Solid electrolytic capacitor and method for manufacturing the same
By forming conductive and organic solvent layers with benzenetriol derivatives in specific concentration ratios, the electrolytic capacitor maintains low E.S.R. in high-temperature environments, addressing the limitations of conventional capacitors.
Patent Information
- Application Number
- JP2021070650
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-19
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2041-04-19
AI Technical Summary
Existing electrolytic capacitors fail to maintain low equivalent series resistance (E.S.R.) in high-temperature environments, both initially and over time.
The electrolytic capacitor is manufactured by impregnating a capacitor element with a first liquid containing a conductive polymer and an antioxidant, followed by a second liquid with an organic solvent and antioxidant, forming conductive and organic solvent layers, using benzenetriol or its derivatives as antioxidants, with specific concentration ratios to suppress thermal oxidative deterioration.
The capacitor achieves low initial E.S.R. and maintains a lower E.S.R. than conventional capacitors in high-temperature environments, reducing leakage current and thermal oxidative deterioration.
Smart Images

Figure 0007574133000002 
Figure 0007574133000003 
Figure 0007574133000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolytic capacitor and a method for manufacturing an electrolytic capacitor. [Background technology]
[0002] A known electrolytic capacitor includes a capacitor element having an anode with a dielectric oxide film, a cathode, and a separator disposed between the anode and the cathode, and an exterior body that houses the capacitor element.
[0003] Patent Document 1 describes an electrolytic capacitor in which a polyhydroxy compound is contained in a conductive polymer layer formed on a dielectric oxide film. Patent Document 1 describes that when a polyhydroxy compound having a melting point of 40° C. or more and 150° C. or less is used, it is possible to improve the conductivity and reduce the ESR (equivalent series resistance).
[0004] Patent Document 2 describes that the electrolyte of an electrolytic capacitor contains a first aromatic compound having a hydroxyl group as a solute acid component. Patent Document 2 also describes that the first aromatic compound having a hydroxyl group can maintain a low ESR for a long period of time. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6767630 [Patent Document 2] International Publication No. 2017 / 056447 Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, there has been a demand for electrolytic capacitors that can maintain a lower ESR than conventional capacitors in high-temperature environments. In addition, electrolytic capacitors are required to have a low initial ESR.
[0007] An object of the present invention is to provide an electrolytic capacitor which has a low initial ESR and can maintain an ESR lower than that of conventional capacitors in a high temperature environment. [Means for solving the problem]
[0008] Techniques capable of reducing the ESR are described in Patent Documents 1 and 2, etc. However, the inventors' research has revealed that even if these techniques are adopted, they are insufficient to achieve a desired low ESR in the initial state and in a high-temperature environment.
[0009] The inventors have further conducted research and found that the following invention provides an electrolytic capacitor capable of maintaining a lower ESR than conventional capacitors in high-temperature environments, and that the initial ESR can be reduced by using this electrolytic capacitor.
[0010] The method for producing an electrolytic capacitor of the present invention is a method for producing an electrolytic capacitor including a capacitor element body having an anode with a dielectric oxide film, a cathode, and a separator disposed between the anode and the cathode, the method comprising: a first step of impregnating the capacitor element body with a first liquid containing a conductive polymer and an antioxidant at 0.2 wt% or more and 2.0 wt% or less, and then heat treating the capacitor element body to form a conductive polymer layer on the dielectric oxide film; and a second step of impregnating the capacitor element body with a second liquid containing an organic solvent and an antioxidant at 0.2 wt% or more and 10.0 wt% or less, to form an organic solvent layer after the conductive polymer layer is formed, the capacitor element body being impregnated with a second liquid containing an organic solvent and an antioxidant at 0.2 wt% or more and 10.0 wt% or less, the antioxidant contained in the first liquid and the antioxidant contained in the second liquid being at least one selected from benzenetriol and derivatives of benzenetriol, and the concentration of the antioxidant in the second liquid being the same as or higher than the concentration of the antioxidant in the first liquid.
[0011] According to the present invention, the first liquid forming the conductive polymer layer and the second liquid forming the organic solvent layer each contain at least one antioxidant selected from benzenetriol and derivatives of benzenetriol. Within the above range of antioxidant concentration, the concentration of the antioxidant in the second liquid forming the organic solvent layer is set to be the same as that of the first liquid forming the conductive polymer layer, or higher than that of the first liquid. It has been found that this makes it possible to manufacture an electrolytic capacitor that has a low initial ESR and can maintain a lower ESR than conventional electrolytic capacitors in a high temperature environment.
[0012] The organic solvent contained in the second liquid may be at least one selected from polyalkylene glycols, polyglycerols, and derivatives thereof.
[0013] By using an organic solvent such as polyalkylene glycol to form the organic solvent layer, the repair performance of the dielectric oxide film of the anode is improved, and a reduction in leakage current can be expected.
[0014] The polyalkylene glycol may be at least one selected from the group consisting of polyethylene glycol, polypropylene glycol, and a copolymer of ethylene glycol and propylene glycol.
[0015] By using the above-mentioned compounds, which are easily available, to form an organic solvent layer, a reduction in leakage current can be expected.
[0016] The electrolytic capacitor according to the present invention is an electrolytic capacitor including a capacitor element body having an anode having a dielectric oxide film, a cathode, and a separator disposed between the anode and the cathode, wherein a conductive polymer layer containing at least a conductive polymer and an antioxidant, and an organic solvent layer containing at least an organic solvent and an antioxidant are formed in the capacitor element body, the antioxidant contained in the conductive polymer layer and the antioxidant contained in the organic solvent layer are at least one selected from benzenetriol and derivatives of benzenetriol, and the weight ratio of the antioxidant contained in the conductive polymer layer to the antioxidant contained in the organic solvent layer is 1:1 to 1:50.
[0017] According to the above configuration, the conductive polymer layer and the organic solvent layer each contain at least one selected from benzenetriol and a derivative of benzenetriol as an antioxidant. The ratio of the antioxidant in the conductive polymer layer to the antioxidant in the organic solvent layer is 1:1 to 1:50. It has been found that this makes it possible to provide an electrolytic capacitor that has a low initial ESR and can maintain a lower ESR than conventional electrolytic capacitors in a high temperature environment.
[0018] In the above configuration, the organic solvent contained in the organic solvent layer may be at least one selected from polyalkylene glycols, polyglycerols, and derivatives thereof.
[0019] By including an organic solvent such as polyalkylene glycol in the organic solvent layer, the repair performance of the dielectric oxide film of the anode is improved, and a reduction in leakage current can be expected.
[0020] The polyalkylene glycol may be at least one selected from the group consisting of polyethylene glycol, polypropylene glycol, and a copolymer of ethylene glycol and propylene glycol.
[0021] By using the above-mentioned compounds, which are easily available, as the organic solvent, a reduction in leakage current can be expected. Effect of the Invention
[0022] According to the present invention, it is possible to provide an electrolytic capacitor that has a low initial ESR and can maintain an ESR lower than that of conventional capacitors in a high temperature environment. [Brief description of the drawings]
[0023] [Figure 1] 1 is a cutaway front view of a main portion of an electrolytic capacitor according to an embodiment of the present invention; [Diagram 2] FIG. 2 is an exploded perspective view of the capacitor element shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings.
[0025] As shown in FIG. 1, electrolytic capacitor 1 includes exterior body 4 having exterior case 2 and sealing body 3 that seals the opening of exterior case 2, and capacitor element 5 housed in exterior body 4.
[0026] As shown in FIG. 2, capacitor element 5 is formed by winding anode 11 and cathode 12 with separator 13 interposed therebetween into a cylindrical shape, and is secured in place by tape 14 attached to the outer circumferential surface.
[0027] Lead tabs (not shown) are connected to the anode 11 and the cathode 12, respectively. The anode 11 is connected to a lead terminal 21 via a lead tab. The cathode 12 is connected to a lead terminal 22 via a lead tab. The lead terminals 21 and 22 are led out to the outside through holes 31 and 32, respectively, formed in the sealing body 3, as shown in FIG. 1.
[0028] The anode 11 shown in Fig. 2 is a valve metal having a dielectric oxide film formed on its surface. The valve metal may be at least one selected from the group consisting of aluminum, tantalum, niobium, and titanium. The dielectric oxide film is formed, for example, by roughening the surface of a foil of the valve metal by etching, and then subjecting it to a chemical conversion treatment.
[0029] The cathode 12 is formed using a valve metal. For example, a valve metal foil whose surface is roughened by etching, or a foil whose surface is roughened and then chemically treated, is used as the cathode 12. A plain foil that is not etched may be used as the cathode 12. Furthermore, a coating foil in which a metal thin film containing at least one metal selected from the group consisting of titanium, nickel, titanium carbide, nickel carbide, titanium nitride, nickel nitride, titanium carbonitride, and nickel carbonitride is formed on the surface of the roughened foil or plain foil may be used. A coating foil in which a carbon thin film is formed on the surface of the roughened foil or plain foil may be used.
[0030] There is no particular limitation on the material of the separator 13. For example, a material mainly made of cellulose may be used as the separator 13.
[0031] A conductive polymer layer supported by a separator 13 is formed between the dielectric oxide film of the anode 11 and the cathode 12. The conductive polymer layer contains a conductive polymer and an antioxidant. The conductive polymer layer is a layer formed by impregnating the dielectric oxide film with a first liquid containing a conductive polymer and 0.2 wt % to 2.0 wt % of the antioxidant, and then heat-treating the first liquid.
[0032] The polymer contained in the conductive polymer layer may be, for example, polythiophene, polypyrrole, polyaniline, or a derivative thereof. Polyethylenedioxythiophene (PEDOT) is generally used as the polymer. The polymer is not limited to these.
[0033] The conductive polymer layer further includes a dopant. As the dopant, p-toluenesulfonic acid, polystyrenesulfonic acid (PSS), etc. are generally used. The dopant is not limited to these. A self-doped conductive polymer may also be used.
[0034] The conductive polymer layer may contain other additives in addition to the polymer, the dopant, and the antioxidant described above. The antioxidant will be described later.
[0035] Capacitor element 5 shown in FIG. 2 further has an organic solvent layer. The organic solvent layer contains an organic solvent and an antioxidant. The organic solvent layer is a layer formed by impregnating a capacitor element body having anode 11, cathode 12, and separator 13 with a second liquid containing an organic solvent and 0.2 wt % to 10.0 wt % of an antioxidant after the conductive polymer layer is formed. The organic solvent layer is formed or held in the voids of capacitor element 5 on which the conductive polymer layer is formed.
[0036] The organic solvent may be, for example, at least one selected from polyalkylene glycol, polyglycerin, and derivatives thereof. These improve the repair performance of the dielectric oxide film of the anode, so that a reduction in leakage current can be expected. The polyalkylene glycol may be at least one selected from polyethylene glycol, polypropylene glycol, and a copolymer of ethylene glycol and propylene glycol. These compounds are easily available, and are expected to reduce leakage current. The organic solvent contained in the organic solvent layer is not particularly limited.
[0037] The organic solvent layer may contain other additives in addition to the organic solvent and the antioxidant. The organic solvent layer may or may not contain an electrolyte.
[0038] The antioxidant contained in the conductive polymer layer and the antioxidant contained in the organic solvent layer are at least one selected from benzenetriol and derivatives of benzenetriol. Examples of benzenetriol include pyrogallol, hydroxynol, and phloroglucinol. The derivative of benzenetriol may be, for example, a derivative in which the hydrogen group of benzenetriol is etherified, esterified, halogenated, aminated, or carbonylated. Specifically, the derivative of benzenetriol may be a derivative in which the hydrogen group of benzenetriol is replaced with an atom or functional group other than the hydrogen group. Examples of functional groups include an amino group and a carboxyl group. Examples of derivatives of benzenetriol include propyl gallate. The antioxidant contained in the conductive polymer layer and the antioxidant contained in the organic solvent layer may be the same or different.
[0039] The amount of the antioxidant contained in the organic solvent layer is the same as or greater than the amount of the antioxidant contained in the conductive polymer layer. It is presumed that the magnitude relationship between the "amount of the antioxidant contained in the organic solvent layer" and the "amount of the antioxidant contained in the conductive polymer layer" has a tendency similar to the magnitude relationship between the "concentration of the antioxidant in the first liquid" for forming the conductive polymer layer and the "concentration of the antioxidant in the second liquid" for forming the organic solvent layer in the manufacturing method of the electrolytic capacitor 1 described later. In other words, when the "concentration of the antioxidant in the second liquid" for forming the organic solvent layer is the same as the "concentration of the antioxidant in the first liquid" for forming the conductive polymer layer, it is presumed that the "amount of the antioxidant contained in the organic solvent layer" is the same as the "amount of the antioxidant contained in the conductive polymer layer". When the "concentration of the antioxidant in the second liquid" for forming the organic solvent layer is higher than the "concentration of the antioxidant in the first liquid" for forming the conductive polymer layer, it is presumed that the "amount of the antioxidant contained in the organic solvent layer" is greater than the "amount of the antioxidant contained in the conductive polymer layer."
[0040] The conductive polymer layer and / or the organic solvent layer may contain other antioxidants in addition to the above antioxidants.
[0041] The above-mentioned electrolytic capacitor 1 is produced, for example, by the following method.
[0042] Lead tabs for external extraction electrodes are connected to anode 11 and cathode 12 (see FIG. 2) that have been cut to a specified width. Anode 11 and cathode 12 with the lead tabs connected are wound with separator 13 interposed therebetween to produce a capacitor element body. Anode 11 is a valve metal on which a dielectric oxide film is formed.
[0043] In order to repair the cut edge of the capacitor element body or the dielectric oxide film that was damaged during the preparation of the capacitor element body, the capacitor element body is subjected to a chemical conversion treatment. The chemical conversion treatment is performed by applying a voltage to the capacitor element body in a chemical conversion liquid. The chemical conversion liquid used for the chemical conversion treatment can be, for example, an aqueous solution containing at least one of adipic acid and an adipate.
[0044] Next, the capacitor element body is impregnated with a first liquid containing a conductive polymer and 0.2 wt% to 2.0 wt% of an antioxidant, and then heat-treated (for example, heated at 40°C to 220°C) (first step). The antioxidant is at least one selected from benzenetriol and derivatives of benzenetriol. The conductive polymer of the first liquid may be the polymer and dopant exemplified above. The polymer and dopant are not limited to a specific polymer and dopant. A self-doped conductive polymer may also be used. In addition to the polymer and antioxidant, the first liquid may further contain other additives. In addition to the at least one antioxidant selected from benzenetriol and derivatives of benzenetriol, the first liquid may also contain other antioxidants.
[0045] As a result of the above, a conductive polymer layer is formed on the capacitor element body.
[0046] Next, the capacitor element body on which the conductive polymer layer is formed is impregnated with a second liquid containing an organic solvent and 0.2 wt % to 10.0 wt % of the above-mentioned antioxidant (second step). The antioxidant is at least one selected from benzenetriol and derivatives of benzenetriol. The concentration of the antioxidant in the second liquid is the same as or higher than the concentration of the antioxidant in the first liquid. The antioxidant (at least one selected from benzenetriol and derivatives of benzenetriol) contained in the second liquid may be the same as or different from the above-mentioned antioxidant (at least one selected from benzenetriol and derivatives of benzenetriol) contained in the first liquid. The organic solvent may be any of the organic solvents exemplified above. The type of organic solvent is not particularly limited. The second liquid may further contain other additives. The second liquid may contain other antioxidants in addition to the at least one antioxidant selected from benzenetriol and derivatives of benzenetriol.
[0047] As a result of the above, an organic solvent layer is formed, and thus capacitor element 5 is obtained.
[0048] Capacitor element 5 is housed in exterior case 2 (see FIG. 1), and the opening of exterior case 2 is closed with sealing body 3. In this way, electrolytic capacitor 1 is obtained.
[0049] The present inventors have obtained the following findings.
[0050] The increase in ESR in high-temperature environments is believed to be due to the thermal oxidative degradation of the conductive polymer contained in the conductive polymer layer. Conventionally, the reason for the inability to adequately suppress the thermal oxidative degradation of conductive polymers is believed to be, for example, that the conductive polymer is thermally oxidatively deteriorated due to oxygen flowing into the conductive polymer layer. It is also believed that the thermal oxidative degradation caused by the conductive polymer present on the surface of the dielectric oxide film reacting with oxygen in the dielectric oxide film could not be adequately suppressed.
[0051] In contrast, it is believed that the electrolytic capacitor manufactured by the above-mentioned method can sufficiently suppress the thermal oxidative degradation of the conductive polymer. Specifically, it is believed that the benzenetriol and / or derivatives of benzenetriol contained in the conductive polymer layer as an antioxidant suppresses the thermal oxidative degradation of the conductive polymer even if oxygen flows into the conductive polymer layer. In addition, an organic solvent layer containing benzenetriol and / or derivatives of benzenetriol as an antioxidant is formed on the surface of the conductive polymer layer, and the antioxidant present in the organic solvent layer is secured to a certain extent. It is believed that this sufficiently suppresses the thermal oxidative degradation of the conductive polymer present on the surface of the dielectric oxide film. These findings make it possible to maintain a lower ESR than before in high temperature environments.
[0052] In addition, when the conductive polymer layer contains a large amount of antioxidant, the initial ESR tends to be high, but by including an antioxidant in the organic solvent layer, the concentration of the antioxidant in the first liquid that forms the conductive polymer layer can be reduced, which is thought to prevent the initial ESR of the electrolytic capacitor from becoming high.
[0053] As described above, according to the present embodiment, it is possible to manufacture an electrolytic capacitor that has a low initial ESR and can maintain a lower ESR than conventional capacitors in a high-temperature environment. The above-described electrolytic capacitor has a low initial ESR and can maintain a lower ESR than conventional capacitors in a high-temperature environment. EXAMPLES
[0054] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0055] An electrolytic capacitor was produced by the following method.
[0056] Aluminum lead tabs for external extraction electrodes were connected to the anode and cathode foils cut to a specified width. The anode aluminum foil was made by roughening the surface of the aluminum foil, which is a valve metal, by etching, and then forming a dielectric oxide film by chemical conversion treatment at 100 V. The cathode foil was aluminum foil on which carbon was vapor-deposited. The main body of the capacitor element was made by winding the anode aluminum foil and cathode aluminum foil with nylon-based electrolytic paper (separator) between them.
[0057] A chemical conversion treatment was performed to repair the dielectric oxide film that was lost on the cut edge of the anode foil and the attachment part of the lead tab. The chemical conversion treatment was performed by immersing the main body, which will become the capacitor element, in a chemical conversion solution and applying a voltage that is close to the chemical conversion voltage value of the dielectric oxide film. The chemical conversion solution used was an aqueous solution of ammonium adipate with an ammonium adipate concentration of 2 wt%.
[0058] Next, the capacitor element body was impregnated with the first liquid under reduced pressure under the following conditions (see [Conditions for preparing the conductive polymer layer and organic solvent layer] below), and then the capacitor element body was held in a thermostatic chamber set at 40°C for 30 minutes, and then heat-treated in a thermostatic chamber set at 160°C for 30 minutes. This impregnation and heat treatment was repeated twice. As a result, a conductive polymer layer was formed on the capacitor element body.
[0059] Next, the capacitor element body was impregnated with the second liquid under reduced pressure under the following conditions (see [Conditions for preparing the conductive polymer layer and organic solvent layer] below), and then the capacitor element body was left in a thermostatic chamber at 135°C for 30 minutes to form an organic solvent layer.
[0060] The obtained capacitor element was placed in an aluminum case, and the periphery of the opening of the case was curled. The rated voltage (63V) was applied to the capacitor element placed in the case in a thermostatic chamber set at 125°C, and an aging process was performed to produce an electrolytic capacitor. The electrolytic capacitor produced in this experiment has a category upper limit temperature of 125°C, a rated voltage of 63WV, a rated capacitance of 22μF, and a product size of φ8×7L (mm).
[0061] [Conditions for preparing conductive polymer layer and organic solvent layer] <Conventional Condition 1> Conductive polymer layer: Dispersion liquid (containing no antioxidant) made by mixing PEDOT / PSS (concentration 2.0 wt%) and ethylene glycol (concentration 10 wt%) Organic solvent layer: None <Conventional Condition 2> Conductive polymer layer: Dispersion liquid (containing no antioxidant) made by mixing PEDOT / PSS (concentration 2.0 wt%) and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 0.5 wt%) "PEG400" is polyethylene glycol with a number average molecular weight of 400. <Conventional Condition 3> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution (without antioxidant) <Example 1> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.2 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 0.2 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:1 <Example 2> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.2 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:25 <Example 3> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 1.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:2 <Example 4> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Example 5> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 10.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:20 <Example 6> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 2.0 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:2.5 <Example 7> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.2 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 10.0 wt%) Antioxidant contained in conductive polymer layer:Antioxidant contained in organic solvent layer=1:50 <Example 8> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), phloroglucinol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing phloroglucinol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Example 9> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), phloroglucinol (concentration 1.0 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing phloroglucinol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:5 <Example 10> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), hydroxynol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing hydroxynol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Example 11> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), propyl gallate (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing propyl gallate (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Example 12> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing phloroglucinol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Example 13> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), hydroxynol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Comparative Example 1> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 0.2 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 0.1 wt%) Antioxidant contained in conductive polymer layer: Antioxidant contained in organic solvent layer = 1:0.5 <Comparative Example 2> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 1.0 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 0.5 wt%) Antioxidant contained in conductive polymer layer: Antioxidant contained in organic solvent layer = 1:0.5 <Comparative Example 3> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 5.0 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 0.5 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:0.1 <Comparative Example 4> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), pyrogallol (concentration 10.0 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 0.5 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:0.05 <Comparative Example 5> Conductive polymer layer: Dispersion liquid of PEDOT / PSS (concentration 2.0 wt%), catechol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing catechol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Comparative Example 6> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), p-nitrophenol (concentration 0.5 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing p-nitrophenol (concentration 5.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:10 <Comparative Example 7> Conductive polymer layer: Dispersion of PEDOT / PSS (concentration 2.0 wt%), hydroxynol (concentration 5.0 wt%), and ethylene glycol (concentration 10 wt%) Organic solvent layer: Polyethylene glycol (PEG400) solution containing pyrogallol (concentration 1.0 wt%) Antioxidant contained in the conductive polymer layer:Antioxidant contained in the organic solvent layer=1:0.2
[0062] (evaluation) As an initial characteristic, the equivalent series resistance (ESR) of the electrolytic capacitor was measured in an environment of 20°C. Next, the rated voltage (63 V) was applied to the electrolytic capacitor in a high-temperature atmosphere of 150°C for 1,000 hours (hereinafter referred to as "after high-temperature test"), and then the equivalent series resistance (ESR) of the capacitor was measured.
[0063] Table 1 shows the experimental conditions and evaluation results. In Table 1, "Avg." is the arithmetic mean value of ESR (n=30). "cf" in "150°C rated application test after 1000 hours" ("after high temperature test") is the rate of increase in ESR after the high temperature test compared to the initial ESR. "cf" is calculated using the following formula. cf = (Avg. ESR after high temperature test - Initial Avg. ESR) / Initial Avg. ESR
[0064] [Table 1]
[0065] As shown in Table 1, the electrolytic capacitor under conventional condition 1 is a capacitor that does not contain an antioxidant in the conductive polymer layer and does not have an organic solvent layer, the electrolytic capacitor under conventional condition 2 is a capacitor that contains benzenetriol as an antioxidant only in the organic solvent layer, and the electrolytic capacitor under conventional condition 3 is a capacitor that contains benzenetriol as an antioxidant only in the conductive polymer layer. As shown in Table 1, the ESR after high-temperature testing was high under conventional conditions 1 to 3. In addition, the rate of increase (cf) of ESR was large under conventional conditions 1 to 3.
[0066] As shown in Table 1, the electrolytic capacitors of Examples 1 to 13 are capacitors in which both the conductive polymer layer and the organic solvent layer contain benzenetriol or a derivative of benzenetriol as an antioxidant. In Example 1, the concentration of the antioxidant in the second liquid is the same as the concentration of the antioxidant in the first liquid. In this case, it is presumed that the amount of the antioxidant in the organic solvent layer is the same as the amount of the antioxidant in the conductive polymer layer. In Examples 2 to 13, the concentration of the antioxidant in the second liquid is higher than the concentration of the antioxidant in the first liquid. In this case, it is presumed that the amount of the antioxidant in the organic solvent layer is greater than the amount of the antioxidant in the conductive polymer layer.
[0067] In Examples 1 to 13, the initial ESR was low and the ESR after the high-temperature test was also low, as shown in Table 1. Furthermore, the rate of increase in ESR (cf) was small. That is, the electrolytic capacitors of Examples 1 to 13 were electrolytic capacitors that had a low initial ESR and were capable of maintaining a lower ESR than conventional electrolytic capacitors in a high-temperature environment.
[0068] In addition, although the types of antioxidants in Examples 1 to 7 and those in Examples 8 to 13 were different, the effects of Examples 1 to 7 were equivalent to those of Examples 8 to 13. From this, it is considered that when the antioxidant is benzenetriol and / or a derivative of benzenetriol, the initial ESR is low and a lower ESR than conventional ones can be maintained in a high temperature environment regardless of the type of antioxidant.
[0069] As shown in Table 1, in the electrolytic capacitors of Comparative Examples 1 to 4 and 7, both the conductive polymer layer and the organic solvent layer contained benzenetriol or a derivative of benzenetriol as an antioxidant, but the ESR after the high-temperature test was high. In Comparative Examples 1 to 4 and 7, unlike Examples 1 to 12, the concentration of the antioxidant in the first liquid was higher than that in the second liquid. In this case, it is presumed that the amount of the antioxidant in the conductive polymer layer was greater than that in the organic solvent layer. This is considered to have influenced the ESR after the high temperature test.
[0070] The initial ESR was high in Comparative Examples 3 and 4. Moreover, the initial ESR in Comparative Example 7 was higher than that in Example 13 in which the same antioxidant as in Comparative Example 7 was used. In Comparative Examples 3, 4, and 7, the concentration of the antioxidant in the first liquid was higher than in Examples 1 to 13. In these cases, it is presumed that the amount of the antioxidant in the conductive polymer layer was large, which is thought to have affected the initial ESR.
[0071] In Comparative Examples 5 and 6, the ESR after the high-temperature test was high, and the ESR increase rate (cf) was large. In Comparative Example 5, catechol, which is a benzenediol, was used as the antioxidant. In Comparative Example 6, p-nitrophenol, in which the hydrogen atom of phenol is substituted with a nitro group, was used as the antioxidant. It was found that these antioxidants were unable to sufficiently suppress the increase in ESR in a high-temperature environment.
[0072] From the above experiment, the following was found. The first liquid forming the conductive polymer layer and the second liquid forming the organic solvent layer each contain benzenetriol or a derivative of benzenetriol as an antioxidant, the first liquid containing 0.2 wt% to 2.0 wt% of the antioxidant, and the second liquid containing 0.2 wt% to 10.0 wt% of the antioxidant. Furthermore, the concentration of the antioxidant in the second liquid is the same as or higher than the concentration of the antioxidant in the first liquid. In this case, it is presumed that the amount of the antioxidant contained in the organic solvent layer is the same as or higher than the amount of the antioxidant contained in the conductive polymer layer. It was found that the electrolytic capacitor fabricated under the above conditions had a low initial ESR and was capable of maintaining a lower ESR than conventional electrolytic capacitors in high temperature environments.
[0073] In the above experiments, in Examples 1 to 13, benzenetriol or a derivative of benzenetriol was used. However, the effect of the present invention can be obtained even when two or more selected from benzenetriol and a derivative of benzenetriol are used. In addition, in the above experiments, propyl gallate or phloroglucinol was used as a derivative of benzenetriol, but the effect of the present invention can be obtained even when other derivatives of benzenetriol are used.
[0074] In the above experiments, in Examples 1 to 13, PEDOT was used as the polymer and PSS was used as the dopant to form the conductive polymer layer. However, the polymer and dopant are not limited to the above. The effect of the present invention can be obtained even when other polymers are used. The effect of the present invention can be obtained even when other dopants are used.
[0075] In the above experiments, in Examples 1 to 13, polyethylene glycol was used as the organic solvent for the organic solvent layer and the second liquid. However, other organic solvents may be used as the organic solvent for the organic solvent layer and the second liquid. The effects of the present invention can be obtained even when other organic solvents are used as the organic solvent for the organic solvent layer and the second liquid.
[0076] Although the embodiment of the present invention has been described above based on the examples, the specific configuration should not be considered to be limited to these embodiments. The scope of the present invention is indicated by the claims rather than the above description, and includes all modifications within the meaning and scope of the claims.
[0077] In addition, in the above experiment, an electrolytic capacitor was fabricated with an upper category temperature limit of 125°C, a rated voltage of 63 WV, a rated capacitance of 22 μF, and a product size of φ8 × 7L (mm), but the upper category temperature limit, rated voltage, rated capacitance, and product size of the electrolytic capacitor of the present invention are not limited to the above. [Explanation of symbols]
[0078] 1. Electrolytic capacitor 2 Outer case 3 Sealing body 4 Exterior body 5 Capacitor elements 11 Anode 12 Cathode 21, 22 Lead terminal
Claims
1. A method for manufacturing a solid electrolytic capacitor including a capacitor element body having an anode having a dielectric oxide film, a cathode, and a separator disposed between the anode and the cathode, a first step of impregnating the capacitor element body with a first liquid containing a conductive polymer and an antioxidant at 0.2 wt % or more and 2.0 wt % or less, and then performing a heat treatment to form a conductive polymer layer on the capacitor element body; a second step of forming an organic solvent layer by impregnating the capacitor element body with a second liquid containing an organic solvent and an antioxidant at 0.2 wt % or more and 10.0 wt % or less, and not containing an electrolyte, after the conductive polymer layer is formed; having the antioxidant contained in the first liquid and the antioxidant contained in the second liquid are at least one selected from benzenetriol and derivatives of benzenetriol, A method for manufacturing a solid electrolytic capacitor, wherein a concentration of the antioxidant in the second liquid is the same as or higher than a concentration of the antioxidant in the first liquid.
2. 2. The method for producing a solid electrolytic capacitor according to claim 1, wherein the organic solvent contained in the second liquid is at least one selected from the group consisting of polyalkylene glycol, polyglycerin, and derivatives thereof.
3. 3. The method for producing a solid electrolytic capacitor according to claim 2, wherein the polyalkylene glycol is at least one selected from the group consisting of polyethylene glycol, polypropylene glycol, and a copolymer of ethylene glycol and propylene glycol.
4. A solid electrolytic capacitor comprising a capacitor element body having an anode having a dielectric oxide film, a cathode, and a separator disposed between the anode and the cathode, a conductive polymer layer including at least a conductive polymer and an antioxidant in the capacitor element body; An organic solvent layer is formed, the organic solvent layer containing at least an organic solvent and an antioxidant and not containing an electrolyte, the antioxidant contained in the conductive polymer layer and the antioxidant contained in the organic solvent layer are at least one selected from benzenetriol and derivatives of benzenetriol, a weight ratio of the antioxidant contained in the conductive polymer layer to the antioxidant contained in the organic solvent layer being 1:1 to 1:50;
5. 5. The solid electrolytic capacitor according to claim 4, wherein the organic solvent contained in the organic solvent layer is at least one selected from the group consisting of polyalkylene glycol, polyglycerin, and derivatives thereof.
6. 6. The solid electrolytic capacitor according to claim 5, wherein the polyalkylene glycol is at least one selected from the group consisting of polyethylene glycol, polypropylene glycol, and a copolymer of ethylene glycol and propylene glycol.
Citation Information
Patent Citations
Capacitor and its manufacturing method
JP2006186292A
Electrolytic capacitor and method for manufacturing the same
JP2016021453A
Solid electrolytic capacitor and manufacturing method for the same
JP2017017182A
Electrolytic capacitor manufacturing method and electrolytic capacitor
JP2017147466A
Manufacturing method of electrolytic capacitor
JP2020072132A