Water-based finish paint with high toughness and high hardness as well as preparation method and application of water-based finish paint
By using a specific ratio of water-based topcoat components and roller coating process, the contradiction between high toughness and high hardness of metal color-coated sheets is resolved, achieving environmentally friendly and efficient coating applications suitable for home appliances, furniture, elevator decoration, and other fields.
Patent Information
- Application Number
- CN202610187865.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-09
- Publication Date
- 2026-04-03
AI Technical Summary
Existing technologies cannot simultaneously achieve the high toughness and high hardness of metal color-coated sheets, and oil-based coatings pose environmental and safety hazards.
A water-based topcoat with a specific ratio of components, including water-based resin, amino resin, silver powder, film-forming aid, crosslinking agent, nano-ceramic powder, coupling agent and deionized water, is applied to the surface of galvanized or stainless steel coils using a roller coating process to form a high-toughness and high-hardness coating.
It achieves a balance between high toughness and high hardness, reduces VOC content, complies with RoHS environmental standards, improves production safety and efficiency, and reduces production costs.
Smart Images

Figure CN121779992A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water-based topcoat technology, specifically to a water-based topcoat with both high toughness and high hardness, its preparation method, and its application. Background Technology
[0002] Metal color-coated steel sheets are composite materials made by coating an organic coating onto the surface of a substrate and then baking it. They are widely used in the home appliance manufacturing industry due to their good decorative properties, corrosion resistance, and ease of processing. Currently, the mainstream technical solutions in this field mainly face the following challenges: Firstly, regarding coating performance, existing technologies struggle to balance the processing toughness and operational hardness required for color-coated steel sheets. Appliance casings undergo deep processing such as stamping and bending during manufacturing, demanding extremely high coating toughness to prevent cracking or paint peeling. Simultaneously, as exterior components, the finished product requires extremely high surface hardness to resist scratches during daily use. However, in materials science, coating toughness and hardness often exhibit a contradictory relationship of mutual restraint.
[0003] In addition, the currently dominant oil-based coating system contains a large amount of toxic, harmful, volatile, and irritating substances such as ethyl acetate and xylene, which affect the health of employees, are detrimental to environmental protection and VOC reduction at the front end, and pose risks of flammability and explosion in all aspects of transportation, storage, and use. Therefore, there is an urgent need in this field for a coating that can achieve a perfect balance between high toughness and high hardness, and is also environmentally friendly and safe. Summary of the Invention
[0004] In view of the aforementioned problems, this application is made to provide a water-based topcoat with both high toughness and high hardness, a method for preparing the same, and its application, which overcome or at least partially solve the aforementioned problems, comprising: A water-based topcoat that combines high toughness and high hardness, comprising the following components by weight percentage: Water-based resin 45-55%; Amino resin 5-7%; Silver powder 3-6%; Film-forming aids 2-6%; Crosslinking agent 2-3%; 1-5% nano-ceramic powder; Coupling agent 0.3-2%; Deionized water 13-30%; Additives: 0.6-2.4%.
[0005] Preferably, the waterborne resin is a waterborne acrylic resin or a silicone-modified acrylic resin.
[0006] Preferably, the film-forming aid is diethylene glycol butyl ether, propylene glycol butyl ether, or dimethylaminoethanol.
[0007] Preferably, the crosslinking agent is an epoxy phosphate ester and / or an aqueous blocked isocyanate crosslinking agent.
[0008] Preferably, the coupling agent is a titanate silane coupling agent.
[0009] Preferably, the additive comprises the following components by weight percentage: Neutralizing agent 0.1-0.7%; Drying agent 0.1-0.3%; Leveling agent 0.1-0.5%; Defoamer 0.3-0.9%.
[0010] A method for preparing a water-based topcoat with both high toughness and high hardness as described above includes the following steps: Preparation of nano-ceramic slurry; The water-based resin, the amino resin, the silver powder, the film-forming aid, the crosslinking agent, the coupling agent, and the additives are added according to the specified ratio, and finally the nano-ceramic slurry is added to obtain the target finished water-based topcoat.
[0011] Preferably, the step of preparing the nano-ceramic slurry includes: The nano-ceramic powder is ground and dispersed. Add an appropriate amount of water and dispersant to the resin, add the nano-ceramic powder during stirring, and grind to obtain the nano-ceramic slurry.
[0012] An application of the water-based topcoat as described above, wherein the application is the processing of the water-based topcoat on the surface of galvanized or stainless steel coils.
[0013] Preferably, the water-based topcoat of a specified viscosity is applied to the surface of the galvanized coil or stainless steel coil by roller coating, followed by high-temperature baking and cooling to obtain the target color-coated sheet.
[0014] This application has the following advantages: In the embodiments of this application, addressing the problem that existing water-based topcoats cannot simultaneously achieve both toughness and hardness, and are also environmentally unfriendly, this application provides a solution for a water-based topcoat that combines high toughness and high hardness. Specifically, it consists of the following components by weight percentage: 45-55% water-based resin; 5-7% amino resin; 3-6% silver powder; 2-6% film-forming aid; 2-3% crosslinking agent; 1-5% nano-ceramic powder; 0.3-2% coupling agent; 13-30% deionized water; and 0.6-2.4% additives. This water-based topcoat, with its specific components and proportions, enables the product to simultaneously possess both 0T and 4H properties. Compared to oil-based coatings, water-based coatings are more "green, environmentally friendly, healthy, and safe." The product complies with RoHS technical standards, reduces VOC content, and decreases the composition of toxic and harmful substances in the coating, providing a healthy and safe environment for the production, transportation, storage, and use of coatings and metal coils. Attached Figure Description
[0015] To more clearly illustrate the technical solution of this application, the drawings used in the description of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0016] Figure 1 This is a flowchart illustrating the steps of a method for preparing a water-based topcoat that combines high toughness and high hardness, according to an embodiment of this application. Detailed Implementation
[0017] To make the objectives, features, and advantages of this application more apparent and understandable, the application will be further described in detail below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.
[0018] The inventors, through analysis of existing technologies, discovered that for stainless steel substrates, current oil-based coating systems often cannot simultaneously satisfy both high toughness and high hardness. For galvanized substrates, a two-coat process of "primer first, then topcoat" is commonly used to achieve basic adhesion and processability. Attempts to simplify this to a single-coat process using oil-based coatings generally result in poor adhesion and insufficient bending performance, failing to achieve both 0T and 4H properties. This performance contradiction directly leads to low yield rates during production and quality defects in finished appliance casings, such as paint chipping or surface scratches.
[0019] An embodiment of this application provides a water-based topcoat that combines high toughness and high hardness, which, by weight percentage, consists of the following components: Water-based resin 45-55%; Amino resin 5-7%; Silver powder 3-6%; Film-forming aids 2-6%; Crosslinking agent 2-3%; 1-5% nano-ceramic powder; Coupling agent 0.3-2%; Deionized water 13-30%; Additives: 0.6-2.4%.
[0020] In the embodiments of this application, addressing the problem that existing water-based topcoats cannot simultaneously achieve both toughness and hardness, and are also environmentally unfriendly, this application provides a solution for a water-based topcoat that combines high toughness and high hardness. Specifically, it consists of the following components by weight percentage: 45-55% water-based resin; 5-7% amino resin; 3-6% silver powder; 2-6% film-forming aid; 2-3% crosslinking agent; 1-5% nano-ceramic powder; 0.3-2% coupling agent; 13-30% deionized water; and 0.6-2.4% additives. This water-based topcoat, with its specific components and proportions, enables the product to simultaneously possess both 0T and 4H properties. Compared to oil-based coatings, water-based coatings are more "green, environmentally friendly, healthy, and safe." The product complies with RoHS technical standards, reduces VOC content, and decreases the composition of toxic and harmful substances in the coating, providing a healthy and safe environment for the production, transportation, storage, and use of coatings and metal coils.
[0021] The following will further describe a water-based topcoat that combines high toughness and high hardness in this exemplary embodiment.
[0022] In this embodiment, the aqueous resin is an aqueous acrylic resin.
[0023] It should be noted that during the high-temperature baking process, the functional groups of the amino resin and the acrylic resin undergo a cross-linking reaction, which connects the linear resin molecules into a dense three-dimensional network structure. Furthermore, this invention introduces nano-ceramic powder into the formulation, which enhances the flexibility of the coating while increasing surface hardness, raising the pencil hardness from 2H to 4H. This invention also adds a titanate silane coupling agent to the formulation; under high-temperature baking conditions, the titanate silane coupling agent cross-links with the acrylic resin, improving the adhesion between the coating and the substrate and effectively preventing paint peeling during bending.
[0024] As an example, the waterborne resin is a waterborne acrylic resin or a silicone-modified acrylic resin. The waterborne acrylic resin can be waterborne acrylic resin 8700 or Youwo 1701 acrylic resin; the silicone-modified acrylic resin can be 1703 silicone-modified acrylic resin.
[0025] In one specific implementation, the waterborne acrylic resin selected is waterborne acrylic resin 8700, and the amino resin selected is fully etherified and semi-etherified amino resin 303.
[0026] In this embodiment, the film-forming aid is diethylene glycol butyl ether, propylene glycol butyl ether, or dimethylaminoethanol. During the drying and baking process of the water-based coating, the film-forming aid helps the acrylic resin particles to deform and fuse better, forming a continuous, dense, and smooth paint film. Diethylene glycol butyl ether is preferred as the film-forming aid.
[0027] In this embodiment, the crosslinking agent is an epoxy phosphate ester and / or a water-based blocked isocyanate crosslinking agent. The epoxy groups of the epoxy phosphate ester participate in the crosslinking reaction of the resin system, further enhancing the overall density and chemical stability of the coating.
[0028] As an example, water-based blocked isocyanate crosslinking agents such as BI-200, 9500A, Youwo 8224, or Youwo 8220 can be selected.
[0029] In this embodiment, the additive is composed of the following components by weight percentage: Neutralizing agent 0.1-0.7%; Drying agent 0.1-0.3%; Leveling agent 0.1-0.5%; Defoamer 0.3-0.9%.
[0030] As an example, a polyester leveling agent can be selected, and a silicone oil or vegetable oil can be selected as the defoamer.
[0031] Reference Figure 1 This application illustrates a method for preparing a water-based topcoat with both high toughness and high hardness according to an embodiment of the present application, including the following steps: S110, Preparation of nano-ceramic slurry; S120. Add the water-based resin, the amino resin, the silver powder, the film-forming aid, the crosslinking agent, the coupling agent, and the additives according to the specified ratio, and finally add the nano-ceramic slurry to obtain the target finished water-based topcoat.
[0032] In one embodiment of the present invention, the specific process of "preparing nano-ceramic slurry" in step S110 can be further described in conjunction with the following description.
[0033] The nano-ceramic powder is ground and dispersed. Add an appropriate amount of water and dispersant to the resin, add the nano-ceramic powder during stirring, and grind to obtain the nano-ceramic slurry.
[0034] As an example, the nano-ceramic powder was ground and dispersed. An appropriate amount of water and dispersant were added to the resin, and the nano-ceramic powder was slowly added under high-speed stirring for 30 minutes for pre-dispersion. Then it was transferred to a high-speed grinder and ground with 2 mm zirconium beads for 2-3 hours.
[0035] In one specific implementation, the proportions of the components in the preparation of the nano-ceramic powder slurry are as follows: resin 10%, dispersant 6%, nano-ceramics 30%, and the remainder being purified water. The resin used is a water-based polyester and a water-based acrylic resin, and the dispersant is styrene-maleic anhydride.
[0036] In one embodiment of the present invention, the specific process of step S120, which involves "adding the water-based resin, the amino resin, the silver powder, the film-forming aid, the crosslinking agent, the coupling agent, and the additives according to a specified ratio, and finally adding the nano-ceramic slurry to obtain the target finished water-based topcoat," can be further described in conjunction with the following description.
[0037] It should be noted that the relevant proportions of materials are added sequentially to the dispersion tank according to the formula, and finally the ground nano-ceramic slurry is added to obtain the target finished water-based topcoat.
[0038] One embodiment of this application provides an application of a water-based topcoat that combines high toughness and high hardness, wherein the application is the processing of the water-based topcoat on the surface of galvanized coil or stainless steel coil.
[0039] Specifically, the water-based topcoat of a specified viscosity is applied to the surface of the galvanized or stainless steel coil by roller coating, followed by high-temperature baking and cooling to obtain the target color-coated sheet.
[0040] As an example, on galvanized coils, a liquid water-based topcoat of a certain viscosity is directly applied to the galvanized substrate by roller coating (passivation treatment is required), followed by high-temperature baking for 30-100 seconds to bring the plate temperature to 210-241℃, and then it is removed and cooled.
[0041] For galvanized substrates, existing technologies typically require a two-coat process of "primer + topcoat" to achieve sufficient adhesion and processing performance. If an oil-based coating is used for a single coat, there are problems with poor adhesion and insufficient bending performance. It also cannot simultaneously meet 0T and 4H requirements, and it also faces the inherent environmental and safety issues of oil-based coatings.
[0042] The single-coat color-coated steel sheet coated with the water-based topcoat of this application can improve the stamping performance (OT) and processability (4H) of the color-coated steel sheet. Furthermore, under the condition of meeting the requirements of use, it can achieve single-coat by saving a coating process, saving paint, and saving a drying and curing process, thus saving costs.
[0043] As an example, a liquid water-based topcoat of a certain viscosity is directly applied to a stainless steel substrate using a roller coating method (without passivation or other treatments). After baking at a high temperature for 30-100 seconds to bring the plate temperature to 210-241℃, it can be removed and cooled.
[0044] Currently, most stainless steel appliance casings are finished using spraying or electroplating (vacuum coating) techniques. These techniques are more expensive and less efficient than roller coating. Furthermore, oil-based coatings often contain large amounts of toxic, harmful, volatile, flammable, and explosive substances. Moreover, existing oil-based coating systems often cannot simultaneously meet the extreme requirements of high toughness and high hardness for stainless steel substrates.
[0045] The stainless steel color-coated sheets coated with the water-based topcoat of this application can solve a series of problems such as paint peeling and scratches during the stamping process of stainless steel color-coated sheets. At the same time, the use of roller coating water-based paint replaces processes such as spraying and vacuum coating, and makes the paint water-based, safe and healthy, thereby improving production efficiency and reducing production costs.
[0046] Example 1 I. Product Name: Single-coat water-based topcoat for galvanized steel sheet II. Product Model: BXG-1007 III. Product preparation method: Preparation of nano-ceramic slurry: By weight percentage, add 56% pure water to a dispersion tank, then add 10% resin and 6% dispersant. Add 30% nano-ceramic powder to a high-speed disperser while stirring at high speed. After high-speed dispersion for 30 minutes, transfer to a horizontal sand mill for high-speed grinding for 3 hours. The resin is 75% waterborne polyresin and 25% waterborne acrylic resin. Preparation of high-hardness waterborne topcoat: Under high-shear stirring, nano-ceramic slurry is added to the waterborne topcoat and mixed for at least 30 minutes to obtain the high-hardness waterborne topcoat; the waterborne topcoat accounts for 85% and the nano-ceramic slurry accounts for 15% during mixing. The waterborne topcoat, by weight percentage, includes: 8700 waterborne acrylic resin (48%); 303 fully etherified and semi-etherified amino resin (6.5%); silver powder (4%); diethylene glycol butyl ether (5%); epoxy phosphate ester (2.5%); nano-ceramic powder (3.8%); titanate silane coupling agent (1.3%); deionized water (26.8%); and additives (2.1%).
[0047] The nano-ceramic powder is ground and dispersed, and an appropriate amount of water and dispersant are added to the resin. The nano-ceramic powder is added during the stirring process, and the nano-ceramic slurry is obtained by grinding. The ratio is 10% resin, 6% dispersant, 30% nano-ceramic, and the remainder is purified water. The resin is water-based polyester resin and water-based acrylic resin. Aqueous resin, amino resin, silver powder, film-forming aid, crosslinking agent, coupling agent and other additives are added, and finally nano-ceramic slurry is added to obtain a single-coat water-based topcoat for galvanized steel sheets.
[0048] IV. Product Introduction: This is an environmentally friendly, low-VOC, single-coat water-based topcoat specifically developed for galvanized sheet / coil coating production lines. The coating application is safe and efficient, eliminating the need for respirators and goggles, and poses no flammability or explosiveness risks during transportation and storage. The product complies with RoHS environmental requirements, and the coating possesses high hardness and bending resistance, meeting the requirements for stamping, bending, and other processing methods. It can be used in various industries such as home appliances, furniture, and elevator decoration.
[0049] V. Technical Parameters 1. Coating parameters:
[0050] 2. Coating performance
[0051] VI. Product Process Substrate processing: degreasing and cleaning, surface chemical treatment; Coating process: Roller coating (single coating), two-roller or three-roller coating, linear speed <100m / min; Baking conditions: PMT board temperature 224-241℃, baking time 40-80s (determined according to line speed, board thickness, etc.).
[0052] VII. Coating Application For coating application: After cleaning the material tray, roller surface, mixer, etc. for normal color change, wipe once with anhydrous ethanol (alcohol) or ethyl acetate (circulate several times with the circulating pump; water-based coating is recommended).
[0053] Viscosity adjustment: Industrial alcohol is preferred for dilution, but pure water can also be used.
[0054] Paint removal: Scrape the paint from the tray into the large bucket. (It is recommended to discard any remaining small amount of paint from the tray. Note: Do not pour any remaining paint from the tray after cleaning with oil-based thinner into the large bucket to avoid contaminating the paint in the large bucket.)
[0055] VIII. Safety Instructions Before using this product, please refer to the Material Safety Data Sheet (MSDS) for detailed information on product safety, recommended operating and precautionary measures, and product storage methods.
[0056] IX. Transportation Protect from impact and compression, and avoid exposure to sunlight. Transport as general dangerous goods.
[0057] 10. Storage The product must be stored in its original container at the temperature recommended on the product label, away from heat sources.
[0058] Example 2 I. Product Name: Water-based Topcoat for Stainless Steel II. Product Model: BXG76 III. Product preparation method: Preparation of nano-ceramic slurry: By weight percentage, add 56% pure water to a dispersion tank, then add 10% resin and 6% dispersant. Add 30% nano-ceramic powder to a high-speed disperser while stirring at high speed. After high-speed dispersion for 30 minutes, transfer to a horizontal sand mill for high-speed grinding for 3 hours. The resin is 45% water-based polyester and 65% water-based acrylic. Water-based topcoat for stainless steel: A high-hardness water-based topcoat is obtained by adding nano-ceramic slurry to the water-based topcoat under high-shear stirring conditions and mixing for at least 30 minutes. During mixing, the water-based topcoat accounts for 85% and the nano-ceramic slurry accounts for 15%. The water-based topcoat, by weight percentage, includes: 8700% water-based acrylic resin; 303% fully etherified and semi-etherified amino resin; 3.5% silver powder; 4% diethylene glycol butyl ether; 2.5% epoxy phosphate; 5% nano-ceramic powder; 2% titanate silane coupling agent; 23.8% deionized water; and 2.2% additives.
[0059] The nano-ceramic powder is ground and dispersed, and an appropriate amount of water and dispersant are added to the resin. The nano-ceramic powder is added during the stirring process, and the nano-ceramic slurry is obtained by grinding. The ratio is 10% resin, 6% dispersant, 30% nano-ceramic, and the remainder is purified water. The resin is water-based polyester resin and water-based acrylic resin. Aqueous resin, amino resin, silver powder, film-forming aid, crosslinking agent, coupling agent and other additives are added, and finally nano-ceramic slurry is added to obtain a single-coat water-based topcoat for galvanized steel sheets.
[0060] IV. Product Introduction: This is an environmentally friendly, low-VOC, single-coat water-based topcoat specifically developed for stainless steel coil coating production lines. The coating application is safe and efficient, eliminating the need for respirators and goggles, and poses no risks of flammability or explosion during transportation and storage. The product complies with RoHS environmental requirements, and the coating possesses high hardness and bending resistance, meeting the requirements for stamping, bending, and other processing methods. It can be used in various industries such as home appliances, furniture, and elevator decoration.
[0061] V. Technical Parameters 1. Coating parameters:
[0062] 2. Coating performance
[0063] VI. Product Process Substrate processing: degreasing and cleaning, surface chemical treatment; Coating process: Roller coating (single coating), two-roller or three-roller coating, linear speed <100m / min; Baking conditions: PMT board temperature 224-241℃, baking time 40-80s (determined according to line speed, board thickness, etc.).
[0064] VII. Coating Application For coating application: After cleaning the material tray, roller surface, mixer, etc. for normal color change, wipe once with anhydrous ethanol (alcohol) or ethyl acetate (circulate several times with the circulating pump; water-based coating is recommended).
[0065] Viscosity adjustment: Industrial alcohol is preferred for dilution, but pure water can also be used.
[0066] Paint removal: Scrape the paint from the tray into the large bucket. (It is recommended to discard any remaining small amount of paint from the tray. Note: Do not pour any remaining paint from the tray after cleaning with oil-based thinner into the large bucket to avoid contaminating the paint in the large bucket.) VIII. Safety Instructions Before using this product, please refer to the Material Safety Data Sheet (MSDS) for detailed information on product safety, recommended operating and precautionary measures, and product storage methods.
[0067] IX. Transportation Protect from impact and compression, and avoid exposure to sunlight. Transport as general dangerous goods.
[0068] 10. Storage The product must be stored in its original container at the temperature recommended on the product label, away from heat sources.
[0069] Although preferred embodiments of the present application have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present application.
[0070] Finally, it should be noted that in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or terminal device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or terminal device. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or terminal device that includes said element.
[0071] The above provides a detailed description of a water-based topcoat with both high toughness and high hardness, its preparation method, and its application. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.
Claims
1. A water-based topcoat possessing both high toughness and high hardness, characterized in that, By weight percentage, it consists of the following components: Water-based resin 45-55%; Amino resin 5-7%; Silver powder 3-6%; Film-forming aids 2-6%; Crosslinking agent 2-3%; 1-5% nano-ceramic powder; Coupling agent 0.3-2%; Deionized water 13-30%; Additives: 0.6-2.4%.
2. The water-based topcoat with both high toughness and high hardness according to claim 1, characterized in that, The water-based resin is a water-based acrylic resin or a silicone-modified acrylic resin.
3. The water-based topcoat with both high toughness and high hardness according to claim 1, characterized in that, The film-forming aid is diethylene glycol butyl ether, propylene glycol butyl ether, or dimethylaminoethanol.
4. The water-based topcoat with both high toughness and high hardness according to claim 1, characterized in that, The crosslinking agent is an epoxy phosphate ester and / or an aqueous blocked isocyanate crosslinking agent.
5. The water-based topcoat with both high toughness and high hardness according to claim 1, characterized in that, The coupling agent is a titanate silane coupling agent.
6. The water-based topcoat with both high toughness and high hardness according to claim 1, characterized in that, The additive, by weight percentage, comprises the following components: Neutralizing agent 0.1-0.7%; Drying agent 0.1-0.3%; Leveling agent 0.1-0.5%; Defoamer 0.3-0.9%.
7. A method for preparing a water-based topcoat possessing both high toughness and high hardness as described in any one of claims 1-6, characterized in that, Including the following steps: Preparation of nano-ceramic slurry; The water-based resin, the amino resin, the silver powder, the film-forming aid, the crosslinking agent, the coupling agent, and the additives are added according to the specified ratio, and finally the nano-ceramic slurry is added to obtain the target finished water-based topcoat.
8. The preparation method according to claim 7, characterized in that, The step of preparing the nano-ceramic slurry includes: The nano-ceramic powder is ground and dispersed. Add an appropriate amount of water and dispersant to the resin, add the nano-ceramic powder during stirring, and grind to obtain the nano-ceramic slurry.
9. An application of a water-based topcoat as described in any one of claims 1-6, characterized in that, The application is the application of the water-based topcoat on the surface of galvanized or stainless steel coils.
10. The application according to claim 9, characterized in that, On the surface of the galvanized or stainless steel coil, the water-based topcoat of a specified viscosity is applied to the substrate by roller coating, followed by high-temperature baking and cooling to obtain the target color-coated sheet.