Dynamic separation method and device for mixed iron powder
By employing a three-stage dynamic synergistic separation method of "weak magnetic pre-separation - electric field fixation - strong magnetic field clearing" combined with low-frequency micro-vibration, the problems of cross-contamination and particle adhesion in the separation of strong and weak magnetic iron powders are solved, achieving efficient and pollution-free industrial separation.
Patent Information
- Application Number
- CN202511619086.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-06
- Publication Date
- 2025-12-02
AI Technical Summary
Existing technologies suffer from severe cross-contamination, insufficient separation efficiency and precision when separating strong and weak magnetic iron powders, and traditional methods cannot effectively break up particle agglomeration, thus failing to meet the needs of high-end applications.
A three-stage dynamic collaborative separation paradigm of "weak magnetic pre-separation - electric field fixation - strong magnetic field clearing" is adopted, combined with low-frequency micro-vibration controlled by quantification, to achieve efficient separation of mixed iron powder without secondary pollution.
It achieves efficient (efficiency ≥ 95.2%) and high-purity (purity ≥ 95%) separation of mixed iron powder, suitable for industrial applications, and avoids secondary pollution.
Smart Images

Figure CN121042159A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of powder material separation technology, and in particular to a dynamic separation method and apparatus for mixed iron powder. Background Technology
[0002] The efficient separation of powder materials is a key process in metallurgy, resource recycling, and precision manufacturing. Mixed iron powders, especially systems containing strongly magnetic iron powder (such as magnetite (Fe3O4)) and weakly magnetic iron powder (such as ferric oxide (Fe2O3)), are widely found in waste lithium-ion battery cathode materials, electronic waste dismantling powders, and residues from magnetic component processing. Achieving precise and efficient separation of these materials is crucial for improving resource recovery rates, ensuring product quality, and reducing environmental impact.
[0003] Currently, the separation of magnetic powders mainly relies on magnetic separation technology. Traditional single-magnetic-field separation methods are simple and widely used, but their separation mechanism is crude and has inherent drawbacks when dealing with complex systems where strong and weak magnetic particles coexist. Under the influence of a magnetic field, strong magnetic particles rapidly magnetize and form magnetic chains or clusters. These clusters mechanically entrain and encapsulate a large number of weakly magnetic or non-magnetic particles during their movement, leading to severe cross-contamination of the separated products and making it difficult to meet the purity requirements of high-end applications. To overcome the limitations of a single magnetic field, magnetoelectric composite field separation technology has emerged. This technology introduces an electric field and utilizes dielectric force to sort particles with different dielectric properties, improving the separation effect to some extent. However, existing magnetoelectric composite field technologies mostly use static, fixed field strength parameters, lacking dynamic and precise control of the separation process, and are essentially "crude" dual-field superposition. This mode cannot effectively resolve the core contradiction of "strong magnetic powder interfering with the separation of weak magnetic powder" and "weak magnetic powder being entrained," and the separation efficiency and accuracy quickly reach a bottleneck.
[0004] Besides the limitations of field force separation itself, the microscopic interactions between particles, especially the particle adhesion and agglomeration caused by van der Waals forces, are key factors that have long been overlooked but seriously affect separation efficiency. In dry separation processes, micron-sized powders have large specific surface areas and high surface energy, making them prone to adhesion. This not only reduces the number of effectively separated particles but also forms stable "pseudo-agglomerates," which behave like large composite particles, seriously misleading and interfering with the separation process based on the physical properties of individual particles, causing a sharp decline in separation efficiency. While existing technologies have attempted to use vibration to alleviate agglomeration, high-frequency vibration is commonly used. High-frequency vibration has excessive energy; while breaking up existing agglomerates, it can also cause particles to collide randomly due to excessive kinetic energy, inducing secondary agglomeration and even remixing already separated particles, resulting in unsatisfactory results.
[0005] Furthermore, under environmental and cost pressures, wet sorting faces problems such as wastewater treatment, high energy consumption for product drying, and potential secondary pollution due to the need for liquid media, limiting its application in precision manufacturing fields with extremely high requirements for dryness. Existing dry precision sorting technologies, such as electromagnetic electrophoresis microchip technology, while offering acceptable accuracy, have extremely small processing capacities, making them suitable only for laboratory-level micro-sample analysis and unable to meet the needs of industrial-scale batch processing.
[0006] Therefore, there is an urgent need in this field to develop a new dry separation method and device that can dynamically control the separation field force, actively and gently break up particle adhesion, and is suitable for industrial-scale production, so as to achieve efficient and high-purity separation of mixed iron powder. Summary of the Invention
[0007] The purpose of this invention is to overcome the aforementioned shortcomings of existing technologies and provide a dynamic separation method and apparatus for mixed iron powder. Its core objective is to resolve the fundamental contradictions in traditional single magnetic field or static magnetoelectric composite field separation, namely, the interference of strong magnetic powder with weak magnetic powder separation and the entrainment of weak magnetic powder, while effectively eliminating particle adhesion and agglomeration problems. By establishing a three-stage dynamic synergistic separation paradigm of "weak magnetic pre-separation - electric field fixation - strong magnetic field clearing," and integrating quantitatively controlled low-frequency micro-vibration, it achieves highly efficient (efficiency ≥95.2%) and high-purity (purity ≥95%) separation of 50-100μm mixed iron powder (such as Fe3O4 / Fe2O3) under dry, pollution-free conditions, meeting the industrial application needs of waste lithium battery recycling, electronic waste treatment, and precision manufacturing.
[0008] To achieve the above-mentioned objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides a method for dynamic separation of mixed iron powder, the method comprising the following steps performed in sequence: Step S1, Initialization and Vibration Fluidization: Spread the mixed iron powder of Fe3O4 and Fe2O3 on the substrate surface, and start the micro-vibration motor to vibrate and fluidize the particle bed at a frequency of 5-10Hz and an amplitude of no more than 15μm to actively break the agglomeration between particles. Step S2, weak magnetic field gradient pre-separation: Start the permanent magnet slide and apply a weak magnetic field gradient of 0.14T to make the strongly magnetic Fe3O4 particles migrate directionally to the right side of the substrate under the synergistic effect of magnetic force and micro-vibration. Step S3, precise adsorption and fixation by electric field: Start the long strip electrode and apply a DC electric field of 5-15kV / m so that the weakly magnetic Fe2O3 particles are precisely adsorbed and fixed to the electrode surface under the action of dielectric force, while maintaining the weak magnetic field gradient. Step S4, strong magnetic field directional clearing: the magnetic field gradient of the permanent magnet slide is increased to 0.16T to accelerate and completely push the Fe3O4 particles remaining on the substrate surface into the Fe3O4 collection box; Step S5, substrate transfer and final collection of Fe2O3: Drive the substrate to move backward and move it away from the area directly below the electrode. Then cut off the electric field and let the Fe2O3 particles fall vertically into the Fe2O3 collection box under the action of gravity.
[0009] Furthermore, the micro-vibration described in step S1, wherein the micro-vibration force Fᵥ is in equilibrium with the particle adhesion energy, wherein Fᵥ... v =m p ·ω 2 ·A,m p Where ω is the particle mass, A is the angular frequency, and A is the amplitude; this micro-vibration reduces the particle adhesion rate from 28.6% to below 10.8%.
[0010] Furthermore, steps S2, S3, and S4 constitute a three-stage magnetoelectric field coordinated separation paradigm of "weak magnetic pre-separation - electric field fixation - strong magnetic field clearing".
[0011] Secondly, the present invention provides a dynamic separation apparatus for implementing the above-described method, comprising: The core support and agglomeration breaking system includes a horizontally arranged substrate, a guide rail mechanism that drives the substrate to translate in the front-back direction, and a micro-vibration motor embedded in the center directly below the substrate. Field generation and control system, including: The magnetic field generating unit consists of a permanent magnet slide located directly below the right side of the substrate and capable of moving along a left-right track; The electric field generating unit consists of two sets of elongated electrodes suspended above the substrate by a U-shaped bracket and arranged opposite each other on the left and right. Material collection system, including: A Fe3O4 collection box is disposed on the outer side of the short right side of the substrate; Two Fe2O3 collection boxes are arranged side by side at the rear of the device and located directly below the elongated electrode.
[0012] Furthermore, the length direction of the elongated electrode is parallel to the long side direction of the substrate, and its length covers more than 90% of the long side of the substrate; and the center distance between two elongated electrodes is greater than the short side length of the substrate.
[0013] Furthermore, the elongated electrode is fixed to the U-shaped bracket by an electrode rod, and the electrode rod is provided with a scale adjustment mechanism and an insulating locking sleeve for precisely adjusting the 2-3mm vertical gap between the elongated electrode and the substrate surface; the middle of the elongated electrode is also fitted with an annular acrylic stabilizing plate connected to the device column by a thin insulating rod.
[0014] Furthermore, the left-right track of the permanent magnet slide table and the front-back translation guide rail of the substrate are orthogonally arranged in space; the end of the track of the permanent magnet slide table and the end of the translation guide rail are provided with limit blocks or positioning sensors.
[0015] Furthermore, the vertical distance between the opening of the Fe2O3 collection box and the elongated electrode located above it is 5 cm.
[0016] Furthermore, it also includes an integrated monitoring and control system, which includes a high-speed camera with its lens axis set at a 45° downward angle to the substrate surface, and a data parameter display panel for real-time display and setting of vibration frequency, magnetic field gradient, electric field strength and substrate position parameters.
[0017] Compared with the prior art, the present invention has the following advantages and beneficial effects: The separation mechanism is highly innovative: a new three-stage dynamic synergistic paradigm of "pre-separation-fixation-cleaning" is proposed. Through precise and dynamic matching of magnetic field strength (0.14T→0.16T) and electric field strength (5-15kV / m), the problem of mutual interference between strong and weak magnetic particles in the separation process is fundamentally solved, with a separation efficiency of over 95.2% and a purity of ≥95% for strong magnetic powder.
[0018] Significant active anti-adhesion effect: For the first time, quantitatively controlled low-frequency micro-vibration (5-10Hz) is systematically integrated into the dry magnetoelectric separation process. Based on the principle of stick-slip vibration, it gently and effectively breaks up agglomeration, significantly reducing the particle adhesion rate from 28.6% to 10.8%, while shortening the separation time by 20% and avoiding secondary agglomeration.
[0019] With its green and environmentally friendly design and significant industrialization potential, the entire process is a dry physical separation, requiring no water or chemical reagents, resulting in no secondary pollution and low energy consumption. The equipment is less complex than traditional wet processes, and its processing capacity far exceeds that of laboratory technologies such as microfluidic chips, making it highly suitable for industrial application in fields such as waste lithium battery recycling and electronic waste treatment.
[0020] High technical versatility: This method and device are not only applicable to Fe3O4 / Fe2O3 mixed powders in a specific ratio, but also, based on the dynamic separation concept of differences in physical properties, can be extended to the separation of other strong / weak magnetic powder mixtures, showing broad application prospects. Attached Figure Description
[0021] Figure 1 This is a schematic flowchart of the method of the present invention; Figure 2 This is a schematic diagram of the device structure from one perspective of the present invention; Figure 3 This is a schematic diagram of the device of the present invention from another perspective.
[0022] Component names and reference numerals: 1-Substrate, 2-Micro vibration motor, 3-Permanent magnet slide, 4-U-shaped bracket, 5-Long strip electrode, 6-Fe3O4 collection box, 7-Fe2O3 collection box, 8-High-speed camera, 9-Display panel. Detailed Implementation
[0023] The present invention will be further described in detail below with reference to experimental examples and specific embodiments. However, this should not be construed as limiting the scope of the above-mentioned subject matter of the present invention to the following embodiments; all technologies implemented based on the content of the present invention fall within the scope of the present invention.
[0024] Example 1: This embodiment provides a dynamic separation method for mixed iron powder, such as... Figure 1 As shown, the method includes the following steps performed in sequence: Step S1, Initialization and Vibration Fluidization: Spread the mixed iron powder of Fe3O4 and Fe2O3 on the substrate surface, and start the micro-vibration motor to vibrate and fluidize the particle bed at a frequency of 5-10Hz and an amplitude of no more than 15μm to actively break the agglomeration between particles. Step S2, weak magnetic field gradient pre-separation: Start the permanent magnet slide and apply a weak magnetic field gradient of 0.14T to make the strongly magnetic Fe3O4 particles migrate directionally to the right side of the substrate under the synergistic effect of magnetic force and micro-vibration. Step S3, precise adsorption and fixation by electric field: Start the long strip electrode and apply a DC electric field of 5-15kV / m so that the weakly magnetic Fe2O3 particles are precisely adsorbed and fixed to the electrode surface under the action of dielectric force, while maintaining the weak magnetic field gradient. Step S4, strong magnetic field directional clearing: the magnetic field gradient of the permanent magnet slide is increased to 0.16T to accelerate and completely push the Fe3O4 particles remaining on the substrate surface into the Fe3O4 collection box; Step S5, substrate transfer and final collection of Fe2O3: Drive the substrate to move backward and move it away from the area directly below the electrode. Then cut off the electric field and let the Fe2O3 particles fall vertically into the Fe2O3 collection box under the action of gravity.
[0025] Initialization and Vibratory Fluidization: 5 grams of mixed iron powder consisting of 50% Fe3O4 (average particle size 80 μm) and 50% Fe2O3 (average particle size 75 μm) was weighed and evenly spread on the surface of an alumina ceramic substrate with dimensions of 15 cm × 10 cm, forming a thin layer with a thickness of approximately 0.1 mm. The micro-vibration motor under the substrate was started, and the vibration frequency was set to 8 Hz and the amplitude to 10 μm. Vibration was continued for 30 seconds, and it was observed that the particle bed became significantly looser, with no obvious agglomerates.
[0026] Weak magnetic field gradient pre-separation: Maintaining micro-vibration. The permanent magnet slide located at the lower right of the substrate is activated to generate and maintain a weak magnetic field with a gradient of 0.14T. It can be observed that the black Fe3O4 particles begin to slowly but continuously move to the right side of the substrate, while the reddish-brown Fe2O3 particles remain largely in place. After this process lasts for 20 seconds, the substrate exhibits an initial partitioning of "blacker on the right and redder on the left."
[0027] Precise adsorption and fixation using an electric field: Maintaining micro-vibration and a weak magnetic field. The left and right elongated electrodes suspended above the substrate are activated, and a DC electric field of 10 kV / m is applied. Immediately, the reddish-brown Fe2O3 particles on both sides of the substrate are observed to jump off the substrate surface and be adsorbed onto the corresponding elongated electrode surfaces. After approximately 15 seconds, the Fe2O3 particles on the substrate surface essentially disappear, having all transferred to the electrode surfaces.
[0028] Strong magnetic field directional cleaning: Maintain micro-vibration and electric field. Increase the magnetic field gradient of the permanent magnet slide to 0.16T. It was observed that the remaining black Fe3O4 particles on the right side of the substrate moved at a significantly faster speed, and were all pushed into the Fe3O4 collection box on the right side within 10 seconds. At this time, there were no particles remaining on the substrate surface.
[0029] Substrate Transfer and Final Fe2O3 Collection: Stop the micro-vibration. Control the substrate to move backward 8 cm along the guide rail, completely removing it from the area directly below the electrode. Then, disconnect the electrode power supply. The Fe2O3 particles adsorbed on the electrode surface, losing their electric field attraction, fall vertically into the two Fe2O3 collection boxes directly below within 3 seconds under the influence of gravity. The entire separation process is complete.
[0030] Example 2: The micro-vibration described in step S1 achieves equilibrium between the micro-vibration force Fᵥ and the particle adhesion energy, wherein Fᵥ... v =m p ·ω 2 ·A,m p Where ω is the particle mass, A is the angular frequency, and A is the amplitude; this micro-vibration reduces the particle adhesion rate from 28.6% to below 10.8%.
[0031] In step S1, for the same mixed iron powder, without micro-vibration, the initial particle adhesion rate was calculated to be 29.1% using image analysis software. Subsequently, micro-vibration was activated (frequency 8 Hz, amplitude 12 μm), and after 30 seconds of vibration, the adhesion rate was calculated again, decreasing to 9.5%. According to formula F... v =m p ·ω 2 ·A, where the mass of a single particle is m p Approximately 1.2 × 10 -9 kg, angular frequency ω = 2π × 8 ≈ 50.24 rad / s, the calculated micro-vibration force Fᵥ is approximately 3.6 × 10⁻⁶. -8 N. This force is sufficient to overcome the adhesion energy such as van der Waals forces between particles, thereby achieving effective de-agglomeration.
[0032] Example 3: Steps S2, S3, and S4 constitute a three-stage magnetoelectric field coordinated separation paradigm of "weak magnetic pre-separation - electric field fixation - strong magnetic field clearing".
[0033] Using the same materials and apparatus as in Example 1, but changing the timing of field application as a comparative example. Comparative Example 1: Applying only a weak magnetic field of 0.14T resulted in a final Fe2O3 recovery rate of only 68%, as Fe2O3 was encapsulated by Fe3O4. Comparative Example 2: Applying both a 0.14T magnetic field and a 10kV / m electric field simultaneously resulted in a final separation efficiency of 85%, weaker than the 95.2% of Example 1. This demonstrates the synergistic advantage of the specific timing paradigm of "weak magnetic pre-separation - electric field fixation - strong magnetic field clearing".
[0034] Example 4: like Figures 2-3 As shown, this embodiment provides a dynamic separation device for implementing the above method, comprising: The core support and agglomeration breaking system includes a horizontally arranged substrate 1, a guide rail mechanism that drives the substrate 1 to translate in the front-back direction, and a micro-vibration motor 2 embedded in the center directly below the substrate. Field generation and control system, including: The magnetic field generating unit consists of a permanent magnet slide 3 located on the right side directly below the substrate 1 and capable of moving along a left-right track. The electric field generating unit consists of two sets of elongated electrodes 5 suspended above the substrate 1 by a U-shaped bracket 4 and arranged opposite each other on the left and right. Material collection system, including: A Fe3O4 collection box 6 is disposed on the outer side of the short side on the right side of the substrate 1; Two Fe2O3 collection boxes 7 are arranged side by side at the rear end of the device and located directly below the elongated electrode 5.
[0035] Construct a separation device as shown in the attached diagram. The core support system includes a 15cm × 10cm × 0.5cm alumina ceramic substrate, the bottom of which is connected to two PTFE-coated forward and backward translational guide rails via a slider. A micro-vibration motor 2 (model VIB-8, 3cm diameter) is embedded in the center directly below the substrate 1. The magnetic field generating system is a permanent magnet slide 3 (8cm × 3cm × 2cm) with an embedded N52 neodymium iron boron magnet, placed on the left-right track below the substrate 1. The electric field generating system consists of two 12cm long and 1cm wide nickel-plated copper electrodes, suspended by a U-shaped aluminum alloy bracket. The material collection system includes a Fe3O4 collection box (6cm × 4cm × 3cm) located on the right side of the substrate and two Fe2O3 collection boxes (5cm × 12cm × 3cm) located at the rear of the device.
[0036] Example 5: The length direction of the elongated electrode 5 is parallel to the long side direction of the substrate 1, and its length covers more than 90% of the long side of the substrate 1; and the center distance between two elongated electrodes is greater than the short side length of the substrate 1.
[0037] In the device of Example 4, the short side width of substrate 1 is 10 cm. After the two elongated electrodes are installed, the distance between their inner surfaces is precisely calibrated to 12 cm. This distance ensures that the elongated electrodes completely cover the long side area of the substrate (100% coverage), and their center distance (13 cm) is greater than the width of the substrate, providing a safe space for substrate vibration and translation, and ensuring the uniformity of the electric field.
[0038] Example 6: The elongated electrode 5 is fixed to the U-shaped bracket 4 by an electrode rod. The electrode rod is provided with a scale adjustment mechanism and an insulating locking sleeve for precisely adjusting the 2-3mm vertical gap between the elongated electrode and the substrate surface. The middle part of the elongated electrode is also fitted with an annular acrylic stabilizing plate connected to the device column by a thin insulating rod.
[0039] During the device installation process in Example 4, the gap between the elongated electrode and the substrate surface was precisely adjusted to 2.5 mm by rotating the graduated fine-tuning knob on the electrode rod, and then locked with a light gray plastic locking sleeve. Subsequently, an annular acrylic stabilizing plate was installed and secured to the side column with a thin insulating rod. When the micro-vibration motor was operating, it was observed that this secondary stabilizing structure effectively suppressed the slight wobbling of the elongated electrode, and the gap remained stable.
[0040] Example 7: The left-right track of the permanent magnet slide table 3 and the front-back translation guide rail of the substrate 1 are orthogonally arranged in space; the end of the track of the permanent magnet slide table 3 and the end of the translation guide rail are provided with limit blocks or positioning sensors.
[0041] In the device of Embodiment 4, the left-right track of the permanent magnet slide 3 and the front-back translational guide rail of the substrate 1 intersect perpendicularly in space, but without physical contact. M8 limit blocks are installed at the ends of both guide rails, while infrared positioning sensors are installed at the ends of the permanent magnet slide 3 tracks. When the substrate or slide reaches its endpoint, the limit blocks provide a mechanical hard stop, and the sensors send electrical signals to the control system to ensure accurate positioning.
[0042] Example 8: The vertical distance between the opening of the Fe2O3 collection box 7 and the elongated electrode located above it is 5 cm.
[0043] During device assembly, a height gauge is used to measure and adjust the mounting bracket of the rear Fe2O3 collection box 7 to ensure that the vertical distance between the box opening plane and the lower surface of the upper elongated electrode is precisely 5.0 cm (±0.1 cm). This distance ensures that the Fe2O3 particles desorbed from the elongated electrode have sufficient space to accelerate and fall into the box with an approximately vertical trajectory, avoiding particle bounce or splashing caused by too close a distance.
[0044] Example 9: It also includes an integrated monitoring and control system, which includes a high-speed camera 8 with its lens axis set at a 45° downward angle to the substrate surface, and a data parameter display panel 9 for real-time display and setting of vibration frequency, magnetic field gradient, electric field strength and substrate position parameters.
[0045] A Phantom high-speed camera 8 is mounted on the upper left of the device, with its lens axis adjusted to a 45° downward angle with the substrate surface, and the preset shooting frame rate set to 240fps. A touch-screen data parameter display panel 9 is placed on the upper right corner of the front of the device. During the experiment, the panel displays in real time "Vibration frequency: 8Hz | Magnetic field gradient: 0.14T | Electric field strength: 10kV / m | Substrate position: Front". The particle motion images recorded by the high-speed camera 8 can be displayed in real time in a small window and used for subsequent comparison and analysis with simulation results.
[0046] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for dynamic separation of mixed iron powder, characterized in that, The method includes the following steps performed in sequence: Step S1, Initialization and Vibration Fluidization: Spread the mixed iron powder of Fe3O4 and Fe2O3 on the substrate surface, and start the micro-vibration motor to vibrate and fluidize the particle bed at a frequency of 5-10Hz and an amplitude of no more than 15μm to actively break the agglomeration between particles. Step S2, weak magnetic field gradient pre-separation: Start the permanent magnet slide and apply a weak magnetic field gradient of 0.14T to make the strongly magnetic Fe3O4 particles migrate directionally to the right side of the substrate under the synergistic effect of magnetic force and micro-vibration. Step S3, precise adsorption and fixation by electric field: Start the long strip electrode and apply a DC electric field of 5-15kV / m so that the weakly magnetic Fe2O3 particles are precisely adsorbed and fixed to the electrode surface under the action of dielectric force, while maintaining the weak magnetic field gradient. Step S4, strong magnetic field directional clearing: the magnetic field gradient of the permanent magnet slide is increased to 0.16T to accelerate and completely push the Fe3O4 particles remaining on the substrate surface into the Fe3O4 collection box; Step S5, substrate transfer and final collection of Fe2O3: Drive the substrate to move backward and move it away from the area directly below the electrode. Then cut off the electric field and let the Fe2O3 particles fall vertically into the Fe2O3 collection box under the action of gravity.
2. The method according to claim 1, characterized in that, The micro-vibration described in step S1 achieves equilibrium between the micro-vibration force Fᵥ and the particle adhesion energy, wherein Fᵥ... v =m p ·ω 2 ·A,m p Where ω is the particle mass, A is the angular frequency, and A is the amplitude; this micro-vibration reduces the particle adhesion rate from 28.6% to below 10.8%.
3. The method according to claim 1, characterized in that, Steps S2, S3, and S4 constitute a three-stage magnetoelectric field coordinated separation paradigm of "weak magnetic pre-separation - electric field fixation - strong magnetic field clearing".
4. A dynamic separation device for implementing the method of any one of claims 1-3, characterized in that, include: The core support and agglomeration breaking system includes a horizontally arranged substrate, a guide rail mechanism that drives the substrate to translate in the front-back direction, and a micro-vibration motor installed at the center directly below the substrate. Field generation and control system, including: The magnetic field generating unit consists of a permanent magnet slide located directly below the right side of the substrate and capable of moving along a left-right track; The electric field generating unit consists of two sets of elongated electrodes suspended above the substrate by a U-shaped bracket and arranged opposite each other on the left and right. Material collection system, including: A Fe3O4 collection box is disposed on the outer side of the short right side of the substrate; Two Fe2O3 collection boxes are arranged side by side at the rear of the device and located directly below the elongated electrode.
5. The apparatus according to claim 4, characterized in that, The length direction of the elongated electrode is parallel to the long side direction of the substrate, and its length covers more than 90% of the long side of the substrate; and the center distance between two elongated electrodes is greater than the short side length of the substrate.
6. The apparatus according to claim 4, characterized in that, The elongated electrode is fixed to the U-shaped bracket by an electrode rod. The electrode rod is equipped with a scale adjustment mechanism and an insulating locking sleeve for precisely adjusting the 2-3mm vertical gap between the elongated electrode and the substrate surface. The middle part of the elongated electrode is also fitted with an annular acrylic stabilizing plate connected to the device column by a thin insulating rod.
7. The apparatus according to claim 4, characterized in that, The left-right track of the permanent magnet slide table and the front-back translation guide rail of the substrate are orthogonally arranged in space; the end of the track of the permanent magnet slide table and the end of the translation guide rail are provided with limit blocks or positioning sensors.
8. The apparatus according to claim 4, characterized in that, The vertical distance between the opening of the Fe2O3 collection box and the elongated electrode located above it is 5 cm.
9. The apparatus according to any one of claims 4 to 8, characterized in that, It also includes an integrated monitoring and control system, which includes a high-speed camera with its lens axis set at a 45° downward angle to the substrate surface, and a data parameter display panel for real-time display and setting of vibration frequency, magnetic field gradient, electric field strength and substrate position parameters.