Method for efficiently improving wear resistance of Cr12MoV steel

By treating Cr12MoV steel with scanning electron beam surface modification technology, the problem of insufficient wear resistance of mold steel was solved, and its wear resistance and surface properties were significantly improved.

CN121653316APending Publication Date: 2026-03-13GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411267113.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2026-03-13

AI Technical Summary

Technical Problem

Cr12MoV mold steel is prone to wear and fatigue failure in working environments, and existing technologies are unable to effectively improve its wear resistance.

Method used

Scanning electron beam surface modification technology was used to pretreat Cr12MoV steel workpieces to remove surface impurities and oil stains. Electron beam treatment was then performed in a vacuum environment with the following parameters: electron beam accelerating voltage 60kV, focusing current 390mA, scanning frequency 300Hz, moving speed 6mm/s, and electron beam current 10-14mA. This process formed a hardened layer to improve wear resistance.

Benefits of technology

It significantly improved the wear resistance of Cr12MoV steel, reducing the wear amount from 0.036 mm3 to 0.011-0.016 mm3, and changing the wear mechanism from adhesive wear to abrasive wear, thus improving the wear resistance of the material surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a method for improving the wear resistance of Cr12MoV steel. The method comprises the following steps: (1) pretreatment: cleaning the surface of a milled workpiece by using an absolute ethyl alcohol solvent; (2) drying treatment is conducted, specifically, the pretreated workpiece is placed in a drying box and heated to 50-65 DEG C, and the dried workpiece is obtained; and (3) scanning electron beam processing. The process adopted by the invention can quickly and remarkably improve the wear resistance of the Cr12MoV steel, and has wide market popularization value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-energy beam surface modification technology for cold work die steel, and specifically relates to a method for efficiently improving the wear resistance of Cr12MoV steel. Background Technology

[0002] Cr12MoV steel is a widely used Cr12 type high-carbon, high-chromium ledeburitic cold work die steel both domestically and internationally. Its characteristics include high hardness, good wear resistance, and hardenability, making it suitable for manufacturing various complex-shaped cold work dies that can withstand significant impact loads, such as cold-cutting shears, cold extrusion dies, and wire drawing dies. It is currently widely used in the automotive, shipbuilding, railway, and aerospace industries. However, Cr12MoV die steel often endures significant impact, extrusion, and external friction in its working environment, making it prone to wear and fatigue failure modes. Improving the surface wear resistance of die steel has become a current focus. Therefore, efficient surface modification techniques are employed to enhance the wear resistance of Cr12MoV steel.

[0003] Electron beam surface modification is a novel technology that uses an electron beam device to treat the surface of materials. Under high vacuum conditions, an electron beam device bombards the workpiece surface with electrons, causing the surface to rapidly heat up to the micrometer level and melt. Since the substrate is still in a cold state, the heat generated by the electron beam bombardment rapidly diffuses into the substrate structure, creating a large supercooling between the melt and the substrate. This alters the chemical composition and microstructure of the material surface, thereby improving its surface properties. Summary of the Invention

[0004] This invention provides a highly efficient method for processing Cr12MoV steel. The method involves pre-treating the Cr12MoV steel workpiece to remove surface impurities and oil stains; then, it is processed by scanning electron beam to produce the finished product. The process employed in this invention can significantly improve the wear resistance of Cr12MoV steel and has broad market potential.

[0005] Includes the following steps: Step 1: Pretreatment. The original test block is cut and milled to a uniform size of 50mm×50mm×16mm cube. The milled surface is cleaned with anhydrous ethanol solvent to remove oil and impurities from the material surface. Then, the surface of the test piece is dried with a dryer to prevent rusting.

[0006] Proceed to step 2 after step 1 is completed; Step 2: Before scanning electron beam treatment, place the cleaned workpiece on the support block inside the scanning electron beam apparatus chamber. Then, use a molecular pump to evacuate the processing chamber and an ion pump to evacuate the electron gun chamber, ensuring that the vacuum level in both chambers reaches 10. -3Pa. Then, the parameters of the CNC control console of the electron beam welding machine need to be set. Under the conditions of electron beam accelerating voltage of 60kV, electron beam focusing current of 390mA, electron beam scanning frequency of 300Hz, electron gun moving speed of 6mm / s, scanning ring diameter of 6mm, and electron beam current of 10mA, 12mA or 14mA, an electron beam experiment is carried out to obtain the finished product.

[0007] Step 2: Proceed to Step 3 after completion; Step 3: Performance testing. The images after wear were observed using a ZEISS Gemini SEM 300 scanning electron microscope. The wear resistance was tested using a CFT-I material surface performance comprehensive tester with a load of 30 N, a reciprocating length of 4 mm, and a wear time of 30 min. The surface profile of the worn sample was also tested using the CFT-I material surface performance comprehensive tester to measure the amount of wear.

[0008] 2. A method for improving the wear resistance of Cr12MoV steel according to claim 1, characterized in that: step 1, the pretreatment, includes milling the outer surface of the Cr12MoV steel using a CNC milling machine to cut the workpiece into uniform cubic test blocks. During the milling of the outer surface and the cutting process, it is ensured that the feed rate of each workpiece is consistent and the milling speed is the same, ultimately obtaining the milled workpiece.

[0009] 3. The scanning electron beam surface treatment process for Cr12MoV steel according to claim 1, characterized in that: the cleaning agent in step 1 is mainly composed of alcohol-based organic solvents.

[0010] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention employs a scanning electron beam (SEM) method to treat the surface of Cr12MoV steel, rapidly improving its wear resistance. By using the SEM method, the metal surface can quickly reach its melting point, and then, as the SEM torch moves, the surface rapidly cools. This rapid heating and cooling process generates significant supercooling, forming a hardened layer on the workpiece surface, thereby significantly improving wear resistance.

[0011] 2. The entire process of scanning electron beam treatment of Cr12MoV steel surface involved in this invention is carried out in a vacuum environment. Therefore, it effectively isolates the influence of air and other impurities on the material surface, preventing oxidation reactions on the Cr12MoV steel surface and ensuring that other elements do not participate in the reaction. Simultaneously, the electron bombardment surface treatment has high energy transfer efficiency, allowing for rapid completion and improving work efficiency.

[0012] 3. The Cr12MoV steel specimen prepared according to this invention was tested for 30 minutes under a 30N load with a reciprocating length of 3 mm. The initial wear was 0.036 mm. 3 After being scanned by an electron beam, the wear amount was only 0.011 mm. 3 The wear amount was significantly reduced compared to the test block that was not treated with scanning electron beam. Attached Figure Description

[0013] Figure 1 The width of the wear mark before electron beam treatment; Figure 2 The wear mark contour line before electron beam heat treatment; Figure 3 The wear mark width when using an electron beam current of 10mA; Figure 4 The wear track contour when using an electron beam current of 10mA; Figure 5 The wear mark width when using an electron beam current of 12mA; Figure 6 The wear track contour when using an electron beam current of 12mA; Figure 7 The wear mark width when using an electron beam current of 14mA; Figure 8 The wear track contour when using an electron beam current of 14mA; Figure 9 Comparison of wear amounts of Cr12MoV steel after treatment with different electron beam currents; Detailed Implementation

[0014] The following are specific implementation methods of the present invention. The solutions of the present invention will be further described with reference to the accompanying drawings, but the present invention is not limited to these implementation methods.

[0015] Step 1: Pretreatment. After turning, the Cr12MoV steel test block is cut into 50mm×50mm×16mm specimens. Then, the specimens are cleaned with alcohol-based organic solvents to remove impurities and oil stains from the surface of the test block.

[0016] Proceed to step 2 after step 1 is completed; Step 2: Scanning Electron Beam Treatment. Before scanning electron beam treatment, the cleaned workpiece is placed on a support block in the working chamber of the scanning electron beam surface modification device. Then, a molecular pump is used to evacuate the processing chamber and an ion pump to evacuate the electron gun chamber, ensuring that the vacuum level in both chambers reaches 10⁻³ Pa. Next, the parameters of the CNC control console of the electron beam welding machine are set. Electron beam experiments are conducted under the following conditions: electron beam accelerating voltage of 60 kV, electron beam focusing current of 390 mA, electron beam scanning frequency of 300 Hz, electron gun moving speed of 6 mm / s, scanning ring diameter of 6 mm, and electron beam current of 10 mA. The wear measurement after 30 minutes is 0.021 mm. 3 The finished product.

[0017] Step 1: Pretreatment. After turning, the Cr12MoV steel test block is cut into 50mm×50mm×16mm specimens. Then, the specimens are cleaned with alcohol-based organic solvents to remove impurities and oil stains from the surface of the test block.

[0018] Proceed to step 2 after step 1 is completed; Step 2: Scanning Electron Beam Treatment. Before scanning electron beam treatment, the cleaned workpiece is placed on a support block inside the scanning electron beam surface modification device chamber. Then, a molecular pump is used to evacuate the processing chamber and an ion pump to evacuate the electron gun chamber, ensuring that the vacuum level in both the processing chamber and the electron gun chamber reaches 10. -3 Pa. Then, the parameters of the CNC control console of the electron beam welding machine need to be set. An electron beam experiment was conducted under the following conditions: electron beam accelerating voltage of 60kV, electron beam focusing current of 390mA, electron beam scanning frequency of 300Hz, electron gun moving speed of 6mm / s, scanning ring diameter of 6mm, and electron beam current of 12mA. The wear measurement after 30 minutes was 0.011 mm. 3 The finished product.

[0019] Step 1: Pretreatment. After turning, the Cr12MoV steel test block is cut into 50mm×50mm×16mm specimens. Then, the specimens are cleaned with alcohol-based organic solvents to remove impurities and oil stains from the surface of the test block.

[0020] Proceed to step 2 after step 1 is completed; Step 2: Scanning Electron Beam Treatment. Before scanning electron beam treatment, the cleaned workpiece is placed on a support block inside the scanning electron beam surface modification device chamber. Then, a molecular pump is used to evacuate the processing chamber and an ion pump to evacuate the electron gun chamber, ensuring that the vacuum level in both the processing chamber and the electron gun chamber reaches 10. -3Pa. Then, the parameters of the CNC control console of the electron beam welding machine need to be set. An electron beam experiment was conducted under the following conditions: electron beam acceleration voltage of 60kV, electron beam focusing current of 390mA, electron beam scanning frequency of 300Hz, electron gun moving speed of 6mm / s, scanning ring diameter of 6mm, and electron beam current of 14mA. The wear measurement after 30 minutes was 0.016 mm. 3 The finished product.

[0021] Wear resistance test: Friction and wear test was carried out on the surface of Cr12MoV steel in specific implementation examples 1-3 and before treatment. The friction and wear parameters were: load 30N; time 30min; wear track length 4mm; and Si3N4 steel ball.

[0022] From the appendix Figure 1-8 As can be seen, the Cr12MoV steel matrix exhibits numerous grooves, spalling pits, and fragments after wear. However, after electron beam treatment, the surface becomes smoother, and the wear mechanism changes from adhesive wear to abrasive wear. (From the attached...) Figure 9 As can be seen from the data, electron beam treatment can effectively reduce the surface wear rate of Cr12MoV steel and significantly improve its wear resistance.

[0023] The above description is a detailed description of the preferred embodiments of the present invention. However, the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modifications made under the technical spirit of the present invention should fall within the patent scope covered by the present invention.

Claims

1. A method for efficiently improving the wear resistance of Cr12MoV steel, comprising the following steps: Step 1: Pretreatment. The original test block is cut and milled to a uniform size of 50mm×50mm×16mm cube. The milled surface is cleaned with anhydrous ethanol solvent to remove oil and impurities from the material surface. Then, the surface of the test piece is dried with a dryer to prevent rusting.

2. Proceed to step 2 after step 1 is completed; Step 2: Before scanning electron beam treatment, place the cleaned workpiece on the support block inside the scanning electron beam apparatus chamber. Then, use a molecular pump to evacuate the processing chamber and an ion pump to evacuate the electron gun chamber, ensuring that the vacuum level in both chambers reaches 10⁻³ Pa. Next, set the parameters of the CNC control console of the electron beam welding machine. Conduct electron beam experiments under the following conditions: electron beam accelerating voltage of 60 kV, electron beam focusing current of 390 mA, electron beam scanning frequency of 300 Hz, electron gun moving speed of 6 mm / s, scanning ring diameter of 6 mm, and electron beam current of 10 mA, 12 mA, or 14 mA, to obtain the finished product.

3. Step 2: Proceed to Step 3 after completion; Step 3: Performance testing. The images after wear were observed using a ZEISS Gemini SEM 300 scanning electron microscope. The wear resistance was tested using a CFT-I material surface performance comprehensive tester with a load of 30 N, a reciprocating length of 4 mm, and a wear time of 30 min. The surface profile of the worn sample was also tested using the CFT-I material surface performance comprehensive tester to measure the amount of wear.

4. The method for improving the wear resistance of Cr12MoV steel according to claim 1, characterized in that: Step 1, pretreatment, involves using a CNC milling machine to mill the outer surface of Cr12MoV steel, cutting the workpiece into uniform cubic test blocks. During the milling and cutting process, it is ensured that the feed rate and milling speed are consistent for each workpiece, ultimately yielding the milled workpiece.

5. The scanning electron beam surface treatment method for Cr12MoV steel according to claim 1, characterized in that: the cleaning agent in step 1 is mainly composed of alcohol-based organic solvents.

6. Compared with the prior art, the present invention has the following beneficial effects: This invention employs a scanning electron beam (SEM) method to treat the surface of Cr12MoV steel, rapidly improving its wear resistance. By using the SEM method, the metal surface can quickly reach its melting point, and then, as the SEM torch moves, the surface rapidly cools. This rapid heating and cooling process generates significant supercooling, forming a hardened layer on the workpiece surface, thereby significantly improving wear resistance.

7. The entire process of scanning electron beam treatment of Cr12MoV steel surface involved in this invention is carried out in a vacuum environment. Therefore, it effectively isolates the influence of air and other impurities on the material surface, preventing oxidation reactions on the Cr12MoV steel surface and ensuring that other elements do not participate in the reaction. Simultaneously, the electron bombardment surface treatment has high energy transfer efficiency, allowing for rapid completion and improving work efficiency.

8. The Cr12MoV steel specimen prepared according to this invention was tested for 30 minutes under a 30N load with a reciprocating length of 3 mm. The initial wear was 0.036 mm. 3 After being scanned by an electron beam, the wear amount was only 0.011 mm. 3 The wear amount was significantly reduced compared to the test block that was not treated with scanning electron beam.