7.5 with sodium hydroxide. The temperature is raised to 76°C under stirring conditions and the reaction is carried out for 30 minutes. Then, a modifier terephthalaldehyde is added in an amount of 12.5% ​​of the total weight of the melamine. The temperature is maintained and stirring is continued for 1 hour to obtain the melamine body.

[0051] The preparation method of the modified EVA body of this embodiment is: S11: Compounding montmorillonite and silicon dioxide in a weight ratio of 3:2 to form a compound; performing an A-conditioning treatment on the compound, 1-hydroxymethylpyrazole-3-carboxylic acid, polyethylene glycol 400, and phosphorous acid in a weight ratio of 3:5:2:0.08, followed by suction filtration and drying to obtain a conditioning agent A; S12: Preparation of zeolite molecular sieve-organic composite B: S12a: soaking the zeolite molecular sieve in a sufficient amount of 8% by mass sodium hydroxide solution for 2 hours, washing, filtering, and drying to obtain a pretreated zeolite molecular sieve; S12b: γ-aminopropyltriethoxysilane and 60% ethanol solution were mixed in a weight ratio of 3:10, and then hydrochloric acid was added to adjust the pH to 4.5 to obtain an organic solution B; The pretreated zeolite molecular sieve and the organic B solution were subjected to B grinding treatment in a weight ratio of 7:4, and the treatment was completed to obtain a zeolite molecular sieve-organic composite B; S13: adding EVA to tetrahydrofuran at a weight ratio of 5:12 and stirring thoroughly to obtain EVA liquid; mixing the modified A agent and the EVA liquid at a weight ratio of 4:11, and then filtering and drying to obtain the modified EVA agent; S14: The EVA agent prepared in A and the zeolite molecular sieve-organized composite B are subjected to a secondary stirring treatment in a weight ratio of 13:5. After the stirring is completed, the mixture is filtered and dried to obtain a modified EVA body.

[0052] In this embodiment, the A-treatment is carried out by stirring at a speed of 600 r / min for 2 h; the B-milling is carried out by ball milling at a speed of 1250 r / min for 2 h.

[0053] The stirring temperature of the first stirring process in this embodiment is 52.5°C, the stirring speed is 470r / min, and the stirring is carried out for 2h; the stirring temperature of the second stirring process is 50°C, the stirring speed is 750r / min, and the stirring is carried out for 1h; The vinyl acetate content of the EVA is 25%, and the melt index is 2 g / 10 min.

[0054] The preparation method of the enhancer of this embodiment is: S101: Silica powder and an 8% by mass ethyl cellulose aqueous solution are uniformly blended in a weight ratio of 5:12, and then tannic acid (6.5% by weight of the total silica powder) and polyester fiber (17.5% by weight of the total silica powder) are added, and the mixture is thoroughly blended. Finally, the mixture is filtered and dried to obtain a silica powder-polyester fiber modified product. S102: 10 parts by weight of a polyvinyl alcohol solution, 4 parts by weight of a silane coupling agent KH550, and 3 parts by weight of soybean oleic acid are uniformly mixed to obtain a treatment solution; preheating the graphene at 57.5° C. for 1 hour to obtain preheated graphene; ultrasonically treating the preheated graphene and the treatment solution at a mass ratio of 3:7, and completing the ultrasonic treatment to obtain a treatment solution doped with graphene; S103: The silicon micropowder-polyester fiber modification and the graphene-doped treatment liquid are mixed and ball-milled in a weight ratio of 7:3.5 at a ball-milling speed of 1250 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a reinforcing agent.

[0055] The ultrasonic treatment in this embodiment was performed with an ultrasonic power of 375 W and an ultrasonic treatment time of 1 h. The mass fraction of the polyvinyl alcohol solution was 10%.

[0056] The method for preparing a highly elastic and wear-resistant sports shoe material of this embodiment includes the following steps: The raw materials of the high-elasticity and wear-resistant sports shoe material are weighed according to weight, and the raw materials are first mixed at a mixing temperature of 78.5° C. for 5 minutes, then vulcanized, and finally compression molded to obtain the high-elasticity and wear-resistant sports shoe material.

[0057] The vulcanization temperature of the vulcanization treatment in this embodiment is 162° C., and the vulcanization time is 2 minutes. The compression molding pressure is 17.5 MPa, and the compression molding time is 20 minutes.

[0058] Comparative Example 1: The difference from Example 3 is that the modified EVA body is directly replaced by EVA raw material, and the EVA is not processed in any way.

[0059] Comparative Example 2: The difference from Example 3 is that the secondary stirring treatment of the zeolite molecular sieve-organized composite B body is not used in the preparation of the modified EVA body.

[0060] Comparative Example 3: The difference from Example 3 is that no pretreated zeolite molecular sieve is added in the preparation of the zeolite molecular sieve-organized composite B.

[0061] Comparative Example 4: The difference from Example 3 is that no conditioning agent A is used for primary treatment in the preparation of the modified EVA body.

[0062] Comparative Example 5: The difference from Example 3 is that no compounding material is added to the agent A.

[0063] Comparative Example 6: The difference from Example 3 is that no reinforcing agent is added.

[0064] Comparative Example 7: The difference from Example 3 is that the silica powder-polyester fiber modified body is not added in the preparation of the reinforcing agent.

[0065] Comparative Example 8: The difference from Example 3 is that tannic acid and polyester fiber are not added in the preparation of the silica powder-polyester fiber modified body.

[0066] Comparative Example 9: The difference from Example 3 is that no graphene-doped treatment solution is added during the preparation of the reinforcing agent.

[0067] Comparative Example 10: The difference from Example 3 is that no preheated graphene is added in the preparation of the graphene-doped treatment solution.

[0068] The elasticity and wear resistance of the products of Examples 1 to 3 and Comparative Examples 1 to 10 were tested. The test results are shown in Table 1.

[0069] Table 1 Test results of elasticity and wear resistance of products of Examples 1 to 3 and Comparative Examples 1 to 10:

[0070] It can be seen from Comparative Examples 1 to 10 and Examples 1 to 3 that the product of Example 3 has excellent elasticity and wear resistance, and the elasticity and wear resistance of the product can be improved in a coordinated manner; it can be seen from Comparative Examples 1 to 10 and Example 3 that the modified EVA body is directly replaced by EVA raw material and no reinforcing agent is added. The elasticity and wear resistance of the product show a trend of obvious deterioration, and the performance coordination of the product is poor; At the same time, the modified EVA body was not prepared by using the secondary stirring treatment of the zeolite molecular sieve-organized composite B body, the pretreated zeolite molecular sieve was not added in the preparation of the zeolite molecular sieve-organized composite B body, the modified EVA body was not prepared by using the conditioning agent A for primary treatment, and no compound was added to the conditioning agent A. The performance of the product showed a trend of deterioration. The modified EVA body prepared by using the zeolite molecular sieve-organized composite B body in combination with the conditioning agent A had the most significant effect on product performance. The effects of other methods were not as obvious as those of the present invention. The preparation of the modified EVA body was only made by the specific method of the present invention, and the performance effect of the product was the most significant. The performance of the products showed a trend of deterioration when the silicon micropowder-polyester fiber modification was not added in the preparation of the reinforcing agent, tannic acid and polyester fiber were not added in the preparation of the silicon micropowder-polyester fiber modification, the graphene-doped treatment liquid was not added in the preparation of the reinforcing agent, and preheated graphene was not added in the preparation of the graphene-doped treatment liquid. Only the reinforcing agent prepared by using the specific graphene-doped treatment liquid of the present invention and the silicon micropowder-polyester fiber modification had the most significant performance effect. Using other methods as a substitute was not as obvious as the effect of the present invention.

[0071] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the invention can be embodied in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as illustrative and non-restrictive, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations that come within the meaning and range of equivalents of the claims be embraced therein.

[0072] In addition, it should be understood that although this specification is described in terms of implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.

Claims

1. A highly elastic and wear-resistant sports shoe material, characterized in that: It includes the following raw materials in parts by weight: 40-45 parts of modified EVA body, 30-35 parts of natural rubber, 8-12 parts of reinforcing agent, 8-12 parts of nano silver agent, 5-8 parts of zinc oxide, 3-5 parts of calcium stearate, 2-3 parts of AC foaming agent, 2-3 parts of paraffin, 0.5-0.8 parts of crosslinking agent and 1-3 parts of antioxidant.

2. A highly elastic and wear-resistant sports shoe material according to claim 1, characterized in that: The antioxidant is antioxidant RD; the cross-linking agent is sulfur and dicumyl peroxide prepared in a weight ratio of 2:1; The preparation method of the nano silver agent comprises the following steps: adding nano silver powder to a 15% sodium dodecylbenzene sulfonate solution having a mass fraction of 5-8 times the total weight of the nano silver powder, stirring and dispersing the mixture uniformly; then adding a silane solution having a mass fraction of 25-30% of the total weight of the nano silver powder and a triformaldehyde body having a mass fraction of 25-30% of the total weight of the nano silver powder; stirring the mixture at a stirring speed of 350-400 r / min for 1 hour at a stirring temperature of 48-52° C.; and finally filtering and drying the mixture to obtain the nano silver agent.

3. The highly elastic and wear-resistant sports shoe material according to claim 2, characterized in that: The silane liquid is prepared by stirring silane coupling agent KH560, ethanol and water in a weight ratio of (3-5): (8-11): (5-6) at a stirring temperature of 50° C. and a stirring speed of 300-350 r / min for 1 hour; The preparation method of the tripolyformaldehyde body is as follows: melamine and paraformaldehyde are mixed in a weight ratio of 1:(3-5), and then distilled water is added in an amount of 5-8 times the total weight of the melamine. The pH is adjusted to 7.5 with sodium hydroxide. The temperature is raised to 76° C. under stirring conditions, and the reaction is carried out for 30 minutes. Then, a modifier terephthalaldehyde is added in an amount of 10-15% of the total weight of the melamine. The temperature is maintained and stirring is continued for 1 hour to obtain the melamine body.

4. The highly elastic and wear-resistant sports shoe material according to claim 1, characterized in that: The preparation method of the modified EVA body is: S11: montmorillonite and silicon dioxide are compounded in a weight ratio of 3:2 to form a compound; the compound, 1-hydroxymethylpyrazole-3-carboxylic acid, polyethylene glycol 400, and phosphorous acid are subjected to an A-conditioning treatment in a weight ratio of (2-4):(4-6):(1-3):0.08, followed by suction filtration and drying to obtain a conditioning agent A; S12: Preparation of zeolite molecular sieve-organic composite B: S12a: soaking the zeolite molecular sieve in a sufficient amount of 8% by mass sodium hydroxide solution for 2 hours, washing, filtering, and drying to obtain a pretreated zeolite molecular sieve; S12b: Mix γ-aminopropyltriethoxysilane and 55-65% by mass ethanol solution in a weight ratio of 3:(8-11), and then add hydrochloric acid to adjust the pH to 4.5 to obtain organic solution B; The pretreated zeolite molecular sieve and the organic B solution were subjected to B grinding treatment in a weight ratio of 7:(3-5), and the treatment was completed to obtain a zeolite molecular sieve-organic composite B body; S13: adding EVA to tetrahydrofuran in a weight ratio of 5:(11-13) and stirring thoroughly to obtain an EVA liquid; mixing the modified A agent and the EVA liquid in a weight ratio of (3-5):11, and then filtering and drying to obtain the modified EVA agent; S14: The EVA agent prepared by A and the zeolite molecular sieve-organized composite B are subjected to a secondary stirring treatment in a weight ratio of (11-15):

5. After the stirring is completed, the mixture is filtered and dried to obtain a modified EVA body.

5. The highly elastic and wear-resistant sports shoe material according to claim 4, characterized in that: The A-adjustment treatment adopts a stirring method with a stirring speed of 550-750 r / min and stirring for 2 hours; the B-milling treatment adopts a ball milling method with a ball milling speed of 1000-1500 r / min and ball milling for 2 hours.

6. The high-elasticity and wear-resistant sports shoe material according to claim 4, characterized in that: The stirring temperature of the first-stage stirring treatment is 50-55°C, the stirring speed is 450-500r / min, and the stirring is carried out for 2h; the stirring temperature of the second-stage stirring treatment is 48-52°C, the stirring speed is 700-800r / min, and the stirring is carried out for 1h; The vinyl acetate content of the EVA is 25%, and the melt index is 2 g / 10 min.

7. The highly elastic and wear-resistant sports shoe material according to claim 1, characterized in that: The preparation method of the enhancer is: S101: Silica powder and an 8% by mass aqueous solution of ethyl cellulose are uniformly blended in a weight ratio of 5:(11-13), and then tannic acid (5-8% by weight of the total weight of the silica powder) and polyester fiber (15-20% by weight of the total weight of the silica powder) are added, and the mixture is thoroughly blended, and finally filtered and dried to obtain a silica powder-polyester fiber modified product; S102: 8-11 parts by weight of a polyvinyl alcohol solution, 3-5 parts by weight of a silane coupling agent KH550, and 2-4 parts by weight of soybean oleic acid are uniformly mixed to obtain a treatment solution; preheating the graphene at 55-60° C. for 1 hour to obtain preheated graphene; ultrasonically treating the preheated graphene and the treatment solution at a mass ratio of 3:7, and completing the ultrasonic treatment to obtain a treatment solution doped with graphene; S103: The silicon micropowder-polyester fiber modification and the graphene-doped treatment liquid are mixed and ball-milled in a weight ratio of 7:(3-4) at a ball-milling speed of 1000-1500 r / min for 2 h. After the ball-milling is completed, the mixture is filtered and dried to obtain a reinforcing agent.

8. The highly elastic and wear-resistant sports shoe material according to claim 7, characterized in that: The ultrasonic power of the ultrasonic treatment is 350-400W, and the ultrasonic treatment is performed for 1 hour; the mass fraction of the polyvinyl alcohol solution is 8-12%.

9. A method for preparing a highly elastic and wear-resistant sports shoe material, for preparing the highly elastic and wear-resistant sports shoe material according to any one of claims 1 to 8, characterized in that: The following steps are involved: The raw materials of the high-elasticity and wear-resistant sports shoe material are weighed according to weight, and the raw materials are first mixed at a mixing temperature of 75-80° C. for 5 minutes, then vulcanized, and finally compression molded to obtain the high-elasticity and wear-resistant sports shoe material.

10. The method for preparing a highly elastic and wear-resistant sports shoe material according to claim 9, characterized in that: The vulcanization temperature of the vulcanization treatment is 160-165°C, and the vulcanization time is 2 minutes; the pressure of the compression molding is 15-20 MPa, and the compression time is 20 minutes.

Citation Information

Patent Citations

  • Smellless EVA (ethylene-vinyl acetate) material used as shoe sole and preparation method thereof

    CN103910925A

  • Preparation method of flame-retardant polyhydric alcohol and polyurethane foam and polyurethane sealant prepared from flame-retardant polyhydric alcohol

    CN107459620A

  • Preparation method of anti-flaming type shoe upper material

    CN111663200A

  • Metal organic framework granular material as well as preparation method and application thereof

    CN118341408A

  • Sole material, sneaker sole and sneaker

    CN118852746A

Cited By

  • EVA (Ethylene Vinyl Acetate) foaming material, preparation method and application thereof

    CN121086320A