Battery cell, battery, and electrical device

By using the second lithium nickel cobalt manganese oxide with a higher nickel content as the cathode active material in lithium-ion batteries, the problem of delayed electrolyte return due to silicon material is solved, the cycle performance and energy density of the battery are improved, and the battery is extended improved battery life.

WO2024207655A1PCT designated stage expired Publication Date: 2024-10-10CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/112653
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2023-08-11
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Silicon material, as the negative electrode material of lithium-ion batteries, has a large volume change during the charge and discharge process, causing the electrolyte to not flow back in time, resulting in poor battery cycle performance.

Method used

The second lithium nickel cobalt manganese oxide containing a higher nickel content is used as the positive active material. During charging, its lattice shrinks to form gaps to store the squeezed out electrolyte. During discharge, it is beneficial for the electrolyte to flow back to the negative electrode sheet and improve the electrolyte separation. Lithium condition, thereby improving the cycle performance of the battery cells.

Benefits of technology

By reasonably controlling the content of the second lithium nickel cobalt manganese oxide in the positive active material and the proportion of silicon element in the negative active material, the cycle performance of the battery cells is improved, the energy density and stability of the battery are increased, and the battery life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023112653_10102024_PF_FP_ABST
    Figure CN2023112653_10102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of lithium batteries, and in particular to a battery cell, a battery and an electrical device. A positive electrode active material of the battery cell comprises a first lithium nickel manganese cobalt oxide and a second lithium nickel manganese cobalt oxide, and a negative electrode active material thereof comprises a silicon-based material and a carbon-based material, the molar content of nickel elements of the second lithium nickel manganese cobalt oxide amongst all transition metal elements being greater than that of nickel elements of the first lithium nickel manganese cobalt oxide amongst all transition metal elements, and in the second lithium nickel manganese cobalt oxide, the molar content of the nickel elements amongst all of the transition metal elements being greater than or equal to 0.8. In the present application, providing in the positive electrode active material the second lithium nickel manganese cobalt oxide having a relatively high content of nickel elements allows gaps formed by lattice contraction of the second lithium nickel manganese cobalt oxide during a charging process to store an electrolyte extruded by negative electrode silicon expansion, aiding in electrolyte backflow during the next charging process, reducing the occurrence of lithium plating, and thus improving the cycle performance of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Battery cells, batteries and electrical equipment

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310363528.4, filed on April 7, 2023, entitled “Battery Cell, Battery and Electrical Equipment,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the technical field of lithium batteries, and in particular to a battery cell, a battery, and an electrical device. Background Art

[0004] Lithium-ion batteries have made significant progress in recent years, finding widespread application in energy storage systems such as hydropower, thermal, wind, and solar power plants, as well as in electric vehicles, power tools, military equipment, and aerospace. However, in electric vehicles, such as electric bicycles, electric motorcycles, and electric cars, graphite anodes have essentially reached their gram capacity limit as market demands for higher battery life continue to rise, making them incapable of meeting future demands for high-energy-density cells.

[0005] Silicon, as a negative electrode material, boasts an ultra-high specific capacity, more than ten times the theoretical capacity of traditional carbon-based materials, and a comparable discharge platform. Therefore, it is considered the preferred negative electrode material for next-generation lithium-ion batteries. However, silicon, as a negative electrode material, is prone to significant volume changes during charge and discharge, causing a sudden drop in battery capacity and poor cycle performance.

[0006] Summary of the Invention

[0007] In view of this, the main technical problem to be solved by this application is the problem of poor battery cycle performance caused by silicon material as negative electrode material, thereby providing a battery cell, battery and electrical equipment that can improve the situation of untimely electrolyte reflux caused by the expansion of silicon material, and help improve the cycle performance of the battery cell.

[0008] The first aspect of the present application provides a battery cell including a positive electrode sheet and a negative electrode sheet. The positive electrode sheet includes a positive electrode active material, the positive electrode active material includes a first lithium nickel cobalt manganese oxide and a second lithium nickel cobalt manganese oxide, the molar content of nickel in the second lithium nickel cobalt manganese oxide in all its transition metal elements is greater than the molar content of nickel in the first lithium nickel cobalt manganese oxide in all its transition metal elements. In the second lithium nickel cobalt manganese oxide, the molar content of nickel in all transition metal elements is greater than or equal to 0.8. The negative electrode sheet includes a negative electrode active material, the negative electrode active material includes a silicon-based material and a carbon-based material.

[0009] In the technical solution of the embodiment of the present application, the positive electrode active material of the battery cell contains a second type of lithium nickel cobalt manganese oxide with a higher nickel content. During the charging process, the crystal lattice of the second type of lithium nickel cobalt manganese oxide shrinks significantly. This can improve the situation where the electrolyte is squeezed out due to the expansion of the silicon-based material during charging. The gaps formed by the contraction of the crystal lattice of the second type of lithium nickel cobalt manganese oxide are used to store the squeezed electrolyte, which is conducive to the electrolyte reflux to the negative electrode during discharge, thereby improving the occurrence of lithium precipitation due to untimely electrolyte reflux during the next charge, and further improving the cycle performance of the battery cell.

[0010] In any embodiment, the ratio of the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material to the mass fraction of silicon in the negative electrode active material is less than or equal to 10 and greater than 0. The mass fraction X2 of the second lithium nickel cobalt manganese oxide in the positive electrode active material is correlated with the mass fraction X1 of silicon in the negative electrode active material. The greater the silicon content in the negative electrode active material, the greater the content of the second lithium nickel cobalt manganese oxide in the positive electrode active material. In the embodiment of the present application, when Y = X2 / X1, and 0 < Y ≤ 10, the cycling performance of the battery cell is better.

[0011] In any embodiment, the ratio of the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material to the mass fraction of the silicon element in the negative electrode active material is less than or equal to 6 and greater than or equal to 4. When 4≤Y≤6, the cycle performance of the battery cell is better.

[0012] In any embodiment, the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material is less than or equal to 50% and greater than 0. By rationally controlling the content of the second lithium nickel cobalt manganese oxide in the positive electrode active material so that 0 < X2 ≤ 50%, the positive electrode active material is not only more stable, but also the voids formed by the lattice contraction of the second lithium nickel cobalt manganese oxide during charging facilitate the storage of electrolyte squeezed out by the expansion of the negative electrode active material, which is beneficial to the electrolyte backflow during discharge, improves lithium precipitation, and improves the cycle performance of the battery cell.

[0013] In any embodiment, the mass fraction of silicon in the negative electrode active material is less than or equal to 10% and greater than 0. By rationally controlling the silicon content in the negative electrode active material so that 0 < X1 ≤ 10%, the energy density of the battery cell can be improved while ensuring the stability of the negative electrode active material, thereby improving the cycle performance of the battery cell.

[0014] In any embodiment, in the first lithium nickel cobalt manganese oxide, the molar content of nickel in the total transition metal elements is less than or equal to 0.75 and greater than or equal to 0.5. By controlling the molar content of nickel in the first lithium nickel cobalt manganese oxide in the total transition metal elements, the stability of the positive electrode active material is improved and the cycle performance of the battery cell is improved.

[0015] In any embodiment, the first lithium nickel cobalt manganese oxide comprises a first lithium nickel cobalt manganese oxide or a doping modified material of the first lithium nickel cobalt manganese oxide or a surface modified material of the first lithium nickel cobalt manganese oxide, and the structural formula of the first lithium nickel cobalt manganese oxide is LiNi x Co y Mn z O2, wherein x+y+z=1, 0.5≤x≤0.75, 0.03≤y≤0.3, 0.2≤z≤0.4. The doping modification material of the first lithium nickel cobalt manganese oxide may be a modification material in which a trace amount of titanium, zirconium, aluminum, magnesium and lanthanum is doped into the first lithium nickel cobalt manganese oxide. The surface modification material may be any one or more modification materials such as MgO, ZrO2, TiO2, Al2O3, AlPO4, AlF3, LiAlO2 and LiTiO2 coated on the surface of the first lithium nickel cobalt manganese oxide. The technical solution of the present application is not limited to the surface modification material. It should be noted that in the later stage of formation or cycling of the battery cell in the embodiment of the present application, the atomic number ratio of the Li element in the atomic number ratio of the constituent elements of the first lithium nickel cobalt manganese oxide may be greater than 1, or less than 1 and greater than 0; the atomic number ratio of the O element may be greater than 2, or less than 2 and greater than 0.

[0016] In any embodiment, the second lithium nickel cobalt manganese oxide comprises a second lithium nickel cobalt manganese oxide or a doping modified material of the second lithium nickel cobalt manganese oxide or a surface modified material of the second lithium nickel cobalt manganese oxide, and the structural formula of the second lithium nickel cobalt manganese oxide is LiNi a Co b Mn cO2, wherein a+b+c=1, 0.8≤a≤0.98, 0.01≤b≤0.15, 0.01≤c≤0.15. The doping modification material of the second type of lithium nickel cobalt manganese oxide can be a modification material in which a trace amount of titanium, zirconium, aluminum, magnesium and lanthanum is doped into the second type of lithium nickel cobalt manganese oxide. The surface modification material can be any one or more modification materials such as MgO, ZrO2, TiO2, Al2O3, AlPO4, AlF3, LiAlO2 and LiTiO2 coated on the surface of the first type of lithium nickel cobalt manganese oxide. The technical solution of this application is not limited to the surface modification material. It should be noted that in the later stage of formation or cycling of the battery cell in the embodiment of this application, the atomic number ratio of the Li element in the atomic number ratio of the constituent elements of the first type of lithium nickel cobalt manganese oxide can be greater than 1, or less than 1 and greater than 0; the atomic number ratio of the O element can be greater than 2, or less than 2 and greater than 0.

[0017] In any embodiment, the volume average particle size Dv50 of the secondary particles of the first lithium nickel cobalt manganese oxide is 3 microns to 5 microns. By controlling the volume average particle size Dv50 of the first lithium nickel cobalt manganese oxide to be 3 microns to 5 microns, the specific surface area of ​​the first lithium nickel cobalt manganese oxide is within a preferred range, and the first lithium nickel cobalt manganese oxide has fewer side reactions when used as a positive electrode active material, thereby improving the cycle performance retention rate of the battery cell.

[0018] In any embodiment, the volume average particle size Dv50 of the secondary particles of the second lithium nickel cobalt manganese oxide is 8 microns to 12 microns. By controlling the volume average particle size Dv50 of the second lithium nickel cobalt manganese oxide to be 8 microns to 12 microns, the specific surface area of ​​the second lithium nickel cobalt manganese oxide is within a preferred range, resulting in larger sites for lithium insertion and removal when the second lithium nickel cobalt manganese oxide is used as a positive electrode active material, thereby ensuring better power performance of the battery cell.

[0019] In any embodiment, the volume average particle size Dv50 of the primary particles of the first lithium nickel cobalt manganese oxide is in the range of 1 μm to 3 μm.

[0020] In any embodiment, the volume average particle size Dv50 of the primary particles of the second lithium nickel cobalt manganese oxide is in the range of 100 nm to 500 nm.

[0021] In any embodiment, the compacted density of the positive electrode sheet is 2.8-3.7 g / cm 3 The compaction density of the positive electrode sheet is relatively high, which increases the energy density of the positive electrode sheet.

[0022] In any embodiment, the silicon-based material includes any one or more of silicon, a silicon-carbon composite material, silicon monoxide, and a silicon monoxide-carbon composite material.

[0023] In any embodiment, the carbon-based material comprises graphite.

[0024] The second aspect of the present application further provides a battery, comprising the battery cell of the first aspect of the present application. Since the battery of the present application comprises the battery cell provided by the present application, it has at least the same advantages as the battery cell.

[0025] The third aspect of the present application further provides an electrical device comprising the battery cell of the first aspect of the present application and / or the battery of the second aspect of the present application. Since the electrical device of the present application comprises the battery cell and / or the battery provided herein, it has at least the same advantages as the battery cell.

[0026] The beneficial effects of the present application are: different from the prior art, the battery cell of the present application, by including a second lithium nickel cobalt manganese oxide with a higher nickel content in the positive electrode active material, the second lithium nickel cobalt manganese oxide lattice shrinks significantly during the charging process. This can improve the situation where the electrolyte is squeezed out due to the expansion of the silicon-based material during the charging process. The gaps formed by the contraction of the second lithium nickel cobalt manganese oxide lattice are used to store the squeezed electrolyte, which is conducive to the electrolyte reflux to the negative electrode during the discharge process, thereby improving the occurrence of lithium precipitation due to untimely electrolyte reflux during the next charge, and can improve the cycle performance of the battery cell.

[0027] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] FIG1 is a schematic structural diagram of a battery cell according to an embodiment of the present application.

[0029] FIG2 is a schematic diagram of the exploded structure of a battery according to an embodiment of the present application.

[0030] FIG3 a is a schematic diagram of a partial structure of an electrical device according to an embodiment of the present application.

[0031] FIG3 b is a schematic diagram of an electrical device according to an embodiment of the present application.

[0032] FIG4 a is a scanning electron microscope image of the first lithium nickel cobalt manganese oxide of Example 1 of the present application.

[0033] FIG4 b is another scanning electron microscope image of the first lithium nickel cobalt manganese oxide of Example 1 of the present application.

[0034] FIG5 a is a scanning electron microscope image of the second lithium nickel cobalt manganese oxide of Example 1 of the present application.

[0035] FIG5 b is another scanning electron microscope image of the second lithium nickel cobalt manganese oxide of Example 1 of the present application. DETAILED DESCRIPTION

[0036] Below, the embodiments of the battery cells, batteries, and electrical equipment of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0037] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0038] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0039] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0040] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, a method includes steps (a) and (b), which indicates that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, a method may further include step (c), which indicates that step (c) may be added to the method in any order, for example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.

[0041] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may indicate that other components not listed may also be included or that only the listed components are included.

[0042] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0043] Silicon, as the negative electrode active material, undergoes significant volume changes during charge and discharge, with a volume expansion rate reaching 300%, leading to problems with particle pulverization and electrode expansion. This is especially true when used with low-nickel ternary materials (where the nickel content of all transition metal elements is less than 0.8%) as the positive electrode active material. This causes significant electrolyte extrusion, preventing the electrolyte from flowing back during discharge, leading to lithium deposition, a sharp decrease in battery capacity, and poor cycle performance.

[0044] Based on this, the present application proposes a battery cell, including a positive electrode sheet and a negative electrode sheet, the positive electrode sheet including a positive electrode active material, the positive electrode active material including a first lithium nickel cobalt manganese oxide (NCM1) and a second lithium nickel cobalt manganese oxide (NCM2), the molar content of nickel in the second lithium nickel cobalt manganese oxide in all transition metal elements is greater than the molar content of nickel in the first lithium nickel cobalt manganese oxide in all transition metal elements. In the second lithium nickel cobalt manganese oxide, the molar content of nickel in all transition metal elements is greater than or equal to 0.8. The negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes a silicon-based material and a carbon-based material.

[0045] In the embodiment of the present application, the positive electrode active material of the battery cell contains a second lithium nickel cobalt manganese oxide with a higher nickel content. During the charging process, the crystal lattice of the second lithium nickel cobalt manganese oxide shrinks significantly, which can improve the situation where the electrolyte is squeezed out due to the expansion of the silicon-based material during the charging process. The gaps formed by the contraction of the crystal lattice of the second lithium nickel cobalt manganese oxide are used to store the squeezed electrolyte. During the discharge process, the expansion of the crystal lattice of the second lithium nickel cobalt manganese oxide is conducive to the reflux of the electrolyte to the negative electrode sheet, thereby improving the occurrence of lithium precipitation due to untimely electrolyte reflux during the next charge, and improving the cycle performance of the battery cell.

[0046] In the embodiment of the present application, the molar content of nickel in the total transition metal elements in the first lithium nickel cobalt manganese oxide (NCM1) is less than 0.8 and greater than 0. In the embodiment of the present application, the first lithium nickel cobalt manganese oxide can be an oxide including lithium nickel cobalt manganese. The second lithium nickel cobalt manganese oxide can also be an oxide including lithium nickel cobalt manganese.

[0047] In an embodiment of the present application, the positive electrode active material of the battery cell contains a second lithium nickel cobalt manganese oxide with a higher nickel content, and a first lithium nickel cobalt manganese oxide with a lower nickel content. Among them, the first lithium nickel cobalt manganese oxide has a lower activity and a higher stability during the charge and discharge process. During the charge and discharge process, as the reaction proceeds, the stability of the second lithium nickel cobalt manganese oxide decreases. The positive electrode active material contains the first nickel cobalt manganese oxide with low nickel content and the second nickel cobalt manganese oxide with high nickel content, so that the overall activity of the positive electrode active material is mild and the stability is high. At the same time, the lattice of the second nickel cobalt manganese oxide shrinks during the charging process, forming gaps to store the electrolyte squeezed out by the expansion of silicon.

[0048] In embodiments of the present application, the negative electrode active material includes a silicon-based material and a carbon-based material. The carbon-based material exhibits stable performance, while the silicon-based material is susceptible to expansion during charge and discharge. The combination of the silicon-based and carbon-based materials improves the overall stability of the negative electrode active material. Furthermore, the silicon-based material has a higher theoretical capacity of up to 4200 mAh / g. Compared to pure graphite as the negative electrode active material, the addition of the silicon-based material can increase the theoretical capacity of the negative electrode active material.

[0049] For ease of description, the mass fraction of silicon is represented by X1 based on the total mass of the negative electrode active material. The total mass of the negative electrode active material is the sum of the masses of the silicon-based material and the carbon-based material. The mass fraction of the second lithium nickel cobalt manganese oxide is represented by X2 based on the total mass of the positive electrode active material. The total mass of the positive electrode active material is the sum of the mass of the first lithium nickel cobalt manganese oxide and the mass of the second lithium nickel cobalt manganese oxide. The ratio of the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material to the mass fraction of silicon in the negative electrode active material is represented by Y, that is, Y = X2 / X1.

[0050] In some embodiments of the present application, the mass fraction X2 of the second lithium nickel cobalt manganese oxide in the positive electrode active material is related to the mass fraction X1 of the silicon-based material in the negative electrode active material. The higher the silicon content in the negative electrode active material, the higher the content of the second lithium nickel cobalt manganese oxide in the positive electrode active material.

[0051] In some embodiments of the present application, 0<Y≤10. When 0<Y≤10, the cycle performance of the battery cell is better. During the charging process, the gaps formed by the lattice contraction of the second lithium nickel cobalt manganese oxide can better store the electrolyte squeezed out by the expansion of the silicon-based material. During the discharge process, the lattice expansion of the second lithium nickel cobalt manganese oxide is conducive to the reflux of the electrolyte; and the stability of the positive electrode active material and the negative electrode active material is relatively high, so that the cycle performance of the battery cell is better. Among them, the value of Y can be 0.1, 1, 1.5, 2, 2.4, 3, 3.2, 4, 4.8, 5, 5.1, 5.7, 6, 6.5, 7, 7.7, 8, 8.5, 9, 9.3, 10, etc., or a range consisting of any two of the above values, for example, 1.5-3.2, 2-8, 7-9.3, etc.

[0052] In some embodiments of the present application, when 4≤Y≤6, the cycle performance of the battery cell is better.

[0053] In some embodiments of the present application, 0<X2≤50%. For example, X2 can be 0.001%, 0.1%, 1%, 5%, 6.3%, 8%, 10%, 15%, 18.5%, 20%, 25%, 30%, 33.2%, 35%, 38%, 40%, 42%, 44.5%, 45%, 47%, 50%, etc., or a range consisting of any two of the above values, for example, 0.001%-5%, 6.3%-15%, 15%-20%, 25%-35%, 38%-42%, 45%-50%, etc.

[0054] By reasonably controlling the content of the second lithium nickel cobalt manganese oxide in the positive electrode active material so that 0<X2≤50%, the positive electrode active material is more stable on the one hand, and on the other hand, the gaps formed by the lattice contraction of the second lithium nickel cobalt manganese oxide during the charging process are convenient for storing the electrolyte squeezed out by the expansion of the negative electrode active material. During the discharge process, the lattice expansion of the second lithium nickel cobalt manganese oxide is conducive to the reflux of the electrolyte, improving the lithium precipitation situation, and making the cycle performance of the battery cell better.

[0055] In some embodiments of the present application, 0<X1≤10%. By reasonably controlling the content of silicon in the negative electrode active material so that 0<X1≤10%, the energy density of the battery cell can be improved, the stability of the negative electrode active material can be ensured, and the cycle performance of the battery cell can be better. For example, X1 can be 0.001%, 0.1%, 1%, 2%, 2.3%, 3%, 3.6%, 4%, 4.7%, 5%, 5.5%, 6%, 6.5%, 7%, 7.4%, 8%, 8.3%, 8.8%, 9%, 9.2%, 9.4%, 10%, etc., or a range consisting of any two of the above values, for example, 0.001%-5%, 65.5%-10%, 2%-10%, 2%-8%, etc.

[0056] In some embodiments of the present application, in the first lithium nickel cobalt manganese oxide, the molar content of nickel in all transition metal elements is less than or equal to 0.75 and greater than or equal to 0.5. By controlling the molar content of nickel in all transition metal elements in the first lithium nickel cobalt manganese oxide, the stability of the positive electrode active material is improved, which is beneficial to improving the cycle performance of the battery cell. For example, the molar content of nickel in all transition metal elements can be 0.50, 0.51, 0.55, 0.6, 0.62, 0.65, 0.68, 0.7, 0.72, 0.75, etc., or a range consisting of any two of the above values, for example, 0.51-0.65, 0.68-0.75, etc.

[0057] In some embodiments of the present application, the first lithium nickel cobalt manganese oxide includes a first lithium nickel cobalt manganese oxide or a doping modified material of the first lithium nickel cobalt manganese oxide or a surface modified material of the first lithium nickel cobalt manganese oxide, and the structural formula of the first lithium nickel cobalt manganese oxide is LiNi x Co y Mn zO2, wherein x+y+z=1, 0.5≤x≤0.75, 0.03≤y≤0.3, 0.2≤z≤0.4. The doping modification material of the first lithium nickel cobalt manganese oxide may be a first lithium nickel cobalt manganese oxide doped with a trace amount of metal elements, for example, it may be a modified material doped with any one or more of titanium, zirconium, aluminum, magnesium and lanthanum elements, wherein the molar content of the doped metal element is less than or equal to 0.01. The surface modification material may be a modified material in which the surface of the first lithium nickel cobalt manganese oxide is coated with other substances. In the embodiment of the present application, the first lithium nickel cobalt manganese oxide has a small lattice change during the charge and discharge process and has strong stability. The first lithium nickel cobalt manganese oxide includes but is not limited to LiNi 0.6 Co 0.2 Mn 0.2 O2 (also abbreviated as N6C2M2), LiNi 0.5 Co 0.2 Mn 0.3 O2 (can also be abbreviated as N5C2M3), LiNi 0.7 Co 0.1 Mn 0.2 O2 (also abbreviated as N7C1M2) and LiNi 0.75 Co 0.05 Mn 0.2 O2 (also abbreviated as N 7.5 C 0.5 M 2.5 ) at least one of .

[0058] In some embodiments of the present application, the second lithium nickel cobalt manganese oxide includes a second lithium nickel cobalt manganese oxide or a doping modified material of the second lithium nickel cobalt manganese oxide or a surface modified material of the second lithium nickel cobalt manganese oxide, and the structural formula of the second lithium nickel cobalt manganese oxide is LiNi a Co b Mn c O2, wherein a+b+c=1, 0.8≤a≤0.98, 0.01≤b≤0.15, 0.01≤c≤0.15. The doping modification material of the second type of lithium nickel cobalt manganese oxide can be a modification material in which a trace amount of any one or more of titanium, zirconium, aluminum, magnesium and lanthanum elements are doped in the second type of lithium nickel cobalt manganese oxide, and the molar content of nickel element in all transition metal elements is less than or equal to 0.01. The surface modification material can be a modification material in which the surface of the second type of lithium nickel cobalt manganese oxide is coated with other substances. In the embodiment of the present application, the crystal form of the second type of lithium nickel cobalt manganese oxide is a hexagonal layered rock salt structure. During the charging process, the Li in the layered rock salt structure of the second type of lithium nickel cobalt manganese oxide + During the discharge process, the second type of lithium nickel cobalt manganese oxide is inserted into the layered rock salt structure of lithium nickel cobalt manganese oxide. +, so that the lattice returns to its initial state or nearly to its initial state, and the gaps formed by the second type of lithium nickel cobalt manganese oxide are reduced, which helps the electrolyte to reflux.

[0059] In some embodiments of the present application, the second lithium nickel cobalt manganese oxide may include but is not limited to LiNi 0.8 Co 0.1 Mn 0.1 O2 (can also be abbreviated as N8C1M1), LiNi 0.85 Co 0.1 Mn 0.05 O2 (also abbreviated as N 8.5 C1M 0.5 ), LiNi 0.9 Co 0.05 Mn 0.05 O2 (also abbreviated as N9C 0.5 M 0.5 ), LiNi 0.97 Co 0.02 Mn 0.01 O2 (also abbreviated as N 9.7 C 0.2 M 0.1 ), LiNi 0.98 Co 0.01 Mn 0.01 O2 (also abbreviated as N 9.8 C 0.1 M 0.1 ) and LiNi 0.98 Co 0.01 Mn 0.01 O2 (also abbreviated as N 9.8 C 0.1 M 0.1 ) at least one of .

[0060] In some embodiments of the present application, the volume average particle size Dv50 of the secondary particles of the first lithium nickel cobalt manganese oxide is 3 microns to 5 microns. By controlling the volume average particle size Dv50 of the first lithium nickel cobalt manganese oxide to be 3 microns to 5 microns, the specific surface area of ​​the first lithium nickel cobalt manganese oxide is within a preferred range, resulting in fewer side reactions when the first lithium nickel cobalt manganese oxide is used as a positive electrode active material, and a higher cycle performance retention rate of the battery cell. The volume average particle size Dv50 of the first lithium nickel cobalt manganese oxide can be 3 microns, 3.3 microns, 3.5 microns, 4 microns, 4.6 microns, or 5 microns, or a range consisting of any two of the above values, for example, 3.3 microns to 4.6 microns, 3.5 microns to 4 microns, etc.

[0061] In some embodiments of the present application, the volume average particle size Dv50 is common knowledge in the art, has a meaning commonly known in the art, and can be measured by methods and instruments in the art.

[0062] In some embodiments of the present application, the volume average particle size Dv50 of the secondary particles of the second lithium nickel cobalt manganese oxide is 8 microns to 12 microns. By controlling the volume average particle size Dv50 of the second lithium nickel cobalt manganese oxide to be 8 microns to 12 microns, the specific surface area of ​​the second lithium nickel cobalt manganese oxide is within a preferred range, so that the second lithium nickel cobalt manganese oxide has larger sites for lithium insertion and removal when used as a positive electrode active material, thereby ensuring better power performance of the battery cell. Among them, the volume average particle size Dv50 of the second lithium nickel cobalt manganese oxide can be 8 microns, 8.5 microns, 9 microns, 9.7 microns, 10 microns, 10.6 microns, 11 microns, 11.4 microns or 12 microns, or a range consisting of any two of the above values, for example, 8.5 microns to 10.6 microns, 9 microns to 11.4 microns, etc.

[0063] In some embodiments of the present application, the volume average particle size Dv50 of the primary particles of the first lithium nickel cobalt manganese oxide is in the range of 1 μm to 3 μm. The volume average particle size Dv50 of the primary particles of the first lithium nickel cobalt manganese oxide can be 1 μm, 1.5 μm, 2 μm, 2.2 μm, 2.5 μm, or 3 μm, or a range consisting of any two of the foregoing values, for example, 1.5 μm to 2.5 μm, 2 μm to 3 μm, etc.

[0064] In some embodiments of the present application, the volume average particle size Dv50 of the primary particles of the second lithium nickel cobalt manganese oxide ranges from 100 nm to 500 nm. In the embodiments of the present application, the volume average particle size Dv50 of the primary particles of the second lithium nickel cobalt manganese oxide is relatively small, so that the secondary particles of the formed second lithium nickel cobalt manganese oxide have a larger specific surface area. The volume average particle size Dv50 of the primary particles of the second lithium nickel cobalt manganese oxide can be 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 360 nm, 400 nm, 440 nm or 500 nm, or a range consisting of any two of the above values, for example, 150 nm to 300 nm, 360 nm to 500 nm, etc.

[0065] In some embodiments of the present application, the compaction density of the positive electrode sheet is 2.8 g / cm 3 -3.7g / cm 3 The compaction density of the positive electrode sheet is relatively large, which is beneficial to increasing the energy density of the positive electrode sheet. In the embodiment of the present application, the particle size of the secondary particles of the first lithium nickel cobalt manganese oxide and the second lithium nickel cobalt manganese oxide are different, which is beneficial to increasing the compaction density of the positive electrode sheet. The compaction density of the positive electrode sheet can be 2.8g / cm3 , 3.0g / cm 3 、3.1g / cm 3 、3.2g / cm 3 , 3.3g / cm 3 , 3.5g / cm 3 、3.6g / cm 3 or 3.7g / cm 3 etc., or a range consisting of any two of the above values, for example, 3.0 g / cm 3 -3.7g / cm 3 , 2.8g / cm 3 -3.3g / cm 3 wait.

[0066] In some embodiments of the present application, the compacted density is common knowledge in the art, has a meaning commonly known in the art, and can be measured by methods and instruments in the art.

[0067] In some embodiments of the present application, the silicon-based material includes any one or more of silicon, a silicon-carbon composite, silicon monoxide, or a silicon monoxide-carbon composite. In the embodiments of the present application, the silicon-based material may be pure silicon or pure silicon monoxide. The silicon-based material may also be a silicon-carbon composite, such as a silicon-carbon surface coated with a carbon layer; or a silicon monoxide-carbon composite, such as a silicon monoxide surface coated with a carbon layer. In other embodiments, the silicon-based material also includes a silicon-nitrogen complex and / or a silicon alloy.

[0068] In some embodiments of the present application, the carbon-based material includes graphite. In the embodiments of the present application, the graphite can be natural graphite or artificial graphite; the carbon-based material can also include soft carbon or hard carbon.

[0069] In addition, the battery cell, battery, and electric device of the present application will be described below with reference to the drawings as appropriate.

[0070] In the embodiment of the present application, a battery cell refers to the smallest unit that makes up a battery. A battery cell also includes an electrolyte and a separator. The separator is provided between the positive electrode and the negative electrode. It mainly prevents the positive and negative electrodes from short-circuiting while allowing ions to pass through. During the charge and discharge process of the battery, the active ions Li + The electrolyte is inserted and removed back and forth between the positive electrode and the negative electrode, and acts as a conductor of ions between the positive electrode and the negative electrode.

[0071] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, and the positive electrode film layer includes the positive electrode active material of the above embodiment of the present application.

[0072] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0073] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0074] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.

[0075] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0076] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0077] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes the negative electrode active material of the above embodiment.

[0078] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0079] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0080] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0081] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0082] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0083] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0084] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. This application has no specific restrictions on the type of electrolyte, and it can be selected according to needs.

[0085] In some embodiments, the electrolyte solution includes an electrolyte salt and a solvent.

[0086] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0087] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0088] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.

[0089] In some embodiments, the battery cell further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0090] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0091] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be made into a battery cell assembly through a winding process or a lamination process.

[0092] In some embodiments, as shown in FIG1 , a battery cell 10 may include an outer packaging. The outer packaging may be used to encapsulate the battery cell assembly 11 and the electrolyte. The outer packaging includes an end cap 12 , a housing 13 , and other functional components.

[0093] The end cap 12 refers to a component that covers the opening of the shell 13 to isolate the internal environment of the battery cell 10 from the external environment. Without limitation, the shape of the end cap 12 can be adapted to the shape of the shell 13 to match the shell 13. Optionally, the end cap 12 can be made of a material with a certain hardness and strength (such as an aluminum alloy). In this way, the end cap 12 is not easily deformed when squeezed or collided, so that the battery cell 10 can have a higher structural strength and improved safety performance. Functional components such as electrode terminals 12a can be provided on the end cap 12. The electrode terminals 12a can be used to electrically connect to the battery cell assembly 11 for outputting or inputting electrical energy into or out of the battery cell 10. In some embodiments, the end cap 12 can also be provided with a pressure relief mechanism for releasing internal pressure when the internal pressure or temperature of the battery cell 10 reaches a threshold. The material of the end cap 12 can also be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose any special restrictions on this. In some embodiments, an insulating member (not shown) may be provided inside the end cap 12 to isolate the electrical connection components in the housing 13 from the end cap 12 to reduce the risk of short circuits. For example, the insulating member may be made of plastic, rubber, or the like.

[0094] The housing 13 is a component that cooperates with the end cap 12 to form the internal environment of the battery cell 10. This internal environment can be used to accommodate the battery cell assembly 11, electrolyte, and other components. The housing 13 and the end cap 12 can be separate components. An opening can be provided in the housing 13, and the end cap 12 is placed over the opening to form the internal environment of the battery cell 10. Alternatively, the end cap 12 and the housing 13 can be integrated. Specifically, the end cap 12 and the housing 13 can form a common connection surface before other components are inserted into the housing. When the interior of the housing 13 needs to be enclosed, the end cap 12 is placed over the housing 13. The housing 13 can have a variety of shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the housing 13 can be determined based on the specific shape and size of the battery cell assembly 11. The housing 13 can be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and this embodiment of the present application does not impose any specific limitations on this.

[0095] The housing 13 may contain one or more battery cell assemblies 11. The portions of the positive and negative electrode sheets that do not contain active material each form a tab 11a. The positive and negative tabs may be located together at one end of the main body or separately at opposite ends. During the battery's charge and discharge processes, the positive and negative active materials react with the electrolyte, and the tabs 11a connect to the electrode terminals to form a current circuit.

[0096] Please refer to Figure 2, which is a schematic diagram of the exploded structure of a battery 100 provided in some embodiments of the present application. The battery 100 includes a housing 20 and a battery cell 10, with the battery cell 10 housed within the housing 20. The housing 20 provides a storage space for the battery cell 10 and can have various structures. In some embodiments, the housing 20 can include a first portion 21 and a second portion 22, which overlap each other and together define a storage space for the battery cell 10. The second portion 22 can be a hollow structure with one end open. The first portion 21 can be a plate-like structure, with the first portion 21 overlapping the open side of the second portion 22, so that the first and second portions 21 and 22 together define a storage space. Alternatively, the first and second portions 21 and 22 can each be a hollow structure with one end open, with the open side of the first portion 21 overlapping the open side of the second portion 22. Of course, the housing 20 formed by the first and second portions 21 and 22 can have various shapes, such as a cylinder or a rectangular parallelepiped.

[0097] In the battery 100, there may be multiple battery cells 10, and the multiple battery cells 10 may be connected in series, in parallel, or in a hybrid connection. A hybrid connection refers to a combination of series and parallel connections among the multiple battery cells 10. The multiple battery cells 10 may be directly connected in series, in parallel, or in a hybrid connection, and then the entire battery cell 10 may be housed within the housing 20. Of course, the battery 100 may also be formed by first connecting multiple battery cells 10 in series, in parallel, or in a hybrid connection to form a battery module, and then the multiple battery modules may be connected in series, in parallel, or in a hybrid connection to form an entire battery cell, and then housed within the housing 20. The battery 100 may also include other structures, for example, the battery 100 may further include a busbar component for electrically connecting the multiple battery cells 10.

[0098] The battery 100 in the embodiment of the present application includes a lithium-ion battery as a battery cell 10. In other embodiments, the battery 100 may further include any one or more of a lithium-sulfur battery, a sodium-ion battery, and a magnesium-ion battery, but is not limited thereto. The battery cell 10 may be cylindrical, flat, rectangular, or in other shapes.

[0099] In some embodiments, batteries may be assembled into a battery module. The number of batteries contained in the battery module may be one or more. The specific number may be selected by those skilled in the art based on the application and capacity of the battery module.

[0100] In addition, the present application also provides an electric device, which includes at least one of the battery cells and / or batteries provided in the present application. The battery cells or battery packs can be used as power sources for electric devices, or as energy storage units for electric devices. Electric devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0101] As an electrical device, a battery cell and / or battery can be selected according to its usage requirements.

[0102] Figures 3a and 3b show an electric device as an example. The electric device is a vehicle such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. A structural schematic diagram of a vehicle 1000 is specifically provided. A battery 100 is provided inside the vehicle 1000, and the battery 100 can be provided at the bottom, head, or tail of the vehicle 1000. The battery 100 can be used to power the vehicle 1000, for example, the battery 100 can serve as an operating power source for the vehicle 1000. The vehicle 1000 may also include a controller 200 and a motor 300, and the controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating, and operating power requirements of the vehicle 1000 during driving.

[0103] In some embodiments of the present application, the battery 100 can serve not only as an operating power source for the vehicle 1000, but also as a driving power source for the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.

[0104] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.

[0105] Example 1

[0106] Preparation method of positive electrode sheet:

[0107] The first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1O2, abbreviated as N8C1M1), conductive carbon black (Super-P), and polyvinylidene fluoride (PVDF) in a weight ratio of 90:10:3:1.5 were mixed with N,N-dimethylpyrrolidone (NMP) and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry was evenly coated on both sides of aluminum foil. The electrode was cold pressed and sliced ​​to produce the positive electrode sheet.

[0108] Among them, the first type of lithium nickel cobalt manganese oxide and the second type of lithium nickel cobalt manganese oxide are used as positive electrode active materials, conductive carbon black (Super-P) is used as a conductive agent, polyvinylidene fluoride (PVDF) is used as a binder, and N,N-dimethylpyrrolidone (NMP) is used as a slurry solvent.

[0109] Among them, as shown in Figures 4a and 4b, the volume average particle size Dv50 of the secondary particles of the first type of lithium nickel cobalt manganese oxide is 3.6 μm, and the volume average particle size Dv50 of the primary particles of the first type of lithium nickel cobalt manganese oxide is 1.5 μm. As shown in Figures 5a and 5b, the volume average particle size Dv50 of the secondary particles of the second type of lithium nickel cobalt manganese oxide is 10.5 μm, and the volume average particle size Dv50 of the primary particles of the second type of lithium nickel cobalt manganese oxide is 300 μm. In the embodiment of the present application, the morphology of the secondary particles of the first type of lithium nickel cobalt manganese oxide is particles with edges and corners. The morphology of the secondary particles of the second type of lithium nickel cobalt manganese oxide is a spherical structure with a smooth surface. In the embodiment of the present application, the compaction density of the positive electrode sheet is 3.5 g / cm 3 In other embodiments, the compaction density of the positive electrode sheet can also be 2.8g / cm 3 -3.7g / cm 3 other values.

[0110] In the embodiment of the present application, in the first type of lithium nickel cobalt manganese oxide, the molar content of nickel in all transition metal elements is 0.6. In the second type of lithium nickel cobalt manganese oxide, the molar content of nickel in all transition metal elements is 0.8. Among them, the content of nickel in the first type of lithium nickel cobalt manganese oxide and the second type of lithium nickel cobalt manganese oxide are both known amounts. By performing scanning electron microscopy on the positive electrode sheet and taking advantage of the different morphologies of the first type of lithium nickel cobalt manganese oxide and the second type of lithium nickel cobalt manganese oxide: energy spectrum analysis (EDS) is performed on the secondary particles with angular surfaces, the molar content of nickel in the secondary particles in all transition metal elements can be obtained; energy spectrum analysis (EDS) is performed on the secondary particles with a spherical structure with a smooth surface, and the molar content of nickel in the secondary particles in all transition metal elements can be obtained. Of course, the embodiment of the present application is not limited to a specific testing method, and the molar content of nickel in all transition metal elements of the first type of lithium nickel cobalt manganese oxide and the second type of lithium nickel cobalt manganese oxide in the positive electrode active material can also be obtained by other methods.

[0111] Preparation method of negative electrode sheet:

[0112] In the embodiments of the present application, a negative electrode active material, a conductive agent, a thickener, and a binder are mixed with deionized water to form a slurry for the negative electrode sheet. Specifically, in the embodiments of the present application, the negative electrode active material includes a silicon-based material and a carbon-based material. The carbon-based material is artificial graphite, and the silicon-based material is nano-silicon. The conductive agent is conductive carbon black (Super-P) and carbon nanotubes. The thickener is sodium carboxymethyl cellulose (CMC-Na). The binder is styrene-butadiene rubber (SBR).

[0113] Specifically, in the embodiment of the present application, artificial graphite, nano-silicon, conductive carbon black (Super-P), carbon nanotubes, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) are mixed with deionized water in a weight ratio of 95:5:0.5:0.1:1:1.5 and stirred evenly to obtain a slurry for coating the negative electrode sheet. The viscosity can be adjusted by adding deionized water during the stirring process. Then, the slurry is coated on both sides of the negative electrode current collector with a certain width, and the negative electrode sheet is obtained by cold pressing and slicing. In the embodiment of the present application, the negative electrode current collector is a 6μm thick copper foil. The embodiment of the present application does not limit the material and thickness of the negative electrode current collector.

[0114] Preparation method of battery monomer:

[0115] The positive electrode sheet, the separator and the negative electrode sheet are wound into a battery cell assembly, and the battery cell is produced through the steps of tab welding, aluminum shell packaging, liquid injection, packaging formation and vacuum molding. The width of the battery cell assembly is 148mm, the thickness is 28mm, the height is 98mm, and the capacity is 60Ah. Among them, the injected electrolyte is a 1mol / L LiPF6 solution, the solvent of the LiPF6 solution is ethylene carbonate (EC) and dimethyl carbonate (DMC), and the volume ratio of ethylene carbonate (EC) and dimethyl carbonate (DMC) is 1:2. In the embodiment of the present application, the separator adopts 7μm thick polyethylene (PE). In the embodiment of the present application, the energy density of the negative electrode active material of the negative electrode sheet is 1.07 times the energy density of the positive electrode active material of the positive electrode sheet.

[0116] The battery cell obtained in the embodiment of the present application includes a positive electrode sheet and a negative electrode sheet, the positive electrode sheet includes a positive electrode active material, and the positive electrode active material includes a first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2 and the second lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 O2). The negative electrode sheet includes a negative electrode active material, which includes a silicon-based material and a carbon-based material. The first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2The molar content of nickel in all transition metal elements is 0.6. 0.8 Co 0.1 Mn 0.1 The molar content of nickel in all transition metal elements is 0.8.

[0117] Example 2

[0118] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 The weight ratio of the conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 80:20:3:1.5. Other details are the same as those in Example 1 and will not be repeated here.

[0119] Example 3

[0120] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 The weight ratio of the conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 75:25:3:1.5. Other details are the same as those in Example 1 and will not be repeated here.

[0121] Example 4

[0122] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1The weight ratio of the conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 70:30:3:1.5. Other details are the same as those in Example 1 and will not be repeated here.

[0123] Example 5

[0124] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 The weight ratio of the conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 60:40:3:1.5. Other details are the same as those in Example 1 and will not be repeated here.

[0125] Example 6

[0126] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 The weight ratio of the conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 50:50:3:1.5. Other details are the same as those in Example 1 and will not be repeated here.

[0127] Example 7

[0128] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1The weight ratio of the negative electrode sheet is 70:30:3:1.5. The weight ratio of artificial graphite, nano-silicon, conductive carbon black (Super-P), carbon nanotubes, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) is 90:10:0.5:0.1:1:1.5. Other details are the same as in Example 1 and are not repeated here.

[0129] Example 8

[0130] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 The weight ratio of the negative electrode sheet is 60:40:3:1.5. The weight ratio of artificial graphite, nano-silicon, conductive carbon black (Super-P), carbon nanotubes, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) is 90:10:0.5:0.1:1:1.5. Other details are the same as in Example 1 and are not repeated here.

[0131] Example 9

[0132] The battery cell and the preparation method of the battery cell of the embodiment of the present application are different from those of the embodiment 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 O2, abbreviated as N8C1M1), conductive carbon black (Super-P), and polyvinylidene fluoride (PVDF) are prepared in a weight ratio of 50:50:3:1.5. In the negative electrode preparation method, the weight ratio of artificial graphite, nano-silicon, conductive carbon black (Super-P), carbon nanotubes, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) is 90:10:0.5:0.1:1:1.5. All other components are the same as in Example 1 and are not further described here.

[0133] Example 10

[0134] The difference between the battery cell and the preparation method of the battery cell in the embodiment of the present application and that in the preparation method of the positive electrode sheet is that the first lithium nickel cobalt manganese oxide has the structural formula LiNi 0.5 Co 0.2 Mn 0.3 O2, abbreviated as N5C2M3. The second type of lithium nickel cobalt manganese oxide has the structural formula LiNi 0.85 Co 0.1 Mn 0.05 O2, abbreviated as N 8.5 C1M 0.5 The weight ratio of the first type of lithium nickel cobalt manganese oxide, the second type of lithium nickel cobalt manganese oxide, conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 75:25:3:1.5. 0.5 Co 0.2 Mn 0.3 O2), the molar content of nickel in all transition metal elements is 0.5. The second type of lithium nickel cobalt manganese oxide (LiNi 0.85 Co 0.1 Mn 0.05 O2), the molar content of nickel in all transition metal elements is 0.85. Other details are the same as those in Example 1 and will not be repeated here.

[0135] Example 11

[0136] The difference between the battery cell and the preparation method of the battery cell in the embodiment of the present application and that in the preparation method of the positive electrode sheet is that the first lithium nickel cobalt manganese oxide has the structural formula LiNi 0.7 Co 0.1 Mn 0.2 O2, abbreviated as N7C1M2. The second type of lithium nickel cobalt manganese oxide has the structural formula LiNi 0.9 Co 0.05 Mn 0.05 O2, abbreviated as N9C 0.5 M 0.5 The weight ratio of the first type of lithium nickel cobalt manganese oxide, the second type of lithium nickel cobalt manganese oxide, conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 75:25:3:1.5. 0.7 Co 0.1 Mn 0.2 The molar content of nickel in all transition metal elements is 0.7. 0.9 Co 0.05 Mn 0.05 The molar content of nickel in all transition metal elements is 0.9. Other details are the same as those in Example 1 and will not be described again.

[0137] Example 12

[0138] The difference between the battery cell and the preparation method of the battery cell in the embodiment of the present application and that in the preparation method of the positive electrode sheet is that the first lithium nickel cobalt manganese oxide has the structural formula LiNi 0.75 Co 0.5 Mn 0.2 O2, abbreviated as N 7.5 C 0.5 M2. The structural formula of the second type of lithium nickel cobalt manganese oxide is LiNi 0.98 Co 0.01 Mn 0.01 O2, abbreviated as N 9.8 C 0.1 M 0.1 The weight ratio of the first type of lithium nickel cobalt manganese oxide, the second type of lithium nickel cobalt manganese oxide, conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) is 75:25:3:1.5. 0.75 Co 0.5 Mn 0.2 The molar content of nickel in all transition metal elements is 0.75. 0.98 Co 0.01 Mn 0.01 The molar content of nickel in all transition metal elements in the reaction mixture is 0.98. Other details are the same as those in Example 1 and will not be described again.

[0139] Example 13

[0140] The battery cells and their preparation methods in this embodiment differ from those in Example 1 in that, in the negative electrode sheet preparation method, the silicon-based material is silicon oxide. The weight ratio of artificial graphite, silicon oxide, conductive carbon black (Super-P), carbon nanotubes, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) is 95:7.5:0.5:0.1:1:1.5. All other components are the same as in Example 1 and are not further described here.

[0141] Comparative Example 1

[0142] The battery cell and the preparation method of the battery cell of this comparative example are different from those of Example 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1O2, abbreviated as N8C1M1), conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) weight ratio is 100:0:3:1.5. That is, the positive electrode active material in this comparative example is the first nickel cobalt manganese oxide LiNi 0.6 Co 0.2 Mn 0.2 O2, does not contain the second type of lithium nickel cobalt manganese oxide, and the rest is the same as in Example 1 and will not be repeated here.

[0143] Comparative Example 2

[0144] The battery cell and the preparation method of the battery cell of this comparative example are different from those of Example 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.8 Co 0.1 Mn 0.1 O2, abbreviated as N8C1M1), conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) weight ratio is 100:0:3:1.5. That is, the positive electrode active material in this comparative example is the first nickel cobalt manganese oxide LiNi 0.6 Co 0.2 Mn 0.2 O2, and does not contain the second type of lithium nickel cobalt manganese oxide. In the preparation method of the negative electrode sheet, the weight ratio of artificial graphite, nano-silicon, conductive carbon black (Super-P), carbon nanotubes, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) is 90:10:0.5:0.1:1:1.5. All other aspects are the same as in Example 1 and are not repeated here.

[0145] Comparative Example 3

[0146] The battery cell and the preparation method of the battery cell of this comparative example are different from those of Example 1 in that, in the preparation method of the positive electrode sheet, the first lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2, abbreviated as N6C2M2), the second type of lithium nickel cobalt manganese oxide (LiNi 0.7 Co 0.1 Mn 0.2 The weight ratio of the conductive carbon black (Super-P) and polyvinylidene fluoride (PVDF) was 75:25:3:1.5. This means that the molar content of nickel in the total transition metal content of the second type of lithium nickel cobalt manganese oxide, the positive electrode active material in this comparative example, was 0.7, less than 0.8. All other aspects were the same as in Example 1 and are not further described here.

[0147] The battery performance test was conducted on the battery cells of Examples 1-13 and Comparative Examples 1-3. Specifically, the battery cell cycle capacity retention rate test was conducted. The specific test conditions were:

[0148] At 25℃, 1 / 3C 标 (Nominal capacity) Constant current charge to the end voltage of 4.4V, then constant voltage charge to 0.05C 标 , let it sit for 5 minutes, then 1 / 3C 标 Discharge to the discharge cut-off voltage of 2.5V, and obtain the discharge energy E and capacity C. The obtained capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery cell and record the discharge capacity C of the battery after the nth cycle. n , then the battery capacity retention rate P after each cycle n =C n / C0×100%. In this test process, the first cycle corresponds to n=1, the second cycle corresponds to n=2, ..., the 1500th cycle corresponds to n=1500. The corresponding battery capacity retention rate data in Table 1 are the data measured after 1500 cycles under the above test conditions.

[0149] According to the test results shown in Table 1, (1) the cycle capacity retention rate of the battery cells of Examples 1 to 13 is relatively good, ranging from 81% to 93.5%. When the positive electrode active material of Comparative Examples 1 and 2 is the first lithium nickel cobalt manganese oxide N6C2M2 with a lower nickel content, and the negative electrode active material includes a silicon-based material and a carbon-based material, the cycle capacity retention rate is between 60% and 80%. Specifically, in the first lithium nickel cobalt manganese oxide, the molar content of nickel in all transition metal elements is 0.6, which is less than 0.8. The positive electrode active material of Comparative Example 3 includes lithium nickel cobalt manganese oxide N6C2M2 with a lower nickel content and lithium nickel cobalt manganese oxide N7C1M2 with a lower nickel content, that is, the molar content of nickel in all transition metal elements in both lithium nickel cobalt manganese oxides is less than 0.8, and the cycle capacity retention rate of the battery cell is 80%. The cycle capacity retention rates of the battery cells of Examples 1 to 13 are all higher than those of Comparative Examples 1-3. It is described that the positive electrode active materials of Examples 1 to 13 of the present application are increased by adding a second lithium nickel cobalt manganese oxide with a higher nickel content, wherein the molar content of nickel element in all transition metal elements in the second lithium nickel cobalt manganese oxide is greater than or equal to 0.8, thereby improving the battery capacity retention rate of the battery cell. After the battery cell is cycled 1500 times, the battery cell cycle capacity retention rate can be as high as 93.5%.

[0150] Table 1: Parameters and performance test results of Examples 1-13 and Comparative Examples 1-3

[0151] Note: Carbon weight parts are the weight parts of carbon-based materials in the negative electrode material; Silicon weight parts are the weight parts of silicon-based materials in the negative electrode material; NCM1:NCM2 is the weight ratio of NCM1 to NCM2; X1 represents the mass fraction of silicon in the negative electrode active material; X2 represents the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material; Y represents the ratio of the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material to the mass fraction of silicon in the negative electrode active material, that is, Y=X2 / X1.

[0152] (2) From the test results of Examples 1 to 3, it can be seen that, when the negative electrode active material and X1 are the same, as the content of the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material increases, the cycle capacity retention rate of the battery cell gradually increases. When the ratio Y value of the mass fraction of the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material to the mass fraction of the silicon element in the negative electrode active material reaches 5, the cycle capacity retention rate can be as high as 93%. This shows that as the content of the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material increases, during the charging process, the voids formed by the lattice contraction of the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material increase, and the voids formed by the positive electrode sheet increase, so that the electrolyte squeezed out due to the expansion of the negative electrode silicon-based material reaches the voids formed by the positive electrode sheet, which facilitates the electrolyte to flow back from the voids formed by the positive electrode sheet to the negative electrode during discharge, facilitates the reflux of the electrolyte, reduces the occurrence of lithium precipitation during the charging process, and thus can improve the cycle capacity retention rate. When the Y value reaches 5, the volume of the gap formed by the positive electrode sheet is equivalent to or similar to the volume of the electrolyte squeezed out by the expansion of the negative electrode sheet, so that the gap volume for storing the electrolyte reaches a better state and the battery's cycle capacity retention rate reaches a better rate.

[0153] The test results of Examples 4-6 and Comparative Example 1 show that, given the same negative electrode active material and X1, as the content of the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material further increases, the cycle capacity retention rate shows a downward trend. When the Y value reaches 10, the cycle capacity retention rate drops to 83%. This indicates that as the content of the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material of the positive electrode sheet increases (X2 increases) and the Y value increases, the instability of the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material increases its impact on the cycle capacity retention rate of the battery cell, causing the cycle capacity retention rate of the battery cell to weaken to a certain extent. In Comparative Example 1, the positive electrode active material does not contain the second lithium nickel cobalt manganese oxide (NCM2), and its cycle capacity retention rate is 80%. Examples 1-6 show that when 0<Y≤10, the cycle capacity retention rate of the battery cell is improved, and the cycle capacity retention rate can reach 83%-93%. When 4≤Y≤6, the cycle capacity retention rate of the battery cell is as high as 89%-93%, and the cycle capacity retention rate is greatly improved. When 0<X2≤50%, the cycle capacity retention rate of the battery cell is also improved.

[0154] (3) It can be seen from Example 2, Example 8, Comparative Example 1 and Comparative Example 2 that, based on the fact that the positive electrode active material in Comparative Example 1 and Comparative Example 2 does not contain the second lithium nickel cobalt manganese oxide (NCM2), when X1 = 5%, the cycle capacity of the battery cell is 80%; when X1 = 10%, the cycle capacity of the battery cell is 70%. The positive electrode active materials of Example 2 and Example 8 both include the first lithium nickel cobalt manganese oxide (NCM1) and the second lithium nickel cobalt manganese oxide (NCM2). When the Y value is the same, both being 4, when X1 is 5%, the cycle capacity retention rate is 89%, which is higher than the 80% of Comparative Example 1; when X1 is 10%, the cycle capacity retention rate is 83%, which is higher than the 70% of Comparative Example 2. When the Y value is the same, 0<X1≤10%, the cycle capacity retention rate of the battery cell is improved. Specifically, when Y=4, 0<X1≤10%, the cycle capacity retention rate is as high as 83%-89%.

[0155] (4) Examples 7 to 9 and Comparative Example 2 illustrate that, when X1 = 10% and 0 < X2 ≤ 50%, the cycle capacity retention rate of the battery cell is improved, with the cycle capacity retention rate being 81% to 85%, which is higher than the cycle capacity retention rate of 70% when the positive electrode active material does not contain the second lithium nickel cobalt manganese oxide (NCM2).

[0156] (5) In Examples 3, 10, and 12, the positive electrode active material contains a second lithium nickel cobalt manganese oxide (NCM2), the negative electrode active material is the same (artificial graphite and nano-silicon), X1 is the same (5%), X2 is the same (25%), and Y is the same (5), but the second lithium nickel cobalt manganese oxide (NCM2) in the positive electrode active material is different. In the second lithium nickel cobalt manganese oxide, the molar content of nickel in all transition metal elements increases successively and is greater than or equal to 0.8. The cycle capacity retention rate of the battery cell is between 91% and 93.5%, showing a trend of first increasing and then decreasing. When the molar content of nickel in all transition metal elements is 0.8, the cycle capacity retention rate of the battery cell is 93%. When the molar content of nickel in all transition metal elements is 0.85, the cycle capacity retention rate of the battery cell reaches the highest, and is as high as 93.5%. When the molar content of nickel in all transition metal elements is 0.98, the cycle capacity retention rate of the battery cell decreases to 91%.

[0157] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present application, embodiments having substantially the same structure as the technical concept and exerting the same effects are all included in the technical scope of the present application. In addition, within the scope of the subject matter of the present application, various modifications that can be conceived by those skilled in the art to the embodiments, and other methods constructed by combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A battery cell, comprising: A positive electrode sheet, the positive electrode sheet comprising a positive electrode active material, the positive electrode active material comprising a first lithium nickel cobalt manganese oxide and a second lithium nickel cobalt manganese oxide, the molar content of nickel in the second lithium nickel cobalt manganese oxide in all transition metal elements is greater than the molar content of nickel in the first lithium nickel cobalt manganese oxide in all transition metal elements, wherein the molar content of nickel in the second lithium nickel cobalt manganese oxide in all transition metal elements is greater than or equal to 0.8; The negative electrode sheet comprises a negative electrode active material, wherein the negative electrode active material comprises a silicon-based material and a carbon-based material.

2. The battery cell according to claim 1, wherein: The ratio of the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material to the mass fraction of the silicon element in the negative electrode active material is less than or equal to 10 and greater than 0.

3. The battery cell according to claim 1 or 2, wherein: The ratio of the mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material to the mass fraction of the silicon element in the negative electrode active material is less than or equal to 6 and greater than or equal to 4.

4. The battery cell according to any one of claims 1 to 3, wherein: The mass fraction of the second lithium nickel cobalt manganese oxide in the positive electrode active material is less than or equal to 50% and greater than 0.

5. The battery cell according to any one of claims 1 to 4, wherein: The mass fraction of silicon in the negative electrode active material is less than or equal to 10% and greater than 0.

6. The battery cell according to any one of claims 1 to 5, wherein: In the first lithium nickel cobalt manganese oxide, the molar content of nickel element in all transition metal elements is less than or equal to 0.75 and greater than or equal to 0.

5.

7. The battery cell according to any one of claims 1 to 6, wherein: The first lithium nickel cobalt manganese oxide comprises a first lithium nickel cobalt manganese oxide or a doping modification material of the first lithium nickel cobalt manganese oxide or a surface modification material of the first lithium nickel cobalt manganese oxide. The structural formula of the first lithium nickel cobalt manganese oxide is LiNi x Co y Mn z O2, where 0.5≤x≤0.75, 0.03≤y≤0.3, 0.2≤z≤0.

4.

8. The battery cell according to any one of claims 1 to 7, wherein: The second lithium nickel cobalt manganese oxide comprises a second lithium nickel cobalt manganese oxide or a doping modified material of the second lithium nickel cobalt manganese oxide or a surface modified material of the second lithium nickel cobalt manganese oxide. The structural formula of the second lithium nickel cobalt manganese oxide is LiNi a Co b Mn c O2, where 0.8≤a≤0.98, 0.01≤b≤0.15, 0.01≤c≤0.

15.

9. The battery cell according to any one of claims 1 to 8, wherein: The volume average particle size Dv50 of the secondary particles of the first lithium nickel cobalt manganese oxide is 3 microns to 5 microns; and / or, The volume average particle size Dv50 of the secondary particles of the second lithium nickel cobalt manganese oxide is 8 microns to 12 microns.

10. The battery cell according to any one of claims 1 to 9, wherein: The volume average particle size Dv50 of the primary particles of the first lithium nickel cobalt manganese oxide is in the range of 1 micron to 3 microns; and / or, The volume average particle size Dv50 of the primary particles of the second lithium nickel cobalt manganese oxide is in the range of 100 nanometers to 500 nanometers.

11. The battery cell according to any one of claims 1 to 10, wherein: The compaction density of the positive electrode sheet is 2.8 g / cm 3 -3.7g / cm 3 .

12. The battery cell according to any one of claims 1 to 11, wherein: The silicon-based material includes any one or more of silicon, a silicon-carbon composite material, silicon monoxide, and a silicon monoxide-carbon composite material.

13. The battery cell according to any one of claims 1 to 12, wherein: The carbon-based material includes graphite.

14. A battery comprising the battery cell according to any one of claims 1 to 13.

15. An electrical device comprising the battery cell according to any one of claims 1 to 13 and / or the battery according to claim 14.

Citation Information

Patent Citations

  • Nickel-based positive electrode material with core-shell structure and preparation method thereof

    CN110085845A

  • Cathode active material, cathode plate and electrochemical device

    CN110970602A

  • Electrolyte and electrochemical device

    CN111342129A

  • Positive pole piece and preparation method thereof and lithium ion secondary battery

    CN111640912A

  • Positive electrode material, positive electrode plate and lithium ion battery

    CN111653732A

Cited By

  • Positive plate and lithium ion secondary battery

    CN119480904A

  • Positive electrode sheet and lithium ion secondary battery

    CN119480904B

  • Lithium ion cylindrical battery with hot gas safety and power utilization device