Layered material, electrode active material for electrochemical devices, electrochemical device, and electrochemical capacitor

By using novel layered materials, the problem of insufficient specific capacitance in electrochemical devices has been solved, and electrochemical capacitors with high specific capacitance and high energy density have been realized.

CN122422960APending Publication Date: 2026-07-17PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480080777.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-27
Filing Date
2024-09-24
Publication Date
2026-07-17

AI Technical Summary

Technical Problem

In existing technologies, the specific capacity of the electrode active materials in electrochemical devices is insufficient, making it difficult to meet the requirements for high performance.

Method used

A novel layered material is used, the main body of which is composed of M1(1-a)mM2amXn, where M1 and M2 are different atoms from Ti, Sc, Y, La, Zr and Hf, and X is a carbon or nitrogen atom. The terminal contains atoms with high electronegativity. The terminal is formed by selective etching, which improves the specific capacity of the electrode active material.

Benefits of technology

It significantly improves the specific capacitance and energy density of electrochemical devices, enhancing the performance of electrochemical capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122422960A_ABST
    Figure CN122422960A_ABST
Patent Text Reader

Abstract

The layered material (1a) has a layer (10). The layer (10) has a main body (11) and a terminal (12). The main body (11) has M1 (1‑a)m M2 am X n The composition. In this composition, M1 and M2 are different atoms selected from Ti, Sc, Y, La, Zr and Hf. X contains at least one of carbon and nitrogen atoms. a is greater than 0 and less than 1. n is greater than 1 and less than 4. m is greater than n and less than 5. Terminal (12) is present on the surface of the body (11).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to layered materials, electrode active materials for electrochemical devices, electrochemical devices, and electrochemical capacitors. Background Technology

[0002] In recent years, a material called MXene has attracted much attention. MXene is a two-dimensional (2D) material, as described below, which is a layered material with one or more layers. MXene typically has the particle morphology of this layered material, and the particles can be in the form of powder, plates, or sheets.

[0003] Currently, the application of MXene in electrochemical capacitors is being studied. For example, Non-Patent Literature 1 describes a case where, in the production of two-dimensional titanium carbide as a type of MXene by etching Al from Ti3AlC2, the electrostatic capacitance per unit volume increases when a solution of lithium fluoride and hydrochloric acid is used.

[0004] Prior art literature

[0005] Non-patent document 1: Michael Ghidiu et al., "Conductive two-dimensionaltitanium carbide 'clay' with high volumetric capacitance", Nature volume 516, pages78-81 (2014) Summary of the Invention

[0006] The problem that the invention aims to solve

[0007] This disclosure provides a novel layered material that is advantageous from the viewpoint of improving the performance of electrochemical devices.

[0008] Methods for solving problems

[0009] The layered material disclosed herein comprises a body and layers having terminals present on the surface of the body, the body having M1 (1-a)m M2 am X n The composition,

[0010] In the composition,

[0011] M1 and M2 are distinct atoms selected from Ti, Sc, Y, La, Zr, and Hf.

[0012] X contains at least one selected from carbon and nitrogen atoms.

[0013] a is greater than 0 and less than 1.

[0014] n is 1 or more and 4 or less

[0015] m is greater than n and less than 5.

[0016] The effects of the invention

[0017] According to this disclosure, a novel layered material that is advantageous from the viewpoint of improving the performance of electrochemical devices can be provided. Attached Figure Description

[0018] Figure 1 This is a diagram that schematically represents an example of a layered material.

[0019] Figure 2 This is a diagram schematically representing an example of an electrochemical capacitor.

[0020] Figure 3A The graphs represent the X-ray diffraction (XRD) results of the precursors of the layered materials in Examples 1, 2, 3 and Comparative Example 1.

[0021] Figure 3B These are graphs showing the XRD measurement results of the layered materials of Example 1, Example 2, Example 3 and Comparative Example 1.

[0022] Figure 4 The graph shows the XRD results of the precursor, Ti2SnC, and Zr2SnC of Reference Example 1.

[0023] Figure 5 This is a graph showing the particle size distribution of the layered materials in Example 1, Example 2 and Comparative Example 1.

[0024] Figure 6A This is a scanning electron microscope (SEM) image of the layered material in Example 1.

[0025] Figure 6B This is an SEM image of the layered material from Example 2.

[0026] Figure 6C This is a SEM image of the layered material in Comparative Example 1. Detailed Implementation

[0027] (The insights that form the basis of this disclosure)

[0028] As described in Non-Patent Document 1, MXene is considered as an electrode active material for electrochemical devices such as electrochemical capacitors. In such electrochemical devices, the capacitance per unit volume or per unit mass of the electrode active material [F / cm³] is important. 3[Or F / g] indicates a high specific capacity. Therefore, the inventors conducted in-depth research on MXene, which can be used as an electrode active material in at least one of the negative and positive electrodes of electrochemical devices. As a result, it was newly discovered that by using a prescribed layered material as the electrode active material, the specific capacity in an electrochemical device can be easily increased. Based on this new insight, the inventors completed the layered material of this disclosure.

[0029] (Implementation Method)

[0030] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. The present disclosure is not limited to the following embodiments.

[0031] Figure 1 An example of a layered material of this disclosure is schematically shown. For example... Figure 1 As shown, the layered material 1a includes a layer 10. Layer 10 includes a main body 11 and a terminal 12. The main body 11 has M1 (1-a)m M2 am X n The composition of the layer 10 is as follows: M1 and M2 are distinct atoms selected from Ti, Sc, Y, La, Zr, and Hf. X is selected from at least one of carbon and nitrogen atoms. a is greater than 0 and less than 1. n is greater than 1 and less than 4. m is greater than n and less than 5. Terminal 12 is an atom or functional group present on the surface of the body 11. If the atom or functional group forming terminal 12 is denoted as T, then layer 10 has M1. (1-a)m M2 am X n T s The composition of . s is any number.

[0032] As described above, in the layered material 1a, the main body 11 has M1 (1-a)m M2 am X n The composition of the material is such that, for example, when layered material 1a is used as the electrode active material in an electrochemical device, a higher specific capacity is more easily achieved compared to when MXene containing only Ti as a transition metal is used as the electrode active material in an electrochemical device. The reason for this is not yet clear. The atomic radii of M1 or M2 contained in the above composition are relatively large. It is believed that this affects the configuration of the functional groups or atoms at the terminal 12, making it easier to reduce the thickness of the electric double layer generated in the electrochemical device. Therefore, it is believed that a high specific capacity is easily achieved when layered material 1a is used as the electrode active material in an electrochemical device.

[0033] In the main body 11, the configuration of M1, M2, and X is not limited to a specific configuration. For example, in the main body 11, M1 and M2 are arranged at the vertices of the octahedron in an arrangement of multiple octahedrons forming a common edge, i.e., an octahedral array. Furthermore, X is arranged inside each octahedron.

[0034] M1 and M2 are not limited to specific atoms as long as they are different atoms selected from Ti, Sc, Y, La, Zr, and Hf. M1 and M2 are preferably different atoms selected from Ti, Zr, and Hf. In this case, when the layered material 1a is used as the electrode active material of the electrochemical device, it is easier to achieve a high specific capacity.

[0035] In the above composition, it is more preferable that M1 is Ti and M2 is Zr. In this case, when the layered material 1a is used as the electrode active material of the electrochemical device, it is easier to achieve a high specific capacity.

[0036] In the above composition, M1 can be Ti or Zr, and M2 can be Sc, Y, or La. In this case, when the layered material 1a is used as the electrode active material of the electrochemical device, it is easier to achieve a high specific capacity.

[0037] In the above composition, as long as n is greater than or equal to 1 and less than or equal to 4, and m is greater than n and less than or equal to 5, n and m are not limited to specific values. n can be, for example, 1, 2, 3, or 4, or a value satisfying the conditions 1 < n < 2, 2 < n < 3, or 3 < n < 4. For example, if defects such as vacancies exist in the crystal forming the main body 11, then n may not be an integer. m can, for example, satisfy the condition m = n + 1.

[0038] In the above composition, n is preferably 2 and m is 3. In this case, when the layered material 1a is used as the electrode active material of the electrochemical device, it is easier to achieve a high specific capacity.

[0039] In the above composition, 'a' is not limited to a specific value as long as it is greater than 0 and less than 1. 'a' is preferably greater than 0 and less than 0.33. In this case, when the layered material 1a is used as the electrode active material of the electrochemical device, it is easier to achieve a high specific capacity.

[0040] In the above composition, a can be greater than 0 and less than 0.2.

[0041] In the above composition, a can be greater than 0 and less than 0.1.

[0042] In the above composition, a can be greater than 0 and less than 0.67, or greater than 0 and less than 0.5.

[0043] In the above composition, M1 can be Ti or Zr, and M2 can be Hf, Sc, Y, or La. In this case, a can be greater than 0 and less than 0.67. In this case, when the layered material 1a is used as the electrode active material of the electrochemical device, it is easier to achieve a high specific capacity. In this case, further, a can be greater than 0 and less than 0.5, or a can be greater than 0 and less than 0.33.

[0044] In the above composition, X may contain carbon atoms. In this case, when layered material 1a is used as the electrode active material of an electrochemical device, it is easier to achieve a high specific capacity. X may contain only carbon atoms, only nitrogen atoms, or both carbon and nitrogen atoms.

[0045] In the above composition, X may also contain oxygen atoms. The oxygen content in X can be 20% to 80%, or 30% to 75%. Furthermore, even when X is not intended to contain oxygen atoms, oxygen atoms from the raw materials may sometimes replace carbon atoms and be included in X. The oxygen content in X, based on the number of atoms, can be less than 20%, and can be less than 10%, less than 5%, less than 1%, or less than 0.1%. X may also not contain oxygen atoms.

[0046] Terminal 12 is not limited to any specific atom or group of atoms that can exist on the surface of the body 11. For example, terminal 12 may contain atoms with electronegativity greater than that of M1 and M2 contained in the body 11. In this case, terminal 12 is likely to exist on the surface of the body 11 in a desired state. Examples of atoms with electronegativity greater than M1 and M2 include hydrogen atoms, oxygen atoms, halogen atoms, chalcogenides, nitrogen atoms, phosphorus atoms, carbon atoms, and antimony atoms. Electronegativity is defined based on polarization.

[0047] Terminal 12 may contain, for example, at least one selected from hydroxyl, hydrogen, halogen, chalcogen, amino, phosphorus, and antimony atoms. In this case, terminal 12 is more likely to exist on the surface of body 11 in the desired state.

[0048] like Figure 1 As shown, the layered material 1a, for example, comprises multiple layers 10. In this case, the layered material 1a has, for example, a multilayer structure in which multiple layers 10 are separated from each other and stacked. In this case, two adjacent layers 10 may not be completely separated and may include contact areas. The layered material 1a may also have a single-layer structure consisting of only one layer 10. An assembly of single-layer or multilayer structures composed of the layered material 1a can be particles such as powders and flakes.

[0049] The thickness of layer 10 is not limited to a specific value. The thickness of layer 10 may be, for example, 0.5 nm or more and 5 nm or less, or 0.5 nm or more and 3 nm or less. This thickness can vary depending on the number of atomic layers formed by M1 and M2.

[0050] The maximum size of layer 10 in the in-plane direction perpendicular to the thickness direction of layer 10 is not limited to a specific value. Its maximum size is, for example, 0.1 μm or more and 200 μm or less, or 1 μm or more and 40 μm or less.

[0051] When the layered material 1a has a multilayer structure, the distance d between the layers 10 in the multilayer structure is not limited to a specific value. The distance d can be, for example, 0.1 nm or more and 10 nm or less, 0.1 nm or more and 5 nm or less, or approximately 1 nm.

[0052] When the layered material 1a has a multilayer structure, the maximum size of the layered material 1a in the in-plane direction perpendicular to the thickness direction of layer 10 is not limited to a specific value. For example, its maximum size is 0.1 μm or more and 100 μm or less, or it can be 1 μm or more and 20 μm or less.

[0053] When the layered material 1a has a multilayer structure, cations can exist between adjacent layers 10 in the thickness direction of the layers 10. Examples of cations include protons (H). + Alkali metal ions, alkaline earth metal ions, and quaternary ammonium ions, etc., can exist. Anions or solvents coordinated with cations in layer 10 can also exist. Examples of anions and solvents coordinated with cations include halide ions, H₂O, and propylene carbonate.

[0054] When the layered material 1a has a multilayer structure, the number of layers 10 contained in the layered material 1a is 2 or more, and can be 20 or more but less than 100,000 or more but less than 20,000. In the thickness direction of the layers 10, the thickness of the layered material 1a is not limited to a specific value. Its thickness is, for example, 0.1 μm or more but less than 200 μm, or 1 μm or more but less than 40 μm.

[0055] When the layered material 1a has a multi-layered structure, the number of layers 10 contained in the layered material 1a can be 6 or less. In this case, the layered material 1a is referred to as a low-layered structure.

[0056] In an assembly of layered material 1a, for example, the majority of the assembly may be a single-layer structure of layered material 1a and / or a low-layer structure. For example, more than 50% by volume of the assembly may be a single-layer structure of layered material 1a and / or a low-layer structure.

[0057] The aforementioned dimensions and distances can be calculated, for example, by arithmetic averaging based on microscope images from scanning electron microscopes (SEM), transmission electron microscopes (TEM), atomic force microscopes (AFM), etc. In this case, for example, the aforementioned dimensions and distances can be calculated by arithmetic averaging of more than 40 data points. Alternatively, the aforementioned dimensions and distances can also be calculated as actual spatial distances based on the positions of the (002) planes in the reciprocal lattice space determined by X-ray diffraction (XRD).

[0058] The method for manufacturing the layered material 1a is not limited to a specific method. For example, the layered material 1a can be manufactured from materials having M... m AX n The precursor is synthesized by selectively etching A atoms in its composition. In the composition of the precursor, M represents the metal atoms corresponding to M1 and M2 in the body 11 of the layered material 1a, and m and n correspond to m and n in the body 11, respectively. A can be an element from Group 12, Group 13, Group 14, Group 15 or Group 16, and A can be at least one element selected from Al, Zn, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, S and Cd. A is preferably Al. This precursor is called MAX, having a composition of M... m X n The two layers represent a crystalline structure consisting of one layer of A atoms positioned between them. In M... m X n In each layer, M is arranged at the vertices of the octahedron in an octahedral array, forming multiple octahedrons sharing a common edge. Furthermore, X is positioned inside each octahedron. In other words, M... m X n Each layer of MAX has M atoms arranged in an octahedral manner and X atoms arranged inside the octahedron. The structure of MAX is not limited to a specific structure; for example, it has a structure in which one layer of X atoms is arranged between (n+1) M atomic layers, provided that m=n+1. In addition, it has repeating units with A atomic layers arranged adjacent to the (n+1)th M atomic layer.

[0059] In MAX, the A-atom layer is removed by selectively etching A atoms. This exposes the M-atom layer. m X n On the surface of the layer, atoms or groups of atoms from the etching solution modify its surface, forming terminal 12.

[0060] Etching solutions used for selective etching of A atoms, for example, those containing fluoride ions F. -The etching solution can be a mixture of lithium fluoride and hydrochloric acid or hydrofluoric acid. Selective etching of A atoms can be performed using molten salts of Lewis acids such as CuCl2, high-temperature and high-pressure HCl, halogen gases such as Br2 and I2, or organic solutions containing dissolved halogens such as Br2 and I2.

[0061] Layered material 1a can be prepared from precursors other than MAX. For example, it can be prepared by using precursors from two M... m X n Layered materials 1a are fabricated by selectively etching A atoms in a precursor with two or more A atom layers between the layers.

[0062] After selectively etching A atoms from precursors such as MAX, treatments such as ultrasonic treatment, manual shaking, or vibration using an automatic oscillator can be performed. These treatments promote the separation (delamination) of layers 10 in the layered material 1a. Thus, for example, a layered material 1a with a monolayer structure or as a low-layer structure can be obtained. For example, by using manual shaking or vibration using an automatic oscillator, shear stresses desired from the viewpoint of layer 10 separation can be applied between the layers 10. For example, consider the case where the layered material 1a has a monolayer structure or is a low-layer structure. In this case, the ratio of the size of the layered material 1a in the thickness direction of layer 10 to the size of the layered material 1a in the in-plane direction of layer 10 is small. Even in such cases, by using manual shaking or vibration using an automatic oscillator, shear stresses desired from the viewpoint of layer 10 separation can be applied between the layers 10, making the layered material 1a difficult to break and easily maintaining its desired size.

[0063] In the layered material 1a, a portion of the A atoms from the precursor such as MAX may remain. The amount of A atoms remaining in the layered material 1a is, for example, 10% by mass or less of the content of A atoms in the precursor, preferably 8% by mass or less, and more preferably 6% by mass or less. The amount of A atoms remaining in the layered material 1a may also be greater than 10% by mass of the content of A atoms in the precursor, depending on the application of the layered material 1a.

[0064] Layered material 1a can also be manufactured by methods other than selectively etching A atoms from precursors such as MAX. For example, it can be manufactured by heat treatment of metal M1, metal M2, graphite, or a halide of M1 or M2 inside a sealed tube. The sealed tube is, for example, a quartz tube. Layered material 1a can also be manufactured by chemical vapor deposition (CVD) using metal M1, metal M2, a halide of M1 or M2, and CH4 or N2.

[0065] For example, it is possible to provide an electrode active material for electrochemical devices containing a layered material 1a. As described above, by using such an electrode active material in an electrochemical device, a high specific capacity can be easily achieved in the electrochemical device.

[0066] An electrode containing a layered material 1a as the electrode active material can be provided. In this case, the surface of the electrode may be substantially composed solely of the layered material 1a, or there may be an adhesive between the layered materials 1a. The adhesive may include, for example, a resin, comprising at least one selected from polytetrafluoroethylene, polyvinylidene fluoride, and styrene-butadiene rubber. The electrode containing the layered material 1a as the electrode active material can be manufactured by molding an assembly of the layered material 1a, or a mixture of an assembly of the layered material 1a and an adhesive, into a film or sheet. For example, methods including suction filtration can be applied in the manufacture of the electrode. Alternatively, coating methods such as spraying, rod coating, or dip coating can be used to manufacture the electrode.

[0067] The electrode described above can also be fabricated using a precursor of layered material 1a or a modified version of layered material 1a. For example, layered material 1a is used to coat the surface of polymer particles such as polystyrene in a solvent to obtain coated particles. Next, the solvent is removed, and the aggregate of coated particles is formed into a film. Then, the polymer is removed by high-temperature treatment or the like, leaving behind shell-like hollow particles of layered material 1a. This method can also be used to fabricate the electrode. In this case, the specific capacity of the electrochemical device using the electrode can easily be increased, and the coulombic efficiency can easily be improved.

[0068] The density of the aforementioned electrodes is not limited to a specific value. For example, its density is 1.5 g / cm³. 3 Above, 2.0g / cm 3 Above, or 2.5g / cm 3 The above, preferably 3.0 g / cm³ 3 The above. Its density is more preferably 3.5 g / cm³. 3 The above is further optimized to 4.0 g / cm³. 3 The above, especially preferred, is 4.5 g / cm³. 3 The above. Its density is, for example, 10 g / cm³. 3 the following.

[0069] The thickness of the aforementioned electrodes is not limited to a specific value. For example, its thickness may be 3 μm or more, 5 μm or more, or less than 500 μm.

[0070] An electrochemical device, for example, includes a pair of electrodes and an electrode active material configured to contact at least one of the electrodes. The electrode active material may contain a layered material 1a.

[0071] Figure 2This is a schematic diagram illustrating an example of an electrochemical capacitor. (See diagram for example.) Figure 2 As shown, the electrochemical capacitor 2a includes a positive electrode 3a and a negative electrode 3b. In the electrochemical capacitor 2a, the positive electrode 3a and the negative electrode 3b are disposed separately in the electrolyte 4. At least one of the positive electrode 3a and the negative electrode 3b contains a layered material 1a as the electrode active material. According to this structure, the electrochemical capacitor 2a can easily achieve a high specific capacitance.

[0072] The energy density stored in an electrochemical capacitor is typically calculated as (1 / 2) × CV. 2 Where C is the specific capacity [F / cm³] 3 [or F / g], where V is the operating potential range [V]. The unit of energy density can be FV. 2 / cm 3 or FV 2 / g. On the other hand, the energy density stored in an electrochemical capacitor can usually be expressed in units of Wh / L or Wh / kg.

[0073] Suppose that for either the positive or negative electrode of an electrochemical capacitor, the specific capacitance C of that electrode is determined by measuring it using a half-cell method with a three-electrode approach. 3p [F / cm] 3 Or in the case of F / g]. In this case, the specific capacity C of the full cell formed by using this electrode for both the positive and negative electrodes is... f [F / cm] 3 [F / g] can be calculated to be equal to (1 / 4)C 3p .

[0074] Electrolyte 4 is not limited to a specific electrolyte. For example, electrolyte 4 can be a non-aqueous electrolyte. In this case, the operating potential range of electrochemical capacitor 2a can be easily increased. From the viewpoint of increasing the energy density stored in electrochemical capacitor 2a, a large operating potential range is advantageous. Electrolyte 4 can also be an aqueous electrolyte. In this case, to prevent water electrolysis, the operating potential range can be adjusted to below 1.2V. Furthermore, the usable temperature range of electrochemical capacitor 2a can be adjusted to a temperature range that allows water, as a solvent, to exist stably in a liquid state and prevents freezing and vaporization (e.g., -40°C to 80°C). On the other hand, when electrolyte 4 is a non-aqueous electrolyte, compared to when electrolyte 4 is an aqueous electrolyte, there are fewer restrictions on the operating potential range and usable temperature range of electrochemical capacitor 2a.

[0075] like Figure 2As shown, in the electrochemical capacitor 2a, an electrolyte 4 is contained inside a cell 5. The interior of cell 5 is divided by a diaphragm 7 into a space containing a positive electrode 3a and a space containing a negative electrode 3b. The positive electrode 3a and the negative electrode 3b are electrically connected to terminals 6a and 6b located outside cell 5, respectively.

[0076] The diaphragm 7 is not limited to a specific type of diaphragm as long as it does not impede the movement of electrolyte ions contained in the electrolyte 4. For example, the diaphragm 7 can be a dielectric membrane. Examples of dielectric membranes include porous membranes of polyolefins such as polypropylene and polytetrafluoroethylene. The diaphragm 7 may contain glass fibers.

[0077] The material of unit 5 is not limited to a specific material. The material of unit 5 can be metal materials such as stainless steel, resin materials such as polytetrafluoroethylene, or other materials. Unit 5 can be closed or open. There may or may not be gaps inside unit 5.

[0078] For example, the positive electrode 3a and the negative electrode 3b can be inside the unit 5, with a separator 7 disposed between the positive electrode 3a and the negative electrode 3b, and the stack containing the positive electrode 3a, the separator 7 and the negative electrode 3b are wound up.

[0079] As described above, at least one of the positive electrode 3a and the negative electrode 3b contains a layered material 1a as the electrode active material. The electrode active material, for example, performs electron transfer with electrolyte ions contained in the electrolyte 4.

[0080] For example, the positive electrode 3a may contain only layered material 1a as the electrode active material. In this case, the negative electrode 3b may contain activated carbon, carbon nanotubes, and carbon materials such as graphene or Li4Ti5O. 12 The positive electrode 3a may contain layered material 1a as the electrode active material, or only the negative electrode 3b may contain layered material 1a as the electrode active material. In this case, the positive electrode 3a may contain graphite, activated carbon, or carbon nanotubes as the electrode active material. When only the positive electrode 3a or the negative electrode 3b contains layered material 1a as the electrode active material, the electrode without layered material 1a may be substantially composed solely of the electrode active material, or it may be configured such that there is a binder between the electrode active materials. The binder may contain, for example, a resin. The binder may contain, for example, at least one selected from polytetrafluoroethylene, polyvinylidene fluoride, and styrene-butadiene rubber. Both the positive electrode 3a and the negative electrode 3b may contain layered material 1a as the electrode active material.

[0081] The positive electrode 3a and the negative electrode 3b can be configured as independent freestanding films, or they can have a structure in which a thin film and / or membrane containing electrode active material is formed on the current collector (not shown). The current collector is not limited to a specific type as long as it is conductive. For example, the current collector may contain materials such as stainless steel, aluminum, or aluminum alloy.

[0082] Electrolyte 4 may contain an electrolyte and a non-aqueous solvent. Electrolyte 4 may contain both an electrolyte and an aqueous solvent, or it may be an ionic liquid. The electrolyte is dissolved in either a non-aqueous or aqueous solvent and exists in the form of cations or anions.

[0083] Electrolyte 4 contains, for example, at least one cation selected from the group of cations below and at least one anion selected from the group of anions below as an electrolyte.

[0084] <Cation Group>

[0085] Sodium ions (Na) + ),

[0086] Magnesium ions (Mg 2+ ),

[0087] 1-Ethyl-3-methylimidazolium ion (EMI) + ),

[0088] Tributylmethylammonium ion (TrBMAm) + ),

[0089] Tetrabutylammonium ion (TeBAm) + ),

[0090] Tributylethylphosphonium ion (TrBEPh) + ),

[0091] Tributylmethylphosphonium ion (TrBMPh) + ),

[0092] 1-Butyl-1-methylpyrrolidine ononium ion (1B1MPy) + ),

[0093] 1-Methyl-1-propylpyrrolidineonium ion (1M1PPy) + ),

[0094] Tetraethylammonium ion (Et4N+).

[0095] Lithium ion (Li + ),as well as

[0096] Proton (H) + ).

[0097] <Anion group>

[0098] Diethyl phosphate ion (DEPh) - ),

[0099] bis(fluorosulfonyl)imide ion (FSI) - ),

[0100] Perchlorate ions (ClO3O) - ),

[0101] bis(trifluoromethanesulfonyl)imide ion (TFSI) - ),

[0102] Trifluoromethanesulfonate ion (Triflate - ),

[0103] Hexafluorophosphate ion (P-F6).

[0104] Tetrafluoroborate ion (B-F4).

[0105] sulfate ions (SO4) 2- ),

[0106] Chloride ions (Cl) - ),as well as

[0107] Iodide ions (I - ).

[0108] The non-aqueous solvent that may be included in the electrolyte 4 is not limited to a specific non-aqueous solvent. For example, the electrolyte 4 may contain at least one solvent selected from the group consisting of the following solvents. The non-aqueous solvent may be only one solvent or may be a mixture of multiple solvents.

[0109] <Solvent Group>

[0110] propylene carbonate (PC)

[0111] γ-Butyrolactone (gBL)

[0112] Ethylene carbonate (EC).

[0113] Ethyl methyl carbonate (EMC).

[0114] Dimethoxyethane (DME)

[0115] Dimethyl carbonate (DMC).

[0116] Diethyl carbonate (DEC), and

[0117] Acetonitrile (AN).

[0118] Electrolyte 4 may contain specified additives in addition to solvents and electrolytes, as required.

[0119] When terminals 6a and 6b of the electrochemical capacitor 2a are connected to a load, the electrochemical capacitor 2a discharges. On the other hand, when terminals 6a and 6b of the electrochemical capacitor 2a are connected to a power source, the electrochemical capacitor 2a is charged.

[0120] Depending on the combination of the electrode active material and the electrolyte 4, the electrochemical capacitor 2a can also be configured as a pseudo capacitor or a hybrid capacitor that includes a Faraday reaction.

[0121] (Postscript)

[0122] Based on the above description, the following technical solution is disclosed.

[0123] (Technical Solution 1)

[0124] A layered material comprising a body and terminals present on the surface of the body, the body having M1 (1-a)m M2 am X n The composition,

[0125] In the composition,

[0126] M1 and M2 are distinct atoms selected from Ti, Sc, Y, La, Zr, and Hf.

[0127] X contains at least one selected from carbon and nitrogen atoms.

[0128] a is greater than 0 and less than 1.

[0129] n is 1 or more and 4 or less

[0130] m is greater than n and less than 5.

[0131] (Technical Solution 2)

[0132] According to the layered material described in technical solution 1

[0133] The terminal contains atoms with electronegativity greater than that of M1 and M2.

[0134] (Technical Solution 3)

[0135] The layered material according to technical solution 1 or 2

[0136] The terminal comprises at least one selected from hydroxyl, hydrogen, halogen, chalcogen, amino, phosphorus and antimony atoms.

[0137] (Technical Solution 4)

[0138] The layered material according to any one of technical solutions 1 to 3,

[0139] n is 2, m is 3.

[0140] (Technical Solution 5)

[0141] The layered material according to any one of technical solutions 1 to 4,

[0142] X contains carbon atoms.

[0143] (Technical Solution 6)

[0144] The layered material according to any one of technical solutions 1 to 5,

[0145] M1 and M2 are distinct atoms selected from Ti, Zr, and Hf.

[0146] (Technical Solution 7)

[0147] The layered material according to any one of technical solutions 1 to 6,

[0148] M1 is Ti, and M2 is Zr.

[0149] (Technical Solution 8)

[0150] According to the layered material described in technical solution 7

[0151] a is greater than 0 and less than 0.33.

[0152] (Technical Solution 9)

[0153] According to the layered material described in technical solution 7

[0154] a is greater than 0 and less than 0.2.

[0155] (Technical Solution 10)

[0156] According to the layered material described in technical solution 5

[0157] a is greater than 0 and less than 0.1.

[0158] (Technical Solution 11)

[0159] The layered material according to any one of technical solutions 1 to 5,

[0160] M1 is either Ti or Zr.

[0161] M2 is Sc, Y, or La.

[0162] (Technical Solution 12)

[0163] The layered material according to any one of technical solutions 1 to 5,

[0164] M1 is either Ti or Zr.

[0165] M2 is Hf, Sc, Y, or La.

[0166] a is greater than 0 and less than 0.67.

[0167] (Technical Solution 13)

[0168] The layered material according to technical solution 12

[0169] a is greater than 0 and less than 0.5.

[0170] (Technical Solution 14)

[0171] The layered material according to technical solution 12

[0172] a is greater than 0 and less than 0.33.

[0173] (Technical Solution 15)

[0174] An electrode active material for an electrochemical device comprises the layered material described in any one of technical solutions 1 to 14.

[0175] (Technical Solution 16)

[0176] An electrochemical device comprising a pair of electrodes and an electrode active material disposed in contact with at least one of the pair of electrodes.

[0177] The electrode active material comprises the layered material described in any one of technical solutions 1 to 14.

[0178] (Technical Solution 17)

[0179] An electrochemical capacitor having a positive electrode and a negative electrode.

[0180] The positive electrode and the negative electrode are configured separately in the electrolyte.

[0181] The layered material selected from at least one of the positive electrode and the negative electrode comprises any one of technical solutions 1 to 14 as the electrode active material.

[0182] (Technical Solution 18)

[0183] The electrochemical capacitor according to technical solution 17

[0184] The negative electrode contains the layered material as the electrode active material.

[0185] Example

[0186] The present disclosure will now be described in more detail through examples. However, the following examples are merely illustrative and the present disclosure is not limited to them.

[0187] (Example 1)

[0188] TiC powder, ZrC powder, Ti powder, and Al powder were mixed in a zirconia mortar to obtain the mixed powder of Example 1. These powders were provided by the High Purity Chemical Research Institute, Ltd. The molar ratio of TiC:ZrC:Ti:Al in the mixed powder of Example 1 was 1.7:0.3:1:1. The mixed powder of Example 1 was calcined at 1500°C for 1 hour in an argon atmosphere to obtain the calcined body (block) of Example 1. The calcined body of Example 1 was then pulverized in a zirconia mortar. This yielded a product containing Ti... 2.7 Zr 0.3 The powder of the precursor of AlC2 in Example 1.

[0189] The precursor powder, CuCl2 powder, and NaCl powder from Example 1 were mixed in a zirconia mortar to obtain a mixed powder. The molar ratio of Ti in this mixed powder was... 2.7 Zr 0.3 The AlC2:CuCl2:NaCl ratio was 1:3:4. This mixed powder was calcined at 650°C for 10 hours under an argon atmosphere to obtain a calcined body (block). The calcined body was then pulverized in a zirconia mortar. The resulting powder was washed with pure water to remove chlorides. Next, Cu was removed by washing the calcined body with 0.1M ammonium persulfate. The washed calcined body was then filtered and vacuum dried at room temperature (15°C–28°C). This yielded a product containing Ti. 2.7 Zr 0.3 C2T s The composition of the layered material powder in Example 1. T represents the atoms or functional groups that form the terminals of the layered material, and s is an arbitrary number.

[0190] While adding N-methyl-2-pyrrolidone, the powder of the layered material from Example 1, acetylene black powder, and polyvinylidene fluoride were mixed to obtain a slurry. The slurry was applied to an aluminum foil with an etched surface using a coater, and the resulting coating was vacuum dried at 60°C to obtain a film containing MXene. The laminate of the aluminum foil and the MXene-containing film was cut into rectangles with a short side length of 10 mm and a long side length of 20 mm when viewed from top view to obtain the electrode of Example 1.

[0191] Next, a three-electrode electrochemical capacitor, serving as a half-unit for evaluation, was assembled. This half-unit was configured such that the applied voltage was entirely applied to the electrode of Example 1. The assembly and evaluation of the electrochemical capacitor were carried out inside a glove box under an argon atmosphere simulating actual manufacturing and usage conditions.

[0192] The electrode of Example 1 was used as the working electrode of the 3-electrode unit. An activated carbon electrode (AC) was used as the counter electrode of the 3-electrode unit. Activated carbon and polytetrafluoroethylene (PTFE) as a binder were mixed at a mass ratio of 95:5 to obtain a mixture containing activated carbon. This mixture containing activated carbon was molded on a Ti mesh, and Pt wires were mounted on the resulting molded product to obtain the activated carbon electrode. This activated carbon electrode has a capacitance approximately 10 times greater than that of the electrode of Example 1. An Ag / Ag electrode manufactured by EC Frontier was used as the reference electrode of the 3-electrode unit. + Reference electrode. A commercially available 1M Li-PF6 / EC-DMC electrolyte was used as the electrolyte for the 3-electrode unit.

[0193] The main body of the 3-electrode unit used a plate electrode evaluation unit (product code 011951) manufactured by BAS Corporation. A rectangular aluminum substrate with a short side length of approximately 10 mm and a long side length of approximately 20 mm was placed on a lower block made of fluororesin, serving as the base. Next, the electrode of Example 1 was placed on the aluminum substrate with the MXene-containing film of Example 1 facing upwards. A main body block with cylindrical through-holes and attached fluororesin O-rings was placed on the electrode of Example 1. A pair of screws located at both ends of the main body block were screwed in evenly, clamping the electrode of Example 1 between the lower block and the main body block. 1 mL of electrolyte was added to the space within the main body block. A counter electrode and a reference electrode were installed on the unit cap and fixed by embedding them into the main body block. Thus, an evaluation half-unit, i.e., an electrochemical capacitor, was assembled as a plate electrode evaluation unit. After assembly, the electrochemical capacitor was allowed to stand for 1 hour.

[0194] (Electrochemical measurement)

[0195] Electrochemical measurements were performed using the assembled electrochemical capacitor, i.e., the evaluation half-unit. In an argon-atmospheric glove box, the working electrode and reference electrode of the assembled electrochemical capacitor were connected to an external electrode. Using an electrochemical measuring device 1287A (Solartron Analytical) and CorrWare software, the scan rate was set to 1 mV / s, and the scan range relative to the reference electrode was set to 0 V (or open potential) to -2 V. Cyclic voltammetry (CV) measurements were then performed. Based on the CV measurement results of the evaluation half-unit, the capacitance per unit mass [F / g] of the MXene-containing film of the electrode in Example 1 was calculated. The results are shown in Table 1A.

[0196] (Quantitative elemental analysis)

[0197] Elemental analysis of the sample obtained from the powder of the layered material of Example 1 was performed using a scanning fluorescence X-ray analyzer ZSX-Primus IV manufactured by Rigaku Corporation, employing wavelength dispersive X-ray fluorescence analysis (WD-XRF). Table 2 shows the elements with a content exceeding 0.01 mol%. The upper section of Table 2 represents the content of each element on a mass basis, and the lower section represents the result of converting the content of each element on a mass basis to the content of each element on a substance basis by dividing the content of each element on a mass basis by the atomic weight of each atom [g / mol]. The composition of the powder of the layered material of Example 1, based on the amount of feed, is Ti, as described above. 2.7 Zr 0.3 C2T s On the other hand, based on the elemental quantitative analysis, as shown in Table 2, the Ti and Zr composition of the layered material in Example 1 is expressed as Ti 2.692 Zr 0.308 This is very close to the composition based on the amount of feed added. Furthermore, the mass ratio of O atoms is approximately 87% relative to the total mass of O, Cl, and S atoms, which are considered to exist as terminals of the layered material. This is similar to the condition of surface functional groups in the calculation model of double-layer capacitance, which will be discussed later.

[0198] (Example 2)

[0199] Except as described below, the powder of the layered material of Example 2 was prepared in the same manner as in Example 1. TiC powder, ZrC powder, Ti powder, Al powder, and Si powder were mixed in a zirconia mortar to obtain the mixed powder of Example 2. These powders were provided by the High Purity Chemical Research Institute, Ltd. The molar ratio of TiC:ZrC:Ti:Al:Si in the mixed powder of Example 2 was 1.7:0.3:1:0.9:0.1. Except that the mixed powder of Example 2 was used instead of the mixed powder of Example 1, the powder of the layered material of Example 2 was obtained in the same manner as in Example 1. Except that the layered material of Example 2 was used instead of the layered material of Example 1, the electrode of Example 2 was obtained in the same manner as in Example 1. Except that the electrode of Example 2 was used instead of the electrode of Example 1, the half-unit for evaluation was assembled and electrochemical measurements were performed in the same manner as in Example 1. The results are shown in Table 1A.

[0200] (Comparative Example 1)

[0201] Except as described below, the powder of the layered material of Comparative Example 1 was prepared in the same manner as in Example 1. TiC powder, Ti powder, and Al powder were mixed in a zirconia mortar to obtain the mixed powder of Comparative Example 1. These powders were provided by the High Purity Chemical Research Institute, Ltd. The molar ratio of TiC:Ti:Al in the mixed powder of Comparative Example 1 was 2:1:1. Except that the mixed powder of Comparative Example 1 was used instead of the mixed powder of Example 1, and the firing temperature of the mixed powder was adjusted to 1400°C, the powder of the layered material of Comparative Example 1 was obtained in the same manner as in Example 1. Except that the layered material of Comparative Example 1 was used instead of the layered material of Example 1, the electrode of Comparative Example 1 was obtained in the same manner as in Example 1. Except that the electrode of Comparative Example 1 was used instead of the electrode of Example 1, the half-unit for evaluation was assembled and electrochemical measurements were performed in the same manner as in Example 1. The results are shown in Table 1A.

[0202] (Example 3)

[0203] Except as described below, the powder of the layered material of Example 3 was prepared in the same manner as in Example 1. TiC powder, ZrC powder, Ti powder, and Al powder were mixed in a zirconia mortar to obtain the mixed powder of Example 3. These powders were provided by the High Purity Chemical Research Institute, Ltd. The molar ratio of TiC:ZrC:Ti:Al in the mixed powder of Example 3 was 1.4:0.6:1:1.1. The powder of the layered material of Example 3 was obtained in the same manner as in Example 1, except that the mixed powder of Example 3 was used instead of the mixed powder of Example 1. The molar ratio of Zr / (Ti+Zr) in the powder of the layered material of Example 3 was 0.2.

[0204] (See Example 1 for reference)

[0205] Except as described below, the precursor powder of Reference Example 1 was prepared in the same manner as in Example 1. ZrC powder, Ti powder, and Sn powder were mixed in a zirconia mortar to obtain the mixed powder of Reference Example 1. The molar ratio of ZrC:Ti:Sn in the mixed powder of Reference Example 1 was 1:1:1. The precursor powder of Reference Example 1 was obtained in the same manner as in Example 1, except that the mixed powder of Reference Example 1 was used instead of the mixed powder of Example 1 and the firing temperature of the mixed powder was adjusted to 1200°C.

[0206] (X-ray diffraction)

[0207] X-ray diffraction (XRD) was performed on the powders of the precursors of the layered materials of Examples 1, 2, 3, and Comparative Example 1, as well as on the powders of these layered materials, using an X'Pert PRO MPD X-ray diffraction apparatus manufactured by PANalytical. The results are shown in... Figure 3A and Figure 3B .

[0208] Figure 3A These are graphs showing the XRD measurement results of the precursors of the layered materials in Examples 1, 2, 3 and Comparative Example 1. Figure 3B These are graphs showing the XRD measurement results of the layered materials of Example 1, Example 2, Example 3 and Comparative Example 1. Figure 3A and Figure 3B The vertical axis represents diffraction intensity, and the horizontal axis represents the diffraction angle 2θ. The diffraction intensity on the vertical axis represents the relative relationship of diffraction intensity in a single XRD measurement, not the relative result of diffraction intensity in multiple XRD measurements.

[0209] Figure 3A and Figure 3B The comparison shows that the layered materials of Examples 1, 2, 3 and Comparative Example 1 do not contain a precursor, and the layered material MXene is generated from the precursor MAX. According to Figure 3A Comparing Examples 1-3 with Comparative Example 1, the diffraction peaks corresponding to the (110) plane of the precursor in Examples 1-3 are shifted to a lower angle compared to the diffraction peaks corresponding to the (110) plane of the precursor in Comparative Example 1. This means that the lattice size of the precursors in Examples 1-3 is larger than that of the precursor in Comparative Example 1. Therefore, it is believed that in the lattices of the precursors and layered materials in Examples 1-3, a portion of Ti in the lattices of the precursors and layered materials in Comparative Example 1 is replaced by Zr, which has an atomic radius larger than Ti. Compared to the diffraction peaks corresponding to the (110) plane of the precursors in Examples 1 and 2, the diffraction peaks corresponding to the (110) plane of the precursor in Example 3 are shifted to a lower angle. Therefore, it is believed that the amount of Zr replacement in the lattices of the precursors and layered materials in Example 3 is greater than the amount of Zr replacement in the lattices of the precursors and layered materials in Examples 1 and 2.

[0210] XRD was performed on the precursor powder, Ti₂SnC powder, and Zr₂SnC powder of Reference Example 1 using an X'Pert PRO MPD X-ray diffractometer manufactured by PANalytical. The results are as follows: Figure 4 As shown. Figure 4 The graph shows the XRD results of the precursor, Ti2SnC, and Zr2SnC of Reference Example 1. Figure 4 The vertical axis represents diffraction intensity, and the horizontal axis represents the diffraction angle 2θ. The diffraction intensity on the vertical axis represents the relative relationship of diffraction intensity in a single XRD measurement, not the relative result of diffraction intensity in multiple XRD measurements.

[0211] like Figure 4As shown, the position of the XRD diffraction peak of the precursor powder in Reference Example 1 was determined to be midway between the positions of the XRD diffraction peaks of Ti2SnC powder and Zr2SnC powder. Therefore, the precursor of Reference Example 1 is considered to be TiZrSnC, a solid solution of Ti2SnC and Zr2SnC. Therefore, it is believed that by etching the precursor of Reference Example 1 in the same manner as the precursor of Example 1, a layered material TiZrCT corresponding to TiZrSnC can be generated. s .

[0212] (Particle size distribution determination)

[0213] The particle size distribution of the layered materials in Examples 1, 2, and Comparative Example 1 was determined using a Microtrac MT3000EXII laser diffraction particle size distribution measuring device. The results are as follows: Figure 5 As shown. Figure 5 This is a graph showing the particle size distribution of the layered materials in Example 1, Example 2, and Comparative Example 1. Figure 5 In the diagram, the left vertical axis represents frequency (%), the right vertical axis represents cumulative amount (%), and the horizontal axis represents particle size.

[0214] (SEM observation)

[0215] SEM images of the layered materials of Example 1, Example 2 and Comparative Example 1 were obtained using a VE-8800 scanning electron microscope manufactured by KEYENCE. Figure 6A These are SEM images of the layered material from Example 1. Figure 6B These are SEM images of the layered material from Example 2. Figure 6C This is a SEM image of the layered material in Comparative Example 1.

[0216] As shown in Tables 1A and 1B, the electrostatic capacitance per unit mass of the MXene-containing film of the electrodes of Examples 1 and 2 is greater than that of the MXene-containing film of the electrode of Comparative Example 1. Figure 5The particle size of the layered material powders in Examples 1 and 2 is larger than that of the layered material powder in Comparative Example 1. Generally, the smaller the particle size of a material, the larger its specific surface area, and the larger the specific surface area, the easier it is to increase the capacitance. However, referring to Tables 1A and 1B, the capacitance per unit mass of the MXene-containing film of the electrodes of Examples 1 and 2 with larger particle sizes is greater than that per unit mass of the MXene-containing film of the electrode of Comparative Example 1 with smaller particle sizes. This is believed to be due to the inherent characteristics of the layered material itself. For example, consider the case where the specific surface area of ​​the layered materials in Examples 1 and 2 is the same as that of the layered material in Comparative Example 1. In this case, the difference between the capacitance per unit mass of the MXene-containing film of the electrodes of Examples 1 and 2 and the capacitance per unit mass of the MXene-containing film of the electrode of Comparative Example 1 is considered to be even larger.

[0217] (Examples 4-16 and Comparative Examples 1-16)

[0218] Using the compositions of MXene shown in Tables 1A and 1B, the double-layer capacitance [μF / cm] of the layered materials in Examples 4-16 and Comparative Examples 1-16 was calculated using the ESM-RISM method, a first-principles calculation. 2 The ESM-RISM method describes the electronic states of electrodes and reactants using density functional theory and the electrolyte distribution using RISM, a classical solution theory, thus enabling rapid prediction of the electronic states under an applied electric field. The calculation model used the following approach: a lattice mitigation was performed using standard first-principles calculations on a MAX precursor structure. A surface model was then created by removing one layer of the MAX structure and assigning O atoms to the surface for atomic mitigation. Based on the ESM-RISM calculations, the model was electron-assigned as described in the literature below. A QV curve representing the relationship between surface charge Q and applied voltage V was constructed based on the Fermi energy change relative to the assigned charge, and the electrostatic capacitance was evaluated based on its slope. The charge was varied from 0 to -10 μC / cm. 2 The calculations used Quantum Espresso code. The results are shown in Tables 1A and 1B.

[0219] Reference: Chemistry of Materials (USA), 2022, 34, 5, 2069-2075

[0220] https: / / pubs.acs.org / doi / full / 10.1021 / acs.chemmater.1c03328

[0221] The double-layer capacitance of the layered materials in Examples 1 and 2 was not calculated, but it is assumed that there is a correspondence between the double-layer capacitance and the electrostatic capacitance. The electrostatic capacitance per unit mass of the MXene-containing film of the electrodes in Examples 1 and 2 is greater than that per unit mass of the MXene-containing film of the electrode in Comparative Example 1. Therefore, it can be considered that the double-layer capacitance of the layered materials in Examples 1 and 2 is higher than that of the layered material in Comparative Example 1.

[0222] Based on the comparison between the embodiments and comparative examples, if the layered material contains two or more elements selected from Ti, Sc, Y, La, Zr, and Hf, the specific capacitance and double-layer capacitance tend to be higher compared to the case where the layered material contains only one metal. According to the embodiments, if the layered material contains two or more elements selected from Ti, Sc, Y, La, Zr, and Hf, the double-layer capacitance of the layered material can reach 12 μF / cm. 2 above.

[0223] Table 1A

[0224]

[0225] Table 1B

[0226]

[0227] Table 2

[0228]

[0229] Industry availability

[0230] The layered material disclosed herein can be used as the electrode active material of the electrode in an electrochemical capacitor, which can be used for energy storage in various fields.

Claims

1. A layered material comprising a body and terminals present on the surface of the body, the body having M1 (1-a)m M2 am X n The composition, In the composition, M1 and M2 are distinct atoms selected from Ti, Sc, Y, La, Zr, and Hf. X contains at least one selected from carbon and nitrogen atoms. a is greater than 0 and less than 1. n is 1 or more and 4 or less m is greater than n and less than 5.

2. The layered material according to claim 1, The terminal contains atoms with electronegativity greater than that of M1 and M2.

3. The layered material according to claim 1, The terminal comprises at least one selected from hydroxyl, hydrogen, halogen, chalcogen, amino, phosphorus and antimony atoms.

4. The layered material according to claim 1, n is 2, m is 3.

5. The layered material according to claim 1, X contains carbon atoms.

6. The layered material according to claim 1, M1 and M2 are distinct atoms selected from Ti, Zr, and Hf.

7. The layered material according to claim 1, M1 is Ti, and M2 is Zr.

8. The layered material according to claim 7, a is greater than 0 and less than 0.

33.

9. The layered material according to claim 7, a is greater than 0 and less than 0.

2.

10. The layered material according to claim 7, a is greater than 0 and less than 0.

1.

11. The layered material according to claim 1, M1 is either Ti or Zr. M2 is Sc, Y, or La.

12. The layered material according to claim 1, M1 is either Ti or Zr. M2 is Hf, Sc, Y, or La. a is greater than 0 and less than 0.

67.

13. The layered material according to claim 12, a is greater than 0 and less than 0.

5.

14. The layered material according to claim 12, a is greater than 0 and less than 0.

33.

15. An electrode active material for an electrochemical device, comprising the layered material according to any one of claims 1 to 14.

16. An electrochemical device comprising a pair of electrodes and an electrode active material disposed in contact with at least one of the pair of electrodes. The electrode active material comprises the layered material according to any one of claims 1 to 14.

17. An electrochemical capacitor having a positive electrode and a negative electrode, The positive electrode and the negative electrode are configured separately in the electrolyte. The electrode active material is selected from at least one of the positive electrode and the negative electrode, comprising any one of claims 1 to 14.

18. The electrochemical capacitor according to claim 17, The negative electrode contains the layered material as the electrode active material.