A method for preparing a bundle-distributed vanadium carbide reinforced steel matrix composite

By forming a precursor film on the surface of vanadium wire and combining it with vacuum solid-state pre-alloying and multi-stage in-situ reaction diffusion heat treatment, the problems of agglomeration and uneven distribution of vanadium carbide reinforcing phase were solved, realizing the formation of a three-dimensional bundle structure and the stable bonding of the reinforcing phase with the steel substrate, thus improving the mechanical properties of the composite material.

CN122358077APending Publication Date: 2026-07-10YULIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610781501.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-02
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

In existing preparation processes, vanadium carbide reinforcing phases tend to agglomerate and are unevenly distributed; high-temperature molten steel casting causes the vanadium metal skeleton to melt and burn off, making it impossible to form a three-dimensional bundle structure; and the bonding strength between the reinforcing phase and the steel substrate is insufficient.

Method used

A precursor film is formed on the surface of a vanadium wire using a pre-treatment chemical isolation liquid. Combined with vacuum solid-phase pre-alloying, liquid casting and multi-stage in-situ reaction diffusion heat treatment are then performed to form a three-dimensional bundled uniformly distributed vanadium carbide reinforcing phase, which avoids melting and burning of the vanadium wire and improves the interfacial bonding strength.

Benefits of technology

The uniform bundled distribution of vanadium carbide in the steel matrix was achieved, which solved the problems of easy agglomeration and uneven distribution of the reinforcing phase, and improved the mechanical properties and interfacial bonding strength of the composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122358077A_ABST
    Figure CN122358077A_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal matrix composite material preparation technology, and discloses a method for preparing a bundled vanadium carbide reinforced steel matrix composite material, comprising: immersing vanadium wire in a pretreatment chemical isolation liquid and drying it to form a precursor solid film on the surface; fabricating a preform from the vanadium wire with the solid film on the surface using a three-dimensional orthogonal weaving process; placing the preform in a vacuum sintering furnace and heating it to complete solid-phase pre-alloying; fixing the preform in a mold and preheating it under a protective atmosphere; melting a high-carbon steel matrix material until it is completely liquefied, injecting it into the mold to immerse the preform, and cooling it to obtain a composite preform block; subjecting the composite preform block to in-situ reaction diffusion heat treatment to obtain the composite material. This invention prevents the thermal loss of vanadium wire during liquid casting and, through in-situ diffusion reaction, allows the generated vanadium carbide to inherit the initial weaving morphology, achieving a three-dimensional bundled uniform distribution of the reinforcing phase within the steel matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal matrix composite material preparation technology, specifically a method for preparing a bundled vanadium carbide reinforced steel matrix composite material. Background Technology

[0002] Vanadium carbide reinforced steel matrix composites are hybrid structural materials formed by introducing vanadium carbide reinforcing phases into steel materials. By using vanadium carbide with high hardness and steel matrix with toughness, they can exhibit good mechanical properties in industrial applications such as wear-resistant parts manufacturing.

[0003] Existing composite material preparation processes mainly include powder metallurgy and external particle casting. External particle casting involves directly adding prepared vanadium carbide powder into liquid steel for mechanical stirring, followed by cooling and molding. Another method involves mixing iron powder and vanadium carbide powder, then pressing and sintering at high temperature. There is also a process where metallic vanadium material is pre-placed in a mold, followed by casting high-temperature liquid high-carbon steel, which promotes the in-situ reaction of vanadium with carbon in the steel to generate vanadium carbide ceramic phase.

[0004] Current preparation methods using added particles are limited by the specific gravity difference between vanadium carbide and steel, as well as the interfacial wetting state. This leads to agglomeration of the reinforcing phase within the matrix, resulting in uneven distribution of physical properties within the material. When using metallic vanadium in conjunction with molten high-carbon steel for direct casting, the high-temperature steel directly thermally shocks the vanadium material, causing melting and burning of the vanadium skeleton. This disrupts the pre-defined spatial arrangement, making it difficult for the generated vanadium carbide to form a regular and stable three-dimensional bundle structure within the matrix. Furthermore, conventional in-situ reactions lack sufficient solid-state diffusion, resulting in insufficient interfacial bonding strength between the vanadium carbide reinforcing phase and the steel substrate, thus limiting the improvement of the overall mechanical properties of the composite material.

[0005] Therefore, the purpose of this invention is to provide a method for preparing a bundled vanadium carbide reinforced steel matrix composite material to overcome the shortcomings of the prior art. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a method for preparing vanadium carbide-reinforced steel-based composite materials with bundled distribution. This method solves the problems in existing preparation processes, such as the easy agglomeration and uneven distribution of the vanadium carbide reinforcing phase, the inability to form a three-dimensional bundled structure due to melting and burning of the vanadium skeleton caused by high-temperature molten steel casting, and the insufficient interfacial bonding strength between the reinforcing phase and the steel substrate.

[0007] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a bundled vanadium carbide reinforced steel matrix composite material includes the following steps: The vanadium wire was completely immersed in a pre-treatment chemical isolation solution for constant temperature impregnation. After being removed, it was placed in a forced-air drying oven for drying, forming a precursor solid film on the surface of the vanadium wire. A preform is made by using a three-dimensional orthogonal weaving process to fabricate vanadium wires with a precursor solid film on the surface. The preform is placed in a vacuum sintering furnace for heating and holding, and then cooled to room temperature to complete solid-phase pre-alloying. The preform that has undergone solid-phase pre-alloying is fixed in the mold and preheated and kept at a temperature under a first protective gas atmosphere. Simultaneously melt high-carbon steel matrix material until it is completely liquefied and keep the melt temperature constant. Inject the completely liquefied high-carbon steel matrix material into a mold to immerse the preform, and let it cool naturally to room temperature to obtain a composite preform block. The composite preforms were placed in an electric resistance furnace with a second protective gas for in-situ reaction diffusion heat treatment, and then cooled to room temperature with the furnace to obtain a bundle-shaped vanadium carbide reinforced steel matrix composite material.

[0008] By adopting the above technical solution, a precursor film is formed on the surface of the vanadium wire using a pre-treatment chemical isolation liquid, combined with vacuum solid-phase pre-alloying, followed by liquid casting and multi-stage in-situ reaction diffusion heat treatment. Therefore, a composite material in which vanadium carbide generated in situ is uniformly distributed in a three-dimensional bundle in the steel matrix is ​​obtained, while avoiding the burn-off of vanadium wire during the casting process.

[0009] The specific reaction mechanism and innovative aspects are as follows: During the impregnation and drying stages, the solute in the isolation liquid adheres to and crystallizes on the surface of the vanadium wire, forming a precursor solid film.

[0010] During solid-state pre-alloying, the precursor solid film undergoes a solid-state transformation upon heating, forming a protective layer on the surface of the vanadium wire. This protective layer isolates the vanadium wire from the direct thermal shock of the high-temperature molten high-carbon steel during subsequent high-temperature casting, preventing the vanadium wire from melting and burning, ensuring the structural integrity of the three-dimensional orthogonal braided preform, and improving the wettability between the molten steel and the vanadium wire.

[0011] During in-situ reactive diffusion heat treatment, carbon atoms in the high-carbon steel matrix diffuse into the interior of vanadium wires under thermal driving force, and react in-situ with vanadium atoms to form vanadium carbide. The three-dimensional orthogonal braided structure of the vanadium wires provides spatial constraints for the in-situ reaction, allowing the generated vanadium carbide to inherit the original arrangement of the vanadium wires and form a regular bundle-like distribution of reinforcing phase within the steel matrix, thereby improving the mechanical properties of the composite material.

[0012] Preferably, the pretreatment chemical isolation solution is made from raw materials comprising the following parts by weight: Boric acid 3.0-5.0 parts; Urea 1.0-2.0 parts; 93.0-96.0 parts of deionized water.

[0013] By employing the above technical solution, boric acid and urea are dissolved in deionized water to form a solution. After constant-temperature impregnation and drying, boric acid and urea crystallize and adhere to the surface of the vanadium wire. Under the subsequent high-temperature conditions of solid-phase pre-alloying, urea decomposes and releases gas, while boric acid melts or reacts, forming a boron-containing transition film on the surface of the vanadium wire that provides both isolation and wetting. This film is resistant to the erosion of liquid high-carbon steel and does not hinder the subsequent diffusion and penetration of carbon atoms.

[0014] Preferably, the preparation method of the pretreatment chemical isolation solution includes: adding boric acid and urea in corresponding weight parts to deionized water, and mechanically stirring for 30-45 minutes under constant temperature water bath heating conditions of 40-50℃ until the solute is completely dissolved.

[0015] By adopting the above technical solution, controlling the water bath temperature and stirring time, boric acid and urea are fully dissolved and dispersed in deionized water to form a uniform chemical isolation liquid, ensuring the consistency of the film formation process.

[0016] Preferably, during the process of completely immersing the vanadium wire in the pretreatment chemical isolation solution for constant temperature impregnation, the temperature of constant temperature impregnation is 40-50℃ and the impregnation time is 3-5 minutes; during the process of drying the removed vanadium wire in a forced-air drying oven, the drying temperature is 110-120℃ and the drying time is 30-45 minutes.

[0017] By adopting the above technical solution, the immersion temperature and time are set to form a liquid film on the surface of the vanadium wire by the isolation liquid, and the drying temperature and time are controlled to make the water in the liquid film evaporate and the solute crystallize to form a dense precursor solid film, thus avoiding the film cracking caused by excessive drying or the water residue caused by incomplete drying.

[0018] Preferably, during the process of forming a preform from vanadium wires with a precursor solid film on the surface, the spacing between the vanadium wires is controlled to be 1.5-2.0 mm.

[0019] By adopting the above technical solution, the arrangement spacing is set to ensure that the liquid high carbon steel can flow into the grid gaps of the preform during casting, fully filling and wrapping the preform, avoiding casting defects caused by too small a spacing, and also avoiding sparse distribution of the reinforcing phase caused by too large a spacing.

[0020] Preferably, during the heating and heat preservation process of the preform in a vacuum sintering furnace, the absolute pressure inside the vacuum sintering furnace is less than 0.01 Pa, the temperature is raised to 750-800℃ at a heating rate of 8-10℃ / min, and the heat preservation time is 1.5-2.5h.

[0021] By employing the above technical solution, the vacuum environment eliminates the influence of oxygen, preventing oxidation of the vanadium wire and its surface film during heating. Controlling the heating rate and the isothermal holding time causes the precursor film to undergo a structural transformation and form a strong bond with the surface of the vanadium wire, completing the pre-alloying process.

[0022] Preferably, the mold is a graphite mold; during the process of fixing the preform that has undergone solid-phase pre-alloying in the mold for preheating and heat preservation, the preheating temperature is 350-400℃, the heat preservation time is 0.5-1.5h, and the first protective gas used is argon.

[0023] By adopting the above technical solution, the mold and preform are preheated under argon protection before casting, which reduces the temperature gradient between the high-temperature molten steel and the preform, reduces the thermal shock force during casting, avoids thermal stress deformation of the preform due to rapid cooling, and improves the fluidity of the molten steel.

[0024] Preferably, the melt temperature of the high-carbon steel matrix material after complete liquefaction is kept constant at 1450-1480℃; the operation of injecting the completely liquefied high-carbon steel matrix material into the mold is carried out by gravity casting.

[0025] By adopting the above technical solution, the melt temperature is kept constant at 1450-1480℃ to ensure the fluidity of high carbon steel, which can fill the mold gap. At the same time, the heat input is limited to the range that the isolation layer on the surface of the preform can withstand, preventing the isolation layer from failing and the vanadium wire from melting.

[0026] Preferably, the in-situ reaction diffusion heat treatment process is as follows: heating to 1050-1080℃ at a heating rate of 5-8℃ / min, and holding at the temperature isothermally for 1.5-2.5h; then heating to 1160-1180℃ at a heating rate of 4-6℃ / min, and holding at the temperature isothermally for 3-4h; finally cooling to 850℃ at a cooling rate of 8-12℃ / min, and holding at the temperature isothermally for 1-1.5h.

[0027] By adopting the above technical solution, the heat treatment process is divided into three stages to control the diffusion and reaction mechanism of carbon atoms: The first stage of heating and holding provides the initial thermal driving force, which causes carbon atoms in the high-carbon steel matrix to cross the interface isolation layer and begin to diffuse to the surface of the vanadium wire. The second stage involves further heating and holding the temperature to increase the atomic diffusion coefficient, allowing carbon atoms to penetrate into the vanadium wire core and combine with vanadium in situ to form vanadium carbide. The temperature and holding parameters ensure the conversion of metallic vanadium into vanadium carbide. The third stage involves cooling and heat preservation, which promotes the stability of the internal structure of the composite material and releases the thermal and structural stresses accumulated during the earlier reaction and cooling processes.

[0028] Preferably, when the composite preform is placed in an electric resistance furnace for in-situ reaction diffusion heat treatment, the second protective gas introduced is high-purity argon.

[0029] By adopting the above technical solution, high-purity argon gas provides an inert atmosphere to prevent oxidation and decarburization of the composite material during high-temperature diffusion heat treatment, thus ensuring the carbon content of the matrix and the full progress of the in-situ reaction.

[0030] This invention provides a method for preparing a bundled vanadium carbide reinforced steel-based composite material. It has the following beneficial effects: 1. This invention forms a structurally stable solid film and protective layer on the surface of vanadium wire by setting up a constant temperature immersion in a pretreatment chemical isolation liquid and a vacuum solid-phase pre-alloying step. The protective layer can isolate the direct thermal shock of the high temperature molten steel during the casting of liquid high carbon steel, prevent the vanadium wire from melting and burning, and ensure the integrity of the vanadium wire preform structure.

[0031] 2. This invention uses a three-dimensional orthogonal weaving process to form a preform from the treated vanadium wire, providing spatial arrangement constraints for subsequent in-situ reactions. This allows the generated vanadium carbide reinforcing phase to directly inherit the weaving morphology of the vanadium wire, achieving a bundled and uniform distribution of vanadium carbide in the steel matrix. This solves the problems of easy agglomeration and uneven distribution of the reinforcing phase in the prior art.

[0032] 3. This invention sets up an in-situ reaction diffusion heat treatment step, using thermal driving force to promote the solid-phase diffusion and reaction of carbon atoms in the high-carbon steel matrix into the interior of the vanadium wire, generating vanadium carbide reinforcing phase in situ. This not only completes the transformation of the metal phase to the ceramic phase, but also realizes the interdiffusion of elements between the reinforcing phase and the steel matrix interface, ensuring the bonding strength inside the composite material. Attached Figure Description

[0033] Figure 1 This is a radial micro-Vickers hardness distribution diagram of the cross-section of the composite material of the present invention; Figure 2 This is a distribution diagram of the test results of porosity and actual density of the composite material of the present invention; Figure 3 This is a comparison chart of the volume porosity and actual measured density of the composite materials in Example 2 and Comparative Example 2 of the present invention. Figure 4 This is a comparison chart of the room temperature tensile and compressive strength of the composite materials of Example 2 of the present invention with those of Comparative Examples 1 and 5. Figure 5 This is a comparison diagram of the fracture toughness and impact toughness of the composite materials in Example 2 of the present invention with those in Comparative Examples 3 and 4.

[0034] Figure 6This is a comparison chart of the volume porosity and room temperature compressive strength of the composite materials in Example 2 and Comparative Example 6 of the present invention. Detailed Implementation

[0035] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] Preparation Examples 1-3: Preparation Example 1: This preparation example provides a method for preparing a pretreatment chemical isolation solution, including the following steps: 3.0 parts by weight of boric acid and 1.0 parts by weight of urea were slowly added to 96.0 parts by weight of deionized water. The mixture was heated in a constant temperature water bath at 40°C and mechanically stirred at 200 rpm for 30 minutes until the solutes were completely dissolved, resulting in a uniform and transparent pretreated chemical isolation solution.

[0037] Preparation Example 2: This preparation example provides a method for preparing a pretreatment chemical isolation solution, including the following steps: 4.0 parts by weight of boric acid and 1.5 parts by weight of urea were slowly added to 94.5 parts by weight of deionized water. The mixture was heated in a constant temperature water bath at 45°C and mechanically stirred at 250 rpm for 35 minutes until the solutes were completely dissolved, resulting in a uniform and transparent pretreated chemical isolation solution.

[0038] Preparation Example 3: This preparation example provides a method for preparing a pretreatment chemical isolation solution, including the following steps: 5.0 parts by weight of boric acid and 2.0 parts by weight of urea were slowly added to 93.0 parts by weight of deionized water. The mixture was heated in a constant temperature water bath at 50°C and mechanically stirred at 300 rpm for 45 minutes until the solutes were completely dissolved, resulting in a uniform and transparent pretreated chemical isolation solution.

[0039] Examples 1-3: Example 1: This embodiment provides a method for preparing a bundled vanadium carbide reinforced steel-based composite material, including the following steps: (1) Surface chemical impregnation pretreatment: The metal vanadium wire is completely immersed in the pretreatment chemical isolation liquid described in Preparation Example 1, and is immersed at a constant temperature of 40°C for 3 min. After being taken out, it is placed in a forced-air drying oven and dried at 110°C for 30 min to form a precursor solid film on the surface of the metal vanadium wire. (2) Preform weaving and solid-state pre-alloying: The vanadium wires processed in step (1) are made into a preform using a three-dimensional orthogonal weaving process, and the spacing of the vanadium wires is controlled to be 1.5 mm. The preform is placed in a vacuum sintering furnace and heated to 750°C at a heating rate of 8°C / min under an absolute pressure of less than 1.0E-2Pa. It is kept at a constant temperature for 1.5 h and then cooled to room temperature with the furnace. (3) Liquid casting of steel matrix: The preform after step (2) is fixed in the graphite mold, preheated to 350°C under argon protection and kept at that temperature for 1 hour; high carbon steel matrix material is melted simultaneously, and after complete liquefaction, the melt temperature is kept constant at 1450°C. Liquid high carbon steel is injected into the graphite mold to immerse the preform by gravity casting, and then naturally cooled to room temperature to obtain composite preform. (4) In-situ reaction diffusion heat treatment: The composite preform is placed in a resistance furnace with high-purity argon gas and heated to 1050°C at a heating rate of 5°C / min and held isothermally for 1.5h; then heated to 1160°C at a heating rate of 4°C / min and held isothermally for 3h; finally cooled to 850°C at a cooling rate of 8°C / min and held isothermally for 1h at this temperature, and then cooled to room temperature with the furnace.

[0040] Example 2: This embodiment provides a method for preparing a bundled vanadium carbide reinforced steel-based composite material, including the following steps: (1) Surface chemical impregnation pretreatment: The metal vanadium wire is completely immersed in the pretreatment chemical isolation liquid described in Preparation Example 2, and is impregnated at a constant temperature of 45°C for 4 min. After being taken out, it is placed in a forced-air drying oven and dried at 115°C for 35 min to form a precursor solid film on the surface of the metal vanadium wire. (2) Preform weaving and solid-state pre-alloying: The metal vanadium wires processed in step (1) are made into a preform using a three-dimensional orthogonal weaving process, and the spacing of the vanadium wires is controlled to be 1.75 mm. The preform is placed in a vacuum sintering furnace and heated to 775°C at a heating rate of 9°C / min under an absolute pressure of less than 1.0E-2Pa. It is kept at a constant temperature for 2 hours and then cooled to room temperature with the furnace. (3) Liquid casting of steel matrix: The preform after step (2) is fixed in the graphite mold, preheated to 375°C under argon protection and kept at that temperature for 1 hour; high carbon steel matrix material is melted simultaneously, and after complete liquefaction, the melt temperature is kept constant at 1465°C. Liquid high carbon steel is injected into the graphite mold to immerse the preform by gravity casting, and then naturally cooled to room temperature to obtain composite preform. (4) In-situ reaction diffusion heat treatment: The composite preform is placed in a resistance furnace with high-purity argon gas and heated to 1065°C at a heating rate of 6°C / min and held isothermally for 2 hours; then heated to 1170°C at a heating rate of 5°C / min and held isothermally for 3.5 hours; finally cooled to 850°C at a cooling rate of 10°C / min and held isothermally for 1.2 hours at this temperature, and then cooled to room temperature with the furnace.

[0041] Example 3: This embodiment provides a method for preparing a bundled vanadium carbide reinforced steel-based composite material, including the following steps: (1) Surface chemical impregnation pretreatment: The metal vanadium wire is completely immersed in the pretreatment chemical isolation liquid described in Preparation Example 3, and is immersed at a constant temperature of 50°C for 5 min. After being taken out, it is placed in a forced-air drying oven and dried at 120°C for 45 min to form a precursor solid film on the surface of the metal vanadium wire. (2) Preform weaving and solid-state pre-alloying: The vanadium wires processed in step (1) are made into a preform using a three-dimensional orthogonal weaving process, and the spacing of the vanadium wires is controlled to be 2.0 mm. The preform is placed in a vacuum sintering furnace and heated to 800°C at a heating rate of 10°C / min under an absolute pressure of less than 1.0E-2Pa. It is kept at a constant temperature for 2.5 h and then cooled to room temperature with the furnace. (3) Liquid casting of steel matrix: The preform after step (2) is fixed in the graphite mold, preheated to 400°C under argon protection and kept at that temperature for 1 hour; high carbon steel matrix material is melted simultaneously, and after complete liquefaction, the melt temperature is kept constant at 1480°C. Liquid high carbon steel is injected into the graphite mold to immerse the preform by gravity casting, and then naturally cooled to room temperature to obtain composite preform. (4) In-situ reaction diffusion heat treatment: The composite preform is placed in a resistance furnace with high-purity argon gas and heated to 1080°C at a heating rate of 8°C / min and held isothermally for 2.5h; then heated to 1180°C at a heating rate of 6°C / min and held isothermally for 4h; finally cooled to 850°C at a cooling rate of 12°C / min and held isothermally for 1.5h at this temperature, and then cooled to room temperature with the furnace.

[0042] Comparative Examples 1-6: Comparative Example 1: Compared with Example 2, the difference is that the surface chemical impregnation pretreatment process of step (1) is omitted, and the vanadium wire is not impregnated with the pretreatment chemical isolation liquid and proceeds directly to the subsequent steps. The rest are the same.

[0043] Comparative Example 2: Compared with Example 2, the difference is that in step (2), the vacuum solid-phase pre-alloying degassing treatment is omitted, and the precursor solid film is formed on the surface of the metal vanadium wire before the liquid casting of the steel matrix in step (3) is carried out directly. The rest are the same.

[0044] Comparative Example 3: Compared with Example 2, the difference is that in the in-situ reaction diffusion heat treatment in step (4), the first stage (1065℃) isothermal heat preservation process is omitted, and the composite preform directly enters the second stage (1170℃) for isothermal heat preservation after heating. The rest are the same.

[0045] Comparative Example 4: Compared with Example 2, the difference is that in the in-situ reaction diffusion heat treatment in step (4), the third stage (850°C) isothermal heat preservation process is omitted, and the furnace is directly cooled to room temperature after the second stage heat preservation is completed. The rest are the same.

[0046] Comparative Example 5: Compared with Example 2, the difference is that in the preparation of the pretreatment chemical isolation solution, the mass fraction of boric acid is reduced to 1.0%, while the proportions of the remaining components and the process parameters are the same.

[0047] Comparative Example 6: Compared with Example 2, this comparative example provides a method for preparing vanadium carbide reinforced iron-based composite materials using powder metallurgy hot pressing sintering, the specific steps of which are as follows: (1) Ball milling and mixing of iron and carbon powder: 2.5g of high-purity graphite powder (4wt%) with a particle size of 2μm was added to 60ml of anhydrous ethanol and placed in an ultrasonic cleaner for ultrasonic dispersion for 20min, during which it was manually stirred once every 5 minutes; 62g of 325-mesh high-purity iron powder and the dispersed suspension were added to an agate grinding jar, and agate grinding balls were added at a ball-to-material ratio of 5:1. The ball mill was set to a speed of 300r / min and alternated between forward and reverse rotation (switching every 30min) for 4h in a planetary ball mill; after the end, the mixture was taken out and placed in a vacuum drying oven, heated to 80℃ at a vacuum of 0.01MPa at 5℃ / min and kept at the temperature for 3h until completely dry, and passed through a 200-mesh sieve to obtain a uniform iron and carbon mixed powder.

[0048] (2) Mold loading and pre-pressing: A 0.1mm thick layer of graphite paper is evenly laid on the inner wall and upper and lower surfaces of the graphite mold and coated with a graphite lubricating coating; 30g of iron-carbon mixed powder is poured into the mold and compacted at a frequency of 50Hz for 30s, followed by light pressure of 2MPa for 10s; 10 metal vanadium wires with a diameter of 1mm and a length of 40mm are placed horizontally in the powder layer, arranged in parallel in one direction with an adjacent spacing of 2mm; the remaining iron-carbon mixed powder is poured into the mold to cover the vanadium wires, compacted again for 30s, and lightly pressured at 2MPa for 10s, and the upper and lower end caps are pressed tightly to seal, with the filling density controlled at approximately 3.0g / cm³. 3 .

[0049] (3) Hot pressing sintering and in-situ reaction: The mold is placed in a vacuum hot pressing sintering furnace, and the vacuum is evacuated to a background vacuum of ≤1.0E-3MPa and maintained for 10min; the first stage of preheating is carried out by heating to 900℃ at a heating rate of 5℃ / min and holding for 45min (without applying pressure); the second stage is carried out by heating to 1180℃ at a rate of 5℃ / min, and after the temperature stabilizes, the pressure is increased step by step (0-10MPa takes 2min, 10-30MPa takes 5min, 30-50MPa takes 3min) to a total pressure of 50MPa, and then held at 1180℃, 50MPa and ≤1.0E-3MPa vacuum for 1.5h.

[0050] (4) Controlled cooling treatment: After the heat preservation and pressure preservation are completed, the temperature is cooled to 600℃ at a cooling rate of 2℃ / min, and isothermally held at 600℃ for 2 hours. Then, the temperature is naturally cooled to room temperature with the furnace. The sample is demolded and polished to remove the surface oxide layer.

[0051] Test Examples 1-6: Test Example 1: This test example uses the micro Vickers hardness test method to determine the hardness gradient of the interface region of the composite materials prepared in Examples 1 to 3. The specific experimental steps are as follows: (1) Using a wire cutting device, composite preform samples of Examples 1 to 3 were cut along a direction perpendicular to the axial direction of the vanadium metal fiber. The cut samples were placed in an embedding machine and embedded and cured with cold embedding resin.

[0052] (2) The cured sample surface was subjected to coarse grinding, semi-fine grinding and fine grinding with silicon carbide sandpaper of different grits in sequence. Then, diamond polishing paste with a particle size of 1μm was used to polish the sample surface on a mechanical polishing machine until the sample surface reached a mirror state without obvious scratches. The residual polishing liquid on the surface was cleaned, ultrasonically cleaned with anhydrous ethanol and then dried with cold air.

[0053] (3) A micro Vickers hardness tester was used to perform a linear point test on the cross section. The test load was set to 200 gf and the indenter holding time was 15 s.

[0054] (4) Select a single reinforcing fiber section on the sample surface and set the starting point of the indentation in the steel matrix about 30 μm away from the outer edge of the reinforcing fiber. Perform linear continuous indentation tests along the radial direction of the section towards the fiber center at equal intervals of 10 μm. Read and record the micro Vickers hardness value corresponding to each test indentation and summarize the data.

[0055] Table 1. Radial micro-Vickers hardness gradient distribution data of composite material sections in Examples 1-3

[0056] Conclusion: Based on the data in Table 1 and Figure 1 The hardness distribution trend shows that the composite material exhibits a staged hardness gradient change from the steel matrix to the interior of the reinforcing fibers. Within the test range of 0-20μm, the hardness value is distributed in the range of 358-403HV0.2, which is within the normal hardness range of high carbon steel matrix, indicating that the matrix side is less affected by interfacial reaction.

[0057] Within the range of 30-50 μm from the starting point, Figure 1 Both the broken line and the bar graph showed a significant increase, with the hardness value increasing to 1385-1754HV0.2. The jump in hardness measured was caused by the cubic V8C7 phase generated in the second stage of diffusion heat treatment (1160-1180℃). In the high-temperature stage, the interstitial solid solution formed at the interface in the early stage underwent desolvation, and boron and nitrogen atoms diffused into the outer matrix. The diffusion channels of carbon atoms were thus opened. Driven by the carbon concentration gradient, the local carbon activity increased, which promoted the continuous precipitation of the high-hardness V8C7 phase.

[0058] In the 60-80μm range, Figure 1 The hardness value further increases, reaching a peak region of 2011-2267 HV0.2. This peak hardness region corresponds to the hexagonal V2C phase generated during the first stage of diffusion heat treatment (1050-1080℃). During the isothermal process of this first stage, the dissolved boron and nitrogen atoms cause lattice distortion, creating a steric hindrance effect on the long-range diffusion of carbon atoms. This suppresses the carbon diffusion flux at the interface, resulting in a low-carbon activity state. Due to the thermodynamic constraints of the phase transition, a low-carbon V2C phase is preferentially generated and stabilized at the microscopic level. In the 90-100 μm range, the hardness value rapidly decreases to 218-345 HV0.2. Figure 1 The downward trend in the numerical value and the low hardness value indicate that the dot test location has reached the core of the residual vanadium metal fiber that did not participate in the reaction.

[0059] The above cross-sectional radial hardness distribution data and corresponding Figure 1The hardness variation characteristics shown in the table demonstrate that the current preparation method constructs a gradient transition layer composed of V8C7 and V2C phases between the metal fibers and the matrix. The multi-level hardness gradient distribution eliminates mechanical abrupt changes and stress concentration defects that are easily caused by single-phase interfaces.

[0060] Test Example 2: This test example uses Archimedes' displacement method to determine the actual density and macroscopic porosity of the composite materials prepared in Examples 1 to 3. The specific experimental steps are as follows: (1) Using an electrical discharge wire cutting machine, block-shaped samples with dimensions of 10mm × 10mm × 10mm were cut from the center of the composite precast blocks of Examples 1 to 3. The surface and edges of the samples were polished with silicon carbide sandpaper, and then ultrasonically cleaned for 15 minutes in a beaker containing anhydrous ethanol to remove surface oil and debris. The cleaned samples were placed in a forced-air drying oven and dried at 80°C to constant weight, and then removed and cooled to room temperature.

[0061] (2) Use an electronic analytical balance with an accuracy of 0.1 mg to measure the dry weight of the sample in air and record the dry weight data.

[0062] (3) The sample was saturated with water using a vacuum immersion device. The sample was placed in deionized water in a vacuum vessel, and the vacuum was drawn to an absolute pressure below 2000 Pa and maintained for 30 min to remove the gas from the sample surface and the pores. Then the pressure was restored to normal to allow the deionized water to be completely injected into the micropores.

[0063] (4) Place the beaker containing deionized water on the dedicated density component support of the electronic balance. Suspend the saturated sample with a thin metal wire and completely immerse it in the water. After the reading stabilizes, record the suspended mass of the sample in the water.

[0064] (5) Remove the sample from the water, quickly absorb the water adhering to the surface of the sample with a wet and wrung-out filter paper, and weigh the saturated mass of the sample in an electronic balance.

[0065] (6) Calculate the theoretical density of the composite material using the mixing principle based on the volume fractions and standard densities of the matrix material and reinforcing fibers. Calculate the actual density and volumetric porosity of the sample using Archimedes' displacement method, and summarize the test data.

[0066] Table 2. Test data of actual density and porosity of composite materials in Examples 1-3

[0067] Conclusion: Based on the data in Table 2 and Figure 2The porosity and density distribution shown are as follows: the volumetric porosity values ​​of Examples 1 to 3 are in the range of 0.13% to 0.32%, and the difference between the actual measured density and the theoretical calculated density is small. Figure 2 The bar charts visually demonstrate that the volumetric porosity values ​​of the three embodiments are all below 0.5%, and the line graphs show that the actual measured densities remain between 7.59 and 7.65 g / cm³. 3 Within the specified range, test results showed that no macroscopic pores or air entrapment defects were generated inside the composite material, and the matrix metal and reinforcing fibers achieved a dense encapsulation and bonding.

[0068] The increase in the density of the composite material depends on the vacuum solid-phase pre-alloying process. Before entering the high-temperature liquid steel casting process above 1450℃, the preform is kept at a constant temperature in a vacuum environment of 750-800℃ and an absolute pressure of less than 1.0E-2Pa. During this stage, the chemical isolation liquid precursor on the surface of the vanadium wire undergoes thermal decomposition. Urea decomposes to release ammonia and carbon monoxide, and boric acid dehydrates to release water vapor. Under the dual action of high temperature and high vacuum environment, volatile gases are continuously extracted from the reaction chamber by the vacuum pump, and the precursor completes the solid-phase degassing process in advance.

[0069] If solid-phase pre-alloying is not performed and casting is carried out directly, the residual crystal water and organic matter inside the precursor film will vaporize upon contact with the liquid high-temperature metal. The encapsulation and obstruction of the external liquid metal will prevent the expansion gas from escaping and venting, causing a boiling phenomenon at the solid-liquid interface. Ultimately, after the composite material solidifies, it will form through-hole or closed macroscopic pores.

[0070] Table 2 and Figure 2 The data showing low porosity and high density confirms that the vacuum degassing process eliminates the interference of volatile substances in the early stage of high-temperature reaction. The fiber interface after degassing exhibits a stable physical state, avoiding gas disturbance during the casting of liquid high-carbon steel. The matrix molten metal can completely fill the gaps in the preform, ensuring the overall structural density of the composite material.

[0071] Test Example 3: This test example uses Archimedes' method of drainage to compare the interfacial compactness and macroscopic defects of the composite precast blocks prepared in Example 2 and Comparative Example 2. The specific experimental steps are as follows: (1) Test samples with dimensions of 15mm × 15mm × 10mm were cut from the composite precast blocks of Example 2 and Comparative Example 2 using an electrical discharge wire cutting machine. The burrs on the cut surface were smoothed with silicon carbide sandpaper, and the samples were ultrasonically cleaned in anhydrous ethanol for 20 minutes to remove oil and metal debris adhering to the surface. After cleaning, the samples were placed in a forced-air drying oven and dried at a constant temperature of 85℃ for 120 minutes. After being removed, they were placed in a desiccator to cool to room temperature.

[0072] (2) Use an electronic analytical balance with an accuracy of 0.1 mg to measure the mass of the dried sample in air and record the value as the dry weight.

[0073] (3) Turn on the vacuum immersion device and completely immerse the sample in deionized water. Start the vacuum pump to reduce the absolute pressure inside the container to below 1500 Pa and maintain the evacuation state for 45 min to allow the air in the open pores inside the sample to escape. Turn off the vacuum pump and restore normal pressure, and let it stand for 30 min to allow water to enter the pores under atmospheric pressure.

[0074] (4) Place the measuring beaker containing deionized water on the density testing assembly below the electronic balance. Suspend the sample using a fine wire mesh bag, ensuring the sample is completely immersed in the water without touching the inner wall of the beaker. After the balance reading stabilizes, record the suspended mass of the sample in the water.

[0075] (5) Remove the sample from the water, quickly wipe away excess water droplets on the surface with a moistened and wrung-out degreased cotton ball, weigh it in an electronic balance and record the saturated mass of the sample.

[0076] (6) Calculate the theoretical density of the composite material based on the volume fraction ratio of the high-carbon steel matrix and the vanadium fiber and the standard density. Apply Archimedes' displacement method to calculate the actual density and volume porosity of the sample, and summarize and compare the two sets of test data.

[0077] Table 3. Comparison of Porosity and Density Test Data of Composite Materials in Example 2 and Comparative Example 2

[0078] Conclusion: Based on the data in Table 3 and Figure 3 The displayed comparison test results Figure 3 The bar chart corresponding to the left vertical axis shows that the volumetric porosity of Example 2 is 0.13%, while the volumetric porosity of Comparative Example 2 increases to 12.14%. Figure 3 The line graph corresponding to the right-hand vertical axis shows that the actual measured density in Example 2 was 7.65 g / cm³. 3 This is essentially equivalent to 7.66 g / cm³. 3 The theoretically calculated density; the actual measured density of Comparative Example 2 decreased to 6.73 g / cm³. 3 It is lower than the theoretical value.

[0079] In Comparative Example 2, the vacuum solid-phase pre-alloying degassing step was removed from the preparation process. A vanadium wire with a precursor film attached to its surface was directly fixed in a graphite mold and then contacted with liquid high-carbon steel at 1465°C. The boric acid and urea components in the precursor decomposed upon contact with the high-temperature molten metal, generating water vapor, ammonia, and carbon monoxide. Because the external liquid high-carbon steel surrounded the vanadium wire, it blocked the physical channels for the decomposed gases to escape to the external environment. A large amount of gas accumulated at the interface between the vanadium wire and the liquid high-carbon steel, expanding under heat and causing exhaust disturbances within the melt. After the molten metal solidified, the unexpelled gases were trapped inside the composite material, forming large pores and interface delamination defects along the fiber arrangement direction.

[0080] Example 2 retains the vacuum degassing step. The precursor completes the decomposition and vaporization process in advance during the vacuum holding stage before liquid metal casting. The generated gas is extracted by vacuum equipment. (Table 3 and...) Figure 3 The presented data differences prove that the vacuum solid phase degassing step eliminates the interference of gas release accompanying the precursor reaction. The early venting of gas ensures that the subsequent high-temperature metal melt can flow stably and fully fill the interior of the preform, avoiding the generation of macroscopic pore defects inside the composite material and ensuring the compactness of the final material.

[0081] Test Example 4: This test example uses an electronic universal testing machine to compare the room temperature tensile strength and compressive strength of the composite materials prepared in Example 2, Comparative Example 1, and Comparative Example 5. The specific experimental steps are as follows: (1) Using a CNC wire EDM machine, mechanical property test specimens were cut along the axial direction of the fiber arrangement in the composite precast blocks of Examples 2, Comparative Examples 1 and 5. The tensile specimens were processed into standard plate-shaped specimens with a gauge length of 30 mm and a rectangular cross-section size of 5 mm × 2 mm. The compression specimens were processed into cylinders with a diameter of 8 mm and a height of 12 mm.

[0082] (2) Use silicon carbide sandpaper of different mesh sizes to mechanically grind the cut surface along the length of the sample to remove surface machining marks and heat-affected zone. Place the ground sample into a beaker containing anhydrous ethanol and ultrasonically clean it for 15 minutes to remove surface debris. After cleaning, take it out and dry it in cold air for later use.

[0083] (3) Tensile properties were tested at room temperature. The plate-shaped tensile specimen was vertically clamped between the upper and lower wedge-shaped grips of the electronic universal testing machine, and the displacement loading rate of the testing machine beam was set to 0.5 mm / min. A contact extensometer was installed at the center of the gauge length of the specimen to record real-time strain data. The equipment was started and the load was continuously applied until the specimen fractured. The maximum fracture load recorded by the testing machine was read, and the room temperature tensile strength was calculated based on the cross-sectional area of ​​the specimen.

[0084] (4) Replace the compression test flat platen fixture of the universal testing machine. Place the cylindrical compression specimen in the center of the lower platen, and apply a small amount of molybdenum disulfide grease to both ends of the specimen to reduce the interference of end-face friction effect on the test results. Set the compression displacement rate of the testing machine to 1.0 mm / min. Start the equipment to load downwards, and stop the test when macroscopic cracks appear on the specimen surface or crushing failure occurs. Record the peak load in the load-displacement curve and calculate the room temperature compressive strength value.

[0085] (5) Prepare 5 tensile specimens and 5 compression specimens for each group of materials and perform repeated tests. After removing invalid data that are prematurely fractured due to specimen processing defects, calculate the arithmetic mean of the remaining valid data as the final output result.

[0086] Table 4. Room temperature tensile and compressive strength test data of composite materials from Example 2 and Comparative Examples 1 and 5

[0087] Conclusion: From Table 4, Figure 4 The data shows that, Figure 4 The gray bar chart corresponding to the left vertical axis shows that the room temperature tensile strength of Example 2 is 1142.8 MPa. Figure 4 The line graph corresponding to the vertical axis on the right shows that the room temperature compressive strength of Example 2 is 2456.4 MPa, the tensile strength of Comparative Example 1 without chemical impregnation pretreatment decreases to 437.2 MPa, and the compressive strength decreases to 1189.3 MPa. The tensile strength of Comparative Example 5, with the boric acid mass fraction in the pretreatment solution reduced to 1.0%, is 681.5 MPa, and the compressive strength is 1624.7 MPa. Both test values ​​are between those of Example 2 and Comparative Example 1.

[0088] In Example 2, the surface of the vanadium wire is coated with boric acid and urea precursors of a set concentration. During the in-situ reaction diffusion heat treatment stage, the boron and nitrogen atoms generated by the precursors dissolve into the interstitial positions of the vanadium lattice, causing local lattice distortion. The boron and nitrogen atoms in the interstitial positions exert a steric hindrance effect on the inward diffusion of carbon atoms, limiting the diffusion flux of carbon atoms. The elemental barrier effect induces the formation of a multilayer gradient transition structure, avoiding the interface stress concentration caused by the excessively large span of elastic modulus between the reinforced ceramic phase and the metal matrix, enabling the composite material to withstand high loads.

[0089] Comparative Example 1 omitted the chemical pretreatment process, and the surface of the vanadium metal fiber lacked a barrier medium. In a high-temperature environment, free carbon atoms in the liquid high-carbon steel directly entered the interior of the vanadium metal fiber. The carbon supply caused the formation of a large single vanadium carbide phase at the interface. The large ceramic phase directly contacted the metal matrix and generated internal stress. When subjected to external force for tension or compression, microcracks were initiated and propagated at the interface, resulting in a decrease in the macroscopic load-bearing capacity of Comparative Example 1.

[0090] Comparative Example 5 underwent chemical impregnation, but the boric acid concentration in the pretreatment solution was set to 1.0%. Insufficient boron content prevented the formation of a continuous and complete interstitial solid solution barrier layer on the vanadium fiber surface after solid-phase pre-alloying. The localized absence of the barrier layer weakened the system's ability to block carbon diffusion, resulting in uncontrollable carbon flux in some areas and the formation of brittle phases with poor morphology. (Table 4) Figure 4 The moderate intensity values ​​reflect that low-concentration isolation fluid cannot establish an anti-carbon penetration layer, as shown in Table 4. Figure 4 The discrepancies in the test data confirm that the chemical precursor film and the set concentration range are prerequisites for avoiding coarsening of the brittle phase and ensuring the strength of the composite material.

[0091] Test Example 5: This test example uses the single-sided notched beam method and the unnotched impact test method to compare the fracture toughness and room temperature impact toughness of the composite materials prepared in Example 2, Comparative Example 3, and Comparative Example 4. The specific experimental steps are as follows: (1) Mechanical test specimens were cut from the composite material preforms of Examples 2, 3, and 4 using an electrical discharge wire cutting machine. Fracture toughness tests were performed using single-sided notched beam specimens, with dimensions of 4 mm × 8 mm × 36 mm. Impact toughness tests were performed using unnotched cuboid specimens, with dimensions of 10 mm × 10 mm × 55 mm. The length of the specimen was parallel to the direction of the internal vanadium fiber arrangement.

[0092] (2) Use sandpaper to grind the surface of the sample step by step to eliminate the surface micro-cracks and remelted layer generated by wire cutting. Immerse the ground sample in anhydrous ethanol and clean it with an ultrasonic cleaner for 15 minutes. After cleaning, take it out and dry it at room temperature.

[0093] (3) Use a diamond wire saw to cut an initial straight groove with a depth of 2 mm at the middle position on one side of the fracture toughness specimen in the width direction. Install the specimen on a high-frequency fatigue testing machine and pre-fabricate a fatigue crack with a length of about 1.5 mm at the bottom of the straight groove to ensure that the initial total crack length meets the requirements of the fracture toughness test standard.

[0094] (4) Place the pre-existing fatigue cracked specimen on the three-point bending fixture of the electronic universal testing machine, with the support span set to 32 mm. Apply a bending load to the specimen at a constant beam displacement rate of 0.5 mm / min until the specimen completely fractures. Record the load-displacement curve during the test. Calculate the fracture toughness of the composite material by combining the maximum failure load, the specimen cross-sectional dimensions, and the initial pre-existing crack length.

[0095] (5) Place the unnotched impact specimen on the anvil of the pendulum impact testing machine, ensuring that the center of the specimen is aligned with the falling trajectory of the pendulum impact blade. The pendulum, releasing energy of 300J, breaks the specimen, and the impact absorption energy value displayed on the dial of the testing machine is read. Five parallel specimens are tested for each group of materials. After removing outliers with excessive dispersion, the arithmetic mean is calculated as the final test result.

[0096] Table 5. Test data of fracture toughness and impact toughness of composite materials in Example 2 and Comparative Examples 3 and 4

[0097] Conclusion: From Table 5 and Figure 5 The data shows that, Figure 5 The bar chart corresponding to the left vertical axis shows that the fracture toughness test value of Example 2 is 57.82 MPa·m. 1 / 2 , Figure 5 The line graph corresponding to the right-hand vertical axis shows that the impact absorption energy test value of Example 2 is 41.63 J. Comparative Example 3, which omits the first stage of heat treatment and insulation, shows a decrease in fracture toughness to 19.24 MPa·m. 1 / 2 The impact absorption energy decreased to 10.45 J. In Comparative Example 4, which omitted the third-stage heat treatment and heat preservation process, the fracture toughness was 31.57 MPa·m. 1 / 2 The impact absorption energy is 23.81 J.

[0098] Example 2 employed a three-stage in-situ reactive diffusion heat treatment process. In the first stage at 1065℃, the reaction interface was in a low-carbon activity state, and the hexagonal V2C phase preferentially precipitated at the interface. In the third stage at 850℃, the rate of carbon atom inward diffusion decreased, and the previously formed high aspect ratio V8C7 phase underwent morphological evolution, transforming from sharp ends to a smooth morphology. The smooth phase interface reduced the stress concentration phenomenon caused by the interface geometry, and the underlying V2C phase alleviated the mismatch of elastic modulus between the ceramic and metallic phases. The multi-level interface structure can deflect and bridge microcracks when the material is under stress, increasing the deformation energy absorption of the composite material during fracture.

[0099] From Table 5 and Figure 5 Data shows that Comparative Example 3 omitted the first-stage heat preservation process, and the composite precast block directly entered the high-temperature phase transformation stage of 1170℃. The reaction system skipped the thermodynamic generation range of the V2C phase, resulting in the direct generation of the cubic V8C7 phase inside the matrix. The high-hardness V8C7 phase directly contacts the metal matrix. The lack of the buffering effect of the equiaxed V2C phase leads to a modulus mismatch on both sides of the interface. Under stress, the crack directly penetrates the ceramic phase, and the crack deflection and energy absorption mechanisms cannot be activated, resulting in brittle fracture of the material. The toughness test value is at the lowest level.

[0100] Comparative Example 4 removed the 850°C isothermal test platform and directly cooled to room temperature after the second stage of heat preservation. Under these conditions, the rod-shaped V8C7 phase generated in the early stage maintained the sharp morphology of the initial growth. The lack of the isothermal morphology passivation process resulted in the retention of the unique interface geometry in the matrix. When subjected to external impact loads or test pre-existing crack propagation, stress concentration occurred at the sharp edge and new microcracks were induced to start. The propagation of microcracks caused the fracture toughness and impact absorption energy values ​​of Comparative Example 4 to be lower than those of Example 2.

[0101] Table 5 and Figure 5 The data distribution confirms that the first stage of heat treatment and the third stage of cooling and passivation are necessary steps to eliminate stress concentration at the internal interface of the material and improve the fracture toughness and impact toughness of the composite material.

[0102] Test Example 6: This test example compares the density, microstructure, and mechanical properties of the composite materials prepared in Example 2 and Comparative Example 6. The specific experimental steps are as follows: (1) According to the Archimedes drainage method described in Test Example 2, the actual density and volume porosity of the samples of Example 2 and Comparative Example 6 were tested respectively (the average value of 3 parallel samples was calculated for Comparative Example 6).

[0103] (2) The interface morphology and phase composition of the two groups of samples were observed and analyzed by scanning electron microscope (SEM) and X-ray diffraction (XRD).

[0104] (3) The room temperature compressive strength of the specimens of Example 2 and Comparative Example 6 was tested and evaluated according to the standards and procedures described in Test Example 4 (compression rate 0.3 mm / min).

[0105] (4) Summarize and compare the relevant test data.

[0106] Table 6. Comparison Test Data of Comprehensive Performance of Composite Materials in Example 2 and Comparative Example 6

[0107] Conclusion: Based on Table 6 and Figure 6 The comparative test data shows that the volumetric porosity of Comparative Example 6 is 2.85% (although it reaches the experimental lower limit of conventional density ≥95%, there are still obvious macroscopic pores), while the volumetric porosity of Example 2 is only 0.13%, which is at a low level. This is because Comparative Example 6 uses solid-phase powder pressing. Although a high pressure of 50MPa is applied, the rigid vanadium wire inside the mold will produce a bridging effect and spatial obstruction on the powder, which will cause the iron and carbon powder under the vanadium wire and the adjacent gaps to not be completely compacted. Micropores are easily left at the interface. Example 2 uses high-temperature liquid high-carbon steel for direct casting. Liquid metal has excellent fluidity. Combined with the pre-vacuum solid-phase degassing, it can fill all the mesh gaps of the three-dimensional woven preform without dead corners, and achieve a nearly fully dense metallurgical encapsulation.

[0108] According to Table 6 and Figure 6 It can be seen that Comparative Example 6 successfully generated a continuous pure V8C7 shell on the surface of vanadium wire through a high-temperature in-situ reaction at 1180℃. However, since the carbon source (graphite powder) in the powder metallurgy method is in direct contact with the vanadium wire, the barrier and flow-limiting effect of the boron-containing transition film formed by boric acid and urea precursor in Example 2 of this invention is lacking. At the same time, the thermodynamic control range of 1065℃, which preferentially generates the V2C phase, is also lacking. As a result, Comparative Example 6 generates a single, coarse V8C7 brittle phase shell. Example 2 formed a gradient transition layer composed of V8C7 and V2C, which alleviated the sharp change in elastic modulus between the metal and the ceramic.

[0109] Combined with Table 6 Figure 6As shown in the gray bar chart corresponding to the left vertical axis, the room temperature compressive strength of Example 2 reached 2456.4 MPa, which is higher than that of Comparative Example 6 (1682.3 MPa). Comparative Example 6, due to the simple unidirectional two-dimensional flat laying of vanadium wire, lacked three-dimensional spatial constraints. Furthermore, the high porosity (2.85%) at the interface and the stress concentration effect brought about by the single V8C7 phase caused the sample to easily develop cracks along the weak areas of powder bonding or brittle interfaces and fail prematurely when subjected to compressive stress. Example 2, benefiting from the macroscopic reinforcement of the three-dimensional orthogonal braided structure, low porosity, and gradient interface microstructure, exhibited excellent compressive bearing capacity, confirming the advanced nature and irreplaceability of the preparation method of this invention.

Claims

1. A method for preparing a bundled vanadium carbide reinforced steel-based composite material, characterized in that, Includes the following steps: The vanadium wire is completely immersed in a pre-treatment chemical isolation solution for constant temperature impregnation, and then placed in a forced-air drying oven for drying, forming a precursor solid film on the surface of the vanadium wire. The vanadium metal wire with the precursor solid film on its surface is made into a preform using a three-dimensional orthogonal weaving process; The preform is placed in a vacuum sintering furnace for heating and holding, and then cooled to room temperature to complete solid-phase pre-alloying. The preform that has undergone solid-phase pre-alloying is fixed in a mold and preheated and kept at a temperature under a first protective gas atmosphere. Simultaneously melt high-carbon steel matrix material until it is completely liquefied and keep the melt temperature constant. Inject the completely liquefied high-carbon steel matrix material into the mold to immerse the preform, and let it cool naturally to room temperature to obtain a composite preform block. The composite preform is placed in a resistance furnace with a second protective gas for in-situ reaction diffusion heat treatment, and then cooled to room temperature with the furnace to obtain the bundled vanadium carbide reinforced steel matrix composite material.

2. The preparation method according to claim 1, characterized in that, The pretreatment chemical isolation solution is made from raw materials comprising the following parts by weight: Boric acid 3.0-5.0 parts; Urea 1.0-2.0 parts; 93.0-96.0 parts of deionized water.

3. The preparation method according to claim 2, characterized in that, The preparation method of the pretreatment chemical isolation liquid includes: Add the corresponding weight parts of the boric acid and the urea to the deionized water, and heat under a constant temperature water bath at 40-50°C for 30-45 minutes with mechanical stirring until the solutes are completely dissolved.

4. The preparation method according to claim 1, characterized in that, During the process of completely immersing the vanadium wire in the pretreatment chemical isolation solution for constant temperature impregnation, the temperature of constant temperature impregnation is 40-50℃ and the impregnation time is 3-5 minutes. During the drying process of the removed vanadium metal wire in the blower drying oven, the drying temperature is 110-120℃ and the drying time is 30-45 minutes.

5. The preparation method according to claim 1, characterized in that, During the process of forming the preform from the vanadium wires with the precursor solid film on the surface, the spacing between the vanadium wires is controlled to be 1.5-2.0 mm.

6. The preparation method according to claim 1, characterized in that, During the heating and heat preservation process of the preform placed in a vacuum sintering furnace, the absolute pressure inside the vacuum sintering furnace is less than 0.01 Pa, and the temperature is raised to 750-800℃ at a heating rate of 8-10℃ / min, and the constant temperature holding time is 1.5-2.5h.

7. The preparation method according to claim 1, characterized in that, The mold is a graphite mold; During the process of fixing the preform that has undergone solid-phase pre-alloying in the mold for preheating and heat preservation, the preheating temperature is 350-400℃, the heat preservation time is 0.5-1.5h, and the first protective gas used is argon.

8. The preparation method according to claim 1, characterized in that, The melt temperature of the high-carbon steel matrix material after complete liquefaction is constant at 1450-1480℃. The operation of injecting the fully liquefied high-carbon steel matrix material into the mold is carried out by gravity casting.

9. The preparation method according to claim 1, characterized in that, The in-situ reaction diffusion heat treatment process is as follows: Heat to 1050-1080℃ at a heating rate of 5-8℃ / min, and hold at that temperature isothermally for 1.5-2.5 hours. Then continue heating at a heating rate of 4-6℃ / min to 1160-1180℃, and hold at that temperature isothermally for 3-4 hours; Finally, the temperature is reduced to 850℃ at a cooling rate of 8-12℃ / min, and isothermal held at 850℃ for 1-1.5 hours.

10. The preparation method according to claim 1, characterized in that, When the composite preform is placed in a resistance furnace for in-situ reaction diffusion heat treatment, the second protective gas introduced is high-purity argon.