Grass suppression material solidifier, method for producing grass suppression material solidifier

A solidified weed suppressing material with inhibitory components and organic acids allows for continuous control of plant growth, addressing the inefficiencies of traditional herbicide use and labor-intensive maintenance in greening areas.

JP2024179268APending Publication Date: 2024-12-26CENTRAL RESEARCH INSTITUTE OF ELECTRIC POWER INDUSTRY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023097981
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Existing methods for maintaining greening areas around infrastructure like power transmission lines require significant labor and cost due to excessive plant growth, and using herbicides can harm the landscape and safety, necessitating a more controlled and efficient method to manage plant growth.

Method used

A solidified weed suppressing material containing a suppressing member with inhibitory components and a promoting material that uses organic acids to elute and adjust plant morphology, allowing continuous control of plant growth without regular maintenance.

Benefits of technology

The material effectively adjusts and maintains plant morphology over time, reducing the need for frequent maintenance and ensuring aesthetic and functional integrity of greening areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024179268000001_ABST
    Figure 2024179268000001_ABST
Patent Text Reader

Abstract

To continuously maintain (control) a plant morphology by adjusting the plant morphology (size and color, flowering time and so on) over a long time, by installing in a desired place.SOLUTION: An inhibitory member (solidified coal ash) containing a component element having a herbic suppression effect that inhibits plant growth and suppresses growth, and a peat (peat moss) granular molded product containing an organic acid that is an acidic substance that promotes the elution of the component element of the suppression member, and the organic acid 6 of the promoting material 3 is dissolved in rainwater 5 or the like. The elution of the component element 7 having the herbic suppression effect of the suppression member 2 continues to be efficiently eluted by rainwater 5 in which the organic acid 6 is dissolved.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solidified weed-suppressing material containing an inhibitory component that regulates (inhibits) plant growth, and a method for producing the solidified weed-suppressing material. [Background technology]

[0002] Plants are often planted on power line sites, river banks, road slopes, medians, airport landing strips, etc. to prevent erosion, ensure safety, maintain the landscape, prevent foundation erosion, and prevent flying sand. Plants used for greening can have a negative impact on crime prevention, appearance, and functionality if they grow too much, so regular maintenance such as weeding is required. However, because such greening areas are difficult for people to access, the current situation is that maintenance requires a great deal of labor, time, and money.

[0003] For this reason, conventionally, instead of regular weeding, plants are killed using herbicides or the like to prevent them from growing, eliminating the adverse effects of excessive plant growth (for example, Patent Document 1). The technology shown in Patent Document 1 is a technology that reduces the burden of weeding by mixing a growth inhibitor with a herbicide.

[0004] In greening areas, it is important for the area to continue to exist even if the amount of vegetation decreases, in terms of environmental image, etc., but when the technology of Patent Document 1 is used, since it is a weeding technology, after the weeding, there will be no vegetation in the greening area. If weeding is carried out in a greening area and the vegetation is removed, the scenery, including the appearance and impression of safety, will be damaged, and under the current circumstances, it is not advisable to carry out weeding in greening areas. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2013-540775 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a solidified weed-suppressing material which, when placed in a desired location, can accurately dissolve the inhibitory components, adjust the morphology of the plant (size, color, flowering period, etc.), and continuously maintain (control) the morphology of the plant.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a method for producing a solidified weed-suppression material that, by placing it in a desired location, accurately dissolves the inhibitory component, adjusts the morphology of the plant (size, color, flowering time, etc.), and continuously maintains (controls) the morphology of the plant. [Means for solving the problem]

[0008] In order to achieve the above-mentioned object, the solidified weed-suppressing material of the present invention according to claim 1 is characterized in that it comprises an inhibitory member containing component elements having a weed-suppressing effect of inhibiting and suppressing plant growth, and a promoting material containing an acidic substance that promotes the dissolution of the component elements of the inhibitory member.

[0009] In the present invention as claimed in claim 1, as rainwater etc. permeates the solidified weed-suppressing material and flows through it, the acidic substances of the promoting material are dissolved in the rainwater etc., and the dissolution of the component elements having the weed-suppressing effect of the suppressing material is promoted by the rainwater etc. having the acidic substances dissolved therein, and the component elements having the weed-suppressing effect continue to be efficiently dissolved out, so that the component elements having the weed-suppressing effect are dissolved out for the desired period of time.

[0010] Therefore, by placing it in the desired location, the inhibitory components can be accurately dissolved, the plant's morphology (size, color, flowering period, etc.) can be adjusted, and the plant's morphology can be continuously maintained (controlled).

[0011] A solidified weed-suppressing material according to a second aspect of the present invention is characterized in that, in the solidified weed-suppressing material according to the first aspect, the acidic substance of the promoting material is an organic acid.

[0012] In the present invention according to claim 2, the elution of the component elements of the suppressing member can be promoted by using an organic acid. As the organic acid, for example, organic compounds exhibiting acidity having a sulfo group (-SO3H) or a carboxyl group (-COOH) in their structure, such as fumaric acid, citric acid, malic acid, tartaric acid, succinic acid, lactic acid, acetic acid, propionic acid, butyric acid, formic acid, itaconic acid, phytic acid, and benzoic acid, are applicable.

[0013] Furthermore, the solidified weed-suppression material of the present invention according to claim 3 is characterized in that, in the solidified weed-suppression material according to claim 1, the component elements of the suppressing member include at least one of boron (B), aluminum (Al), copper (Cu), molybdenum (Mo), iron (Fe), lithium (Li), cobalt (Co), zinc (Zn) and sodium (Na).

[0014] According to the present invention as set forth in claim 3, plant growth can be regulated within a predetermined concentration range while satisfying environmental standards.

[0015] Furthermore, the solidified weed-suppression material of the present invention according to claim 4 is characterized in that, in the solidified weed-suppression material according to claim 1, the promotion material contains an acidic component or is a carrier to which an acidic component is attached.

[0016] In the present invention according to claim 4, the elution of the component elements of the suppressing member can be promoted by using a carrier that contains an acidic component or has an acidic component attached thereto.

[0017] Further, a solidified weed-suppressing material according to the present invention as set forth in claim 5 is the solidified weed-suppressing material according to claim 1, characterized in that the promoting material is peat (peat moss) in which plants have been humified.

[0018] In the present invention according to claim 5, the elution of the component elements of the inhibitor can be promoted by using peat moss in which plants (bryophytes, reeds, sedges, marsh grass, willows, etc.) have been humified.

[0019] Peat moss in which plants have been humified is, for example, dehydrated, crushed, and sorted, and a thickener is added to mold it into a solid form, and the molded form is mixed with a suppressing material (coal ash paste) to form a solidified weed suppression material. In addition, peat moss in which plants have been humified is kneaded into a paste-like suppressing material to form a solidified weed suppression material.

[0020] In addition, the weed-suppression material solidified product of the present invention according to claim 6 is characterized in that, in the weed-suppression material solidified product according to claim 5, the peat (peat moss) is molded into granular peat, and the granular peat is mixed with the suppression member.

[0021] In the present invention according to claim 6, a solidified weed-suppressing material can be obtained by mixing granular peat with a suppressing material (for example, coal ash paste).

[0022] Furthermore, the solidified weed-suppression material of the present invention according to claim 7 is characterized in that, in the solidified weed-suppression material according to claim 5, the peat (peat moss) is made into a fibrous form to form a bag-shaped member, and the bag-shaped member is arranged around the solidified suppression member.

[0023] In the present invention according to claim 7, a solidified weed-suppressing material is prepared by containing a solidified suppressing material in peat (peat moss) formed into a bag-shaped member.

[0024] In addition, the solidified weed-suppression material of the present invention according to claim 8 is characterized in that, in the solidified weed-suppression material according to any one of claims 1 to 7, the volume ratio of the promotion material is in the range of 5.0% to 10.0%.

[0025] In the present invention according to claim 8, the volume ratio of the promotion material is set to 5.0% to 10.0%, thereby controlling the porosity to a desired level, ensuring the strength of the solidified body, and enabling the suppression member to be dissolved at a desired concentration.

[0026] In order to achieve the above-mentioned object, the method for producing a solidified weed-suppressing material of the present invention according to claim 9 comprises dehydrating and crushing peat containing organic acids, molding the crushed material into granules of a desired size, placing the granules in a formwork, adding paste-like coal ash containing component elements having a weed-suppressing effect of inhibiting and suppressing plant growth to the formwork with the granules placed in it, heating and hardening the sample in the formwork for a predetermined period of time, and after the predetermined period has passed, demolding to produce a solidified material.

[0027] In addition, in order to achieve the above-mentioned object, the manufacturing method of the present invention as set forth in claim 10 for solidifying weed-suppressing material comprises pouring a paste-like coal ash containing component elements having a weed-suppressing effect of inhibiting and suppressing plant growth into a formwork, kneading peat containing organic acids into the casting material inside the formwork, heating and hardening the sample inside the formwork for a predetermined period of time, and after the predetermined period has passed, removing it from the formwork to produce a solidified material.

[0028] In the present invention according to claims 9 and 10, as rainwater etc. permeates and flows through the solidified weed-suppression material, the promoting material dissolves in the rainwater etc., and the dissolution of the suppression member is promoted by the rainwater etc. with the promoting material dissolved in it, so that the suppression member continues to dissolve efficiently, making it possible to produce a solidified weed-suppression material in which the suppression member dissolves for a desired period of time.

[0029] Therefore, by placing it in the desired location, the inhibitory components can be accurately dissolved, the plant's morphology (size, color, flowering period, etc.) can be adjusted, and a solidified weed-suppressing material can be produced that continuously maintains (controls) the plant's morphology. Effect of the Invention

[0030] By placing the solidified weed-suppressing material of the present invention in a desired location, it is possible to accurately elute the suppressive components, adjust the morphology of the plant (size, color, flowering time, etc.), and continuously maintain (control) the morphology of the plant.

[0031] Furthermore, the method for producing solidified weed-suppression material of the present invention makes it possible to produce a solidified weed-suppression material that, by placing it in a desired location, accurately dissolves the suppressive components, adjusts the morphology of the plant (size, color, flowering time, etc.), and continuously maintains (controls) the morphology of the plant. [Brief description of the drawings]

[0032] [Figure 1] FIG. 2 is a conceptual diagram of a solidified weed suppression material according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram showing the elution of boron by an organic acid. [Diagram 3] FIG. 2 is an explanatory diagram showing the elution of lithium by an organic acid. [Figure 4] This is a conceptual diagram of an example of the use of peat (peat moss). [Diagram 5] FIG. 2 is a process diagram of one embodiment of a method for producing a solidified weed suppression material. [Figure 6] FIG. 11 is a process diagram of another embodiment of a method for producing a solidified weed suppression material. [Figure 7] This is a conceptual diagram of an example of the use of peat (peat moss). [Figure 8] FIG. 11 is a process diagram of another embodiment of a method for producing a solidified weed suppression material. [Figure 9] 1 is a graph showing the relationship between the volume ratio and the eluted concentration of boron. [Figure 10] 1 is a graph showing the relationship between the volume ratio and the eluted lithium concentration. [Figure 11] 1 is a graph showing the change over time in the amount of eluted boron. [Figure 12] 1 is a graph showing the change over time in the amount of eluted lithium. [Figure 13] FIG. 2 is an explanatory diagram of an example of use of the solidified weed suppression material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Figure 1 shows a conceptual diagram of the state in which a solidified weed control material according to one embodiment of the present invention is installed, Figure 2 shows an explanation of the situation in which boron is eluted by organic acid, and Figure 3 shows an explanation of the situation in which lithium is eluted by organic acid.

[0034] As shown in the figure, the solidified weed-suppressing material 1 is a mixture for maintaining the growth of plants in a specified condition, and comprises an inhibitory member 2 containing component elements that have a weed-suppressing effect of inhibiting and suppressing plant growth, and a promoting material 3 containing an organic acid, which is an acidic substance that promotes the dissolution of the component elements of the inhibitory member 2.

[0035] As rainwater 5 and the like permeates and flows through the solidified weed-suppressing material 1, the organic acid 6 of the promoting material 3 dissolves in the rainwater 5 and the like, and the dissolution of the component element 7 having the weed-suppressing effect of the suppression member 2 is promoted by the rainwater 5 and the like having the organic acid 6 dissolved therein, and the component element 7 having the weed-suppressing effect continues to dissolve efficiently, so that the component element 7 having the weed-suppressing effect is dissolved for the desired period of time.

[0036] As the organic acid 6, for example, organic compounds exhibiting acidity having a sulfo group (-SO3H) or a carboxyl group (-COOH) in their structure, such as fumaric acid, citric acid, malic acid, tartaric acid, succinic acid, lactic acid, acetic acid, propionic acid, butyric acid, formic acid, itaconic acid, phytic acid, and benzoic acid, are applicable.

[0037] Examples of the suppressing material 2 include solidified coal ash, purpose sludge ash, blast furnace slag powder, and unburned shell powder that have been made into a paste (containing water).The component elements 7 having a weed suppressing effect include at least one of boron (B), aluminum (Al), copper (Cu), molybdenum (Mo), iron (Fe), lithium (Li), cobalt (Co), zinc (Zn), and sodium (Na).

[0038] Therefore, within a predetermined concentration range, plant growth can be regulated while satisfying environmental standards.

[0039] The state of dissolution of boron and lithium will be explained based on Figs. 2 and 3.

[0040] As shown in Figure 2, when the inhibitors using Ash A and Ash B were used with the organic acids fumaric acid, citric acid, malic acid, tartaric acid, succinic acid, and lactic acid, higher concentrations of boron were eluted compared to the comparison samples.

[0041] As shown in Figure 3, when the inhibitors using Ash A and Ash B were used and the organic acids fumaric acid, citric acid, malic acid, tartaric acid, succinic acid, and lactic acid were used, lithium was eluted at higher concentrations than in the comparison samples.

[0042] An embodiment of the method for producing the solidified weed suppression material will be described with reference to Figures 4 and 5. Figure 4 shows the concept of an example of the use of peat (peat moss), and Figure 5 shows the manufacturing process.

[0043] As shown in Fig. 4, the promotion material is peat moss 11, which is humified plants (bryophytes, reeds, sedges, marshes, willows, etc.), which is dehydrated, crushed, and sorted, and a thickener is added to form a solid (granules of a desired size: spherical) into spheres 12. The promotion material may contain an acidic component or may be a carrier to which an acidic component is attached.

[0044] As shown in Fig. 5, spheres 12 are placed in a form 14, and paste-like coal ash 15 (suppressing material) containing component elements having a weed-suppressing effect of inhibiting and suppressing plant growth is added to the form 14 with the spheres 12 placed in it. The sample in the form 14 is heated (e.g., 40°C) for a predetermined period (e.g., two weeks) to harden, and after the predetermined period has passed, it is removed from the form and solidified to become a solidified weed-suppressing material 16.

[0045] The volume ratio of the spheres 12, which are granular peat (peat moss) serving as the promotion material, is set to a range of 5.0% to 10.0%. By setting the volume ratio of the spheres 12 (promotion material) to 5.0% to 10.0%, the porosity is kept to a desired level (for example, about 20% or less), ensuring the strength of the weed-suppression material solidified matter 16 and enabling the suppression material to elute at a desired concentration.

[0046] As rainwater etc. seeps into and flows through the solidified weed-suppression material 16, the components of the spheres 12 (components of the promotion material) dissolve in the rainwater etc., and the rainwater etc. with the promotion material dissolved in it promotes the dissolution of the weed-suppression components from the coal ash 15 (suppression material), and the weed-suppression components continue to dissolve efficiently.

[0047] Therefore, by placing the solidified weed-suppressing material 16 in the desired location, the suppressing components can be appropriately dissolved, the plant's morphology (size, color, flowering period, etc.) can be adjusted, and the plant's morphology can be continuously maintained.

[0048] Another embodiment of the method for producing a solidified weed suppression material will be described with reference to Fig. 6. Fig. 6 shows the process status of another embodiment of the method for producing a solidified weed suppression material.

[0049] As shown in Fig. 6, paste-like coal ash 15 (suppressing member) containing component elements having a weed-suppressing effect of inhibiting and suppressing the growth of plants is poured into formwork 21. Peat moss 11, which is humusified plants (bryophytes, reeds, sedges, marsh grass, willows, etc.), is kneaded into the paste-like coal ash 15 (suppressing member). The sample in formwork 21 is heated (for example, at 40°C) for a predetermined period (for example, two weeks) to harden, and after the predetermined period has elapsed, it is removed from the formwork and solidified, resulting in solidified weed-suppressing material 22 in which peat moss 11 is kneaded into coal ash 15 (suppressing member).

[0050] The volume ratio of the peat (peat moss) 11, which is the promotion material, is in the range of 5.0% to 10.0%. Since the volume ratio of the peat (peat moss) 11 is set to 5.0% to 10.0%, the porosity is kept to a desired level (for example, about 20% or less), the strength of the weed-suppression material solidified matter 16 is ensured, and the suppression material can be eluted at a desired concentration.

[0051] As rainwater etc. seeps into and flows through the solidified weed-suppression material 22, the components of the peat (peat moss) 11 (components of the promotion material) dissolve in the rainwater etc., and the rainwater etc. with the promotion material dissolved in it promotes the dissolution of the weed-suppression components from the coal ash 15 (suppression material), and the weed-suppression components continue to dissolve efficiently.

[0052] Therefore, by placing the solidified weed suppression material 22 in the desired location, the suppression components can be appropriately dissolved, the plant's morphology (size, color, flowering period, etc.) can be adjusted, and the plant's morphology can be continuously maintained.

[0053] Another embodiment of the method for producing a solidified weed suppression material will be described with reference to Figures 7 and 8. Figure 7 shows the concept of an example of using peat (peat moss), and Figure 8 shows the manufacturing process.

[0054] As shown in Fig. 7, peat moss 11, which is made by humifying plants (bryophytes, reeds, sedges, marshes, willows, etc.), is made into a fibrous form to form bag-shaped member 25. Also, as shown in Fig. 8, paste-like coal ash containing component elements having a weed-suppressing effect of inhibiting and suppressing plant growth is solidified into pieces of appropriate size to form solidified material 26. The solidified material 26 is contained in bag-shaped member 25, and the bag-shaped member 25 containing the solidified material 26 constitutes solidified weed-suppression material 27.

[0055] The weed suppression material solidified material 27 is constituted by storing peat (peat moss) 11, which is an accelerating material, in a fibrous bag-shaped member 25, and can be easily manufactured into any size and shape. The volume ratio of the peat (peat moss) 11 is in the range of 5.0% to 10.0%. Since the volume ratio of the bag-shaped member 25 is set to 5.0% to 10.0%, the suppression material of the solidified material 26 can be eluted at a desired concentration.

[0056] The state of the elution concentration according to the volume ratio will be explained with reference to Figures 9 and 10. Figure 9 shows the relationship between the volume ratio and the elution concentration of boron, and Figure 10 shows the relationship between the volume ratio and the elution concentration of lithium.

[0057] As shown in Figure 9, it was confirmed that when the volume ratio of the promotion material (granular peat moss) was set between 5.0% and 10.0%, the eluted concentration of boron was higher (for example, from 300 mg / L to 600 mg / L) compared to solidified coal ash without the promotion material.

[0058] As shown in Figure 10, it was confirmed that when the volume ratio of the promotion material (granular peat moss) was between 5.0% and 10.0%, the lithium elution concentration was higher (for example, from 7 mg / L to 12 mg / L) compared to the coal ash solidified material without the promotion material.

[0059] The state of dissolution will be explained with reference to Figs.

[0060] Figure 11 shows the time-dependent change in the amount of boron dissolved, and Figure 12 shows the time-dependent change in the amount of lithium dissolved. The results in the figures were obtained by dripping water simulating rain onto the solidified weed control material for 40 consecutive months, and examining the state of dissolution in relation to the monthly relative amount of precipitation.

[0061] As shown in Figure 11, in both cases where the volume ratio of the promotion material (granular peat moss) was 10.0% (shown by the solid line) and where the volume ratio of the promotion material (granular peat moss) was 5.0% (shown by the dotted line in the figure), it was confirmed that boron was continuously eluted and that the specified eluted concentration (mg / L) was maintained for a long period of time (equivalent to 40 months).

[0062] As shown in FIG. 12, in both cases where the volume ratio of the promotion material (granular peat moss) was 10.0% (shown by the solid line) and where the volume ratio of the promotion material (granular peat moss) was 5.0% (shown by the dotted line in the figure), it was confirmed that lithium was continuously eluted and that the specified elution concentration (mg / L) was maintained for a long period of time (equivalent to 40 months).

[0063] Aluminum and sodium also continued to be eluted, and it was confirmed that the specified elution concentrations (mg / L) were maintained for a long period of time (equivalent to 40 months).

[0064] An example of the use of the solidified weed suppression material 1 will be described with reference to Fig. 13. Fig. 13 shows a situation in which the solidified weed suppression material 1 (16, 22, 27) according to one embodiment of the present invention is applied to the site of a power transmission line.

[0065] Power lines are often located in places where it is difficult for people to access, so the areas around the lines are greened for aesthetic reasons. However, if the plants grow too much, they can have a negative impact on crime prevention, appearance, and functionality.

[0066] As shown in the figure, a plurality of solidified weed suppression materials 1 (16, 22, 27) are spread around the base of a steel tower 32 on the site of a power transmission line 31. A plurality of solidified weed suppression materials 1 (16, 22, 27) are spread in a desired range around a foundation block 32a of the steel tower 32. In addition, a plurality of solidified weed suppression materials 1 (16, 22, 27) are spread along an access road 33 to the steel tower 32.

[0067] The solidified weed-suppressing material 1 (16, 22, 27) contains suppressing components containing component elements that have a weed-suppressing effect of inhibiting and regulating the growth of plants 34, and the component elements are continuously eluted. Therefore, around the base block 32a of the pylon 32 and on the access road 33 to the pylon 32, the size, color, flowering time, and other characteristics of the leaves, roots, and stems, which are the form of the plants 34, can be arbitrarily adjusted, the growth state can be controlled to a desired state continuously over a long period of time, and the desired size, color, and other conditions can be maintained without maintenance.

[0068] By simply laying the weed-suppressing solidified material 1 (16, 22, 27), the form of the plants 34 around the foundation block 32a of the pylon 32 and on the access road 33 to the pylon 32 is adjusted, the growth state is controlled, and the desired size, color, and other conditions are continuously maintained for a long period of time. This makes it possible to maintain (control) the form of the plants 34 (size, color, flowering time, etc.) within a predetermined range, and it is possible to suppress the plants from growing more than necessary around the foundation block 32a of the pylon 32 and on the pylon 32 for a long period of time.

[0069] In other words, the vegetation around the foundation block 32a of the steel tower 32 (at the base of the steel tower 32), which is a place that is difficult to access, can be maintained at low grass for a long period of time, which is advantageous for protecting the scenery and facilities. Also, by constructing the weed-suppressing solidified material 1 (16, 22, 27) on the access road 33 to the steel tower 32 in the mountain area and controlling (adjusting) the vegetation 34 to be maintained at low grass for a long period of time, the access road 33 can be secured for a long period of time without requiring special maintenance.

[0070] Although an example of constructing the weed suppression material solidified material 1 (16, 22, 27) around the pylon 32 has been described, for example, by spreading the weed suppression material processed into a predetermined shape around the periphery of the curb, such as the corner of the sidewalk at an intersection, the growth of plants growing around the curb can be continuously suppressed for a long period of time. Sand, soil, fallen leaves, etc. tend to accumulate on the curb, and there is a risk of plants (weeds) growing in the compost. By spreading the weed suppression material solidified material, the growth of plants (weeds) around the curb can be continuously suppressed for a long period of time, even if sediment accumulates.

[0071] By placing the solidified weed-suppressing material of the present invention in a desired location, it is possible to adjust the morphology (size, color, flowering time, etc.) of plants over the long term, and continuously maintain (control) the morphology of the plants. [Industrial Applicability]

[0072] INDUSTRIAL APPLICABILITY The present invention can be utilized in the industrial fields of solidified weed suppression materials and methods for producing solidified weed suppression materials. [Explanation of symbols]

[0073] 1, 16, 22, 27 Weed suppression material solidification 2 Weed suppression materials 3 Promotional materials 5 Rainwater 6 Organic acids 7 component elements 11 Peat moss 12 Sphere 14, 21 Formwork 15 Coal ash 25 Bag-shaped member 26 Solidified materials 31 Power Lines 32 Steel Tower 32a Foundation block 33 Access Road 34 Plants

Claims

1. An inhibitory member containing a component element having a weed-suppressing effect of inhibiting and suppressing the growth of plants; and a promotion material including an acidic substance that promotes the elution of the component elements of the suppression member. A solidified weed suppression material.

2. In the solidified weed suppression material according to claim 1, The acidic substance of the promotion material is an organic acid. A solidified weed suppression material.

3. In the solidified weed suppression material according to claim 1, The component elements of the suppression member are Contains at least one of boron (B), aluminum (Al), copper (Cu), molybdenum (Mo), iron (Fe), lithium (Li), cobalt (Co), zinc (Zn), and sodium (Na). A solidified weed suppression material.

4. In the solidified weed suppression material according to claim 1, The promoting material is A carrier that contains an acidic component or has an acidic component attached thereto A solidified weed suppression material.

5. In the solidified weed suppression material according to claim 1, The promoting material is It is peat (peat moss) in which plants have humified. A solidified weed suppression material.

6. The solidified weed suppression material according to claim 5, The peat (peat moss) is molded into granular peat, and the granular peat is mixed with the suppression member. A solidified weed suppression material.

7. The solidified weed suppression material according to claim 5, The peat (peat moss) is fibrous and formed into a bag-shaped member, The bag-shaped member is disposed around the solidified suppression member. A solidified weed suppression material.

8. In the solidified weed suppression material according to any one of claims 1 to 7, The volume ratio of the promoting material is in the range of 5.0% to 10.0%. A solidified weed suppression material.

9. Peat containing organic acids is dehydrated and crushed, and the crushed material is molded into granules of a desired size. The granules are placed in a formwork. A paste-like coal ash containing a component element having a weed-suppressing effect of inhibiting and suppressing plant growth is added to the formwork with the granules placed in it. The sample in the formwork is heated and hardened for a predetermined period of time. After the predetermined period has passed, the sample is removed from the formwork to form a solidified product. A method for producing a solidified weed suppression material, comprising the steps of:

10. Paste-like coal ash containing component elements with a weed-suppressing effect that inhibits plant growth and suppresses growth is poured into a formwork, peat containing organic acids is kneaded into the pouring material inside the formwork, and the sample in the formwork is heated and hardened for a specified period of time. After the specified period has passed, the sample is removed from the formwork to form a solidified product. A method for producing a solidified weed suppression material, comprising the steps of:

Citation Information

Patent Citations

  • Pyrox slum inhibits the growth of perennial forage grasses.

    JP2013540775A