Preparation method and application of BiOBr-based composite material

By synthesizing TPP/BOB Z-type heterojunction composite material through a one-step solvothermal method, the problems of low visible light utilization and poor stability of Bi24O31Br10 photocatalyst were solved, and the effects of efficient photocatalytic degradation of tetracycline hydrochloride and inactivation of Staphylococcus aureus were achieved.

CN120961236APending Publication Date: 2025-11-18SOUTH CHINA NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511078946.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-02
Publication Date
2025-11-18

AI Technical Summary

Technical Problem

Bi24O31Br10 photocatalysts have limited visible light utilization, high photogenerated carrier recombination rate, poor stability, and are difficult to prepare on a large scale. Furthermore, there are no reports on the application of TPP and BOB heterojunction systems in the photocatalytic treatment of wastewater.

Method used

A one-step solvothermal method was used to synthesize TPP/Bi24O31Br10 (TPP/BOB) Z-type heterojunction composite material. Nanosheet-like TPP/BOB materials were prepared through a simple one-step reaction for photocatalytic degradation of tetracycline hydrochloride and inactivation of Staphylococcus aureus.

Benefits of technology

The material exhibits highly efficient photocatalytic performance, significantly improving photocatalytic reaction efficiency and application range, and demonstrating excellent sterilization activity and degradation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120961236A_ABST
    Figure CN120961236A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a BiOBr-based composite material, and the preparation method of the BiOBr-based composite material comprises the following steps: (1) adding a bromine-containing precursor solution into a bismuth-containing precursor solution to obtain a mixed solution, and dropwise adding ethanolamine into the mixed solution; and (2) adding TPP into the solution after the reaction in the step (1), carrying out ultrasonic dispersion, transferring into a hydrothermal reaction kettle after dispersion, carrying out hydrothermal reaction, and carrying out centrifugal separation after the reaction to obtain the BiOBr-based composite material. The TPP / BOBZ type heterojunction material prepared by the invention is a nanosheet, the synthesis steps are simple, the obtained material integrates the characteristics of a bismuth oxybromide-based material and a TPP material, and TPP / BOB shows excellent sterilization activity.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application relates to the field of photocatalytic materials, in particular to a preparation method of a BiOBr-based composite material and application thereof. BACKGROUND

[0002] Bi 24 O 31 Br 10 (BOB) is one of the new photocatalysts in the Bi x O y Br z family, and has unique layered structure, adjustable band gap, high thermal stability and biocompatibility, and the valence band position is suitable for application in the field of photocatalytic water treatment. However, the development and utilization of BOB still face challenges such as limited visible light utilization, high recombination rate of photo-generated carriers, poor stability and difficulty in large-scale preparation.

[0003] In order to improve the light response effect of a single material, different material modification methods are adopted in the prior art, wherein, constructing a heterojunction is an effective strategy for improving the photocatalytic performance of a semiconductor, and the method has multiple advantages such as promoting charge separation, broadening light absorption, improving catalytic activity, enhancing stability and optimizing energy band structure. By reasonably designing a heterojunction material, the efficiency and application range of photocatalytic reaction can be significantly improved, which provides a train of thought for the design and synthesis of BOB composite materials.

[0004] 5,10,15,20-tetraphenylporphyrin (TPP) is a classic porphyrin compound, and can act as a photosensitizer to improve the photocatalytic performance of a semiconductor in photocatalytic application due to its strong visible light absorption and excellent photoelectric performance. The introduction of TPP not only expands the spectral response range, promotes the generation of photo-generated electron-hole pairs, but also promotes the interface charge migration and separation, and inhibits the recombination of photo-generated carriers. At present, there is no report on the construction of a heterojunction system of TPP and BOB for photocatalytic treatment of wastewater. SUMMARY

[0005] In order to overcome the shortcomings of the prior art, the application provides a method for preparing a TPP / Bi 24 O 31 Br 10 (TPP / BOB) Z-type heterojunction composite material, which adopts a one-step solvothermal method strategy, and successfully synthesizes a nanosheet-shaped TPP / BOB material through a simple one-step reaction. The material has good photocatalytic performance, is suitable for being used as a photocatalyst for sewage, and can efficiently degrade tetracycline hydrochloride (TC) and inactivate Staphylococcus aureus (S.aureus).

[0006] The first aspect of the present application provides a preparation method of a BiOBr-based composite material, comprising the following steps:

[0007] (1) adding a bromine-containing precursor solution into a bismuth-containing precursor solution to obtain a mixed solution, and dropping ethanolamine into the mixed solution;

[0008] (2) adding TPP into the solution after the reaction of step (1), performing ultrasonic dispersion, transferring to a hydrothermal reaction kettle after the dispersion to perform a hydrothermal reaction, and obtaining the BiOBr-based composite material after centrifugal separation.

[0009] Preferably, the bromine-containing precursor solution comprises a KBr solution.

[0010] Preferably, the bismuth-containing precursor solution is prepared from Bi(NO3)3 and / or Bi(NO3)3·5H2O.

[0011] Preferably, the addition amount of the TPP is 0.5% to 3% of the mass of BOB generated by the reaction of the bromine-containing precursor solution and the bismuth-containing precursor solution, and the addition amount of the TPP is 0.5% to 3% of the mass of BOB generated in theory; further preferably, the addition amount of the TPP is 1% to 3% of the mass of BOB; in some specific preferred embodiments of the present application, the addition amount of the TPP is 2% of the mass of BOB.

[0012] Preferably, the ultrasonic dispersion time is 20 to 40 min.

[0013] Preferably, the temperature of the hydrothermal reaction is 120 to 220℃, and the time is 10 to 14 h.

[0014] The second aspect of the present application provides the BiOBr-based composite material prepared by the above preparation method.

[0015] The BiOBr-based composite material of the present application has an irregular nanosheet structure, and the irregular nanosheets are stacked with each other, and the nanosheet thickness is 20 to 30 nm.

[0016] The third aspect of the present application provides the application of the BiOBr-based composite material in photocatalytic degradation of tetracycline hydrochloride.

[0017] The fourth aspect of the present application provides the application of the BiOBr-based composite material in photocatalytic sterilization.

[0018] Preferably, the application of the BiOBr-based composite material in photocatalytic inactivation of Staphylococcus aureus.

[0019] Compared with the prior art, the present application has the following beneficial effects:

[0020] The TPP / BOBZ type heterojunction material prepared by the method has the characteristics of bismuth oxybromide-based material and TPP material, and the TPP / BOB shows excellent sterilization activity. BRIEF DESCRIPTION OF DRAWINGS

[0021] Figure 1 XRD patterns of TPP, BOB and TPP / BOB;

[0022] Figure 2 FTIR patterns of TPP, BOB and 2% TPP / BOB;

[0023] Figure 3 Raman patterns of TPP, BOB and 2% TPP / BOB;

[0024] Figure 4 SEM images of BOB and 2% TPP / BOB;

[0025] Figure 5 Full spectrum scanning patterns and high resolution patterns of Bi 4f, O 1s and Br 3d of BOB and 2% TPP / BOB;

[0026] Figure 6 UV-visible diffuse reflectance spectra of TPP, BOB and TPP / BOB;

[0027] Figure 7 Photoluminescence patterns of TPP, BOB and TPP / BOB;

[0028] Figure 8 Photocurrent response and electrochemical impedance of BOB and 2% TPP / BOB;

[0029] Figure 9 Photocatalytic degradation experiments of TPP, BOB and TPP / BOB on 10 mg / L TC;

[0030] Figure 10 Photocatalytic sterilization experiments of TPP, BOB and TPP / BOB on S.aureus;

[0031] Figure 11 Photocatalytic mechanism of TPP / BOB. DETAILED DESCRIPTION

[0032] The specific embodiments of the present application will be further described below. It should be noted that the description of these embodiments is used to help understand the present application, but does not constitute a limitation on the present application. In addition, the technical features involved in each embodiment of the present application described below can be combined with each other as long as they do not conflict with each other.

[0033] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods, and the experimental materials used in the following embodiments are all available through conventional commercial channels.

[0034] Example 1

[0035] This embodiment provides a method for preparing TPP / BOB Z-type heterojunction composite material, specifically including the following steps:

[0036] (1) First, weigh 0.97g Bi(NO3)3·5H2O and ultrasonically disperse it in 20mL ethylene glycol (EG). Stir for 30 minutes to ensure complete dissolution, and label this solution A. Weigh 0.6g KBr and dissolve it in 25mL deionized water. Stir for 30 minutes and label this solution B. Then, slowly add solution B dropwise to solution A to form a mixture. After stirring for 10 minutes, transfer 1.2mL of ethanolamine and slowly add it dropwise to the mixture. Continue stirring for 30 minutes.

[0037] (2) Next, a certain amount of TPP (3mg, 5mg, 11mg, 16mg) was weighed and ultrasonically dispersed in the mixture from step (1). After stirring for 30 minutes, the mixture was transferred to a 75mL hydrothermal reactor and placed in an oven at 160℃ for 12 hours. Finally, after the reactor was completely cooled, the product was collected by washing it several times with deionized water and anhydrous ethanol and then dried overnight in an oven at 60℃. The obtained samples were labeled as Z-type heterojunction composite materials of 0.5% TPP / BOB, 1% TPP / BOB, 2% TPP / BOB, and 3% TPP / BOB (theoretical mass ratio of TPP to BOB).

[0038] BOB was prepared according to the preparation method of TPP / BOB Z-type heterojunction composite material, wherein no TPP was added during the preparation of BOB, and the other steps were the same as those for the preparation of TPP / BOB Z-type heterojunction composite material.

[0039] The following tests were performed on the BOB and TPP / BOB Z-type heterojunction composite materials obtained above:

[0040] (1) Powder X-ray diffraction measurement

[0041] Figure 1 XRD spectra of TPP, BOB, and TPP / BOB, such as Figure 1 As stated above, the introduction of TPP via solvothermal induction does not alter the phase structure and crystallinity of BOB. With increasing theoretical TPP mass, no characteristic TPP diffraction peaks were observed in the XRD pattern of the TPP / BOB composite material. This may be due to the low TPP content and weak intensity of the characteristic diffraction peaks in the composite material.

[0042] (2) Infrared spectra

[0043] Figure 2 The infrared spectra of TPP, BOB and 2% TPP / BOB, the characteristic peaks of TPP and BOB in 2% TPP / BOB composite still appeared, the vibration peaks of TPP at 732 cm -1 and 800 cm -1 moved to 742 cm -1 and 800 cm -1 respectively, the vibration peak of BOB at 1470 cm -1 moved to 1475 cm -1 , which indicated that TPP and BOB were successfully composited.

[0044] (3) Raman spectra

[0045] Figure 3 The Raman spectra of TPP, BOB and 2% TPP / BOB, the peaks of TPP at 827 cm -1 , 1001 cm -1 can be attributed to the existence of pyrrole ring bending vibration, breathing vibration respectively, the peak at 1329 cm -1 can be attributed to the existence of semi-pyrrole stretching vibration, the peaks at 1075 cm -1 , 1240 cm -1 , 1457 cm -1 and 1556 cm -1 can be attributed to the existence of C-H in-plane bending vibration, C m -phenyl stretching vibration, aromatic ring skeleton vibration, C β -C β stretching vibration respectively. New Raman bands from TPP can be observed in 2% TPP / BOB composite, which indicated that TPP was successfully introduced into BOB.

[0046] (4) SEM images

[0047] Figure 4 The SEM images of BOB and 2% TPP / BOB, where Fig. a is the SEM image of BOB, Fig. b is the SEM image of 2% TPP / BOB, pure BOB was formed by large-scale irregular nanosheets stacked with each other, the thickness of nanosheet was about 20-30 nm. Compared with pure BOB, the SEM image of 2% TPP / BOB composite did not change significantly, which indicated that the introduction of TPP did not change the morphology of BOB.

[0048] (5) XPS analysis

[0049] Figure 5Full scan spectra and high resolution spectra of Bi 4f, O 1s, Br 3d for BOB and 2%TPP / BOB. Figure 5 (a) XPS full scan spectra of pure BOB and 2%TPP / BOB composite, both of which show characteristic peaks of Bi 4f, Br 3d and O 1s. In addition to the above characteristic peaks, the full scan spectrum of 2%TPP / BOB composite also shows a characteristic peak of C 1s. The C element in 2%TPP / BOB composite comes from the introduced TPP, which indicates that TPP and BOB are successfully composited. Figure 5 (b) High resolution spectra of Bi 4f, BOB shows two prominent peaks at the binding energy of 159.18 eV and 164.52 eV, which correspond to Bi 4f 7 / 2 and Bi 4f 5 / 2 characteristic peaks, respectively. In 2%TPP / BOB composite, Bi 4f 7 / 2 and Bi 4f 5 / 2 characteristic peaks are both shifted to the direction of higher binding energy, appearing at 159.35 eV and 164.67 eV, respectively. Figure 5 (c) High resolution spectra of O 1s, the characteristic peaks at the binding energy of 530.28 eV and 532.28 eV are attributed to lattice oxygen and external hydroxyl, respectively. Figure 5 (d) High resolution spectra of Br 3d, BOB shows Br 3d 5 / 2 and Br 3d 3 / 2 characteristic peaks at the binding energy of 68.58 eV and 69.63 eV, respectively. In 2%TPP / BOB composite, Br 3d 5 / 2 and Br 3d 3 / 2 characteristic peaks are both shifted to the direction of higher binding energy, appearing at 68.73 eV and 69.86 eV, respectively. The reason for this result may be that in 2%TPP / BOB composite, TPP and BOB are in close contact and electron transfer occurs. BOB transfers some electrons to TPP, resulting in a decrease in the electron density of BOB and an increase in the binding energy.

[0050] (6) UV-Vis diffuse reflectance spectra

[0051] Figure 6For the UV-Vis diffuse reflectance spectra of TPP, BOB and TPP / BOB, pure TPP shows a strong Soret band at ~341 nm and four weak Q absorption bands at ~501 nm, 552 nm, 594 nm and 649 nm, respectively. The light absorption edge of pure BOB is about 510 nm. The light absorption of TPP / BOB composite shows the combined characteristics of BOB and TPP, again confirming the successful introduction of TPP into BOB. The red shift of the characteristic Soret band, the significant expansion and enhancement of light absorption in the composite are conducive to generating more photo-generated carriers to participate in the photocatalytic reaction.

[0052] (7) Photoluminescence spectra

[0053] Figure 7 For the photoluminescence spectra of TPP, BOB and TPP / BOB, pure BOB shows a characteristic emission peak at 472 nm. Due to the rapid recombination of photo-generated electron-hole pairs, the characteristic emission peak of pure BOB has the highest intensity. Compared with pure BOB, the characteristic emission peak intensity of TPP / BOB composite is significantly reduced. This indicates that the introduction of TPP can enhance the charge transfer and reduce the recombination rate of photo-generated carriers, which is conducive to improving the photocatalytic performance of the material.

[0054] (8) Photocurrent response and electrochemical impedance

[0055] Figure 8 For the photocurrent response and electrochemical impedance of BOB and 2% TPP / BOB, as shown in Figure 8 (a), both BOB and 2% TPP / BOB composite can produce photocurrent response, and the composite shows higher photocurrent response intensity. The intensity of photocurrent response is positively correlated with the separation ability of photo-generated carriers, which indicates that 2% TPP / BOB composite shows higher separation efficiency of photo-generated electron-hole pairs than BOB. As shown in Figure 8 (b), 2% TPP / BOB composite shows smaller semicircle radius than BOB. The size of the semicircle radius is positively correlated with the impedance of charge transfer, which indicates that 2% TPP / BOB composite has lower charge transfer impedance. The i-t result is consistent with the EIS test result, further confirming that the introduction of TPP can effectively promote the interface charge migration and separation rate, which is conducive to improving the photocatalytic activity.

[0056] Example 2

[0057] To ensure that the reaction system maintains a constant temperature condition during the photocatalytic process, a multi-channel photocatalytic reaction system equipped with a circulating water constant temperature device was used. The specific experimental steps are as follows:

[0058] -1

[0059]

[0060]

[0061] Figure 9 For the photocatalytic degradation of 10 mg / L TC, the TPP / BOB composite material has higher photocatalytic degradation efficiency of TC, 0.5% TPP / BOB is 77.41%, 1% TPP / BOB is 80.10%, 2% TPP / BOB is 85.73%, and 3% TPP / BOB is 83.05%. Among them, the 2% TPP / BOB composite material shows the best degradation performance.

[0062] Example 3

[0063] The material prepared in Example 1 was subjected to photocatalytic sterilization experiment, and Staphylococcus aureus (S. aureus) was selected as a representative of gram-positive bacteria as a research model for photocatalytic sterilization experiment to test the photocatalytic sterilization performance of the sample. The specific experimental process is as follows:

[0064] 8 -1 The reaction system was first dark reacted under light shielding conditions for 60 minutes, then the light source was turned on to simulate sunlight, and every 30 minutes 100 μL of bacterial solution was taken out for gradient dilution, and the bacterial solution was evenly coated on the nutrient agar plate with a disposable plastic coating rod. After sealing with a sealing film, it was placed in a shaking bed at 37.5°C for 20 hours.

[0065]

[0066] ​​​​​​​Figure 10 For the photocatalytic sterilization experiment of TPP, BOB and TPP / BOB on S. aureus, after 1 hour of dark reaction, TPP, BOB and TPP / BOB composite materials all did not show obvious sterilization effect, indicating that they had no significant toxicity effect on bacterial growth. After 3 hours of light irradiation, TPP and BOB made the bacterial concentration decrease by 1.60lg and 0.88lg respectively, which indicated that both of them had certain photocatalytic sterilization performance. TPP / BOB composite material had more excellent photocatalytic sterilization performance, 0.5% TPP / BOB, 1% TPP / BOB, 2% TPP / BOB and 3% TPP / BOB made the bacterial concentration decrease by 2.69lg cfu mL -1 , 3.62lg cfu mL -1 , 5.14lg cfu mL -1 , 4.49lg cfu mL -1 respectively. Among them, 2% TPP / BOB composite material showed the most excellent sterilization effect.

[0067] The photocatalytic mechanism of TPP / BOB is as Figure 11 , the band gap of TPP and BOB is 1.73eV and 2.25eV respectively, and both of them can be excited to produce photo-generated electrons and holes under visible light irradiation. The E CB and E VB of TPP are-0.41V and 1.32V respectively, and the valence band potential is more negative than the redox potential of OH - / ·OH (1.99V vs.NHE), which cannot oxidize OH - to generate ·OH. The E CB and E VB of BOB are-0.17V and 2.08V respectively, and the conduction band potential is more positive than the redox potential of O2 / ·O2 - (-0.33V vs.NHE), which cannot reduce O2 to generate ·O2 - . Based on the above research results, the charge transfer behavior of TPP / BOB heterojunction photocatalyst in the process of photocatalytic degradation and sterilization is Z-type mechanism.

[0068] As can be seen from the above, the TPP / BOB Z-type heterojunction composite material of the application has a nanosheet structure and exhibits excellent photocatalytic efficiency.

[0069] The above detailed description of the embodiments of the application, but the application is not limited to the described embodiments. For those skilled in the art, various changes, modifications, replacements and variations of these embodiments without departing from the principles and spirit of the application, still fall within the scope of the application.

Claims

1. A method for preparing a BiOBr-based composite material, characterized in that, Includes the following steps: (1) Add the bromine-containing precursor solution to the bismuth-containing precursor solution to obtain a mixture, and add ethanolamine dropwise to the mixture; (2) TPP is added to the solution after the reaction in step (1) and ultrasonically dispersed. After dispersion, it is transferred to a hydrothermal reactor for hydrothermal reaction. After the reaction, the BiOBr-based composite material is obtained by centrifugation.

2. The method for preparing the BiOBr-based composite material according to claim 1, characterized in that, The bromine-containing precursor solution includes a KBr solution.

3. The method for preparing the BiOBr-based composite material according to claim 1, characterized in that, The bismuth-containing precursor solution is prepared from Bi(NO3)3 and / or Bi(NO3)3·5H2O.

4. The method for preparing the BiOBr-based composite material according to claim 1, characterized in that, The amount of TPP added is 0.5% to 3% of the mass of BOB generated by the reaction of the bromine-containing precursor solution and the bismuth-containing precursor solution.

5. The method for preparing the BiOBr-based composite material according to claim 1, characterized in that, The ultrasonic dispersion time is 20–40 min.

6. The method for preparing the BiOBr-based composite material according to claim 1, characterized in that, The hydrothermal reaction is carried out at a temperature of 120–220°C for 10–14 hours.

7. The BiOBr-based composite material prepared by the preparation method according to claims 1 to 6.

8. The application of the BiOBr-based composite material according to claim 7 in the photocatalytic degradation of tetracycline hydrochloride.

9. The application of the BiOBr-based composite material according to claim 7 in photocatalytic sterilization.

10. The application according to claim 9, characterized in that, Application of the BiOBr-based composite material in photocatalytic inactivation of Staphylococcus aureus.