Method for producing metal-modified metal oxide
A redox reaction-based method for modifying metal oxides with metal ions of lower oxidation numbers addresses the limitations of existing methods, enabling efficient and stable antibacterial and catalytic applications on various substrates, including those with low heat resistance.
Patent Information
- Application Number
- JP2022111699
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-12
- Publication Date
- 2024-10-21
- Estimated Expiration
- 2042-07-12
AI Technical Summary
Existing methods for producing metal-modified metal oxides face challenges in achieving long-term stability, substrate versatility, and efficient utilization of antibacterial and catalytic functions, particularly on substrates with low heat resistance or complex shapes, and require heating or light irradiation, limiting their applicability.
A method involving a redox reaction to modify the surface of metal oxides with metal ions, using metal oxides with oxidation numbers lower than their maximum, allowing for the production of metal-modified metal oxides that can be applied to various substrates without heating or light, maintaining the modified metal in a dispersed state, and enhancing antibacterial and catalytic properties.
The method enables the production of metal-modified metal oxides with improved antibacterial and catalytic properties, applicable to diverse substrates including those with low heat resistance, without the need for heating or light, ensuring efficient utilization and long-term stability.
Smart Images

Figure 0007569971000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal-modified metal oxide having antibacterial, catalytic, and electrode functions. Regarding the manufacturing method . [Background technology]
[0002] Metal oxides are materials used for various purposes such as catalysts, semiconductor materials, electrodes, etc. In addition to being used as powders, they are often used by being fixed to the surface of a substrate.
[0003] When the compound is applied to a substrate to be used as a film, it is possible to impart functions derived from the metal oxide to the substrate surface, and it is also possible to obtain the effects of the metal oxide with a small amount of the compound.
[0004] As an application method, there is a method using a coating agent in which metal oxide fine particles are dispersed in a liquid such as water, as described in Patent Document 1. A wet film-forming method using such a coating agent allows application to a large area, and allows application using less expensive equipment compared to dry processes such as vacuum processes.
[0005] Metals are known to have functions such as antibacterial properties and catalytic properties for chemical reactions. For example, the antibacterial properties of silver and the catalytic properties of palladium in the initial deposition reaction of electroless plating are well known.
[0006] Materials in which the surface of a metal oxide is modified with a metal are also widely used. For example, materials in which metal particles are supported on a metal oxide carrier are used as catalysts or sensor electrodes.
[0007] It is known that the combination of metal oxide and metal can impart visible light responsiveness to titanium oxide photocatalyst, improve the properties of gas sensors compared to metal oxide alone, etc. Furthermore, by fixing a metal to a support such as metal oxide, metal particles that tend to aggregate can be maintained in a highly dispersed state, making it possible to effectively utilize the functions of the supported metal.
[0008] Known methods for supporting a metal on a support include impregnation, coprecipitation, etc. In these supporting methods, a metal salt, a metal hydroxide, etc. are applied to the surface of the support, and then steps such as calcination and hydrogen reduction are performed.
[0009] As described in Non-Patent Document 1, palladium is used as a catalyst in the initial reaction of electroless plating. One form of use is a method in which a ceramic or resin substrate is immersed in a solution containing +2-valent tin ions to allow the ions to be adsorbed onto the substrate, and then immersed in a solution of palladium chloride to precipitate palladium on the substrate surface through a substitution reaction.
[0010] When the metal support is a material with photocatalytic function such as titanium oxide, it is known that the metal can be obtained on the support surface by photoprecipitation. For example, Patent Document 2 proposes titanium oxide carrying platinum by photoprecipitation as a visible light responsive photocatalyst. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2020-105274 A [Patent Document 2] Patent Publication No. 2021-154233 [Non-patent literature]
[0012] [Non-Patent Document 1] "Modern Plating Textbook," edited by the Electroplating Research Group, Nikkan Kogyo Shimbun, December 2011, pp. 160-179 [Non-Patent Document 2] Yoshiyoshi Baba et al., "Recent Advances in Electrochromic Materials," Metal Surface Technology, Vol. 35, No. 11, 1984, pp. 498-506 [Non-Patent Document 3] Masayuki Nogami (ed.), "Latest Applications and Prospects of the Sol-Gel Method," Popular Edition, CMC Publishing Co., Ltd., December 2020, pp. 199-200 Summary of the Invention [Problem to be solved by the invention]
[0013] In the production of metal-modified metal oxides in which a metal oxide is modified with a metal, it is desirable that a coating agent for forming a film on a substrate has long-term stability, that there is no restriction on the type of substrate to which the coating agent can be applied, and that the coating film can utilize the modifying metal with high efficiency. It is also desirable that the production method of metal-modified metal oxides has few restrictions on the type and shape of the substrate and has simple steps.
[0014] A method that requires high-temperature heating when modifying a metal oxide with a metal is difficult to apply to a metal oxide that has been applied to a substrate with low heat resistance, such as a resin. In this case, a composite of a metal and a metal oxide must be applied to the substrate with low heat resistance in advance. However, when preparing composite particles, it is difficult to keep the composite particles in a nano-sized particle state suitable for application without agglomeration using a method that requires a heating step.
[0015] In addition, coating agents for applying large aggregated particles to a substrate often require a binder, and since the particle surface is covered with the binder, it is difficult to fully exert the antibacterial and catalytic functions except for the part of the particle surface that is not covered with the binder.
[0016] The functionality of the metal oxide and metal components in the areas covered with the binder is reduced, resulting in low material utilization efficiency. Therefore, if metal could be modified only on the metal oxide surface exposed from the binder, the material could be used more efficiently.
[0017] The photodeposition method on the surface of a material with photocatalytic function can efficiently utilize modified metals because it can modify only the surface of the material with metals. However, since the photodeposition method utilizes the photocatalytic function of a base material such as a metal oxide, it is necessary to highly control the crystallinity, which determines the photocatalytic performance of the metal oxide, and there is also the issue that metal deposition occurs only in the area irradiated with light.
[0018] The treatment of applying palladium to a substrate used in the pretreatment of electroless plating is a method that can perform metal modification without being restricted by the shape of the substrate. On the other hand, the solution containing +2-valent tin ions for adsorbing and reducing palladium is strongly acidic, so the type of substrate may be limited. Furthermore, the tin solution is easily decomposed, so it is difficult to use it for a long period of time. Furthermore, it is difficult to utilize the synergistic effect that occurs when a metal oxide and a modifying metal are used in combination with each other with the adsorbed tin component.
[0019] The present invention has been made in view of the above circumstances, and provides a new method for producing a metal-modified metal oxide, a method for producing an antibacterial member, a method for producing a plated product, and a method for producing a device, which are applicable regardless of the material or shape of a substrate. The present invention also provides a coating agent suitable for applying a metal oxide and a method for producing the coating agent. [Means for solving the problem]
[0020] As a result of intensive research into solving the above problems, the present inventors have The present inventors have developed a method for producing a metal-modified metal oxide, the method comprising the steps of: preparing a metal oxide of any one of the metal elements selected from the group consisting of tungsten, molybdenum, vanadium, niobium, titanium, and tantalum, wherein at least a portion of the metal element contained in the oxide has an oxidation number smaller than the maximum oxidation number in the oxide; and contacting the metal oxide with a solution containing ions of a modifying metal to oxidize the metal element in the metal oxide to a higher oxidation number, while modifying the surface of the metal oxide with the modifying metal through an oxidation-reduction reaction that reduces the modifying metal ions in the solution.
[0021] The coating agent according to the present invention contains a metal oxide, and at least a part of the metal element contained in the metal oxide has an oxidation number smaller than the maximum oxidation number that can be taken in the oxide. The metal oxide includes not only solids such as particles, but also components that can be dissolved in the coating agent, such as ionic molecules or complexes in a state in which a metal oxo acid is condensed. The components become solid metal oxides by drying or heating. Furthermore, the metal oxides include cases in which they are hydrates or hydroxides.
[0022] The method for producing a coating agent according to the present invention includes an embodiment in which the constituent elements of a metal oxide are one or more metals selected from the elements of groups 4 to 7 of the periodic table, and the method includes the steps of preparing a solution containing the metals, acidifying the solution, and reducing at least a portion of the metal elements after acidifying the solution.
[0023] The method for producing a metal-modified metal oxide according to the present invention is characterized by comprising the steps of: preparing a metal oxide in which at least a part of the metal elements contained in the metal oxide has an oxidation number smaller than the maximum oxidation number in the metal oxide; and contacting the metal oxide with a solution containing ions of a modifying metal to oxidize the metal elements in the metal oxide having the small oxidation number and to modify the surface of the metal oxide with a metal through an oxidation-reduction reaction in which the metal elements in the metal oxide having the small oxidation number are oxidized and the metal ions in the solution are reduced. Here, the metal oxide includes not only solids such as particles, but also ionic molecules and complexes in which metal oxoacids are condensed.
[0024] In the present invention, the metal oxide can be formed as a film on the surface of a substrate, and the film can be modified with the modifying metal by contacting the film with the solution. In other words, the method for producing a film made of a metal-modified metal oxide according to the present invention is characterized by comprising the steps of preparing a substrate, forming a film containing a metal oxide on the surface of the substrate, in which at least a part of the metal element contained in the metal oxide has an oxidation number smaller than the maximum oxidation number in the metal oxide, and contacting the film with a solution containing ions of the modifying metal, oxidizing the metal element in the metal oxide, and modifying the surface of the metal oxide film with a metal by a redox reaction in which the ions of the metal in the solution are reduced. Here, there is no particular method for the step of preparing a metal oxide film, but wet coating using a coating agent containing a metal oxide containing a metal element having an oxidation number smaller than the maximum oxidation number in the metal oxide can be applied regardless of the material of the substrate. In addition, for example, a film of a metal oxide heated in a reducing atmosphere can be applied.
[0025] The method for producing an antibacterial member according to the present invention is characterized in that the antibacterial member is produced using the metal-modified metal oxide produced by the above-mentioned production method.
[0026] The method for producing a plated product according to the present invention is characterized in that the metal-modified metal oxide produced by the above-mentioned production method is used as a base layer and electroplating or electroless plating is performed.
[0027] The method for producing a device according to the present invention is characterized in that the film produced by the above method is provided as an electrode in a device. Effect of the Invention
[0028] The coating agent, the method for producing the coating agent, and the method for producing the metal-modified metal oxide of the present invention can be used for substrates having low heat resistance or chemical resistance, and the metal-modified metal oxide can be obtained regardless of the shape of the substrate. Furthermore, antibacterial members, plated products, and devices can be produced by utilizing a film made of the metal-modified metal oxide.
[0029] The metal-modified metal oxide produced by the method of the present invention can be used as a functional material or electrode in which antibacterial properties, catalytic properties, or electrical properties are imparted to the metal oxide.
[0030] The method of modifying a metal oxide with a metal in the present invention does not require a heating step or light irradiation, and therefore can be applied to substrates with low heat resistance such as resins, and substrates with complex shapes that cannot be reached by light. [Brief description of the drawings]
[0031] [Figure 1] 1 is a process diagram showing a method for producing a coating agent and a metal-modified metal oxide according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The present invention will be described in detail with reference to the drawings showing embodiments. Note that the present invention is not limited to these descriptions. Various modifications of the embodiments may be made as long as the effects of the present invention are achieved.
[0033] FIG. 1 is a process diagram showing a method for producing a coating agent and a metal-modified metal oxide according to the present invention. In FIG. 1, the coating agent of this embodiment contains a metal oxide. The metal oxide is in a state in which at least a part of the metal elements contained therein has an oxidation number smaller than the maximum oxidation number that can be taken in the oxide. Transition metals and the like show multiple oxidation numbers in addition to the metal state of 0 valence. An example of the state of the metal oxide is a compound in a mixed valence state. A mixed valence state is a state in which the same element has two or more oxidation numbers for the metal elements constituting the compound. Taking tungsten oxide as an example, the maximum oxidation number of tungsten (W) in the oxide is +6, but in a mixed valence state, at least a part of tungsten has an oxidation number smaller than the maximum oxidation number, such as +5. All metal elements may have an oxidation number smaller than the maximum oxidation number, such as WO2 consisting of +4 valence tungsten.
[0034] Metal oxides containing metal elements with oxidation numbers smaller than the maximum oxidation number are produced by oxidation-reduction reactions of the metal elements that make up the metal oxide, such as electrolysis, ultraviolet light irradiation, and chemical reactions with reducing and oxidizing agents.
[0035] The metal elements in the metal oxide according to the present invention that can have an oxidation number smaller than the maximum oxidation number include various elements, mainly transition metal elements. In the present invention, tungsten, molybdenum, vanadium, niobium, Titanium, Tantalum These may be used singly or in combination. Especially tungsten As the metal oxide, a composite oxide containing the above metal elements may be used, and a component other than the above metal elements, for example, a typical metal element such as an alkali metal element, or an ammonium ion, may be included in the composition.
[0036] The metal that modifies the metal oxide can be one that shows a more noble redox potential in solution than the redox potential of the metal element that can undergo an oxidation reaction in the metal oxide. This reaction is similar to the substitution reaction in which metallic copper is immersed in an aqueous palladium chloride solution, causing metallic palladium to deposit on the copper surface, and the substitution reaction in which a substrate with +2-valent tin ions adsorbed is immersed in an aqueous palladium chloride solution in the pretreatment process of electroless plating, resulting in metallic palladium on the substrate.
[0037] On the other hand, in the present invention, since the reaction of metal elements in metal oxides is utilized, there is no occurrence of the elution of ions of relatively less noble metals, as occurs in the case of substitution precipitation between metals. In other words, the present invention can realize a situation in which metal oxides are not lost during the reaction process. As described in Non-Patent Document 1, when metal ions are used, +2-valent tin ions must be used as a strongly acidic solution, and since they are easily decomposed, long-term stability cannot be expected. The metal oxide-containing coating agent targeted in the present invention can also be made neutral, and there are few restrictions on the workability of application and the material of the substrate, and it can be made stable for a long period of time.
[0038] The modifying metals are generally elements known as noble metals. For example, in the case of tungsten oxide, when the +5 tungsten in the oxide is oxidized to +6, the ions of copper and more noble metals such as silver, gold, platinum, and palladium are reduced to metals. However, in the case of copper, for example, it is assumed that after being precipitated as fine particles, the metal does not exist as a metal, but exists as a metal compound such as an oxide, hydroxide, or sulfide. On the other hand, it is also considered that not only the simple substance of the modifying metal but also the metal compound has a function. Therefore, in the present invention, the reduction reaction related to the modifying metal ion is expressed as the modification of the metal, not the support of the metal.
[0039] The mechanism by which metal elements in metal oxides have a state in which they have a smaller oxidation number than the maximum oxidation number will be explained. For example, in the case of tungsten, when all elements have an oxidation number smaller than the maximum oxidation number of +6, such as WO2 consisting of tungsten with a valence of +4, it is often necessary to heat the metal oxide in a reducing atmosphere such as hydrogen to obtain the mixed valence state in which some metal elements in a metal oxide have an oxidation number smaller than the maximum oxidation number. For example, in the case of tungsten oxide, the +6 tungsten in tungsten oxide WO3 is reduced, and some of it becomes +5 tungsten. As conditions for the reduction reaction when the mixed valence state is obtained, various methods other than heating in a hydrogen atmosphere can be applied depending on the properties of the metal oxide.
[0040] In an example of an electrochemical reduction reaction, when tungsten in tungsten oxide is reduced from +6 to +5, hydrogen ions and alkali metal ions in the electrolyte enter the structure of tungsten oxide, compensating for the charge. Since electrons exist in a delocalized state in the structure of tungsten oxide, it exhibits electrical conductivity. In this case, tungsten oxide turns blue (see, for example, Non-Patent Document 2). This reaction is reversible, and when electrochemically oxidized, tungsten oxide returns to the state it was in before the reduction reaction.
[0041] When tungsten oxide is irradiated with light such as ultraviolet light having energy greater than the band gap, excited electrons and holes are generated. The excited electrons reduce the tungsten in the tungsten oxide from +6 to +5. The holes oxidize the surrounding water molecules that are adsorbed on the tungsten oxide, generating oxygen molecules and hydrogen ions (see, for example, Non-Patent Document 3). This creates a state similar to that of an electrochemical reduction reaction.
[0042] It is believed that similar mixed valence states are observed in chemical reactions with reducing agents.
[0043] For example, when the metal oxide is tungsten oxide, the state in which the metal element has an oxidation number smaller than the maximum oxidation number can be exhibited whether the oxide is crystalline or amorphous. The mixed valence state can be exhibited if the structure contains multiple tungsten atoms, such as the state of an ionic molecule in which tungstic acid is condensed.
[0044] The metal oxide may be a hydrate, a phosphate compound, a silicate compound, or the like. Depending on the type of metal, it may be a hydroxide. The composition may contain an alkali metal ion or an ammonium ion. As a constituent element of the metal oxide, the composition may contain a metal that does not have a state having an oxidation number smaller than the maximum oxidation number.
[0045] In the metal oxide containing a metal element having an oxidation number smaller than the maximum oxidation number, the metal element may be not only a single element but also two or more kinds of elements.
[0046] Regarding the coating agent, when the metal oxide contained therein is a particle, the particle size is not particularly limited, but for example, it is desirable that the average dispersed particle size of the aggregate of fine particles or the monodispersed particles is 300 nm or less, and further 200 nm or less. The particle size is measured, for example, by observing the dried particles with an electron microscope or measuring the particles in liquid by the dynamic light scattering method.
[0047] When the aggregates of fine particles or monodisperse particles have an aspect ratio of 3 or more, or when the particles have a two-dimensional sheet structure, the particle size is not limited to the above values, and the length of the longest part may be greater. In such cases, the length of the longest part is desirably 1000 nm or less, preferably 500 nm or less, and more desirably 300 nm or less. Otherwise, dispersibility may decrease.
[0048] There is no limitation on the structure of the metal oxide particles contained in the coating agent. For example, a particle made of another material may be used as a core, and a metal oxide containing a metal element having an oxidation number smaller than the maximum oxidation number of the present embodiment may be coated or supported on the surface of the core.
[0049] The solvent for the coating agent is not particularly limited, but hydrophilic solvents such as water and alcohol, and hydrophobic solvents such as hexane can be used.
[0050] In this embodiment, the metal oxide contained in the coating agent does not have to be a solid such as a particle. For example, a solution containing ionic molecules formed by condensation of a metal oxo acid such as tungstic acid can be applied to a substrate and dried to obtain a solid metal oxide. Such ionic molecules and complexes that are dissolved in the coating agent but become solid metal oxides by drying or heating are also called precursors of metal oxides or simply precursors. Even in the case of a precursor of a metal oxide, a compound containing a metal element in a state of having an oxidation number smaller than the maximum oxidation number can modify a metal with a relatively noble redox potential in a solution.
[0051] The coating agent of the present invention may be used simply to coat metal oxides for various functions other than metal modification.
[0052] The coating agent according to the present invention and its preparation method will be described in detail. The method for producing the coating agent according to the present invention includes a step of preparing a solution containing a metal, a step of acidifying the solution, and a step of reducing at least a part of the metal element after the solution is acidified. The step of reducing a part of the metal element may also include a case where the reduction reaction proceeds naturally over time without any special operation.
[0053] The coating agent according to the present invention may be in the form of a colloidal solution containing the metal oxide in the form of solid particles or the like, or may contain the metal oxide as a precursor such as an ionic molecule or complex.
[0054] Hereinafter, the case where a metal oxide is contained as a precursor in the coating agent will be described. An example of a precursor of a metal oxide is an ionic molecule formed by condensation of a metal oxo acid. Regarding transition metal elements from Group 4 to Group 7 of the periodic table and metal elements M such as tin and indium, [M x Oy ] n- or an ionic molecule in which the oxoacid is condensed, which dissolves in a solvent such as water.
[0055] Ionic molecules formed by condensation of metal oxoacids may have mixed valences because they contain multiple metal elements in the molecule. When a coating agent contains ionic molecules in a mixed valence state, the condensation proceeds further by drying after application to a substrate, or by heating as necessary, to produce a solid that is a metal oxide containing metal elements in a state with an oxidation number smaller than the maximum oxidation number.
[0056] The condensed ionic molecules may be generated not only from oxoacids of a single metal, but also from multiple types of oxoacids. They may be condensed with silicate ions, phosphate ions, etc. The solvent of the coating agent is preferably mainly composed of water from the viewpoint of economy and working environment, but may contain organic solvents such as alcohols such as ethanol in any ratio. The organic solvent components such as alcohols can be expected to suppress the condensation and decomposition of dissolved species such as ionic molecules in the solution, and to extend the use period of the coating agent. Furthermore, alcohols and the like can be expected to play a role as reducing agents to reduce metal elements in ionic molecules. In order to stabilize dissolved species such as ionic molecules, in addition to organic solvents, organic acids, chelating agents, hydrogen peroxide, sulfate ions, ammonium ions, ions of typical elements and transition elements, etc. may be contained.
[0057] The method for producing a coating agent containing the above-mentioned ionic molecule as a precursor is to prepare a coating agent by dissolving [M x O y ] n-The method comprises the steps of preparing a solution containing one or more metal elements that have the property of taking the form of an oxo acid represented by the formula: (a) treating the solution with an ion exchange resin; and (b) heating the ion-exchanged solution at a predetermined temperature, as required. The step of treating with an ion exchange resin also serves as a step of acidifying the solution. Immediately after the treatment with the ion exchange resin, the metal oxo acids in the solution may spontaneously condense to generate ionic molecules. Furthermore, some of the metal elements in the ionic molecules may naturally take on an oxidation number smaller than the maximum oxidation number in the oxide. Such natural changes may also be utilized as a step of reducing the metal elements in the oxide.
[0058] In the process of preparing the solution, for example, ammonium salts or sodium salts of metal acids can be used. There are no restrictions on the solvent, and it may contain organic solvents such as alcohol in addition to water. There are no restrictions on the concentration in the solution, but if the salt dissolves, a relatively high concentration of 0.1 mol / L or more is used, which is good for workability because less liquid needs to be handled. Some ammonium salts and other poorly soluble salts are easily soluble when heated, but they can be used even if they cannot be made into a high concentration.
[0059] In the step of treating with an ion exchange resin, any cation exchange resin may be used. The treatment method may be a continuous method in which the solution is passed through a column-shaped tube filled with an ion exchange resin, or a batch method in which the resin is mixed with the solution and then solid-liquid separation is performed by filtration or centrifugation. In order to remove cationic impurities, the solution may be treated with an ion exchange resin multiple times. This produces a solution containing ions of a metal oxoacid.
[0060] The color of the liquid after cation exchange may change over time depending on the type of metal. For example, when molybdenum is contained, the liquid may become blue. This is presumably due to the condensation of the metal oxoacid to form ionic molecules, and the ionic molecules being in a mixed valence state. A coating agent can be produced based on a solution containing ionic molecules in this mixed valence state. The solution containing the metal oxoacid ions after ion exchange is acidic. The condensation of the metal oxoacid proceeds under acidic conditions, but the condensation state of the ionic molecules may be adjusted by adjusting the pH of the solution at a predetermined stage.
[0061] In particular, solutions containing ions of oxoacids of multiple metal species, such as solutions containing both tungstate ions and molybdate ions, tend to exhibit a dark color due to the mixed valence state after cation exchange treatment, making it easy to utilize the effects of the present invention.
[0062] In the case of a solution containing ionic molecules produced after ion exchange, in which the ionic molecules have the property of being in a mixed valence state, it is possible to add metals such as iron, zinc, aluminum, or +2 valent iron ions or +2 valent tin ions to the solution, and the metals in the ionic molecules can be partially reduced by the action of the reducing agent to promote the mixed valence state. Alternatively, the mixed valence state can be promoted by placing the solution in an environment exposed to ultraviolet light. Furthermore, an electrolysis reaction can be used using an appropriate electrode. The coating film obtained by using a coating agent containing a component in such an advanced mixed valence state has an effect of increasing the amount of substances that undergo an oxidation-reduction reaction when modifying a metal in a later process, for example, increasing the amount of metal modified in the coating film.
[0063] The solution of metal oxoacid ions after ion exchange can be heated to a specified temperature to adjust the form of the oxoacid, such as the degree of condensation. There are no limitations on temperature or time. For example, when a solution containing molybdic acid is continuously heated in a thermostatic bath at 40°C, the blue color exhibited in the mixed valence state becomes darker. When heating, the concentration of the solution may be adjusted with water or an organic solvent to adjust the progress of the condensation reaction.
[0064] Next, a method of preparation will be described for the case where the coating agent is a fine particle dispersion, that is, where the metal oxide contained is fine particles.
[0065] An example of a method for preparing the fine particle dispersion, particularly a fine particle dispersion of metal oxide containing one or more metal elements of groups 4 to 7 of the periodic table, includes the steps of preparing a solution containing a substance that is a source of the metal element, acidifying the solution, heating the acidified solution at a predetermined temperature to generate particles, and separating and redispersing the particles. After the step of acidifying the solution, ionic molecules formed by condensation of metal oxoacids are generated, so that the coating agent according to the present invention can be prepared by going through a step of reducing at least a part of the metal element at any stage.
[0066] In the process of preparing a solution in which a substance serving as a metal element source is dissolved, a salt of a metal acid or the like can be used. The concentration of the metal is not particularly limited. Regardless of the concentration, particles can be synthesized by making the solution into an acidic solution later. For example, the particles can be prepared at a concentration of 0.01 mol / L to 5 mol / L, preferably 0.05 mol / L to 2 mol / L based on the amount of substance of the contained metal element M.
[0067] The solvent may be water alone. Although there is no particular restriction, alcohol such as ethanol, propanol, or ethylene glycol may be mixed in water at a volume ratio of 1% to 70%, preferably 5% to 50%. By adding an organic solvent, the progress of the condensation reaction of the oxo acid can be controlled to obtain a homogeneous product, and the product can be made into a mixed valence state by using the reducing property of the alcohol or the like. If the amount of organic solvent is too small, the effect of controlling the reaction and the effect as a reducing agent are reduced, but if the amount is too large, the salt that is the source of the metal element becomes difficult to dissolve. A surfactant, a water-soluble polymer, an organic acid, an organic acid salt, or the like may be added for the purpose of adjusting the progress of the reaction. When a metal alkoxide is used as the source of the metal element instead of a water-soluble salt, the ratio of the organic component in the solvent may be increased. Some ammonium salts of oxo acids of metals have low solubility in water, so they can be dissolved by heating to a temperature not exceeding the boiling point of the solvent, such as 80°C. In addition to heating, poorly soluble salts may be dissolved by adding an organic acid or hydrogen peroxide.
[0068] In the step of acidifying the solution in which the metal element source is dissolved, various acids such as hydrochloric acid, sulfuric acid, and oxalic acid can be used. The solution may be acidified by cation exchange, as in the case of preparing a precursor of a metal oxide made of ionic molecules. The pH of the solution may take various values depending on the type of metal and coexisting components, for example, 0 to 4, preferably 0 to 3, and more preferably 0 to 2. For example, when preparing tungsten oxide, the pH is adjusted to 0 to 4, preferably 0.5 to 3.5, more preferably 0.5 to 2, and even more preferably 1 to 1.8.
[0069] When the acid is added to the solution, the solution may be heated or at room temperature. When the solution is not heated, the solution may become suspended under low pH conditions, but it is possible to obtain particles with a uniform particle size. When the acid is added to the solution, the solution may be stirred. The metal solution and the acid solution may be prepared separately and flowed through separate flow paths to be mixed by merging them, or they may be combined all at once.
[0070] In the process of heating the acidified solution at a predetermined temperature to mature it, it is desirable to set the temperature at room temperature or below the boiling point of the solvent. Below the boiling point of the solvent, a container made of resin with low strength can be used. Under the condition of a temperature above the boiling point of the solvent, a pressure-resistant container must be used, which is difficult to work with, but has the advantage of allowing a wide variety of particle shapes and crystal structures. If the temperature is low, the reaction time may be extremely long, or particles with low crystallinity and irregular shape may be obtained. In that case, the heating temperature should be 50°C or higher, preferably 60°C or higher. In addition, the mixture may be heated not only at a constant temperature, but also while increasing or decreasing the temperature. The heating time varies depending on the particle precipitation time, but particles can be obtained in a few hours to about 24 hours. Heating may be continued for a longer period of time, up to about 240 hours, for the purpose of adjusting the crystallinity of the particles.
[0071] Any method may be used for the step of separating and redispersing the particles. Centrifugation is particularly effective when the particle diameter is small. The particles are washed by repeatedly adding distilled water to the particles after centrifugation, redispersing them, and centrifuging them again. Finally, a fine particle dispersion can be obtained by adding distilled water or an organic solvent and redispersing them. Fine particles with small particle sizes and components with low crystallinity may be difficult to centrifuge. Furthermore, when discarding the supernatant after centrifugation, some particles may flow away, which tends to reduce the yield. In that case, electrolytes such as salts and acids may be added to facilitate sedimentation of the particles, making centrifugation easier.
[0072] In order to improve the dispersibility of the particles and the adhesion to the substrate when coated, the particle surface may be modified with a functional group using a silane coupling agent, etc. The surface charge of the particles may be adjusted with an anionic or cationic surfactant.
[0073] When various metals such as aluminum, iron, nickel, zinc, or +2valent iron ions or +2valent tin ions are added to the solutions in each step, particularly to the acidified solutions, when the metals or metal ions are oxidized, the ionic molecules formed by condensation of the oxoacids of the metals in the solution or the metals in the generated metal oxides are partially reduced, and for example, a tungsten-based solution turns deep blue, making it easier to obtain metal oxide particles in a mixed valence state. In addition, when any electrode is placed in the acidified solution to perform electrolysis, the liquid near the cathode turns blue, making it easier to obtain metal oxide particles in a mixed valence state.
[0074] When alcohol is added to water, the alcohol has a reducing effect, and so the color may be similar to that of the mixed valence state, making it easier to obtain metal oxide particles in a mixed valence state. This is particularly noticeable when the metal element is molybdenum or vanadium. For example, the color exhibited when producing tungsten oxide is blue. When actively utilizing the reducing effect of adding alcohol, it is effective to use ethylene glycol, which is a dihydric alcohol, or even a polyhydric alcohol.
[0075] A coating agent in which a mixed valence state is promoted may be prepared by adding +2 valent iron ions or +2 valent tin ions to the prepared dispersion of metal oxide particles.
[0076] The metal source may be a multi-metal species, which tends to promote mixed valence states. For example, tungsten may be doped with molybdenum or tantalum to produce an oxide.
[0077] There is no limit to the concentration of metal oxide in the coating agent. Regarding the microparticle dispersion, a concentration of more than 1 mol / L based on the metal element may cause the fluidity to be lost, but it can be diluted appropriately depending on the coating method when used. If the coating agent contains metal oxide in the form of a precursor, it is unlikely to lose fluidity even at high concentrations.
[0078] The metal oxide in the coating agent may be in a form in which it is contained only in a solid form such as particles, in a form in which it is contained only in a precursor of the metal oxide such as an ionic molecule of a metal oxoacid, or in a form in which it contains a mixture of a solid such as particles and a precursor of the metal oxide.
[0079] For the purpose of improving the dispersibility of particles in the dispersion liquid and modifying the adhesiveness and wettability with other materials, the coating agent may contain an organic or inorganic binder, a silane coupling agent, a thickener, a surfactant, or the like.
[0080] The substrate used when forming a film with a coating agent is not particularly limited and may be glass, ceramics, resin, metal, etc. When preparing the film on a device substrate, the film may be formed on a substrate having metal wired to glass or resin.
[0081] The coating agent is attached to the surface of the coated member by dip coating, in which the coated member is immersed in the coating agent of the present invention and then pulled out. By drying the coated member, a coating film with a thickness on the order of nanometers is formed on the surface of the coated member, although the thickness depends on the diameter of the particles in the coating agent. The coating method is not limited to dip coating. Various methods such as spin coating, spray coating, printing, and application using a brush can be applied.
[0082] The present invention provides a method for producing a metal-modified metal oxide, which comprises the steps of: preparing a metal oxide in which at least a portion of the metal elements contained in the metal oxide have an oxidation number smaller than the maximum oxidation number in the metal oxide; and contacting the metal oxide with a solution containing ions of a modifying metal to modify the surface of the metal oxide with a metal component through an oxidation-reduction reaction in which the metal elements in the metal oxide are oxidized and the metal ions in the solution are reduced.
[0083] Here, the metal oxide includes not only solids such as particles, but also precursors of metal oxides such as ionic molecules formed by condensation of metal oxoacids.
[0084] There is no particular limitation on the process for preparing a metal oxide in which at least a part of the metal elements contained in the metal oxide has an oxidation number smaller than the maximum oxidation number in the metal oxide. The metal oxide may be prepared by disposing the metal oxide on a conductive substrate and carrying out an electrochemical oxidation-reduction reaction, or by using a reaction with an oxidizing agent or a reducing agent, a reduction reaction with hydrogen, a reaction with light energy, a reaction with plasma, or a reaction with thermal energy. The coating agent of the present invention may be used.
[0085] In the process of contacting the metal oxide in the above state with a solution containing modifying metal ions and modifying the surface of the metal oxide by an oxidation-reduction reaction, a metal that exhibits a more noble oxidation-reduction potential in the solution than the oxidation-reduction potential of the metal element in the metal oxide can be used as the modifying metal. In addition to platinum, gold, palladium, etc., which are generally recognized as noble metals, silver and copper can be applied to many of the metal oxides in the above state.
[0086] As a method for contacting the metal oxide with a solution containing ions of the modifying metal, if the metal oxide is in the form of particles, the solution of the modifying metal ions can be dripped or sprayed onto the particles with a spray or the like. Alternatively, the particles can be placed in a solution of the modifying metal ions to cause an oxidation-reduction reaction. In the case of a colloidal solution in which metal oxide particles are dispersed in a solvent, or in the case of a metal oxide being an ionic molecule formed by condensation of a metal acid, the solution can be mixed with a solution of the modifying metal to cause an oxidation-reduction reaction and modify the metal oxide with the metal.
[0087] When a solution containing a mixed-valence metal oxide consisting of condensed ionic molecules of a metal acid is mixed with a solution containing ions of a modifying metal, a gel-like precipitate may be formed. If the progress of gelation can be controlled by adjusting the concentration of each solution, a sol of a metal-modified metal oxide can be produced.
[0088] The present invention provides a method for producing a film made of a metal-modified metal oxide, which comprises the steps of: preparing a substrate; forming a film containing a metal oxide on the substrate surface, in which at least a part of a metal element contained in the metal oxide has an oxidation number smaller than the maximum oxidation number in the metal oxide; and contacting the metal oxide film with a solution containing ions of a modifying metal, thereby modifying the surface of the metal oxide film with the metal through a redox reaction in which the metal element in the metal oxide is oxidized and the metal ion in the solution is reduced.
[0089] There is no restriction on the material or shape of the substrate to be prepared. There is no particular method for forming a metal oxide film. For example, various methods of coating using the coating agent of the present invention are applicable. Furthermore, a metal oxide film consisting of only metal elements with the maximum oxidation number in the oxide may be formed, and some metal elements in the metal oxide may be reduced to smaller oxidation numbers by a suitable method such as hydrogen reduction.
[0090] The ratio of metal elements having a small oxidation number contained in the metal oxide constituting the film may be further increased. For example, it can be produced by applying various oxidation-reduction reactions to a film produced using the coating agent of the present invention, or a film produced by a vacuum process, a sol-gel method, or the like. Examples of reactions include electrochemical oxidation-reduction reactions by disposing a metal oxide film on a conductive substrate, reactions by oxidizing agents or reducing agents, reduction reactions by hydrogen, reactions by light energy, reactions by plasma, and reactions by thermal energy.
[0091] In the process of modifying the surface of the metal oxide film with a metal by a redox reaction in which the metal oxide film is brought into contact with a solution containing ions of a modifying metal, the metal element in the metal oxide is oxidized, and the metal ions in the solution are reduced, a method of immersing the substrate on which the film is formed in a solution containing ions of the modifying metal is applicable. When the substrate is large in size, the solution containing ions of the modifying metal may be applied by spraying or the like. Only a specific region of the substrate surface may be modified with the metal by a coating method such as printing.
[0092] The case where the above-mentioned method for producing a metal-modified metal oxide is used for producing an antibacterial material will be described.
[0093] The antibacterial action of metals such as silver is well known and is used in various products. The member modified with a metal exhibiting antibacterial action such as silver by the manufacturing method of the present invention is characterized in that metallic silver or a silver compound is present on the surface of a metal oxide. If the metal oxide exhibits photocatalytic action, it can be used in combination with the antibacterial action of silver, but even if the metal oxide does not exhibit photocatalytic action or is used in an environment such as a dark room, the antibacterial action can be effectively exhibited by the presence of silver on the surface. The metal oxide modifying a metal such as silver may be in the form of a powder, may be fixed to fibers, or may be in the form of a film.
[0094] In the case of using silver nanoparticles for antibacterial purposes, the nanoparticle surface may be covered with a dispersant, etc. Unlike the present invention in which silver is exposed on the surface, it is difficult to maximize the effect of silver.
[0095] Examples of the application of these materials to fields related to plating will be described.
[0096] The following describes the case where a plated product is manufactured by electroless plating. After forming a metal oxide film containing a metal element having an oxidation number smaller than the maximum oxidation number in the metal oxide on the surface of a substrate, the metal oxide film is modified with a metal having a catalytic effect on the initial reaction of electroless plating, such as silver or palladium. The substrate thus treated is then immersed in an electroless plating solution, whereby the initial reaction of electroless plating occurs using the modified metal as a catalyst, and thereafter, a plating reaction occurs continuously due to autocatalysis, thereby manufacturing a plated product. Plating may be performed using a particulate metal-modified metal oxide as a base, rather than a film, to produce a plated product in particulate form.
[0097] Regarding metal oxides, tungsten oxide and molybdenum oxide tend to be hydrolyzed and dissolved in a basic solution. By modifying these metal oxides with metals according to the present invention, it is possible to prevent the metal oxide film from dissolving even in a strongly basic electroless copper plating solution. In this case, the reason is thought to be that the modifying metals such as silver and the metal compounds converted from them have resistance to bases.
[0098] Next, the case where the plating is electroplating will be described. Electroplating is possible when the metal oxide containing a metal element having an oxidation number smaller than the maximum oxidation number in the metal oxide is a material exhibiting electrical conductivity. The element constituting the metal oxide exhibiting electrical conductivity is not particularly limited, but some examples include tungsten, molybdenum, niobium, etc.
[0099] More specifically, the steps of the method for producing plated products using the electrical conductivity of metal oxides are as follows. (1) A step of preparing a substrate. (2) A step of forming a film serving as a base layer on the surface of the substrate, the film containing a metal oxide that exhibits electrical conductivity when it contains a metal element having an oxidation number smaller than the maximum oxidation number in the metal oxide. (3) A step of providing an electrical contact between the underlayer and a power source in the plating solution and arranging it as a cathode. (4) A process in which electrolysis is performed in a plating solution using any anode, whereby the base layer is subjected to a reducing action around the electrical contact, causing a reaction that makes the base layer conductive, causing a reaction that deposits a plating film in the conductive areas of the base layer, and continuing electrolysis to continuously expand the conductive area around the plating film while forming the plating film on the surface of the area, thereby continuously spreading the plating film.
[0100] Here, in the step (1), the material of the substrate is not particularly limited, but by using an insulating material such as resin or glass, the conductivity exhibited by the metal oxide can be effectively utilized. In the device substrate, etc., metal wiring, etc. may be present on the resin or glass. In the step (2), the metal oxide film can be formed by a coating method using a fine particle dispersion of metal oxide. Here, the metal oxide may be a material that can exhibit a state containing a metal element having an oxidation number smaller than the maximum oxidation number in the metal oxide, and may be an insulating material that does not exhibit the above state at this stage. In the step (3), the mechanical contact portion between the underlayer and the cathode becomes an electrical contact between the underlayer and the power source, and the electrical contact is placed in the plating solution. In the step (4), reduction and plating of the metal element in the underlayer are performed. An arbitrary anode, for example, mainly a copper plate in copper plating, mainly a nickel plate in nickel plating, or platinum, carbon, etc., is used as the anode, and the anode is placed in the plating solution. Then, when electrolysis is performed in the plating solution, the following characteristic plating film precipitation reaction occurs in this embodiment. (4-1) The underlayer is subjected to a reducing action around the electrical contact, causing a reaction that exhibits electrical conductivity, in which the underlayer becomes a state in which it contains a metal element having an oxidation number smaller than the maximum oxidation number in a metal oxide, such as a mixed valence state. (4-2) A reaction is caused to occur in the conductive areas of the underlayer to deposit a plating film. (4-3) Electrolysis is continued to continuously expand the conductive region around the plating film while the plating film is formed on the surface of the region, thereby continuously expanding the plating film.
[0101] In the above electroplating method, the plating film spreads continuously, and in the vicinity of the deposited metal, a part of the metal in the metal oxide is reduced, and the metal oxide becomes in a mixed valence state and exhibits electrical conductivity. When a conductive substance is dotted in the metal oxide film that is the plating underlayer, when the front of the spreading plating film touches the conductive substance, a reaction in which the metal element in the metal oxide is reduced proceeds efficiently around the conductive substance.
[0102] Therefore, in the above specific plating process, although there was no restriction on the state of the metal oxide in step (2), by replacing this step with the method for producing a metal-modified metal oxide according to the present invention, the steps (3) and after are entered in a state in which the metal is present on the metal oxide film surface, and therefore the spreading of the plating metal described in step (4) proceeds efficiently.
[0103] The method for producing a metal-modified metal oxide according to the present invention allows the production of a device having the metal-modified metal oxide as an electrode. Examples of such devices include a circuit board produced by plating the metal oxide. Also, examples of such devices include a gas sensor having the metal-modified metal oxide disposed on an interdigital electrode. EXAMPLES
[0104] Next, the present invention will be described with reference to examples, but the present invention is not limited to the following examples.
[0105] (Example 1) Preparation of coating agent (1) Sodium tungstate dihydrate was dissolved in an aqueous solution containing 20% ethanol to a concentration of 0.1 mol / L. The solution was acidified by adding hydrochloric acid or sulfuric acid while stirring. For example, the pH was adjusted to 2 with hydrochloric acid. The container was covered and the acidified liquid was heated. For example, it was placed in a thermostatic bath at 80°C for 24 hours. After heating, a bluish white precipitate was obtained at the bottom of the container. The precipitate was centrifuged and washed by adding distilled water to redisperse the precipitate, and a coating agent with dispersed fine particles was produced. Even if the fine particles were dried once, they were easily redispersed by adding distilled water. X-ray diffraction of the dried particles showed that they were hexagonal tungsten oxide. Scanning electron microscope (SEM) observation showed that the particles were rod-shaped with a diameter of less than 10 nm and a length of about 100 nm.
[0106] The precipitate after centrifugation was easily dispersed in ethanol, 2-propanol, etc. No precipitation occurred even when a non-ionic surfactant was added. The dispersed state was maintained even one year after preparation. In addition to tungsten, coating agents containing oxides of molybdenum and vanadium, as well as composite oxides combining these elements, were obtained using the same method.
[0107] (Example 2) Preparation of coating agent (2) A 0.5 mol / L aqueous solution of sodium tungstate dihydrate was prepared. A cation exchange resin was added to the aqueous solution, stirred, and then filtered. The filtered solution was added to the cation exchange resin again, and the filtering operation was repeated several times, resulting in a yellowish solution. This solution was solidified after drying. Metal acid solutions were also obtained by combining molybdenum, vanadium, and each metal element. A solution made from a salt of molybdic acid and a solution made by mixing tungstate and molybdate in approximately the same amount of substance were blue. A solution made by mixing tungstate and molybdate in approximately the same amount of substance did not produce particles even when heated. In other cases, the color of the solution changed and particles were produced when the solution was left at room temperature or heated at 60°C or 80°C.
[0108] The liquid in which the particles obtained in Example 2 were produced could be used to produce a coating agent by washing the particles as in Example 1. A coating agent could also be produced by mixing the precipitate by stirring or the like without separating the supernatant. A liquid in which tungstic acid and molybdic acid were mixed in approximately equal amounts could be stably used as a coating agent for at least 10 months or more without generating particles or precipitation.
[0109] (Example 3) Coating experiment (1) The liquid prepared in Example 1 was used as a coating agent by adjusting the concentration with water so that it contained 5 wt% oxide particles, and adding a nonionic surfactant. A coating film of tungsten oxide or the like was obtained on the substrate by dip coating, in which a plate-shaped or rod-shaped glass substrate or ABS resin substrate was immersed in the coating agent, pulled up, and dried.
[0110] (Example 4) Coating experiment (2) A liquid that does not contain particles, such as the liquid containing tungsten and molybdenum in equal amounts in Example 2, was directly coated onto a resin substrate as a coating agent by dip coating or the like. After drying, an oxide solid was obtained. No clear peaks derived from crystals were observed in the X-ray diffraction measurement of this solid.
[0111] (Example 5) Metal Modification Tungsten oxide and molybdenum oxide films were prepared by coating once on a glass substrate using the method of Example 3. Vanadium oxide films were obtained by dropping the dispersion onto a resin substrate and drying it. Films were also prepared according to Example 4. For copper and silver modification, 0.1 mol / L aqueous solutions of copper nitrate and silver nitrate were prepared, respectively, and each sample was immersed in the solutions for 1 minute and then washed with distilled water. In addition, gold, palladium, platinum, etc. were also treated using a commercially available standard solution for atomic absorption spectrometry with a concentration of 1000 ppm. When a standard solution was used, the standard solution was dropped onto the sample, and then the sample was washed with distilled water.
[0112] Example 6: Analysis of metal-modified metal oxides The water-based coating agent containing about 5 wt% tungsten oxide used in Example 3 was applied once to a glass substrate by dip coating, resulting in a coating density of 0.04 mg / cm. 2 When this was immersed in a silver nitrate aqueous solution for 1 minute in the same manner as in Example 5, the amount of silver attached was 0.003 mg / cm 2 The ratio of the amount of substance was 0.13 when converted to the ratio of the amount of substance with the silver value as the numerator and the tungsten value as the denominator. A total analysis of the components attached to the glass was performed by dissolving the attached components and using an inductively coupled plasma optical emission spectrometer. The result of an extreme surface analysis using X-ray photoelectron spectroscopy (XPS) showed that the ratio of the amount of substance was 0.19. This confirmed that silver was unevenly distributed on the surface of the tungsten oxide film. Furthermore, to investigate the valence of tungsten, the chemical bond state of the W4f spectrum was analyzed by XPS. The peak-separated W4f 7 / 2 The spectra show that tungsten oxide with and without silver modification It was also confirmed that tungsten with a valence of +6 and +5 was present in the sample. The proportion of tungsten atoms with a valence of +5 was 11% in the sample without silver modification and 4% in the sample with silver modification, and it was confirmed that the proportion of tungsten atoms with a valence of +5 decreased and the proportion of atoms with a valence of +6 increased for tungsten in the oxide after silver modification.
[0113] Magnified observation of silver-modified tungsten oxide films with SEM showed that no silver particles could be clearly identified. X-ray diffraction measurements also showed no clear diffraction peaks for silver or silver compounds. When tungsten was reduced to a valence of +5 to the extent that the tungsten oxide film clearly showed a blue color, the film sometimes took on a blackish color when modified with silver. When such films were observed with SEM, backscattered electron images showed the presence of particles with diameters of about several tens of nanometers on the surface of the tungsten oxide film.
[0114] (Example 7 and Comparative Example 1) Confirmation of catalytic activity A tungsten oxide sample and a molybdenum oxide sample coated on an ABS resin substrate and a glass substrate in the same manner as in Example 3, and a sample containing the same substances tungsten and molybdenum coated on an ABS resin substrate in the same manner as in Example 4 were prepared. Samples modified with silver and samples modified with palladium were prepared for each substrate and immersed in an electroless copper plating solution. OPC-750 manufactured by Okuno Chemical Industries Co., Ltd. was used as the plating solution. Copper plating films were deposited on the tungsten oxide sample, the molybdenum oxide sample, and the samples prepared in the same manner as in Example 4, both modified with silver and palladium. Copper was uniformly deposited even if the substrate had a shape like a round bar. For comparison, no copper deposition was observed in the samples where the glass substrate itself was modified with silver, the sample where a tin oxide film made of tin with a valence of +4, which is the maximum oxidation number among oxides, was modified with silver, and the tungsten oxide sample that was not modified with silver.
[0115] (Example 8 and Comparative Example 2) Confirmation of antibacterial activity Water was poured up to the 100 mL mark into a beaker containing one commercially available 40 g pack of natto and stirred. The supernatant was filtered through filter paper, and the filtrate was collected to produce natto bacteria liquid. Tungsten, molybdenum, and vanadium oxide films were prepared on a glass substrate and immersed in a silver nitrate aqueous solution for one minute. For comparison, a glass substrate and a film made of +4 tin oxide were immersed in a silver nitrate aqueous solution for one minute. In addition, films of tungsten oxide and molybdenum oxide that were not silver-modified were prepared.
[0116] After dropping the natto bacteria liquid onto each sample, they were dried and placed in a desiccator with water at the bottom and left overnight. The natto bacteria liquid-attached surface of each sample was rubbed onto a Petan Check DD general bacteria detection agar medium made by Eiken Chemical Co., Ltd. after one night. The agar medium was placed in a thermostatic chamber at 37°C, and after 9 hours, a color-developing liquid was dropped onto it and the appearance of the natto bacteria colonies was observed. As a result, in the case of samples in which the films of tungsten, molybdenum, and vanadium oxides were silver-modified, no natto bacteria colonies were observed on the agar medium. For the samples prepared for comparison, which were glass material and tin oxide films made of +4 tin treated with a silver nitrate solution, and films of tungsten oxide and molybdenum oxide alone that were not silver-modified, natto bacteria colonies appeared all over the area where the agar medium sample was rubbed. The results were the same even if the natto bacteria liquid was dropped onto the sample without drying and left overnight.
[0117] (Comparative Example 3) Antibacterial properties of tungsten oxide film after oxidation reaction Tungsten oxide was formed on glass with a conductive film of fluorine-doped tin oxide by dip coating in the same manner as in Example 3. In an electrolyte acidified with sulfuric acid, the prepared coating film was used as the working electrode, platinum as the counter electrode, and a silver-silver chloride electrode as the reference electrode, and the potential was scanned from the natural potential to +1000 mV, exposing the tungsten oxide film to an oxidizing atmosphere. The substrate with the tungsten oxide film was washed with water, dried, and subjected to the same operation using the natto bacteria liquid as in Example 8. The presence or absence of colonies was observed on the agar medium, and colonies were observed in the area where the sample was rubbed.
[0118] Example 9: Evaluation of the effect of ultraviolet rays A glass substrate coated with tungsten oxide was prepared in the same manner as in Example 3. In a yellow room that excludes short-wavelength light such as ultraviolet light, a silver nitrate aqueous solution was used for silver modification in the same manner as in Example 5, and the natto bacteria liquid was dropped onto the sample, followed by leaving the sample overnight. After leaving the sample overnight, the sample was removed from the yellow room, and colonies were observed using an agar medium in the same manner as in Example 8. As a result, no colonies were observed on the agar medium in the area where the natto bacteria liquid-adhered portion of the silver-modified tungsten oxide film was rubbed.
[0119] (Example 10 and Comparative Example 4) Use of silver-modified tungsten oxide as a plating undercoat As in Example 3, tungsten oxide was coated onto a 3 cm square ABS resin substrate. As in Example 5, a sample was prepared that was immersed in a silver nitrate aqueous solution to be silver-modified, and a sample with a tungsten oxide film as is. Copper tape was attached to the top of each sample as an electrical contact. A plating solution was prepared by adding a brightener to a copper sulfate plating solution mainly composed of copper sulfate. The substrate was immersed in the plating solution so that a part of the copper tape was in contact with the plating solution, and a copper plate was placed as an anode. Electric plating was performed under a constant current condition of 0.45 A. The time from when the plating film began to spread from the electrical contact until the entire substrate was covered with the copper plating film was 7 minutes in the case of silver modification and 12 minutes in the case of no silver modification.
[0120] (Example 11) Imparting base resistance to tungsten oxide film by silver modification As in Example 10, tungsten oxide was coated on a 3 cm square ABS resin substrate. Only the right half of the substrate was immersed in a 0.1 mol / L silver nitrate aqueous solution for 1 minute, washed with distilled water, and then dried. Next, only the lower half of the substrate was immersed in a pH 12 sodium hydroxide aqueous solution for 1 minute, washed with distilled water, and then dried. Electrical contacts were provided on the substrate, and the substrate was placed in the plating solution so that a part of the electrical contact was immersed in the copper sulfate plating solution, and electroplating was performed. When the plating film was spread from the electrical contact while increasing the current value, the plating film quickly spread in the right half of the coating part, which is the area modified with silver, in the upper half of the substrate. For the lower half of the substrate immersed in a sodium hydroxide aqueous solution, a copper plating film was deposited without defects in the right area modified with silver. Copper deposition did not occur in the left area not modified with silver. It was confirmed that the silver modification made it difficult for tungsten oxide to dissolve even in a basic solution.
[0121] (Example 12) Reduction of metals in metal oxides by adding reducing agents In Example 1, when a polyhydric alcohol, such as ethylene glycol, was added to the solvent instead of ethanol, the resulting particles were more bluish. Also, when a metal that dissolves in acid, such as aluminum, iron, zinc, etc., or +2valent iron ions or +2valent tin ions, was added in the step before heating, blue particles were obtained after heating. Furthermore, when +2valent iron ions or +2valent tin ions were added to the particle dispersion after heating, the color was blue.
[0122] (Example 13) Confirmation of oxidation-reduction reaction A tungsten oxide film was formed on fluorine-doped tin oxide in the same manner as in Example 3. The electrodes and electrolyte were configured in the same manner as in Comparative Example 3, and the potential was swept from the natural potential to -400 mV to increase the proportion of +5 tungsten in the tungsten oxide. At this time, the tungsten oxide film exhibited a blue color. When the film in this state was immersed in plating solutions of various metals, the blue color was maintained in zinc, nickel, and tin plating solutions, but the blue color disappeared in copper plating solutions and silver nitrate aqueous solutions, and the film surface tended to become black. This confirmed that the reaction in which +5 tungsten in the metal oxide is oxidized to +6 tungsten and the reaction in which metal ions in the solution are reduced depend on the redox potential of the metal in the solution, and that ions of a metal that exhibits a relatively noble redox potential are reduced.
Claims
1. A method for producing a metal oxide comprising the steps of: preparing an oxide of any one of a metal element selected from the group consisting of tungsten, molybdenum, vanadium, niobium, titanium, and tantalum, wherein at least a portion of the metal element contained in the oxide has an oxidation number smaller than a maximum oxidation number in the oxide; a step of contacting the metal oxide with a solution containing ions of a modifying metal to oxidize the metal element in the metal oxide to a higher oxidation number while modifying the surface of the metal oxide with the modifying metal by an oxidation-reduction reaction in which the modifying metal ions in the solution are reduced; 2. A method for producing a metal-modified metal oxide comprising the steps of:
2. The method for producing a metal-modified metal oxide according to claim 1, forming the metal oxide as a film on a surface of a substrate; A method for producing a metal-modified metal oxide, comprising contacting the film with the solution to modify the film with the modifying metal.
3. 3. A method for producing an antibacterial material, comprising the steps of: preparing a metal-modified metal oxide by the method for producing a metal-modified metal oxide according to claim 1 or 2; and using the metal-modified metal oxide as at least a part of the antibacterial material.
4. 3. A method for producing a plated product, comprising the steps of: preparing a metal-modified metal oxide by the method for producing a metal-modified metal oxide according to claim 1 or 2; and forming a plating film on a base by using the metal-modified metal oxide as a base.
5. A method for manufacturing a device, comprising preparing a metal-modified metal oxide by the method for manufacturing a metal-modified metal oxide described in claim 2, and providing the metal-modified metal oxide as an electrode.
Citation Information
Patent Citations
Method for preparing vanadium pentoxide
CN102219257A
Method for manufacturing multilayer circuit consisting of conductive path and micro-via
JP2002057460A
Pigment, coating material, and method for producing them
JP2004231927A
Blue particulate-dispersed body, and article using the same
JP2008291157A
Antivirus composition, and method for adding antivirus function
JP2019178076A