Preparation method for producing high-precision casting shell mold through lost foam
By employing a lost foam-shell composite casting process that combines low-temperature demolding and medium-temperature sintering, and using a novel refractory coating, the problems of carbon pollution, insufficient dimensional accuracy, and environmental protection in traditional casting processes have been solved. This process enables high-precision, low-cost casting production and is suitable for multiple high-precision fields.
Patent Information
- Application Number
- CN202511139877.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-14
- Publication Date
- 2025-12-16
Smart Images

Figure CN121131667A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of casting technology, specifically to a method for preparing high-precision casting shells using lost foam casting technology, which is particularly suitable for the production of metal parts in fields such as chemical engineering, aerospace, medical devices, and automobile manufacturing where dimensional accuracy and surface quality requirements are stringent. Background Technology
[0002] 1. Limitations of traditional lost foam casting
[0003] Lost foam casting (EPC) is widely used in the casting industry due to its advantages of near-net-shape forming and simplified processes, but its inherent defects limit its development in high-precision fields:
[0004] Carbon pollution problem: EPS foam decomposes at high temperatures, producing a large number of carbon particles, which can easily lead to carbon enrichment on the surface of castings (carbon content can fluctuate by 0.3-0.5%), affecting the performance of carbon-sensitive materials such as stainless steel and aluminum alloys. For example, when aero-engine blades are cast using traditional lost foam casting, carbon enrichment defects can significantly reduce the fatigue strength of the blades.
[0005] Insufficient dimensional accuracy: Foam molds are prone to thermal expansion and deformation during heating and pouring, resulting in casting dimensional tolerances typically only reaching CT7-9 grade, which is insufficient to meet the aerospace industry's accuracy requirements of CT6 grade and above. When a certain type of satellite bracket was manufactured using traditional processes, excessive dimensional deviations led to a low assembly pass rate.
[0006] Surface quality issues: Foam vaporization residues easily form carbon deposits and pores on the surface of castings, with a surface roughness Ra typically ranging from 12.5 to 25 μm. Additional machining is required to meet the requirements of precision parts, increasing production costs and time.
[0007] 2. Bottlenecks in traditional shell casting
[0008] Shell casting achieves high precision through ceramic molds, but it has the following problems:
[0009] High mold costs: Metal master molds (such as aluminum molds and cast iron molds) have long processing cycles and high costs, and are only suitable for mass production.
[0010] Low process flexibility: Modifying metal master molds is difficult and cannot adapt to the needs of rapid product iteration.
[0011] Significant environmental pressure: Traditional shell casting uses phenolic resin sand, which releases a large amount of harmful gases (such as formaldehyde and benzene compounds) during the casting process, resulting in high environmental treatment costs.
[0012] 3. Shortcomings of existing technological improvement attempts
[0013] To address the above problems, existing technologies have made various attempts:
[0014] Foam material optimization: We developed low-gas-emission foam materials, but the cost was 3-5 times that of EPS, and the gasification residue could not be completely eliminated, with the internal porosity of the casting still reaching 3-5%.
[0015] Improved negative pressure control: Increasing the negative pressure reduces porosity, but it can easily lead to shell breakage and a high scrap rate.
[0016] 4. Industry demand and technological gaps
[0017] With the surge in demand for precision castings in fields such as aerospace (e.g., titanium alloy blades), medical devices (e.g., joint prostheses), and new energy vehicles (e.g., motor housings), the market urgently needs a casting process that combines low cost, high precision, and environmental friendliness. Existing technologies have failed to effectively address issues such as carbon pollution from lost foam casting, high costs of shell casting, and insufficient process flexibility, creating a significant technological gap.
[0018] The above background information is provided only to aid in understanding the inventive concept and technical solution of this invention. It does not necessarily belong to the prior art of this patent application. In the absence of clear evidence that the above information was disclosed on the filing date of this patent application, the above background information should not be used to evaluate the novelty and inventiveness of this application. Summary of the Invention
[0019] The purpose of this invention is to provide a lost foam-shell composite casting process, which avoids carbon pollution by demolding at a low temperature of 200-300℃ and controls the shell shrinkage rate to ≤0.3% by sintering at a medium temperature of 600-800℃, thereby achieving low-cost and environmentally friendly production of CT6 grade precision castings. It is especially suitable for the manufacturing of precision parts in the fields of chemical engineering, aerospace, and medical devices.
[0020] To achieve the above technical objectives, the present invention adopts the following technical solution:
[0021] A method for preparing high-precision casting shell molds using lost foam casting includes the following steps:
[0022] (1) Mold making: The mold is made of EPS material, and the aluminum mold is produced by foaming to create the white mold;
[0023] (2) Mold coating: Apply refractory coating to the surface of the white mold;
[0024] (3) Low-temperature demolding: The white mold after being coated is placed in a resistance furnace and heated to melt the EPS white mold into a liquid and then recycled through a recycling device;
[0025] (4) Medium-temperature sintering mold: Place the demolded shell mold into a resistance heating furnace for sintering;
[0026] (5) Casting: The sintered mold is placed in a negative pressure molding box according to the lost foam molding process, and the molten metal is poured in under negative pressure.
[0027] (6) Casting cleaning and subsequent treatment: After pouring, the casting is kept warm and then removed from the mold. It is then polished and cleaned to obtain the casting blank.
[0028] Preferably, the aluminum mold has a manufacturing precision of ±0.05mm, a surface roughness Ra≤1.6μm, and a uniformly distributed heating channel inside.
[0029] Preferably, the coating thickness is 1.0-3.5 mm.
[0030] Preferably, the coating is applied by a combination of dip coating and spray coating, first dip coating once, then standing for 10-15 minutes before spray coating once.
[0031] Preferably, the low-temperature demolding state is within the temperature range of 200-300°C under atmospheric pressure.
[0032] Preferably, the heating rate for low-temperature demolding is 5-10℃ / min.
[0033] Preferably, the heat preservation time for low-temperature demolding is 30-60 minutes.
[0034] Preferably, the sintering conditions are sintering at a temperature range of 600-800℃ for 5-10 hours.
[0035] Preferably, the vacuum degree of the negative pressure molding box is -0.05 to -0.07 MPa, the metal liquid pouring temperature is 1500-1600℃, and the pouring speed is 1-5 kg / s.
[0036] Preferably, the heat preservation time is 5-10 hours after the casting is removed from the mold, depending on the different material requirements of the casting.
[0037] Invention concept:
[0038] This invention provides a method for preparing high-precision casting shell molds, with the innovative idea of integrating lost foam casting technology and shell mold casting process. By following the lost foam production route and using EPS material as the white mold, and addressing the issue of carbon accumulation during high-temperature vaporization of the lost foam white mold, a novel refractory coating composed of zircon powder, silica sol, binder, nano-alumina, and silicon carbide whiskers is innovatively adopted. Nano-alumina, with its nano-sized particle size, fills the micropores of the coating, increasing its density and significantly enhancing its refractoriness and high-temperature stability, effectively preventing carbon generated during EPS vaporization from diffusing into the molten metal. Silicon carbide whiskers, with their high strength and hardness, form a three-dimensional reinforcing network in the coating, improving its erosion resistance and resisting high-speed erosion during molten metal pouring.
[0039] The coating is evenly applied to the surface of the white mold, and then dried at a low temperature. The white mold melts and precipitates at 200-300℃, allowing for recycling and avoiding the carbon residue problem caused by high-temperature vaporization of EPS in traditional processes. The remaining coating layer is then sintered at a medium temperature of 600-800℃. During this process, the silica sol and refractory aggregate react fully to form a high-strength, highly dense, and appropriately permeable ceramic shell. Finally, the sintered shell is placed in a vacuum negative pressure environment for molding, completing the molten metal pouring. This method, through innovation in refractory materials and synergistic optimization of various process steps, achieves high-precision, low-pollution shell casting, effectively overcoming the limitations of traditional processes in terms of precision, cost, and environmental protection.
[0040] Technological innovation:
[0041] In the process of this invention, the low-temperature demolding step is crucial. By heating the coated white mold in a temperature range of 200-300℃, the EPS white mold melts into a liquid and is then recycled. This effectively overcomes the problem of carbon residue caused by high-temperature vaporization in traditional lost foam casting, avoids carbonization of the metal material, and ensures the purity of the casting. At the same time, it significantly reduces production costs and material waste, achieving green and environmentally friendly production.
[0042] Innovation in refractory materials is also a core highlight of this invention. Traditional refractory coatings, due to their single composition and loose structure, are prone to peeling and cracking under the scouring of high-temperature molten metal, resulting in rough casting surfaces and a high defect rate. The novel refractory coating developed in this invention is composed of zircon powder, silica sol, binder, nano-alumina, and silicon carbide whiskers. Among them, nano-alumina, with its nano-sized particle size advantage, can fill the micropores inside the coating, increasing the density of the coating and significantly enhancing its refractoriness and high-temperature stability; silicon carbide whiskers, with their high strength and high hardness, are uniformly dispersed in the coating to form a three-dimensional reinforcing network, improving the coating's scouring resistance and effectively resisting the high-speed scouring during molten metal pouring. In terms of the preparation process, by pre-treating the raw materials and precisely controlling the mixing, stirring, and grinding parameters, the uniform dispersion of each component is ensured, avoiding agglomeration. The final coating achieves an optimal balance in viscosity, specific gravity, and coating performance, ensuring uniform coating on the white mold surface and tight bonding with the white mold and shell during low-temperature demolding and medium-temperature sintering, thus providing a stable and reliable protective barrier for casting.
[0043] The medium-temperature sintering process is also a core innovation of this invention. The demolded shell mold is sintered at 600-800℃ for 5-10 hours, which reduces energy consumption compared to the high-temperature sintering of 900-1200℃ used in traditional shell casting. Within this temperature range, the silica sol and refractory aggregate react fully to form a high-strength, highly dense, and appropriately permeable ceramic shell mold. This ensures that the surface finish of the casting reaches Ra≤6.3μm, and the dimensional tolerance is controlled within CT6 grade (±0.15mm / 100mm), providing a reliable guarantee for the production of high-precision castings.
[0044] Detailed explanation of the specific functions of each step:
[0045] (a) Making molds
[0046] Using EPS material to create molds is fundamental to the entire production process. For mass production of castings, an aluminum mold with a precision of ±0.05mm, a surface roughness Ra≤1.6μm, and uniformly distributed heating channels is fabricated before foaming to produce a white mold. The high precision of the aluminum mold ensures the dimensional accuracy of the white mold, laying the foundation for obtaining high-precision castings. The internal heating channels make the foaming process more uniform, ensuring consistent density in the white mold and reducing casting defects caused by uneven density. For small batches or single-piece products, manual cutting of EPS boards combined with topology optimization and other technologies can flexibly meet diverse needs and enable the fabrication of complex mold structures.
[0047] (ii) Mold coating
[0048] Applying a refractory coating to the surface of the white mold is a crucial step in ensuring the quality of the casting. The refractory coating of this invention consists of zircon powder, silica sol, binder, nano-alumina, and silicon carbide whiskers. Zircon powder, as the main refractory aggregate, provides basic refractory properties; silica sol and binder enable the coating to adhere firmly to the white mold surface, forming a coating with a certain strength after drying and sintering; nano-alumina significantly improves the coating's refractoriness and high-temperature stability, and its fine particles fill the coating's pores, increasing density; silicon carbide whiskers, with their high strength and hardness, enhance the coating's erosion resistance, preventing corrosion of the coating during molten metal pouring. The coating viscosity is controlled at 18-25 seconds (Ford Cup 4), and the specific gravity is 1.8-2.2 g / cm³. 3 With a thickness of 1.0-3.5mm, a combination of dip coating and spray coating is used. First, dip coating is applied once to fully cover the surface of the white mold. After standing for 10-15 minutes, the coating is allowed to dry and penetrate initially. Then, a second spray coating is applied to fill the gaps, ensuring that the coating is uniform and has good overall performance, effectively avoiding defects such as sand adhesion and porosity in the casting.
[0049] (iii) Low-temperature demolding
[0050] After coating, the white mold is placed in an electric resistance furnace and demolded at a low temperature of 200-300℃ under atmospheric pressure, with a heating rate of 5-10℃ / min and a holding time of 30-60min. This step melts the EPS white mold into a liquid, which is then recycled using a recycling device. Strict control of temperature and time parameters is required in this process. If the temperature is too low, the EPS will not melt completely; if the temperature is too high, the EPS will carbonize, affecting the recycling quality and casting accuracy. Appropriate heating rates and holding times ensure uniform melting and complete demolding of the EPS, while also guaranteeing the reuse of the recycled EPS, reducing production costs and environmental pollution.
[0051] (iv) Medium-temperature sintering mold
[0052] After demolding, the shell mold is placed in a resistance heating furnace and sintered at 600-800℃ for 5-10 hours. This step further solidifies and densifies the coating layer, forming a shell mold with sufficient strength and refractoriness. The sintering temperature and time directly affect the shell mold's performance. Too low a temperature or too short a time results in insufficient shell strength, making it unable to withstand the pressure of molten metal pouring; too high a temperature or too long a time may lead to cracking or performance degradation. Precise control of these parameters allows for optimal compressive strength, refractoriness, and other properties of the shell mold, providing a reliable guarantee for subsequent pouring.
[0053] (v) Pouring
[0054] The sintered mold is placed in a negative pressure molding chamber using the lost foam casting process. Pouring is then completed under a vacuum of -0.05 to -0.07 MPa, at a molten metal pouring temperature of 1500-1600℃, and a pouring speed of 1-5 kg / s. The negative pressure environment enhances the fluidity and filling capacity of the molten metal, ensuring complete filling of the mold cavity and reducing defects such as incomplete filling and cold shuts. Appropriate pouring temperature and speed prevent overheating or undercooling of the molten metal during flow, resulting in a uniform casting structure and good performance.
[0055] (vi) Cleaning and subsequent treatment of castings
[0056] After pouring, the casting is kept at a constant temperature for 5-10 hours, depending on the material requirements of the casting, before being removed from the mold and polished to obtain the casting blank. The heat preservation process allows the casting to cool slowly, reducing internal stress and preventing cracking; polishing removes excess material and impurities from the surface of the casting, improving its surface quality and ensuring it meets design requirements.
[0057] Inter-step synergistic mechanism:
[0058] The high precision of mold making ensures the accuracy of the white mold, providing a foundation for the uniform application of the coating. A high-quality refractory coating layer protects the shell shape during low-temperature demolding, preventing coating peeling. After demolding, medium-temperature sintering ensures a tight bond between the coating layer and the shell, forming a high-strength integral structure. The strong shell can withstand the pressure and erosion of the molten metal during pouring, while negative pressure pouring ensures complete molten metal filling, working in conjunction with the shell to produce a high-quality casting. Finally, cleaning and subsequent treatments further enhance the casting quality. Each step is interconnected and works together to significantly improve the dimensional accuracy, surface quality, and internal properties of the casting.
[0059] For example, if the mold making precision is insufficient, it will lead to deviations in the size of the white mold. Even if the coating performance is good, it will be difficult to compensate for the impact of mold error on the casting precision. If the low-temperature demolding process is not properly controlled, EPS residue or shell damage will occur, and subsequent medium-temperature sintering and pouring steps will not be able to proceed normally, seriously affecting the casting quality.
[0060] The necessity that the steps cannot be changed:
[0061] The order of each step cannot be arbitrarily changed. First, a mold must be made before coating can be applied to its surface; if coating is applied first, the coating will be ineffective without a mold as a support. Second, low-temperature demolding must be performed after coating, as the coating protects the shell during demolding. If demolding occurs before coating, the shell loses its mold support, making it difficult to guarantee the coating effect and shell integrity. Medium-temperature sintering must be performed after demolding, as only the demolded shell is ready for sintering. If sintering is performed prematurely, the undemolded EPS will affect the shell's performance in subsequent processes. Pouring must be performed after sintering, as only a sintered shell has sufficient strength to withstand the pressure of molten metal. Cleaning and subsequent processing can only be carried out after the casting is formed. Therefore, the order of each step strictly follows the production logic and material characteristics; any change will lead to production disruptions or a significant decrease in casting quality.
[0062] The Importance of Optimizing Process Parameters:
[0063] Optimizing process parameters at each step is crucial for producing high-quality casting shells. Taking coatings as an example, the viscosity, specific gravity, and thickness of the coating directly affect its coating effect and performance. Excessive viscosity results in poor coating fluidity and difficulty in uniform application; insufficient viscosity leads to excessive flow and uneven coating thickness. A suitable specific gravity ensures uniform coating composition and avoids sedimentation; an appropriate thickness provides sufficient protection without compromising the dimensional accuracy of the casting. The temperature, heating rate, and holding time parameters for low-temperature demolding determine the melting effect and recycling quality of the EPS (expanded polystyrene); improper parameters can lead to incomplete demolding or EPS carbonization. The temperature and time parameters for medium-temperature sintering affect the shell's strength and performance; unreasonable parameters can result in insufficient shell strength or cracks. The vacuum degree, pouring temperature, and pouring speed parameters during the pouring process directly affect the filling effect of the molten metal and the quality of the casting; inappropriate parameters can lead to defects such as incomplete filling and porosity in the casting. Therefore, accurately optimizing each process parameter is the key to obtaining high-precision casting shells, improving casting quality and production efficiency. Any deviation in parameters may lead to unexpected negative technical effects, seriously affecting product quality and corporate profits.
[0064] The beneficial effects of this invention compared to the prior art include:
[0065] 1. Technological Integration Breakthroughs: The innovative combination of lost foam casting and shell casting leverages the advantages of lost foam casting in complex structure forming while overcoming its limitations in dimensional accuracy and carbon contamination. Simultaneously, it overcomes the restrictions of shell casting, which relies on metal master molds and has a narrow application range. This synergistic effect of the two processes significantly expands the application scenarios of casting technology. In this process, a novel refractory coating composed of zircon powder, silica sol, binder, nano-alumina, and silicon carbide whiskers plays a crucial role. Its high density and erosion resistance ensure stable protection of the shell mold during complex structure forming, further enhancing the applicability of the integrated process.
[0066] 2. Innovation in Coating and Sintering Processes: A specialized shell mold coating composed of zircon powder, silica sol, binder, nano-alumina, and silicon carbide whiskers has been developed. Nano-alumina fills the micropores, achieving a coating density of 92%. Silicon carbide whiskers form a three-dimensional reinforcing network, improving erosion resistance by 40%. Combined with the silica sol binder, a high-strength coating of 1.0-3.5mm is formed, significantly improving the surface finish and anti-sand adhesion properties of castings compared to traditional coatings. Combined with a medium-temperature sintering process of 600-800℃, within this temperature range, the silica sol in the coating reacts fully with the refractory aggregate, forming a high-strength, highly dense ceramic shell with suitable permeability. Compared to traditional high-temperature sintering, this significantly reduces energy consumption and equipment costs while ensuring shell dimensional stability and high-precision casting.
[0067] 3. Versatile Application and Green Production: This invention is applicable to all casting materials, regardless of their complexity, production batch size, or weight, and is particularly effective in manufacturing high-value-added castings (such as precision stainless steel parts). The novel refractory coating, with its excellent high-temperature resistance and erosion resistance, is suitable for various molten metal castings, expanding the range of applicable processes. Low-temperature demolding during production enables efficient recycling of EPS mold materials, reducing solid waste; medium-temperature sintering produces no harmful gas emissions, significantly reducing environmental pollution and offering both economic and environmental benefits. Furthermore, the raw materials in the coating are environmentally friendly and harmless, and the preparation process generates no pollutants, further contributing to green production.
[0068] 4. Simple Operation and Easy Promotion: The process simplifies the cumbersome procedures of traditional casting, with a clear and controllable core workflow. It requires low technical skills from operators, and ordinary workers can master the skills after short-term training. Although the preparation process of the new refractory coating involves multiple steps such as raw material pretreatment and mixing, the process is highly standardized and easy to operate. Furthermore, its application process is highly compatible with existing lost foam casting production lines, allowing for modifications to existing equipment, significantly reducing the cost and time required for technology upgrades, and facilitating rapid industrialization and industry promotion. Attached Figure Description
[0069] Figure 1 A physical image of the casing of a stainless steel impeller used in the chemical industry;
[0070] Figure 2 This is a mold drawing for stainless steel impellers used in the chemical industry. Detailed Implementation
[0071] I. Implementation Plan
[0072] 1. Making molds
[0073] For mass production of castings, high-precision machining equipment is used to fabricate aluminum molds, controlling their manufacturing accuracy to ±0.05mm and surface roughness Ra≤1.6μm. Uniformly distributed heating channels are milled inside the aluminum mold. EPS raw materials are fed into a foaming machine, using the aluminum mold as the template to produce white molds, controlling the density of the white molds within a suitable range. For small batches or single-piece products, based on the casting design drawings, EPS boards are manually cut using cutting equipment to create molds. A topology optimization algorithm is applied to optimize the mold structure, followed by precision machining using a five-axis CNC cutting machine, achieving an accuracy of ±0.05mm. Laser cladding technology is used to repair and strengthen the surface of the cut molds, improving mold quality.
[0074] 2. Refractory Coating Preparation Process
[0075] Selection of refractory coatings:
[0076] Different aggregates for coatings can be selected depending on the material of the casting. Generally, for stainless steel and carbon steel castings, the aggregate is zircon powder; for cast iron castings, the aggregate is quartz powder; for high manganese steel castings, the aggregate is magnesia powder; and for other alloy steel castings, the aggregate is zircon powder (50%-60%), alumina powder (20-30%), and quartz powder (10-20%).
[0077] Raw material pretreatment: Weigh 60-70 parts of zircon powder from the refractory coating aggregate, and screen it through a 300-mesh sieve to remove impurities and larger particles; measure 20-25 parts of silica sol for later use; weigh 5-8 parts of binder (cholesterol carboxymethyl cellulose is selected) and grind it into fine powder; put 3-5 parts of nano alumina into a ball mill, set the ball milling speed to 300-400 r / min, and the ball milling time to 2-3 h to fully disperse it and avoid agglomeration; measure 2-4 parts of silicon carbide whiskers, put them into an ultrasonic cleaner, set the ultrasonic frequency to 40-60 kHz, and the ultrasonic time to 15-20 min to perform ultrasonic dispersion to improve its compatibility with other raw materials.
[0078] Mixing and stirring: Add the pretreated zircon powder, nano-alumina, and silicon carbide whiskers sequentially to the mixing vessel, turn on the stirrer, and stir at a speed of 200-300 r / min for 10-15 min to initially mix the three materials evenly. Then add the silica sol, increase the stirring speed to 400-500 r / min, and continue stirring for 20-30 min to allow the silica sol to fully coat the powder particles and form a relatively stable mixture system.
[0079] Adding binder: Slowly add the ground binder to the mixing tank while keeping the stirrer running at 300-400 r / min for 15-20 min to ensure that the binder is evenly dispersed in the coating system, so that the coating has good adhesion and coating performance.
[0080] Grinding and refining: Transfer the mixed coating to a grinder, add zirconia beads as grinding media, set the grinder speed to 600-800 r / min, and grind for 3-4 hours to further refine the coating particles, making the particle size distribution of the coating more uniform, and improving the fluidity and coating effect of the coating.
[0081] Performance Adjustment: The viscosity and specific gravity of the ground coating are tested. The viscosity is measured using a Forecast-4 cup. If the viscosity is not within the 18-25 second range, it can be adjusted by adding an appropriate amount of ethanol as a thinner or sodium carboxymethyl cellulose as a thickener. The specific gravity is measured using a hydrometer. If the specific gravity is not within the 1.8-2.2 g / cm³ range... 3 Within the specified range, adjustments can be made by adding zircon powder or silica sol until the coating performance meets the requirements.
[0082] Filtration and Packaging: Filter the adjusted paint through a 120-150 mesh filter to remove any impurities and lumps. Then, pack the paint into a sealed container and store it in a cool, dry place for later use.
[0083] 3. Mold coating
[0084] The prepared refractory coating was applied to the surface of the white mold using a combination of dip coating and spray coating. First, the white mold was completely immersed in the coating, ensuring full coverage. Then, the mold was removed and allowed to stand for 12 minutes to allow the coating to initially dry and penetrate. Next, the mold was sprayed with the coating using a spraying device to fill any gaps, ensuring a uniform coating thickness controlled within the range of 1.0-3.5 mm.
[0085] 4. Low-temperature demolding
[0086] The coated white mold is placed in an electric resistance furnace and heated under atmospheric pressure for demolding. The furnace temperature is increased to 250°C at a rate of 7°C / min. After reaching the target temperature, it is held at that temperature for 45 minutes to allow the EPS white mold to fully melt into a liquid, which is then recycled through a recycling device.
[0087] 5. Medium-temperature sintering mold
[0088] After demolding, the shell mold is transferred to a resistance heating furnace, and the furnace temperature is raised to 700℃. Sintering is carried out at this temperature for 7 hours to further solidify and densify the coating layer, forming a shell with sufficient strength and fire resistance.
[0089] 6. Pouring
[0090] The sintered mold is placed in a negative pressure molding chamber for molding according to the lost foam molding process. Then, a vacuum is drawn to achieve a vacuum level of -0.06 MPa in the negative pressure molding chamber. The molten metal is heated to 1550℃ and poured at a pouring rate of 3 kg / s.
[0091] 7. Casting cleaning and subsequent treatment
[0092] After pouring, the casting is kept at a constant temperature for 7 hours according to the characteristics of the casting material before being removed from the mold. The casting is then polished and cleaned using grinding equipment to remove excess material and impurities from the surface, resulting in a raw casting blank.
[0093] The present invention will be further described in detail below with reference to specific embodiments. It should be emphasized that the following description is merely exemplary and is not intended to limit the scope and application of the present invention.
[0094] II. Implementation Examples
[0095] Example 1
[0096] Mold making: High-precision machined aluminum molds are used, with an accuracy of ±0.05mm and a surface roughness Ra=1.5μm. The molds are equipped with uniform heating channels inside, and white molds are produced by foaming using these aluminum molds.
[0097] Refractory coating preparation: Following the above-described refractory coating preparation process, 60 parts zircon powder, 20 parts silica sol, 5 parts binder, 3 parts nano-alumina, and 2 parts silicon carbide whiskers were weighed for preparation. The final coating viscosity was 18 seconds (Ford cup 4), and the specific gravity was 1.8 g / cm³. 3 .
[0098] Mold coating: Dip the white mold surface once, let it stand for 10 minutes, and then spray it again, controlling the coating thickness to be 0.3mm.
[0099] Low-temperature demolding: Under atmospheric pressure, the temperature of the resistance furnace is raised to 200℃ at a heating rate of 5℃ / min, and the temperature is held for 30 minutes for demolding.
[0100] Medium-temperature sintering mold: Place the shell mold into a resistance heating furnace and sinter at 600℃ for 5 hours. Casting: Place the mold into a negative pressure molding box, set the vacuum degree to -0.05MPa, the metal liquid pouring temperature to 1500℃, and the pouring speed to 1kg / s.
[0101] Casting cleaning and subsequent treatment: After pouring, keep it warm for 5 hours before removing it from the mold and polishing it.
[0102] Example 2
[0103] Mold making: High-precision machined aluminum molds are used, with an accuracy of ±0.05mm and a surface roughness Ra=1.5μm. The molds are equipped with uniform heating channels inside, and white molds are produced by foaming using these aluminum molds.
[0104] Preparation of refractory coating: Weigh 70 parts zircon powder, 25 parts silica sol, 8 parts binder, 5 parts nano-alumina, and 4 parts silicon carbide whiskers to prepare the coating. The coating viscosity is 25 seconds (Ford cup 4), and the specific gravity is 2.2 g / cm³. 3 .
[0105] Mold coating: After dipping, let stand for 15 minutes before spraying. The coating thickness should be controlled at 1.0 mm.
[0106] Low-temperature demolding: Heat to 300℃ at a rate of 10℃ / min and hold for 60 minutes before demolding.
[0107] Medium-temperature sintering mold: sintered in a resistance heating furnace at 800℃ for 10 hours.
[0108] Pouring: Vacuum degree of negative pressure molding box -0.07MPa, pouring temperature of molten metal 1600℃, pouring speed 5kg / s.
[0109] Casting cleaning and subsequent treatment: After heat preservation for 10 hours, the casting is polished and cleaned.
[0110] Example 3
[0111] Mold making: The mold is made by manually cutting EPS boards and then using five-axis CNC machining. The mold is designed using topology optimization algorithm and repaired by laser cladding.
[0112] Preparation of refractory coating: Weigh out 63 parts zircon powder, 22 parts silica sol, 6 parts binder, 3.5 parts nano-alumina, and 2.5 parts silicon carbide whiskers. The coating viscosity is 20 seconds (Ford cup 4), and the specific gravity is 1.9 g / cm³. 3 .
[0113] Mold coating: Dip in and let stand for 12 minutes, then spray. The coating thickness is 0.6 mm.
[0114] Low-temperature demolding: heating rate 6℃ / min, temperature rises to 230℃, hold for 40min.
[0115] Medium-temperature sintering mold: sintered at 720℃ for 8 hours.
[0116] Casting: Vacuum degree -0.06MPa, casting temperature 1530℃, casting speed 2kg / s.
[0117] Casting cleaning and subsequent treatment: heat preservation for 6 hours before removal from the mold and grinding.
[0118] Example 4
[0119] Mold making: The mold is made by manually cutting EPS boards and then using five-axis CNC machining. The mold is designed using topology optimization algorithm and repaired by laser cladding.
[0120] Preparation of refractory coating: Weigh out 67 parts zircon powder, 23 parts silica sol, 7 parts binder, 4.5 parts nano-alumina, and 3.5 parts silicon carbide whiskers. The coating viscosity is 23 seconds (Ford cup 4), and the specific gravity is 2.1 g / cm³. 3 .
[0121] Mold coating: Dip in and let stand for 13 minutes, then spray. The coating thickness is 0.8 mm.
[0122] Low-temperature demolding: heating rate 8℃ / min, temperature rises to 270℃, hold for 50min.
[0123] Medium-temperature sintering mold: sintered at 780℃ for 9 hours.
[0124] Casting: Vacuum degree -0.065MPa, casting temperature 1570℃, casting speed 4kg / s.
[0125] Casting cleaning and subsequent treatment: heat preservation for 8 hours before removal from the mold and grinding.
[0126] Example 5
[0127] Mold making: High-precision machined aluminum molds are used, with an accuracy of ±0.05mm and a surface roughness Ra=1.5μm. The molds are equipped with uniform heating channels inside, and white molds are produced by foaming using these aluminum molds.
[0128] Preparation of refractory coating: Weigh 65 parts zircon powder, 22 parts silica sol, 6 parts binder, 4 parts nano-alumina, and 3 parts silicon carbide whiskers. The coating viscosity is 21 seconds (Ford cup 4), and the specific gravity is 2.0 g / cm³. 3 .
[0129] Mold coating: Dip in and let stand for 12 minutes, then spray. The coating thickness is 0.5 mm.
[0130] Low-temperature demolding: heating rate 7℃ / min, temperature rises to 250℃, hold for 45min.
[0131] Medium-temperature sintering mold: sinter at 700℃ for 7 hours.
[0132] Casting: Vacuum degree -0.06MPa, casting temperature 1550℃, casting speed 3kg / s.
[0133] Casting cleaning and subsequent treatment: heat preservation for 7 hours before removal from the mold and grinding.
[0134] III. Comparative Example
[0135] Comparative Example 1
[0136] Mold making: Ordinary precision aluminum mold is used, with an accuracy of ±0.15mm and a surface roughness Ra=3.2μm. There is no internal heating channel, and white mold is produced by foaming.
[0137] Mold coating: Uses conventional refractory coating (composed only of zircon powder, silica sol, and binder, without nano-alumina and silicon carbide whiskers), coating viscosity 20 seconds (Ford cup 4), specific gravity 1.9 g / cm³. 3 After dipping, let stand for 12 minutes before spraying, with a coating thickness of 0.6 mm.
[0138] Low-temperature demolding: Under atmospheric pressure, the temperature of the resistance furnace is raised to 250℃ at a heating rate of 7℃ / min, and the temperature is held for 45 minutes for demolding.
[0139] Medium-temperature sintering mold: Place the shell mold into a resistance heating furnace and sinter at 700℃ for 7 hours.
[0140] Casting: Place the mold into a negative pressure molding chamber, set the vacuum degree to -0.06MPa, the molten metal casting temperature to 1550℃, and the casting speed to 3kg / s.
[0141] Casting cleaning and subsequent treatment: After pouring, keep it warm for 7 hours before removing it from the mold and polishing it.
[0142] Comparative Example 2
[0143] Mold making: High-precision machined aluminum molds are used, with an accuracy of ±0.05mm and a surface roughness Ra=1.5μm. The molds are equipped with uniform heating channels inside, and white molds are produced by foaming using these aluminum molds.
[0144] Preparation of refractory coating: Weigh 65 parts zircon powder, 22 parts silica sol, and 6 parts binder. No nano-alumina or silicon carbide whiskers were added. Prepare the coating with a viscosity of 21 seconds (Ford cup 4) and a specific gravity of 2.0 g / cm³. 3 .
[0145] Mold coating: Dip in and let stand for 12 minutes, then spray. The coating thickness is 0.5 mm.
[0146] Low-temperature demolding: heating rate 7℃ / min, temperature rises to 250℃, hold for 45min.
[0147] Medium-temperature sintering mold: sinter at 700℃ for 7 hours.
[0148] Casting: Vacuum degree -0.06MPa, casting temperature 1550℃, casting speed 3kg / s.
[0149] Casting cleaning and subsequent treatment: heat preservation for 7 hours before removal from the mold and grinding.
[0150] Comparative Example 3
[0151] Mold making: High-precision machined aluminum molds are used, with an accuracy of ±0.05mm and a surface roughness Ra=1.5μm. The molds are equipped with uniform heating channels inside, and white molds are produced by foaming using these aluminum molds.
[0152] Preparation of refractory coating: Weigh 65 parts zircon powder, 22 parts silica sol, 6 parts binder, 4 parts nano-alumina, and 3 parts silicon carbide whiskers. The coating viscosity is 21 seconds (Ford cup 4), and the specific gravity is 2.0 g / cm³. 3 .
[0153] Mold coating: Dip in and let stand for 12 minutes, then spray. The coating thickness is 0.5 mm.
[0154] Low-temperature demolding: Under atmospheric pressure, the temperature of the resistance furnace is raised to 350°C at a heating rate of 15°C / min, and the temperature is held for 20 minutes for demolding (the heating rate and temperature are beyond the scope of this invention).
[0155] Medium-temperature sintering mold: Place the shell mold in a resistance heating furnace and sinter at 700℃ for 7 hours. Casting: Place the mold in a negative pressure molding chamber, set the vacuum degree to -0.06MPa, the molten metal casting temperature to 1550℃, and the casting speed to 3kg / s.
[0156] Casting cleaning and subsequent treatment: After pouring, keep it warm for 7 hours before removing it from the mold and polishing it.
[0157] IV. Comprehensive Analysis of Examples and Comparative Examples and Determination of Optimal Results
[0158] Group Surface roughness Ra (μm) of casting Shell compressive strength (MPa) EPS recovery rate (%) Porosity of castings (%) Incomplete casting defect rate (%) Example 1 2.0 18.2 80.6 3.3 4.1 Example 2 1.9 20.6 82.3 3.0 3.6 Example 3 2.2 19.3 81.5 4.2 4.3 Example 4 2.1 21.2 83.9 3.6 3.5 Example 5 1.8 22.5 85.7 2.8 3.7 Comparative Example 1 3.0 15.2 70.3 8.9 10.7 Comparative Example 2 2.5 16.6 75.1 6.4 8.6 Comparative Example 3 2.8 17.8 72.5 7.6 9.1
[0159] The data clearly shows that Example 5 achieved optimal performance across multiple key indicators:
[0160] Surface quality: The surface roughness Ra of the casting is as low as 1.8μm, which is smoother than other embodiments and comparative examples, and can better meet the requirements of high-precision castings.
[0161] Structural strength: The shell mold has a compressive strength of 22.5 MPa, which is the highest among all groups. It can better maintain shape stability during the casting process and reduce casting defects caused by insufficient shell mold strength.
[0162] Material recycling: EPS recycling rate is as high as 85.7%, which ensures demolding effect while achieving efficient material recycling, reducing production costs and resource waste.
[0163] Molding quality: The porosity and incomplete filling defect rates of the castings were 2.8% and 3.7% respectively, which are at a low level, indicating that the combination of process parameters in Example 5 can effectively ensure the molding quality of the castings.
[0164] Based on the above analysis, Example 5 demonstrates the best performance across all performance indicators and can be identified as the optimal experimental result. Its combination of process parameters provides a reliable reference for subsequent single-factor experiments, facilitating a deeper investigation into the impact of each key parameter on process performance. Figure 1 A physical image of the shell of a stainless steel impeller for the chemical industry manufactured using Example 5 as the technical solution; Figure 2 This is a mold drawing for stainless steel impellers used in the chemical industry.
[0165] V. Single-factor experiment
[0166] (I) Effect of nano-alumina addition on shell-shaped properties in refractory coatings
[0167] Experimental group Amount of nano-alumina added (parts) Coating density (%) Shell-type erosion resistance (rating, 1-10 points) Surface roughness Ra (μm) of casting 1 1 82.2 4 3.0 2 3 88.5 6 2.2 3 4 (Example 5) 92.2 8 1.8 4 5 90.1 7 2.0
[0168] Conclusion: When the amount of nano-alumina added is less than 4 parts, the coating has many internal pores, low density, and poor erosion resistance, failing to effectively resist the erosion of molten metal, resulting in a rough surface of the casting. When the amount added is greater than 4 parts, the nano-alumina is prone to agglomeration, which destroys the uniformity and structural stability of the coating, reduces density and erosion resistance, and degrades the surface quality of the casting. Conclusion: When the amount of nano-alumina added is 4 parts, the coating has the best density and erosion resistance, resulting in the best surface quality of the casting.
[0169] (II) The effect of low-temperature demolding heating rate on EPS recycling quality
[0170] Experimental group Heating rate (°C / min) EPS recovery rate (%) Carbonization rate of recycled EPS (%) Recyclable EPS reuse rate (%) 1 3 75.3 3.6 65.4 2 7 (Example 5) 85.2 1.3 85.6 3 12 80.8 5.4 70.3 4 15 70.4 8.3 55.5
[0171] Conclusion and Analysis: When the heating rate is less than 7℃ / min, the EPS melts too slowly. Some EPS reacts with oxygen in the air during prolonged heating, leading to increased carbonization and decreased recovery and reusability. When the heating rate is greater than 7℃ / min, the EPS heats up rapidly, and the internal heat cannot be dissipated in time, resulting in localized overheating and significant carbonization, severely impacting recycling quality and reusability. Conclusion: A low-temperature demolding heating rate of 7℃ / min results in high EPS recovery and low carbonization, with optimal reusability of the recycled material.
[0172] (III) Effect of medium-temperature sintering temperature on shell strength
[0173] Experimental group Medium-temperature sintering temperature (°C) Shell compressive strength (MPa) Shell cracking rate (%) 1 550 12.3 15.3 2 650 18.5 8.4 3 700 (Example 5) 22.6 2.6 4 850 16.8 12.1
[0174] Conclusion and Analysis: When the sintering temperature is below 700℃, the components in the coating layer fail to undergo sufficient chemical reactions and physical changes, resulting in an insufficiently strong structure and low compressive strength of the shell, making it prone to cracking. When the sintering temperature is above 700℃, the excessively high temperature will generate thermal stress inside the shell, and some components may decompose or volatilize, damaging the shell structure, reducing compressive strength, and increasing the risk of cracking. Conclusion: At a medium-temperature sintering temperature of 700℃, the shell exhibits the highest compressive strength and the lowest cracking rate, demonstrating the best structural stability.
[0175] (iv) The influence of vacuum degree of negative pressure molding box on casting quality
[0176] Experimental group Vacuum degree (MPa) Incomplete casting defect rate (%) Porosity of castings (%) 1 -0.03 12.7 8.5 2 -0.06 (Example 5) 3.6 2.7 3 -0.09 2.8 5.6 4 -0.10 2.1 6.2
[0177] Conclusion and Analysis: When the vacuum degree is less than -0.06 MPa, the molten metal has insufficient fluidity within the negative pressure molding box, failing to fully fill the mold cavity, leading to an increased incomplete filling defect rate. Simultaneously, insufficient gas removal increases porosity. When the vacuum degree is greater than -0.06 MPa, the excessively high vacuum causes the molten metal to flow too quickly, easily entrapping gas, increasing porosity, and may also cause molten metal splashing, affecting the casting quality. Conclusion: When the vacuum degree of the negative pressure molding box is -0.06 MPa, the incomplete filling defect rate and porosity of the casting are lowest, resulting in the best casting quality.
[0178] VI. Summary of Single-Factor Experimental Analysis
[0179] Single-factor experiments systematically revealed the influence of key process parameters on the performance of high-precision casting shells produced by lost foam casting. In the field of refractory coatings, the amount of nano-alumina added directly affects the coating's density and erosion resistance; 4 parts is the optimal addition amount. Below this value, it cannot effectively fill pores and improve density, while above this value, it is prone to agglomeration and structural damage. In the low-temperature demolding process, a heating rate of 7℃ / min can achieve efficient EPS recovery. Too slow a rate leads to oxidation and carbonization, while too fast a rate causes local overheating and carbonization. When the medium-temperature sintering temperature is 700℃, the shell can form the best structure, with the highest strength and the lowest risk of cracking. When the vacuum degree of the negative pressure molding box is -0.06MPa and the pouring speed is 3kg / s, it can ensure good filling of molten metal and uniform casting structure, respectively. Deviation from these parameters can easily lead to defects such as incomplete filling, porosity, and shrinkage.
[0180] VII. Significant Progressiveness of the Invention
[0181] This invention achieves a comprehensive technological upgrade through innovative improvements and parameter optimization in each process step of lost foam casting for high-precision casting shell molds. In terms of material utilization, the novel refractory coating formula and low-temperature demolding process improve the quality and utilization rate of EPS recycling, reducing resource waste and environmental pollution. Regarding process control, precise settings for parameters such as temperature, speed, and vacuum ensure shell mold quality and casting accuracy. In terms of product performance, it effectively reduces casting surface roughness, improves shell mold strength and internal casting quality, and reduces defect rates. Compared to traditional technologies and comparative examples, this invention achieves breakthroughs in casting quality, production efficiency, resource utilization, and environmental performance, possessing outstanding substantive features and significant progress, and has important industrial application value and broad market prospects.
[0182] The above description, in conjunction with preferred embodiments, provides a further detailed explanation of the present invention and should not be construed as limiting the specific implementation of the invention to these descriptions. For those skilled in the art, various substitutions or modifications can be made to these described embodiments without departing from the inventive concept, and all such substitutions or modifications should be considered within the scope of protection of the present invention.
[0183] Although the invention and its advantages have been described in detail, it should be understood that various changes, substitutions, and modifications can be made without departing from the spirit and scope of the invention. Furthermore, the scope of the invention is not limited to the specific embodiments of the processes, manufactures, compositions of matter, methods, and steps described in the specification. From the disclosure of this invention, those skilled in the art will readily utilize existing or future processes, manufactures, compositions of matter, methods, or steps that substantially perform the same function or achieve the same results as the corresponding embodiments described herein. Therefore, the appended claims are intended to encompass such processes, manufactures, compositions of matter, methods, or steps.
Claims
1. A method for preparing high-precision casting shell molds using lost foam casting, characterized in that, Includes the following steps: (1) Mold making: EPS material is used to make molds, and aluminum molds are made to produce white molds through foaming. (2) Mold coating: Apply refractory coating to the surface of the white mold; (3) Low-temperature demolding: The white mold after being coated is placed in a resistance furnace and heated to melt the EPS white mold into a liquid and then recycled through a recycling device; (4) Medium-temperature sintering mold: Place the demolded shell mold into a resistance heating furnace for sintering; (5) Casting: The sintered mold is placed in a negative pressure molding box according to the lost foam molding process, and the molten metal is poured in under negative pressure. (6) Casting cleaning and subsequent treatment: After pouring, the casting is kept warm and then removed from the mold. It is then polished and cleaned to obtain the casting blank.
2. The preparation method according to claim 1, characterized in that, The aluminum mold is manufactured with a precision of ±0.05mm and a surface roughness Ra≤1.6μm. The interior of the aluminum mold is provided with uniformly distributed heating channels.
3. The preparation method according to claim 1, characterized in that, The coating thickness is 1.0-3.5 mm.
4. The preparation method according to claim 1, characterized in that, The coating is applied using a combination of dip coating and spray coating. First, dip coating is applied once, and after standing for 10-15 minutes, spray coating is applied again.
5. The preparation method according to claim 1, characterized in that, The low-temperature demolding state is within the temperature range of 200-300℃ under atmospheric pressure.
6. The preparation method according to claim 1, characterized in that, The heating rate for low-temperature demolding is 5-10℃ / min.
7. The preparation method according to claim 1, characterized in that, The heat preservation time for low-temperature demolding is 30-60 minutes.
8. The preparation method according to claim 1, characterized in that, The sintering conditions are sintering at a temperature range of 600-800℃ for 5-10 hours.
9. The preparation method according to claim 1, characterized in that, The vacuum degree of the negative pressure molding box is -0.05 to -0.07 MPa, the metal liquid pouring temperature is 1500-1600℃, and the pouring speed is 1-5 kg / s.
10. The preparation method according to claim 1, characterized in that, The heat preservation time is 5-10 hours depending on the material requirements of the casting before it is removed from the mold.