Alkaline desulfurization and cyanidation gold leaching agent system for sulphide ore and gold extraction method thereof
By using a ternary reagent system of potassium ferricyanide, low-concentration sodium cyanide, and thioguanine nucleoside, the obstacle of sulfide minerals to gold extraction has been overcome, achieving efficient and environmentally friendly desulfurization of sulfide minerals and gold extraction, reducing costs and environmental risks.
Patent Information
- Application Number
- CN202511613278.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-06
- Publication Date
- 2025-12-05
- Estimated Expiration
- 2045-11-06
AI Technical Summary
Existing technologies are difficult to process gold ores containing sulfide minerals efficiently and in an environmentally friendly manner. Sulfides have a negative impact on the cyanide gold extraction process, resulting in low leaching rates and high costs. Conventional pretreatment methods have problems such as environmental pollution or high equipment costs.
A ternary reagent system consisting of potassium ferricyanide, low-concentration sodium cyanide, and thioguanine nucleoside is used to selectively oxidize sulfides through synergistic effects, forming an efficient chemical cycle to achieve desulfurization of sulfide minerals and efficient extraction of gold.
It achieves high gold recovery rates in refractory sulfide ores, reduces reagent costs, minimizes environmental pollution, realizes efficient sulfide desulfurization and gold extraction, forms an efficient chemical cycle, and reduces equipment investment and operating costs.
Smart Images

Figure CN121065499A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of hydrometallurgy, and particularly relates to a sulfide ore alkaline desulfurization cyanide leaching gold reagent system for sulfur-containing gold ore (especially pyrite, arsenopyrite and other sulfide ores) and a method for extracting gold. BACKGROUND
[0002] In the gold extraction industry, for conventional oxidized ores, direct cyanide leaching is a mature and efficient process. However, for ores containing a large amount of sulfide minerals (such as pyrite FeS2, pyrrhotite Fe (1-x) S, etc.), their treatment has always been a technical problem. The sulfur component in such ores has a serious negative impact on the cyanide gold leaching process: first, sulfides consume a large amount of cyanide and oxygen to generate thiocyanate (SCN - ), greatly increasing the reagent cost; second, gold particles are often tightly wrapped in the form of "encapsulated gold" or "solid solution" by sulfide minerals, hindering the contact between cyanide solution and gold, resulting in extremely low direct leaching rate; third, after the oxidation of sulfides, a dense passivation film (such as sulfur film S 0 ) is formed on the surface of gold particles, further hindering the dissolution of gold.
[0003] To solve the above problems, the industry usually adopts pretreatment processes such as oxidative roasting, biological oxidation, and pressure oxidation to destroy the structure of sulfide minerals and expose the encapsulated gold. However, these methods have the following disadvantages: oxidative roasting produces harmful gases such as SO2, causing serious environmental pollution; biological oxidation has a long cycle and low efficiency; pressure oxidation has high requirements for equipment materials, and the investment and operating costs are huge. Therefore, it has great industrial value to develop a mild, efficient, and environmentally friendly chemical desulfurization pretreatment and leaching integrated technology.
[0004] Chemical oxidation desulfurization in an alkaline environment is a promising alternative. Sodium cyanide (NaCN) itself has a certain oxidative dissolution effect on sulfide ores under alkaline conditions, but its reaction rate is slow, the oxidation of sulfur is not complete, and a passivation layer of elemental sulfur is easily formed on the surface of the mineral, and the use of high-concentration cyanide brings huge environmental and safety risks. Although some studies have tried to use other oxidizing agents (such as potassium permanganate, peroxide, copper-ammonia complex, etc.) in combination with cyanide, the effect is often not ideal, or the introduction of impurity ions interferes with the subsequent gold leaching and recovery.
[0005] Recent studies have found that potassium ferricyanide (K3[Fe(CN)6]), commonly known as red salt, as a mild oxidizing agent, can selectively oxidize sulfides (S 2- ) to higher valence sulfides (such as SO3 2- , SO4 2-), while itself is reduced to potassium ferrocyanide (K4[Fe(CN)6], commonly known as yellow prussiate). The ferrocyanide can be re-oxidized to ferricyanide under the action of oxygen in the air, which theoretically constitutes a recyclable redox system. However, in practical application, the desulfurization rate and depth of the system are still insufficient, and the inhibitory effect on the formation of sulfur film is limited. SUMMARY
[0006] In view of the technical problems existing in the background art, the present application provides a sulfide ore alkaline desulfurization cyanide leaching gold reagent system, the core of which is to construct a unique ternary reagent system composed of potassium ferricyanide, low concentration sodium cyanide and thioguanosine, and a synergistic effect is generated among the three, realizing efficient desulfurization of sulfide ore and gold extraction, and forming an efficient chemical cycle, realizing high recovery rate extraction of gold in refractory sulfide ore.
[0007] The present application provides a sulfide ore alkaline desulfurization cyanide leaching gold reagent system, which comprises a main cyanide reagent and an auxiliary desulfurization reagent; the main cyanide reagent is sodium cyanide; the auxiliary desulfurization reagent is a composite reagent composed of potassium ferricyanide and thioguanosine.
[0008] Further, in the auxiliary desulfurization reagent, the mass ratio of potassium ferricyanide to thioguanosine is (5-10):1.
[0009] The present application also provides a method for extracting gold by using the aforementioned sulfide ore alkaline desulfurization cyanide leaching gold reagent system, comprising the following steps: S1, grinding the low-grade high-sulfur gold ore to obtain a slurry; S2, adjusting the pH value of the slurry to pH ≥10; first adding the composite reagent composed of auxiliary desulfurization reagents potassium ferricyanide and thioguanosine, stirring at room temperature for 1-3h, then adding the main cyanide reagent sodium cyanide, and stirring to obtain a gold-containing pregnant solution and solid residue.
[0010] Further, in step S2, the mass amount of sodium cyanide used per ton of ore is 100-300g / T, the mass amount of potassium ferricyanide used per ton of ore is 50-300g / T, and the mass amount of thioguanosine used per ton of ore is 10-40g / T.
[0011] Further, in step S2, in the composite reagent composed of potassium ferricyanide and thioguanosine, the mass ratio of potassium ferricyanide to thioguanosine is (5-10):1.
[0012] Further, in the low-grade high-sulfur gold ore, the grade of gold is 0.60g / t, and the mass of sulfide ore accounts for 10-20% of the total mass of ore.
[0013] Further, in the grinding process, the low-grade high-sulfur gold ore is crushed to a size of 75% to 85% of -0.074 mm, and water is added to adjust the pulp to a mass percentage of 30% to 35%.
[0014] Further, the pH value of the ore pulp is adjusted by adding a pH value adjusting agent; the pH value adjusting agent is calcium oxide.
[0015] The beneficial effects of the present application are: The present application provides a sulfide ore alkaline desulfurization cyanide leaching gold reagent system, which comprises a main cyanide reagent and an auxiliary desulfurization reagent. The main cyanide reagent is sodium cyanide, and the auxiliary desulfurization reagent is a composite reagent composed of potassium ferricyanide and thioguanine nucleoside. The synergistic effect between potassium ferricyanide, low-concentration sodium cyanide and thioguanine nucleoside realizes efficient desulfurization of sulfide ore and gold extraction, and forms a high-efficiency chemical cycle.
[0016] Specifically, potassium ferricyanide and thioguanine nucleoside form an efficient "oxidation-inhibition" synergistic system. As the main oxidizing agent, potassium ferricyanide selectively attacks the crystal lattice of sulfide minerals, and selectively oxidizes S 2- to soluble sulfonate and other products, efficiently dissociates the mineral structure to expose gold, and avoids the generation of a large amount of elemental sulfur (S 0 ). However, in actual complex mineral phase reactions, a small amount of active sulfur atoms still escape or locally over-oxidize. The thiol group (-SH) and the electron-rich heterocycle in the molecular structure of thioguanine nucleoside can extremely sensitively capture these newly generated, highly reactive S 0 atoms, and "solidify" and "remove" them by rapidly forming stable organic sulfur compounds, thereby preventing the formation of a sulfur film and completely eliminating the threat of passivation layer to gold particle wrapping.
[0017] Moreover, the synergy between potassium ferricyanide and thioguanine nucleoside is far more than simple functional complementation, and extends to mutual promotion at the level of cyanide leaching kinetics, forming a positive feedback enhancement cycle.
[0018] Specifically, thioguanine nucleoside is not only a passive sulfur capture agent, but also an efficient electron transfer medium that can build a "bridge" between potassium ferricyanide and sulfide minerals, significantly accelerating the rate at which potassium ferricyanide extracts electrons from sulfides, thereby greatly improving the kinetic speed of the overall desulfurization reaction. The increase in reaction rate means that more gold is exposed per unit time, and potassium ferricyanide is reduced to ferrocyanide more quickly. The reduced product, ferrocyanide, is regenerated into potassium ferricyanide through electron transfer, thereby making the entire ferricyanide / ferrocyanide catalytic cycle run more quickly and efficiently, and maximizing the utilization efficiency of the reagent.
[0019] Ultimately, such a deep synergy effect will couple desulfurization with gold leaching, achieving the perfect unity of "breaking the wall" and "removing the barrier". The rapid and selective oxidation of potassium ferricyanide proceeds smoothly under the synergistic effect of thioguanosine, with complete mineral decomposition and high surface activity; at the same time, the presence of thioguanosine can more targetedly eliminate the risk of local micro-area passivation and catalyze electron transfer. Both complement each other, together ensuring that the subsequent low-concentration sodium cyanide can smoothly and unobstructedly leach the exposed gold, ultimately achieving high recovery of gold extraction from refractory sulfide ore while reducing total reagent consumption and environmental pollution.
[0020] The above description is only a summary of the technical solutions of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the content of the specification, and in order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the following specific embodiments of the present application are described. BRIEF DESCRIPTION OF DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the present application, the following will briefly introduce the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for those skilled in the art, other drawings can also be obtained without creative labor on the basis of these drawings.
[0022] Figure 1 It is a reflected light microscope photo of low-grade high-sulfur gold ore (from a certain mine area in Inner Mongolia) in the present application.
[0023] Figure 2 It is a gold, copper and iron element surface distribution map of low-grade high-sulfur gold ore in the present application.
[0024] Figure 3 It is a reflected light microscope photo of broken sulfide inclusions in Example 1, wherein (a) is before dissociation, and (b) is after dissociation.
[0025] Figure 4 It is a reflected light microscope photo of sulfide minerals in the ultraviolet wavelength range of 356~365 nm in Comparative Example 4.
[0026] Figure 5 It is a reflected light microscope photo of sulfide minerals in the ultraviolet wavelength range of 356~365 nm in Comparative Example 9. DETAILED DESCRIPTION
[0027] The embodiments of the technical solutions of the present application will be described in detail below with reference to the drawings. The following examples are only used to more clearly illustrate the technical solutions of the present application, and therefore only serve as examples, but cannot limit the protection scope of the present application.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of this application; the use of the terms "including," "comprising," "having" and variations thereof herein is intended to be broad and encompass the terms "consisting of" and "consisting essentially of" and variations thereof. The use of the term "about" in relation to a reference number can include the reference number ±10% of the stated value.
[0029] The embodiment of the application provides a sulfide ore alkaline desulfurization cyanidation gold leaching reagent system, which comprises a main cyanidation reagent and an auxiliary desulfurization reagent; the main cyanidation reagent is sodium cyanide; and the auxiliary desulfurization reagent is a composite reagent composed of potassium ferricyanide and thio-guanosine.
[0030] In the auxiliary desulfurization reagent, the mass ratio of potassium ferricyanide to thio-guanosine is (5-10):1.
[0031] The embodiment of the application further provides a method for extracting gold by using the aforementioned sulfide ore alkaline desulfurization cyanidation gold leaching reagent system, which comprises the following steps: S1, performing grinding treatment on a low-grade high-sulfur gold ore to obtain an ore slurry; In the low-grade high-sulfur gold ore, the grade of gold is 0.60 g / t, and the mass of sulfide minerals accounts for 10-20% of the total mass of the ore.
[0032] In the grinding treatment, the low-grade high-sulfur gold ore is crushed to a size of -0.074 mm, the content of ore powder in the total mass of the material is 75-85%, and water is added to adjust the mass percentage concentration of the ore slurry to 30-35%.
[0033] S2, adjusting the pH value of the ore slurry to pH ≥10; first, a composite reagent composed of potassium ferricyanide and thio-guanosine is added, the composite reagent is stirred at room temperature for 1-3 hours, then the main cyanidation reagent sodium cyanide is added, and stirring is performed to obtain a gold-containing pregnant solution and solid residues.
[0034] The pH value of the ore slurry is adjusted by adding a pH value adjusting agent calcium oxide.
[0035] In the composite reagent composed of potassium ferricyanide and thio-guanosine, the mass ratio of potassium ferricyanide to thio-guanosine is (5-10):1.
[0036] The ore-metered mass of sodium cyanide is 100-300 g / T, the ore-metered mass of potassium ferricyanide is 50-300 g / T, and the ore-metered mass of thio-guanosine is 10-40 g / T.
[0037] Some specific examples are listed below. It should be noted that the examples described below are exemplary and are used only to explain the present application and cannot be understood as limiting the present application. If a specific technique or condition is not specified in the examples, the technique or condition described in the literature in the art or according to the product manual is used. If the manufacturer of the reagent or instrument is not specified, it is a conventional product that can be obtained on the market.
[0038] Example 1 The low-grade high-sulfur gold ore in this example is from a gold mine in Inner Mongolia, wherein the grade of gold is 0.60 g / t, and the mass of sulfide minerals accounts for 10-20% of the total mass of the ore.
[0039] The reflected light microscope photograph of the low-grade high-sulfur gold ore is shown in Figure 1 .
[0040] The gold, copper, and iron element surface distribution map of the low-grade high-sulfur gold ore is shown in Figure 2 .
[0041] The present example provides a method for extracting gold by using a sulfide ore alkaline desulfurization cyanide leaching gold reagent system, comprising the following steps: S1, crushing the low-grade high-sulfur gold ore to an ore particle size of -0.074 mm, and adding water to adjust the pulp to a mass percentage concentration of 35%.
[0042] S2, adjusting the pH of the ore pulp prepared in step S1 to 10.5 with calcium oxide. Subsequently, an auxiliary desulfurization reagent (potassium ferricyanide and sulfide nucleoside complex reagent) is added; in the auxiliary desulfurization reagent, the mass ratio of potassium ferricyanide to sulfide nucleoside is 7:1, the mass amount of potassium ferricyanide is 70 g / T, and the mass amount of sulfide nucleoside is 10 g / T. Stirring at room temperature for 2 h, then adding a main cyanide reagent (sodium cyanide), the mass amount of sodium cyanide is 200 g / T, and stirring leaching at room temperature for 12 h. Solid-liquid separation to obtain a gold-containing liquid and a solid residue (leaching residue).
[0043] The gold concentration in the noble liquid is tested by an ICP-OES analyzer. The gold content in the leaching residue is tested by fire assaying, and the test analysis method refers to “GB / T 7739”.
[0044] Specifically, the gold content in the solid residue is tested by fire assaying, and the test analysis method refers to “GB / T 7739”.
[0045] The leaching rate of gold is calculated to determine the leaching condition of gold.
[0046] ; In the formula, η represents the leaching rate of gold, the unit is %; m1 represents the mass of the original low-grade high-sulfur gold ore, the unit is g; β1 represents the grade of the original low-grade high-sulfur gold ore, the unit is g / t; m2 represents the mass of the solid residue after leaching of the low-grade high-sulfur gold ore, the unit is g; and β2 represents the grade of the solid residue after leaching, the unit is g / t.
[0047] The gold-containing noble liquid is detected by ICP-OES, and the leaching rate of gold obtained by the method of the application is assisted to prove according to the concentration of gold in the gold-containing noble liquid. It can be known that the error of the above two methods is less than 1%, which indicates that the test value of the method is effective data.
[0048] Comparative Example 1 Compared with Example 1, the difference lies in that no auxiliary desulfurization reagent is added in step S2, and the mass amount of sodium cyanide is 5000g / T (the amount of sodium cyanide follows the recommended reagent amount in the industrial feasibility evaluation report), and the other is basically the same as Example 1, which will not be repeated here.
[0049] Comparative Example 2 Compared with Example 1, the difference lies in that no auxiliary desulfurization reagent is added in step S2, and the other is basically the same as Example 1, which will not be repeated here.
[0050] Comparative Example 3 Compared with Example 1, the difference lies in that no component of potassium ferricyanide in the auxiliary desulfurization reagent is added in step S2. The other is basically the same as Example 1, which will not be repeated here.
[0051] Comparative Example 4 Compared with Example 1, the difference lies in that no component of thio-guanosine in the auxiliary desulfurization reagent is added in step S2. The other is basically the same as Example 1, which will not be repeated here.
[0052] Comparative Example 5 Compared with Example 1, the difference lies in that no main cyanide reagent (sodium cyanide) is added in step S2. The other is basically the same as Example 1, which will not be repeated here.
[0053] The leaching rate of gold of Example 1 and Comparative Examples 1-5 is shown in Table 1.
[0054] Table 1 Gold leaching effect of Example 1 and Comparative Examples 1-5 As can be seen from Table 1, potassium ferricyanide, thio-guanosine and sodium cyanide constitute an organic whole that cannot be missed, which is the key to efficient extraction of gold.
[0055] Figure 3The broken sulfide package reflected light microscope photo in Example 1. It can be clearly seen that the originally dense sulfide ore under the action of "potassium ferricyanide-thioguanine nucleoside" complex auxiliary desulfurization reagent chemical dissociation effect, reagent and mineral sulfide effect form crushing ring belt, at the same time show the trend of core dissolution.
[0056] In Comparative Example 3, when the potassium ferricyanide in the auxiliary desulfurization reagent is missing, the gold leaching rate drops from 92% to 14%; in Comparative Example 4, when the thioguanine nucleoside in the auxiliary desulfurization reagent is missing, the gold leaching rate drops from 92% to 21%. It shows that the "potassium ferricyanide-thioguanine nucleoside" complex auxiliary desulfurization reagent is indispensable, and the two can effectively overcome the hindrance of sulfide to gold leaching through synergistic effect.
[0057] Figure 4 The sulfide mineral in Comparative Example 4 is reflected in the ultraviolet wavelength range of 356-365 nm. It can be seen that when the thioguanine nucleoside is not introduced, part of the dissolved sulfide ore will form new inclusions, hindering the subsequent leaching of gold.
[0058] Comparison Figure 3 With Figure 4 It can be seen that thioguanine nucleoside can quickly form stable organic sulfur compounds to "solidify" and "remove" sulfide minerals, thereby blocking the formation of sulfur film and completely eliminating the effect of passivation layer on gold particle inclusions.
[0059] In Comparative Example 5, when the main cyanide reagent sodium cyanide is not used, the gold leaching rate is 0. It shows that sodium cyanide is indispensable as the main reagent for leaching gold, and the leaching process cannot proceed without sodium cyanide.
[0060] And as shown in Table 1, in Example 1, only a very low amount of sodium cyanide (200 g / T) is required to achieve a high leaching rate of 92%; on the contrary, if the auxiliary desulfurization reagent is missing (Comparative Example 1), the amount of sodium cyanide will increase by 25 times (5000 g / T) and the leaching rate will be lower (75%) at a huge cost. It proves that potassium ferricyanide, thioguanine nucleoside and sodium cyanide work together to maximize economic and efficiency.
[0061] Examples 2-8 and Comparative Examples 6-13 Examples 2-8 and Comparative Examples 6-13 provide a method for extracting gold by using a sulfide ore alkaline desulfurization cyanide leaching gold reagent system. Compared with Example 1, the difference is that the amount of potassium ferricyanide and thioguanine nucleoside in the auxiliary desulfurization reagent is different, as shown in Table 2, other experimental parameters and conditions are basically the same as those in Example 1, which will not be repeated here.
[0062] Table 2 Amount of each component of the reagent and gold leaching rate in Examples 2-8 and Comparative Examples 6-13 As can be seen from Table 2, the ratio of potassium ferricyanide to thioguanosine has a significant effect on the leaching rate of gold, and both should be maintained within a suitable range to achieve the best synergistic desulfurization and gold leaching effect.
[0063] When the amount of potassium ferricyanide is in the range of 50-300 g / T and the amount of thioguanosine is in the range of 10-40 g / T (Examples 1-8), the leaching rate of gold is stable at a high level of 91% to 95%. This indicates that within this range, potassium ferricyanide can provide sufficient and moderate oxidation capacity to effectively destroy the structure of sulfide minerals, while sufficient thioguanosine can timely remove any active sulfur atoms that may be generated in the reaction, preventing them from polymerizing into a passivation film, and both promote each other, accelerating the reaction kinetics and the recycling of reagents.
[0064] However, once the ratio of the two reagents is imbalanced, whether one is excessive or insufficient, the synergistic effect of the system will be severely damaged, resulting in a sharp decrease in leaching rate. Specifically, when the amount of potassium ferricyanide is insufficient (Comparative Example 6, 40 g / T), the oxidation capacity is not sufficient to completely dissociate the sulfide minerals, resulting in some gold not being exposed, and the leaching rate decreases to 81%. More critically, when the amount of thioguanosine is too high (Comparative Examples 7-9, 50 g / T), even if the amount of potassium ferricyanide is within the effective range of 100-300 g / T, the leaching rate decreases significantly. This is most likely because the excessive thioguanosine, due to its strong adsorption and complexing ability, not only captures sulfur atoms, but also may excessively adsorb on the mineral or exposed gold surface, forming a new organic barrier layer, hindering the leaching of gold by sodium cyanide, resulting in a negative effect.
[0065] Figure 5 The reflected light microscope photo of the sulfide minerals in Comparative Example 9 in the ultraviolet wavelength range of 356-365 nm.
[0066] Under the excitation of ultraviolet light with a wavelength of 356-365 nm, thioguanosine can exhibit characteristic fluorescence due to its unique conjugated cyclic structure. By observing the photo of Comparative Example 9 in the ultraviolet wavelength range of 356-365 nm, it can be seen that an organic barrier layer is generated on the surface of the minerals, further confirming the above argument.
[0067] It can be seen from the experiment that when the amount of potassium ferricyanide is too high and exceeds the optimal range (comparative examples 10-13, 350-400 g / T), it will also have an adverse effect on the system. A strong oxidative environment may promote the intensification of side reactions, such as the excessive oxidation of sulfides to generate more sulfate, or non-selective reactions with other components in the ore pulp, causing unnecessary reagent loss, and even possibly interfering with the structure or function of thioguanosine. At this time, even if 10-40 g / T of thioguanosine is added, it cannot reverse the decline in leaching rate (from 83% to 63%), which proves that there is a strict, nonlinear synergistic window between the two, and any individual excess of reagents will destroy the chemical balance of the system, ultimately leading to the failure of gold leaching.
[0068] Examples 9-13 and Comparative Examples 14-17 Examples 9-13 and Comparative Examples 14-17 provide a method for extracting gold from a sulfide ore alkaline desulfurization cyanide leaching reagent system, which differs from Example 1 in that the amounts of potassium ferricyanide, thioguanosine, and sodium cyanide are different, as shown in Table 3, and the other experimental parameters and conditions are basically the same as those of Example 1, which are not repeated here.
[0069] Table 3 Amounts of reagent components and gold leaching rates in Examples 9-13 and Comparative Examples 14-17 As can be seen from Table 3, the amount of sodium cyanide has a threshold effect and an economically optimal interval on the gold leaching rate, rather than a simple linear relationship. Under the premise that the synergistic desulfurization system composed of potassium ferricyanide and thioguanosine operates effectively, the amount of sodium cyanide can maintain a very high gold leaching rate (90%-95%) within a large range (100-300 g / T).
[0070] Specifically, when the amount of sodium cyanide increases from 90 g / T (Comparative Example 14) to 100 g / T (Example 9), the gold leaching rate shows a significant jump (from 85% to 90%), which indicates that 100 g / T is a critical effective concentration threshold in this system. Below this value, the total amount of cyanide ions for gold complexation and sulfur film removal is insufficient, resulting in a decline in leaching rate. However, once this threshold is exceeded, increasing the amount of sodium cyanide (e.g., from 100 g / T to 400 g / T) does not significantly improve the leaching rate (Examples 9, 10, and Comparative Examples 15-17 all maintain a high plateau of 90%-94%). This proves that in this ternary synergistic system, the efficient wall breaking of potassium ferricyanide and the perfect passivation of thioguanosine greatly reduce the dependence on the amount of sodium cyanide. Although excessive addition of sodium cyanide (e.g., 400 g / T) has no negative effect on the leaching rate, it is unnecessary from the perspectives of economic benefits and environmental protection.
[0071] In summary, the reagent system of the present application successfully optimizes and stabilizes the dosage of sodium cyanide from a high level (usually much higher than 200 g / T) of the conventional dosage to a relatively low economic interval (100-300 g / T) through the precise synergy of potassium ferricyanide and thioguanosine, significantly reducing the reagent cost and environmental risk while ensuring extremely high gold recovery.
[0072] Note that the present application is not limited to the above-described embodiments. The above-described embodiments are merely examples, and embodiments having substantially the same configuration as the technical idea and exerting the same effects within the scope of the technical solution of the present application are all included in the technical scope of the present application. Furthermore, within the scope of the gist of the present application, various modifications that can be thought of by those skilled in the art, other modes constructed by combining part of the configuration elements of the embodiments are also included in the scope of the present application.
Claims
1. A reagent system for the alkaline de-sulphidation of gold from sulphide ores, characterised in that, The sulfide ore alkaline desulfurization cyanidation gold leaching reagent system comprises a main cyanidation reagent and an auxiliary desulfurization reagent; the main cyanidation reagent is sodium cyanide; the auxiliary desulfurization reagent is a composite reagent composed of potassium ferricyanide and thioguanosine.
2. The sulphide ore alkaline de-sulphidation gold leaching reagent system according to claim 1, c h a r a c t e r i z e d b y, In the auxiliary desulfurization reagent, the mass ratio of potassium ferricyanide to thioguanosine is (5-10):
1.
3. A method of extracting gold from a sulphide ore by alkaline dethiocyanide leaching of gold using a reagent system, characterised in that, The sulfide ore alkaline desulfurization cyanidation gold leaching reagent system of any one of claims 1-2 comprises the following steps: S1, grinding the low-grade high-sulfur gold ore to obtain a slurry; S2, adjusting the pH value of the slurry to pH ≥10; first adding the composite reagent composed of the auxiliary desulfurization reagents potassium ferricyanide and thioguanosine, stirring at room temperature for 1-3 h, then adding the main cyanidation reagent sodium cyanide, and stirring to obtain a gold-containing pregnant solution and solid residues.
4. The method of gold extraction from a sulfide ore by alkaline dethiocyanide leaching according to claim 3, characterized in that, In step S2, the mass amount of sodium cyanide is 100-300 g / T, the mass amount of potassium ferricyanide is 50-300 g / T, and the mass amount of thioguanosine is 10-40 g / T.
5. The method of gold extraction from a sulfide ore by alkaline dethiocyanide leaching according to claim 4, characterized in that, In step S2, the mass ratio of potassium ferricyanide to thioguanosine in the composite reagent composed of potassium ferricyanide and thioguanosine is (5-10):
1.
6. The method of gold extraction from a sulfide ore by alkaline dethiocyanide leaching according to claim 3, characterized in that, In the low-grade high-sulfur gold ore, the grade of gold is 0.60 g / t, and the mass of sulfide minerals accounts for 10-20% of the total ore mass.
7. The method of gold extraction from a sulfide ore by alkaline dethiocyanide leaching according to claim 3, characterized in that, During the grinding process, the low-grade high-sulfur gold ore is crushed to a size of -0.074 mm, and the amount of ore powder accounts for 75-85% of the total mass of the material, and water is added to adjust the slurry to a mass percentage concentration of 30-35%.
8. The method of gold extraction from a sulfide ore by alkaline dethiocyanide leaching according to claim 3, characterized in that, The method for adjusting the pH value of the slurry is to add a pH value adjusting agent; the pH value adjusting agent is calcium oxide.
Citation Information
Patent Citations
Thiosulfate gold extraction method taking Fe (III) cyanide salts as oxidants
CN102534204A
Reinforced leaching method of fine-grained encapsulated gold
CN104694764A
Gold and silver extracting agent and preparation method thereof
CN116287754A
Low-cyanide gold leaching agent system and dump leaching process thereof
CN120666187A
METHOD OF EXTRACTING GOLD FROM CONCENTRATES
RU2009100306A
Cited By
Method for testing gold recovery performance of gold-containing material
CN122345548A