Hollow fiber reinforced aerogel composite material and preparation method thereof

By preparing hollow fiber reinforced aerogel composite materials, the strength and sound insulation problems of aerogel materials in the aerospace field are solved, high-temperature stability and excellent sound insulation performance are achieved, and it is suitable for heat insulation and noise reduction of aircraft.

CN120774690AActive Publication Date: 2025-10-14SHANDONG RES & DESIGN ACADEMY OF IND CERAMICS

Patent Information

Application Number
CN202511247505.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-03
Publication Date
2025-10-14
Estimated Expiration
2045-09-03

AI Technical Summary

Technical Problem

Existing aerogel materials in the aerospace field have problems such as weak strength, poor sound insulation performance, and mismatched thermal expansion coefficients of aluminum-silicon components, which affect their thermal insulation and noise reduction effects.

Method used

A preparation method for hollow fiber reinforced aerogel composite materials is adopted. Through the steps of preparing aluminum silica sol, modified composite, vacuum impregnation, gel aging and supercritical drying, the coating effect of nano-aluminum titanate and nano-zirconium oxide is used to improve the bonding performance between aerogel particles, and the sound insulation performance is improved through the acoustic wave resonance and scattering effect of the hollow fiber.

Benefits of technology

The mechanical properties, thermal insulation and sound insulation properties of aerogel materials have been improved, and their stability and noise isolation capabilities in high temperature environments have been enhanced, making them suitable for the thermal insulation and noise reduction needs of aircraft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a hollow fiber reinforced aerogel composite material and a preparation method thereof, and relates to the field of aerogel materials. The preparation method of the hollow fiber reinforced aerogel composite material comprises the following steps: preparation of aluminum silica sol, modification compounding, vacuum impregnation, gel aging and supercritical drying. According to the hollow fiber reinforced aerogel composite material and the preparation method thereof, the sound insulation performance of the aerogel material can be effectively improved on the premise of overcoming the existing defects (the defect of a porous structure of aerogel, weak binding force among aerogel particles and thermal stress caused by mismatching of thermal expansion coefficients of aluminum and silicon components) of the aerogel material; the strength, the toughness and the heat insulation performance of the aerogel material are synchronously improved.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the field of aerogel materials, in particular to a hollow fiber reinforced aerogel composite material and a preparation method thereof. BACKGROUND

[0002] With the continuous progress and development of science and technology, the flight speed of aircraft is continuously improved. In order to realize the take-off, acceleration, cruising and maneuvering of the aircraft, the gravity of the aircraft itself and the resistance generated by various factors need to be overcome. The aircraft engine can convert energy into controllable thrust and power, and its performance has an important influence on the flight speed, load and endurance time of the aircraft. However, during the operation of the engine, the core engine temperature can exceed 1000℃, which can cause different degrees of thermal damage to the surrounding fuselage and precision equipment area. At the same time, the aerodynamic noise, combustion noise and mechanical noise generated by unstable airflow can cause structural resonance, further threatening the safety of the equipment. Therefore, the heat insulation performance of the heat insulation layer of the aircraft engine is particularly important during flight. In addition, in the short nacelle of the aircraft engine and the special vibration sensitive use scene, the use of the heat insulation layer for auxiliary noise reduction can further play the multifunctionality of the material.

[0003] Aerogel material is a kind of nano-porous material with light weight, temperature resistance and heat insulation performance. Its light weight can reduce the mass of traditional heat insulation materials by more than 50%, saving a lot of space usage. At the same time, its porous structure not only reduces the solid and gas heat conduction of the material, but also absorbs medium and high frequency sound waves, and has good use effect in sound absorption and noise reduction. Among them, in the field of oxide aerogel materials, the temperature resistance of aluminum-silicon aerogel material can reach 1200℃, which has good temperature resistance and heat insulation performance. However, due to the problems of the porous structure of aluminum-silicon aerogel itself, the weak bonding force between aerogel particles, the mismatch of thermal expansion coefficient of aluminum-silicon components causing thermal stress, etc., the strength of the aerogel material is weak, which limits the application of aluminum-silicon aerogel material in the field of aerospace materials.

[0004] At the same time, the existing aerogel material has poor sound insulation performance, and when used as a heat insulation material in the field of aerospace, it has limited effect on blocking the noise of the aircraft. The existing sound insulation processing method for aerogel material affects the strength, toughness and heat insulation performance of the aerogel material, and cannot improve the strength, toughness and heat insulation performance of the aerogel material while improving the sound insulation performance of the aerogel material.

[0005] Therefore, the hollow fiber reinforced aerogel composite and the preparation method thereof are provided, which can effectively improve the sound insulation performance of the aerogel material, and simultaneously improve the strength, toughness and heat insulation performance of the aerogel material under the premise of overcoming the existing defects of the aerogel material (the defect of the porous structure of the aerogel itself, the weak binding force between the aerogel particles, and the thermal stress caused by the mismatch of the thermal expansion coefficients of the aluminum and silicon components), which has important technical significance and research value. SUMMARY

[0006] In order to solve the technical problems in the prior art, the present application provides a hollow fiber reinforced aerogel composite and a preparation method thereof, which can effectively improve the sound insulation performance of the aerogel material, and simultaneously improve the strength, toughness and heat insulation performance of the aerogel material under the premise of overcoming the existing defects of the aerogel material (the defect of the porous structure of the aerogel itself, the weak binding force between the aerogel particles, and the thermal stress caused by the mismatch of the thermal expansion coefficients of the aluminum and silicon components).

[0007] To solve the above technical problems, the technical solutions adopted by the present application are as follows: The preparation method of the hollow fiber reinforced aerogel composite comprises the following steps: preparing an aluminum-silicon sol, modifying and compounding, vacuum impregnation, gel aging, and supercritical drying. The method for preparing the aluminum-silicon sol is to mix aluminum chloride hexahydrate, anhydrous ethanol and deionized water to obtain an aluminum source solution; mix tetraethyl orthosilicate, anhydrous ethanol and deionized water to obtain a silicon source solution; and mix the aluminum source solution and the silicon source solution to obtain the aluminum-silicon sol. The method for modifying and compounding is to obtain pretreated aluminum titanate after heat treatment of nano-aluminum titanate; put the pretreated aluminum titanate and deionized water into anhydrous ethanol, mix uniformly, adjust the pH to 8.5-9.5, heat to 48-52℃, and then drop in the tetraethyl orthosilicate solution while keeping warm; after the dropping is completed, continue to keep warm and stir; separate to obtain a solid, wash and dry the solid to obtain coated aluminum titanate; put the coated aluminum titanate and nano-zirconium oxide into the aluminum-silicon sol, mix uniformly to obtain a modified and compounded sol. The method for vacuum impregnation is to press the hollow alumina fibers into a hollow fiber felt, and use the modified and compounded sol containing an initiator to perform vacuum impregnation on the hollow fiber felt to obtain an impregnated body. The impregnated body is subjected to gel aging and supercritical drying to obtain the hollow fiber reinforced aerogel composite.

[0008] Preferably, the molar ratio of aluminum chloride hexahydrate, anhydrous ethanol and deionized water used in the aluminum source solution is 3-3.1:15-17:55-60; The molar ratio of tetraethyl orthosilicate, anhydrous ethanol and deionized water used in the silicon source solution is 1-1.2:5-6:5-6; The molar ratio of aluminum chloride hexahydrate to tetraethyl orthosilicate is 3-3.1:1-1.2 in the mixing of the aluminum source solution and the silicon source solution.

[0009] Preferably, the weight ratio of the pretreated aluminum titanate to anhydrous ethanol is 1:70-75 in the modification and compounding. The volume of deionized water added is 3.5-4% of the volume of anhydrous ethanol. The weight ratio of tetraethyl orthosilicate to nano-aluminum titanate in the tetraethyl orthosilicate solution is 0.18-0.21:1. The weight ratio of coated aluminum titanate, nano-zirconium oxide, and aluminum-silicon sol is 4.8-5.5:3.4-4.2:100.

[0010] Preferably, the tetraethyl orthosilicate solution in the modification and compounding is an anhydrous ethanol solution of tetraethyl orthosilicate with a concentration of 2.5-2.8wt%. The dropwise addition rate of the tetraethyl orthosilicate solution is 0.4-0.5mL / min. After the completion of the dropwise addition of the tetraethyl orthosilicate solution, the continuous heat preservation and stirring time is 5-6h.

[0011] Further, in the modification and compounding, the nano-aluminum titanate is heat treated at 110-120℃ for 1-2h to obtain the pretreated aluminum titanate. The particle size of the nano-aluminum titanate is 50-60nm. The particle size of the nano-zirconium oxide is 20-30nm.

[0012] Further, the method of vacuum impregnation is to press the hollow alumina fibers into a hollow fiber felt, then place the hollow fiber felt together with the mold into a vacuum impregnation tank in a vacuum environment at room temperature, and use a modified composite sol containing an initiator to vacuum impregnate the hollow fiber felt for 30-40min to obtain an impregnated body. The initiator is propylene oxide, and the molar ratio of the initiator to aluminum chloride hexahydrate used in the modified composite sol is 1:3-5.

[0013] Further, the method of gel aging is to completely immerse the impregnated body in anhydrous ethanol after heat preservation and gelation in a temperature environment of 48-52℃, and then stand for aging under the condition of 48-52℃ to obtain a composite.

[0014] Preferably, in the gel aging, the heat preservation and gelation time is 3-5h. The standing and aging time is 72-96h. The anhydrous ethanol is replaced every 10-12h during the standing and aging process.

[0015] Further, the supercritical drying method is as follows: after the impregnated body is obtained by gel aging to obtain a composite, the temperature of supercritical drying is controlled to be 270-280 DEG C, the pressure is controlled to be 8-9 MPa, and the composite is subjected to supercritical drying for 2-4 h to obtain the hollow fiber reinforced aerogel composite material.

[0016] A hollow fiber reinforced aerogel composite material is prepared by the preparation method.

[0017] Compared with the prior art, the present application has the following advantages: (1) The preparation method of the hollow fiber reinforced aerogel composite material uses specific aluminum and silicon sources to prepare aluminum-silicon sol; in the modification and compounding step, a silica layer is coated on the surface of the nano-aluminum titanate in an in-situ coating manner to obtain coated aluminum titanate; the crack propagation path is blocked by the filling effect of nano-particles (coated aluminum titanate and nano-zirconium oxide), the porous structure defects of the aerogel are improved, and the mechanical properties of the composite material are improved; at the same time, the bonding properties between the aerogel particles are further improved by the bonding effect of the coated aluminum titanate and the active groups of the aluminum-silicon sol; and the near-zero expansion of the coated aluminum titanate offsets the shrinkage of the matrix, the nano-zirconium oxide further compensates for thermal expansion, the interface stress is buffered as a whole, the thermal stress is buffered, the thermal expansion matching of the aluminum-silicon component is effectively improved, and the temperature resistance of the aerogel composite material is improved; then the hollow aluminum oxide fibers are pressed into a hollow fiber felt, the hollow fiber felt is vacuum impregnated with the modified composite sol containing an initiator, and the hollow fiber reinforced aerogel composite material is prepared by gel aging and supercritical drying; by compounding the hollow fibers and the aluminum-silicon aerogel, the mechanical properties of the aerogel composite material are further improved, and the hollow fibers can scatter and absorb sound waves through acoustic resonance and scattering effect, thereby giving the aerogel composite material excellent sound insulation performance.

[0018] (2) The compressive strength of the hollow fiber reinforced aerogel composite material is 0.18-0.20 MPa, the bending strength is 1.4-1.6 MPa, the thermal expansion coefficient is 1.09-1.13 x 10 -6 / K, the room temperature thermal conductivity coefficient is 0.025-0.026 W / m·k, the 800 DEG C thermal conductivity coefficient is 0.036-0.039 W / m·k, the sound transmission loss is 42-45 dB, and the thermal shock cycle number is 52-57 times.

[0019] (3) The preparation method of the hollow fiber reinforced aerogel composite material has a simple process flow, the preparation process is easy to control, the production safety is high, and the method is suitable for large-scale production.

[0020] (4) The hollow fiber reinforced aerogel composite material has high temperature resistance, high strength, heat insulation, sound insulation and other performances, can fully play the multifunctionality of the aerogel material, and further expands the application scenarios of the aerogel composite material. DETAILED DESCRIPTION

[0021] In order to have a clearer understanding of the technical features, objectives and effects of the present application, the specific embodiments of the present application will be described. It should be pointed out that the following detailed description is exemplary and is intended to provide further description of the present application. Unless otherwise specified, all technical and scientific terms used in the present application have the same meaning as generally understood by those skilled in the art to which the present application belongs.

[0022] It should be noted that the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, "first", "second", and the like are used to distinguish similar objects, and are not intended to describe a particular order or sequence, and it should also be understood that when the terms "comprise" and / or "include" are used in the specification, there is a feature, step, operation, device, component and / or combination thereof.

[0023] The present application provides a preparation method of a hollow fiber reinforced aerogel composite material, comprising the following steps: preparing an aluminum-silicon sol, modifying and combining, vacuum impregnation, gel aging, supercritical drying.

[0024] The method for preparing the aluminum-silicon sol is that inorganic aluminum salt and silicon alkoxide precursor are respectively used as aluminum source (aluminum chloride hexahydrate) and silicon source (tetraethyl orthosilicate), a certain amount of aluminum source and silicon source are mixed with a certain proportion of anhydrous ethanol and deionized water, respectively, and each is stirred for 30-50 min to obtain an aluminum source solution and a silicon source solution; the aluminum source solution and the silicon source solution are mixed and continue to be stirred for 30-50 min to form a uniform mixed aluminum-silicon sol, which is ready for use.

[0025] In the present application, preferably, in the preparation of the aluminum source solution, the molar ratio of aluminum chloride hexahydrate, anhydrous ethanol and deionized water used is 3-3.1:15-17:55-60.

[0026] In the present application, preferably, in the preparation of the silicon source solution, the molar ratio of tetraethyl orthosilicate, anhydrous ethanol and deionized water used is 1-1.2:5-6:5-6.

[0027] In the present application, preferably, in the mixing of the aluminum source solution and the silicon source solution, the molar ratio of aluminum chloride hexahydrate to tetraethyl orthosilicate is controlled to be 3-3.1:1-1.2.

[0028] The method for modifying and compounding is as follows: the nano aluminum titanate with a particle size of 50-60 nm is placed in a thermostat, and is treated at 110-120 DEG C for 1-2 h, and then is cooled to obtain pretreated aluminum titanate; then the pretreated aluminum titanate is put into 70-75 times weight of anhydrous ethanol, and is ultrasonically dispersed for 5-15 min, then deionized water is added and mixed uniformly, then ammonia water with a concentration of 25-28 wt% is used to adjust the pH to 8.5-9.5, and the mixture is stirred and heated to 48-52 DEG C and is kept warm; the tetraethyl orthosilicate solution is added dropwise at a dropwise adding rate of 0.4-0.5 mL / min, after the dropwise adding is completed, the mixture is kept warm at 48-52 DEG C and is stirred for 5-6 h; the solid is obtained by centrifugal separation, the solid is washed with anhydrous ethanol for 2-3 times, and is placed in a vacuum drying box, and is dried in a vacuum degree of 0.07-0.08 MPa at 50-55 DEG C until the weight is constant to obtain coated aluminum titanate; then the coated aluminum titanate and nano zirconium oxide (with a particle size of 20-30 nm) are put into aluminum-silicon sol, and are ultrasonically dispersed uniformly to obtain modified and compounded sol.

[0029] In the embodiment of the present application, preferably, the volume of the deionized water is 3.5-4% of the volume of the anhydrous ethanol.

[0030] In the embodiment of the present application, the tetraethyl orthosilicate solution is an ethanol solution of tetraethyl orthosilicate with a concentration of 2.5-2.8 wt%; preferably, the weight ratio of tetraethyl orthosilicate to nano aluminum titanate in the tetraethyl orthosilicate solution is 0.18-0.21:1.

[0031] In the embodiment of the present application, the weight ratio of the coated aluminum titanate, nano zirconium oxide and aluminum-silicon sol is 4.8-5.5:3.4-4.2:100.

[0032] The method for vacuum impregnation is as follows: the hollow alumina fiber is pressed into a hollow fiber felt through a mold, then the hollow fiber felt is placed in a vacuum impregnation tank together with the mold, the vacuum impregnation tank is vacuumized by a vacuum pump, then the initiator is put into the modified and compounded sol and is mixed uniformly, and is siphoned into the vacuum impregnation tank, the modified and compounded sol is controlled to completely impregnate the hollow fiber felt, and the impregnation is kept in a vacuum environment at room temperature for 30-40 min, the impregnation treatment is completed, and an impregnated body is obtained.

[0033] In the embodiment of the present application, the initiator is propylene oxide; preferably, the molar ratio of the initiator to aluminum chloride hexahydrate used in the modified and compounded sol is 1:3-5.

[0034] In the embodiment of the present application, the liquid level height of the modified and compounded sol is 1.2-1.6 times the thickness of the hollow fiber felt.

[0035] The method for aging the gel is as follows: the dip body is placed in an oven together with the mold and heated to 48-52 DEG C, the gel is kept for 3-5 h, then the mold with the dip body is taken out of the gel and completely immersed in anhydrous ethanol, and kept for 72-96 h at a temperature of 48-52 DEG C, and the anhydrous ethanol is replaced every 10-12 h during the aging process, and the composite is obtained after the aging is completed.

[0036] In the embodiment of the present application, the liquid level of the anhydrous ethanol is controlled to be 1.5-2 times the thickness of the dip body during the aging process.

[0037] The method for supercritical drying is as follows: the composite is placed in a supercritical drying reaction kettle together with the mold, the temperature for supercritical drying is controlled to be 270-280 DEG C, the pressure is controlled to be 8-9 MPa, and the supercritical drying is performed for 2-4 h, then the temperature is lowered, the mold is removed, and the hollow fiber reinforced aerogel composite material is obtained.

[0038] In the preparation of the hollow fiber reinforced aerogel composite material, the aluminum-silicon sol is prepared by using specific aluminum source and silicon source; in the modification and compounding step, the silica layer is coated on the surface of the nano-aluminum titanate in an in-situ coating manner to obtain the coated aluminum titanate; the crack propagation path is blocked by the filling effect of the nano-particles (coated aluminum titanate and nano-zirconium oxide), the mechanical properties of the composite material are improved, the bonding properties between the aerogel particles are further improved by the bonding effect of the active groups of the coated aluminum titanate and the aluminum-silicon sol, the coated aluminum titanate and the nano-zirconium oxide are matched with the aluminum-silicon sol to prepare the modified composite sol, the near-zero expansion of the coated aluminum titanate offsets the shrinkage of the matrix, the nano-zirconium oxide further compensates the thermal expansion, the interface stress is buffered, the thermal stress is buffered, the thermal expansion matching of the aluminum-silicon component is effectively improved, and the temperature resistance of the aerogel composite material is improved; then the hollow aluminum oxide fibers are pressed into a hollow fiber felt, the modified composite sol containing an initiator is used for vacuum impregnation of the hollow fiber felt, and the hollow fiber reinforced aerogel composite material is prepared by gel aging and supercritical drying; by compounding the hollow fibers with the aluminum-silicon aerogel, the mechanical properties of the aerogel composite material are further improved, the acoustic wave is scattered and absorbed by the acoustic wave resonance and scattering effect of the hollow fibers, and the aerogel composite material has excellent sound insulation performance.

[0039] The embodiment of the present application also provides a hollow fiber reinforced aerogel composite material prepared by the above preparation method.

[0040] The present application is further described below by combining some specific embodiments.

[0041] Embodiment 1 The present embodiment provides a preparation method of a hollow fiber reinforced aerogel composite material, specifically as follows: 1. Preparation of aluminum-silicon sol An inorganic aluminum salt and a silicon alkoxide precursor were used as the aluminum source (aluminum chloride hexahydrate) and the silicon source (tetraethyl orthosilicate), respectively. A certain amount of the aluminum source and the silicon source were mixed with a certain proportion of anhydrous ethanol and deionized water, respectively, and stirred for 30 min to prepare an aluminum source solution and a silicon source solution. The aluminum source solution and the silicon source solution were mixed and stirred for another 30 min to form a uniform mixed aluminum-silicon sol, which was ready for use.

[0042] In the preparation of the aluminum source solution, the molar ratio of aluminum chloride hexahydrate, anhydrous ethanol, and deionized water was 3:15:55.

[0043] In the preparation of the silicon source solution, the molar ratio of tetraethyl orthosilicate, anhydrous ethanol, and deionized water was 1:5:5.

[0044] In the mixing of the aluminum source solution and the silicon source solution, the molar ratio of aluminum chloride hexahydrate to tetraethyl orthosilicate was controlled to be 3:1.

[0045] 2. Modification and compounding The aluminum titanate nanoparticles with a particle size of 50 nm were placed in a constant temperature oven and treated at 110℃ for 2h, then cooled to obtain pretreated aluminum titanate. Then the pretreated aluminum titanate was added to 70 times the weight of anhydrous ethanol, ultrasonically dispersed for 5 min, then deionized water was added and mixed uniformly, then the pH was adjusted to 9 using 25wt% ammonia water, and the temperature was raised to 48℃ and stirred. Tetraethyl orthosilicate solution was added at a drop rate of 0.4mL / min, and after the addition was completed, the mixture was stirred at 48℃ for 5h. The solid was obtained by centrifugal separation, and the solid was washed with anhydrous ethanol for 3 times, and then placed in a vacuum drying oven at a vacuum degree of 0.07MPa and dried at 55℃ to constant weight to obtain coated aluminum titanate. Then the coated aluminum titanate and nano-zirconium oxide (particle size of 20nm) were added to the aluminum-silicon sol and ultrasonically dispersed to obtain a modified and compounded sol.

[0046] The volume of deionized water added was 3.5% of the volume of anhydrous ethanol.

[0047] The tetraethyl orthosilicate solution was a 2.5wt% tetraethyl orthosilicate ethanol solution, and the weight ratio of tetraethyl orthosilicate to nano-aluminum titanate in the tetraethyl orthosilicate solution was 0.18:1.

[0048] The weight ratio of coated aluminum titanate, nano-zirconium oxide, and aluminum-silicon sol was 4.8:3.4:100.

[0049] 3. Vacuum impregnation The hollow alumina fibers are pressed into a hollow fiber felt through a mold, and then the hollow fiber felt is placed in a vacuum impregnation tank together with the mold. After the vacuum impregnation tank is vacuumized by a vacuum pump, the initiator is put into the modified composite sol and mixed uniformly, and then siphoned into the vacuum impregnation tank. The modified composite sol is controlled to completely impregnate the hollow fiber felt, and the impregnation is carried out at room temperature for 30 min in a vacuum environment. The impregnation is completed, and an impregnated body is obtained.

[0050] In the formula, the initiator is propylene oxide; and the molar ratio of the initiator to aluminum chloride hexahydrate used in the modified composite sol is 1:3.

[0051] The liquid level of the modified composite sol is 1.2 times the thickness of the hollow fiber felt.

[0052] 4. Gel aging The impregnated body is placed in an oven together with the mold and heated to 48℃. After the gel is kept for 3 h, the mold with the impregnated body is taken out of the gel and completely immersed in anhydrous ethanol. Under the condition of 48℃, the aging is carried out for 96 h. During the aging process, the anhydrous ethanol is replaced every 12 h. After the aging is completed, a composite body is obtained.

[0053] In the formula, the liquid level of the anhydrous ethanol is controlled to be 1.5 times the thickness of the impregnated body during the aging process.

[0054] 5. Supercritical drying The composite body is placed in a supercritical drying reaction kettle together with the mold. The temperature of the supercritical drying is controlled to be 270℃, and the pressure is controlled to be 8 MPa. The supercritical drying is carried out for 2 h. After the supercritical drying is completed, the temperature is lowered, the mold is removed, and a hollow fiber reinforced aerogel composite material is obtained.

[0055] The embodiment also provides the hollow fiber reinforced aerogel composite material prepared by the method.

[0056] Example 2 The embodiment provides a preparation method of a hollow fiber reinforced aerogel composite material, in particular to the following steps. 1. Preparation of aluminum-silicon sol Inorganic aluminum salt and silicon alkoxide precursor are respectively used as aluminum source (aluminum chloride hexahydrate) and silicon source (tetraethyl orthosilicate). A certain amount of aluminum source and silicon source are respectively mixed with a certain proportion of anhydrous ethanol and deionized water, and each is stirred for 40 min to prepare an aluminum source solution and a silicon source solution. The aluminum source solution and the silicon source solution are mixed and continuously stirred for 40 min to form a uniformly mixed aluminum-silicon sol, which is ready for use.

[0057] In the preparation of the aluminum source solution, the molar ratio of aluminum chloride hexahydrate, anhydrous ethanol and deionized water is 3.05:16:58.

[0058] In the preparation of the silicon source solution, the mole ratio of tetraethyl orthosilicate, anhydrous ethanol and deionized water used is 1.1:5.5:5.5.

[0059] In the mixing of the aluminum source solution and the silicon source solution, the mole ratio of aluminum chloride hexahydrate and tetraethyl orthosilicate is controlled to be 3.05:1.1.

[0060] 2、Modification and compounding The nano-aluminum titanate with a particle size of 50 nm is placed in a thermostat, and after heat treatment at 115℃ for 1.5 h, it is cooled to obtain pretreated aluminum titanate. Then the pretreated aluminum titanate is put into 72 times by weight of anhydrous ethanol, ultrasonically dispersed for 10 min, and then deionized water is added and mixed uniformly. Then, 25wt% ammonia water is used to adjust the pH to 9, and the temperature is stirred and raised to 50℃. The tetraethyl orthosilicate solution is added at a drop rate of 0.45mL / min, and after the drop is completed, the temperature is maintained at 50℃ for 5.5h. The solid is obtained by centrifugal separation, and the solid is washed with anhydrous ethanol for 3 times, and placed in a vacuum drying box, dried at 52℃ under a vacuum degree of 0.075MPa until the weight is constant, to obtain coated aluminum titanate. Then the coated aluminum titanate and nano-zirconium oxide (particle size of 20 nm) are put into the aluminum-silicon sol and ultrasonically dispersed to obtain a modified and compounded sol.

[0061] The volume of deionized water added is 3.8% of the volume of anhydrous ethanol.

[0062] The tetraethyl orthosilicate solution is an ethanol solution of 2.7wt% tetraethyl orthosilicate; the weight ratio of tetraethyl orthosilicate in the tetraethyl orthosilicate solution to nano-aluminum titanate is 0.2:1.

[0063] The weight ratio of coated aluminum titanate, nano-zirconium oxide and aluminum-silicon sol is 5.1:3.9:100.

[0064] 3、Vacuum impregnation The hollow alumina fiber is pressed into a hollow fiber felt through a mold, and then the hollow fiber felt together with the mold is placed in a vacuum impregnation tank. After the vacuum impregnation tank is vacuumized by a vacuum pump, the initiator is mixed uniformly in the modified and compounded sol and then siphoned into the vacuum impregnation tank. The modified and compounded sol is controlled to completely impregnate the hollow fiber felt, and the vacuum environment is maintained at room temperature for 35 min to complete the impregnation treatment and obtain an impregnated body.

[0065] The initiator is propylene oxide; the mole ratio of the initiator to aluminum chloride hexahydrate in the modified and compounded sol is 1:3.5.

[0066] The liquid level of the modified and compounded sol is 1.5 times the thickness of the hollow fiber felt.

[0067] 4、Gel aging The dip is heated to 50°C in an oven together with the mold, and after the gel is kept at temperature for 4h, the mold with the dip is taken out of the gel and completely immersed in anhydrous ethanol, and is kept at temperature for 96h, and the anhydrous ethanol is replaced every 12h during the keeping at temperature, and after the keeping at temperature is completed, the composite is obtained.

[0068] In the keeping at temperature, the liquid level of the anhydrous ethanol is controlled to be 1.8 times the thickness of the dip.

[0069] 5. Supercritical drying The composite is placed in a supercritical drying reactor together with the mold, and supercritical drying is performed at a temperature of 275°C and a pressure of 8.5MPa for 3h, and after the supercritical drying is completed, the mold is removed, and the hollow fiber reinforced aerogel composite material is obtained.

[0070] The embodiment also provides the hollow fiber reinforced aerogel composite material prepared by the method.

[0071] Example 3 The embodiment provides a preparation method of a hollow fiber reinforced aerogel composite material, and specifically relates to the following steps. 1. Preparation of aluminum-silicon sol Inorganic aluminum salt and silicon alkoxide precursor are respectively used as an aluminum source (aluminum chloride hexahydrate) and a silicon source (tetraethyl orthosilicate), a certain amount of the aluminum source and the silicon source are respectively mixed with a certain proportion of anhydrous ethanol and deionized water, and each is stirred for 50min to prepare an aluminum source solution and a silicon source solution; the aluminum source solution and the silicon source solution are mixed and continuously stirred for 50min to form a uniform mixed aluminum-silicon sol, which is prepared for use.

[0072] In the preparation of the aluminum source solution, the molar ratio of the aluminum chloride hexahydrate, the anhydrous ethanol and the deionized water used is 3.1:17:60.

[0073] In the preparation of the silicon source solution, the molar ratio of the tetraethyl orthosilicate, the anhydrous ethanol and the deionized water used is 1.2:6:6.

[0074] In the mixing of the aluminum source solution and the silicon source solution, the molar ratio of the aluminum chloride hexahydrate and the tetraethyl orthosilicate is controlled to be 3.1:1.2.

[0075] 2. Modification and compounding The nanometer aluminum titanate with a particle size of 50 nm is placed in a thermostat, and is treated at 120℃ for 2 hours, and then is cooled to obtain pretreated aluminum titanate; then the pretreated aluminum titanate is put into 75 times of weight of anhydrous ethanol, and is ultrasonically dispersed for 15 minutes, then deionized water is added and mixed uniformly, then the pH is adjusted to 9 by using 25wt% ammonia water, and is stirred and heated to 52℃, and is kept warm; the tetraethyl orthosilicate solution is added dropwise at a dropwise adding rate of 0.5mL / min, after the dropwise adding is completed, 52℃ is kept warm and stirred for 6 hours; the solid is obtained by centrifugal separation, the solid is washed with anhydrous ethanol for 3 times, and is placed in a vacuum drying box, and is dried at 50℃ under the condition of a vacuum degree of 0.08MPa until the weight is constant, to obtain coated aluminum titanate; then the coated aluminum titanate and nanometer zirconium oxide (with a particle size of 20nm) are put into the aluminum-silicon sol, and are ultrasonically dispersed uniformly to obtain a modified composite sol.

[0076] The volume of the deionized water added is 4% of the volume of the anhydrous ethanol.

[0077] The tetraethyl orthosilicate solution is a 2.8wt% tetraethyl orthosilicate ethanol solution; the weight ratio of the tetraethyl orthosilicate in the tetraethyl orthosilicate solution to the nanometer aluminum titanate is 0.21:1.

[0078] The weight ratio of the coated aluminum titanate, the nanometer zirconium oxide and the aluminum-silicon sol is 5.5:4.2:100.

[0079] 3. Vacuum impregnation The hollow alumina fiber is pressed into a hollow fiber felt through a mold, then the hollow fiber felt is placed in a vacuum impregnation tank together with the mold, the vacuum impregnation tank is vacuumized by using a vacuum pump, then the initiator is added into the modified composite sol and mixed uniformly, and is siphoned into the vacuum impregnation tank, the modified composite sol is controlled to completely impregnate the hollow fiber felt, and the impregnation is kept in a vacuum environment at room temperature for 40 minutes, the impregnation treatment is completed, and an impregnated body is obtained.

[0080] The initiator is propylene oxide; the molar ratio of the initiator to aluminum chloride hexahydrate used in the modified composite sol is 1:3.8.

[0081] The liquid level of the modified composite sol is 1.6 times the thickness of the hollow fiber felt.

[0082] 4. Gel aging The impregnated body is placed in an oven together with the mold, and is heated to 52℃, and is kept warm for 5 hours, then the mold with the impregnated body is taken out of the gel, and is completely immersed in anhydrous ethanol, and is aged for 96 hours at a temperature of 52℃, and the anhydrous ethanol is replaced every 12 hours during the aging process, and after the aging is completed, a composite body is obtained.

[0083] The liquid level of the anhydrous ethanol is controlled to be 2 times the thickness of the impregnated body during the aging process.

[0084] 5. Supercritical drying The composite was placed into a supercritical drying reactor together with the mold, the temperature of the supercritical drying was controlled at 280℃, the pressure was 9MPa, and the supercritical drying was performed for 4h; after the supercritical drying was completed, the temperature was lowered, the mold was removed, and a hollow fiber reinforced aerogel composite material was obtained.

[0085] The example also provides a hollow fiber reinforced aerogel composite material prepared by the foregoing method.

[0086] Comparative Example 1 Comparative Example 1 used the technical solution of Example 2, except that the modification step was omitted, and the aluminum-silicon sol was directly used in the vacuum impregnation step, and the hollow fiber felt was directly vacuum impregnated with the aluminum-silicon sol.

[0087] The compressive strength, bending strength, thermal conductivity at room temperature, thermal conductivity at 800℃, and acoustic transmission loss (acoustic wave frequency 3KHz) of the aerogel composite materials of Examples 1-3 and Comparative Example 1 were detected respectively; at the same time, the aerogel composite materials of Examples 1-3 and Comparative Example 1 were placed in a calcining furnace, the temperature was raised from room temperature to 800℃ at a rate of 10℃ / min, after 30min of heat preservation, the temperature was lowered to room temperature at a rate of 10℃ / min, the aforementioned temperature rising and lowering process was 1 thermal shock cycle, and the number of thermal shock cycles when the aerogel composite materials appeared destructive cracking was counted to verify the thermal shock cycle stability. The specific results are shown in the following table:

[0088] The preparation method of the hollow fiber reinforced aerogel composite material of the present application adopts specific aluminum source and silicon source to prepare aluminum silicon sol; in the modification and compounding step, a silica layer is coated on the surface of nano aluminum titanate in an in-situ coating manner to obtain coated aluminum titanate; the filling effect of nano particles (coated aluminum titanate, nano zirconium oxide) blocks the crack propagation path, improves the aerogel porous structure defects, and improves the mechanical properties of the composite material; at the same time, through the bonding effect of the coated aluminum titanate and the active groups of the aluminum silicon sol, the bonding performance between the aerogel particles is further improved; and by preparing a modified composite sol by combining the coated aluminum titanate, nano zirconium oxide and aluminum silicon sol, the near-zero expansion of the coated aluminum titanate offsets the shrinkage effect of the matrix, the nano zirconium oxide further compensates for thermal expansion, the overall combination buffers the interfacial stress, realizes thermal stress buffering, effectively improves the thermal expansion matching of the aluminum silicon component, and improves the temperature resistance of the aerogel composite material; then the hollow aluminum oxide fibers are pressed into a hollow fiber felt, the modified composite sol containing an initiator is used to vacuum impregnate the hollow fiber felt, and then gel aging and supercritical drying are performed to obtain the hollow fiber reinforced aerogel composite material; by compounding the hollow fibers with the composite aluminum silicon aerogel, the mechanical properties of the aerogel composite material are further improved, and at the same time, the hollow fibers can scatter and absorb sound waves through acoustic resonance and scattering effect, thereby endowing the aerogel composite material with excellent sound insulation performance.

[0089] Unless otherwise specified, the percentages used in the present application are mass percentages.

[0090] Finally, it should be noted that: the above only describes the preferred embodiments of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent replacements to some technical features. Any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a hollow fiber reinforced aerogel composite material, characterized in that: The following steps are involved: Preparation of aluminum silica sol, modified composite, vacuum impregnation, gel aging, supercritical drying; The method for preparing the aluminum silicate sol comprises mixing aluminum chloride hexahydrate with anhydrous ethanol and deionized water to obtain an aluminum source solution; mixing ethyl orthosilicate with anhydrous ethanol and deionized water to obtain a silicon source solution; and mixing the aluminum source solution and the silicon source solution to obtain the aluminum silicate sol. The modified composite method comprises the following steps: heat-treating nano-aluminum titanate to obtain pretreated aluminum titanate; adding the pretreated aluminum titanate and deionized water into anhydrous ethanol, mixing them evenly, adjusting the pH to 8.5-9.5, heating the mixture to 48-52° C., dripping the ethyl orthosilicate solution while maintaining the temperature, and continuing to maintain the temperature and stirring after the dripping is complete; Separating and obtaining a solid, washing and drying the solid to obtain coated aluminum titanate; adding the coated aluminum titanate and nano zirconium oxide into an aluminum silicate sol, mixing them evenly, to obtain a modified composite sol; The vacuum impregnation method comprises pressing hollow alumina fibers into hollow fiber felts, and vacuum impregnating the hollow fiber felts with a modified composite sol containing an initiator to obtain an impregnated body; The impregnated body is subjected to gel aging and supercritical drying to obtain a hollow fiber reinforced aerogel composite material.

2. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 1, characterized in that: The aluminum source solution comprises aluminum chloride hexahydrate, anhydrous ethanol, and deionized water in a molar ratio of 3-3.1:15-17:55-60; The silicon source solution comprises ethyl orthosilicate, anhydrous ethanol, and deionized water in a molar ratio of 1-1.2:5-6:5-6; When the aluminum source solution and the silicon source solution are mixed, the molar ratio of aluminum chloride hexahydrate to tetraethyl orthosilicate is controlled to be 3-3.1:1-1.

2.

3. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 1, characterized in that: In the modified composite, the weight ratio of pretreated aluminum titanate to anhydrous ethanol is 1:70-75; The volume of deionized water added is 3.5-4% of the volume of anhydrous ethanol; The weight ratio of ethyl orthosilicate to nano-aluminum titanate in the ethyl orthosilicate solution is 0.18-0.21:1; The weight ratio of the coated aluminum titanate, nano zirconium oxide and aluminum silica sol is 4.8-5.5:3.4-4.2:

100.

4. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 1, characterized in that: In the modified composite, the ethyl orthosilicate solution is an ethanol solution of ethyl orthosilicate with a concentration of 2.5-2.8 wt%; The dripping rate of the ethyl orthosilicate solution was 0.4-0.5 mL / min; After the ethyl orthosilicate solution is added dropwise, the stirring time is continued to be 5-6 hours.

5. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 1, characterized in that: In the modified composite, the nano-aluminum titanate is subjected to heat treatment at 110-120° C. for 1-2 hours to obtain pretreated aluminum titanate; The particle size of the nano-aluminum titanate is 50-60 nm; The particle size of the nano zirconium oxide is 20-30 nm.

6. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 1, characterized in that: The vacuum impregnation method comprises the following steps: pressing hollow alumina fibers into hollow fiber felt, placing the hollow fiber felt together with the mold into a vacuum impregnation tank, and vacuum impregnating the hollow fiber felt with a modified composite sol containing an initiator for 30-40 minutes under vacuum environment and room temperature to obtain an impregnated body; The initiator is propylene oxide; the molar ratio of the initiator to the aluminum chloride hexahydrate used in the modified composite sol is 1:3-5.

7. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 1, characterized in that: The gel aging method comprises the following steps: placing the impregnated body in a 48-52° C. temperature environment, maintaining the gel, and then completely immersing the body in anhydrous ethanol, and allowing the body to stand for aging at a temperature of 48-52° C. to obtain a composite body.

8. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 7, characterized in that: During the gel aging process, the heat preservation gel time is 3-5 hours; The static aging time is 72-96h; During the static aging process, anhydrous ethanol was replaced every 10-12 hours.

9. The method for preparing the hollow fiber reinforced aerogel composite material according to claim 1, characterized in that: The supercritical drying method is as follows: after the impregnation body is subjected to gel aging to obtain a composite body, the supercritical drying temperature is controlled to be 270-280° C. and the pressure is 8-9 MPa, and the composite body is supercritically dried for 2-4 hours to obtain a hollow fiber reinforced aerogel composite material.

10. A hollow fiber reinforced aerogel composite material, characterized in that: The method is prepared according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of fiber-enhanced aluminum-silicon aerogel heat isolation material

    CN108863429A

  • Enhanced type transparent silicon dioxide aerogel and preparation method thereof

    CN109179428A

  • Preparation method of aluminum-silicon aerogel thermal insulation material

    CN110627475A

  • Infrared shielding coating modified fiber reinforced aerogel thermal insulation material and preparation method thereof

    CN110698101A

  • Dielectric composite film material of silica coated and modified barium titanate / polysulfone and preparation method of dielectric composite film material

    CN110698859A

Cited By

  • Co-woven three-dimensional interpenetrating network reinforced aerogel composite material as well as preparation method and application thereof

    CN121850590A