Rubber composition for tire tread and pneumatic tire

By using rubber compositions containing diene rubber, modified butadiene rubber, silicone group and thermally expandable microcapsules on the tire tread, the ice performance, wet tracking performance and low in the prior art are solved. The problem of insufficient heat generation and wear resistance achieves better tire performance.

CN110168008BActive Publication Date: 2024-11-26THE YOKOHAMA RUBBER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880006134.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-01-12
Filing Date
2018-01-12
Publication Date
2024-11-26
Estimated Expiration
2038-01-12

Smart Images

  • Figure BDA0002121511780000131
    Figure BDA0002121511780000131
  • Figure BDA0002121511780000141
    Figure BDA0002121511780000141
  • Figure BDA0002121511780000142
    Figure BDA0002121511780000142
Patent Text Reader

Abstract

Provided are a rubber composition for tire treads which has excellent ice performance, wet grip performance, low heat build-up and wear resistance when a tire is made, and a pneumatic tire having the rubber composition for tire treads in the tread. The rubber composition for tire treads contains a diene rubber, silica, and a cured product, wherein the content of the silica is 20 to 100 parts by mass relative to 100 parts by mass of the diene rubber, and the content of the cured product is 0.3 to 30 parts by mass relative to 100 parts by mass of the diene rubber. The diene rubber contains natural rubber and modified butadiene rubber having a polyorganosiloxane group at the end, wherein the content of the natural rubber in the diene rubber is 30 to 90% by mass, and the content of the modified butadiene rubber in the diene rubber is 10 to 70% by mass. The cured product is a cured product obtained by curing a crosslinkable oligomer or polymer incompatible with the diene rubber, and the cured product has a JIS A hardness of 3 to 45.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rubber composition for tire tread and a pneumatic tire. Background Art

[0002] In the past, tire rubber compositions used for the tire tread of studless tires are known. For example, [Claim 1] of Patent Document 1 states "A tire rubber composition comprising 100 parts by mass of a diene rubber (A), 30 to 100 parts by mass of carbon black and / or a white filler (B), and 0.3 to 30 parts by mass of a cured product (C) obtained by curing a cross-linking oligomer or polymer (c1) incompatible with the diene rubber (A), wherein the cured product (C) has a JIS A hardness of 3 to 45."

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-067636 Summary of the invention

[0006] Problems to be solved by the invention

[0007] The present inventors have studied the tire rubber composition described in Patent Document 1 and found that at least any one of on-ice performance (friction on ice), wet grip performance, low heat build-up properties, and wear resistance may be insufficient.

[0008] The present invention is proposed in view of the above aspects, and its purpose is to provide a rubber composition for tire tread that has excellent ice performance, wet road grip performance, low heat buildup and wear resistance when the tire is made, and an inflatable tire whose tread uses the above-mentioned rubber composition for tire tread.

[0009] Methods for solving problems

[0010] The present inventors have conducted intensive studies and, as a result, have found that the above-mentioned object can be achieved by using a specific diene rubber, thereby completing the present invention.

[0011] That is, the present invention provides the following [1] to [7].

[0012] [1] A rubber composition for a tire tread, comprising a diene rubber, silica and a cured product, wherein the content of the silica is 20 to 100 parts by mass based on 100 parts by mass of the diene rubber, and the content of the cured product is 0.3 to 30 parts by mass based on 100 parts by mass of the diene rubber, the diene rubber comprises a natural rubber and a modified butadiene rubber having a polyorganosiloxane group at a terminal, the content of the natural rubber in the diene rubber is 30 to 90% by mass, the content of the modified butadiene rubber in the diene rubber is 10 to 70% by mass, and the cured product is a cured product obtained by curing a cross-linking oligomer or polymer incompatible with the diene rubber, and the JIS A hardness of the cured product is 3 to 45.

[0013] [2] According to the rubber composition for tire tread described in [1] above, the polyorganosiloxane group is a group bonded to the end of the butadiene chain via a linking group or an ether group, and the linking group is a linking group formed by a divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent.

[0014] However, a part of -CH2- constituting the above-mentioned divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent may be substituted with -O-.

[0015] Furthermore, a silicon-containing linking group represented by the general formula (Si) described below may exist between the linking group formed of the divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent and the terminal of the butadiene chain.

[0016] [3] The rubber composition for a tire tread according to [1] or [2] above, wherein the cured product is a particulate material having an average particle size of 5 to 250 μm.

[0017] [4] The rubber composition for tire tread according to any one of [1] to [3] above, wherein the crosslinkable oligomer or polymer is a polyether-based or siloxane-based polymer or copolymer and has a silane functional group.

[0018] [5] The rubber composition for tire tread according to any one of [1] to [4] above, further comprising an aromatic modified terpene resin having a softening point of 60 to 150°C, wherein the content of the aromatic modified terpene resin is 2 to 20 parts by mass relative to 100 parts by mass of the diene rubber.

[0019] [6] The rubber composition for tire tread according to any one of [1] to [5] above, further comprising heat-expandable microcapsules, wherein the content of the heat-expandable microcapsules is 0.5 to 20 parts by mass based on 100 parts by mass of the diene rubber.

[0020] [7] A pneumatic tire, the tread of which is formed using the rubber composition for a tire tread according to any one of [1] to [6].

[0021] Effects of the Invention

[0022] According to the present invention, there can be provided a rubber composition for tire tread which, when manufactured into a tire, has excellent performance on ice, wet grip performance, low heat build-up property, and wear resistance, and a pneumatic tire having a tread using the rubber composition for tire tread. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a partial cross-sectional schematic diagram of a tire showing an example of an embodiment of a pneumatic tire of the present invention. DETAILED DESCRIPTION

[0024] Hereinafter, the rubber composition for a tire tread of the present invention and a pneumatic tire having a tread using the rubber composition for a tire tread of the present invention will be described.

[0025] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0026] [Rubber composition for tire tread]

[0027] The rubber composition for tire tread of the present invention (hereinafter also referred to as "the composition of the present invention") is a rubber composition for tire tread, which contains a diene rubber, silica, and a cured product, wherein the content of the silica is 20 to 100 parts by mass relative to 100 parts by mass of the diene rubber, and the content of the cured product is 0.3 to 30 parts by mass relative to 100 parts by mass of the diene rubber. The diene rubber contains natural rubber and modified butadiene rubber having a polyorganosiloxane group at the end, the content of the natural rubber in the diene rubber is 30 to 90% by mass, the content of the modified butadiene rubber in the diene rubber is 10 to 70% by mass, and the cured product is a cured product obtained by curing a cross-linking oligomer or polymer incompatible with the diene rubber, and the JIS A hardness of the cured product is 3 to 45.

[0028] It is believed that the composition of the present invention can achieve the desired effect by adopting the above-mentioned structure. The reason is not clear, but it is roughly estimated as follows.

[0029] As described above, the composition of the present invention contains a diene rubber including natural rubber and a specific modified butadiene rubber, silica, and a specific cured product. According to the research of the present inventors, it is known that the above-mentioned specific cured product has the effect of improving the performance on ice, but is easy to agglomerate, and this tendency becomes stronger when the content of silica increases, and the low heat generation property and wear resistance are reduced.

[0030] On the other hand, in the composition of the present invention, it is considered that the modified terminal of the specific modified butadiene rubber interacts with the cured product to suppress the aggregation thereof.

[0031] As a result, it is estimated that the tire using the composition of the present invention exhibits excellent low heat build-up property and wear resistance in addition to excellent on-ice performance and wet grip performance.

[0032] Hereinafter, each component contained in the composition of the present invention will be described in detail.

[0033] 〈Diene rubber〉

[0034] The diene rubber contained in the composition of the present invention includes natural rubber and modified butadiene rubber having a polyorganosiloxane group at the terminal.

[0035] Natural Rubber

[0036] The natural rubber contained in the above-mentioned diene rubber is not particularly limited.

[0037] The content of the natural rubber in the diene rubber is 30 to 90% by mass, preferably 30 to 85% by mass, and more preferably 35 to 80% by mass.

[0038] 《Modified butadiene rubber》

[0039] The modified butadiene rubber included in the above-mentioned diene rubber is a modified butadiene rubber having a polyorganosiloxane group at a terminal.

[0040] The modified butadiene rubber has polybutadiene (butadiene rubber) as a conjugated diene polymer chain as a main chain, and has a polyorganosiloxane group at the terminal of the main chain.

[0041] Preferred examples of the polyorganosiloxane group include groups derived from the polyorganosiloxane (modifying agent) described in the step (B) below.

[0042] Furthermore, the modified butadiene rubber may have a group derived from a silicon compound (coupling agent) described in the step (A) described later, between the main chain (butadiene chain) and the polyorganosiloxane group.

[0043] The bond between the main chain (butadiene chain) and the polyorganosiloxane group can suppress the excessive reaction between silica and the silane coupling agent described below, and is preferably a bond other than a bond via a nitrogen atom because the processability of the composition is excellent.

[0044] From the perspective of excellent processability of the composition, the polyorganosiloxane group is preferably a group bonded to the terminal of the butadiene chain via a linking group formed by a divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent (hereinafter also referred to as a "hydrocarbon-based linking group") or an ether group, and is more preferably a group bonded to the terminal of the butadiene chain via a hydrocarbon-based linking group.

[0045] The hydrocarbon-based linking group is, for example, a polymethylene group (CH2) having 1 to 20 carbon atoms. k (k is an integer of 1 to 20.)), an arylene group having 6 to 20 carbon atoms, or a cycloalkylene group having 5 to 20 carbon atoms.

[0046] Furthermore, a part of -CH2- constituting the above-mentioned hydrocarbon-based linking group may be replaced by -O-.

[0047] In the hydrocarbon-based linking group, the number of -CH2- replaced by -O- is not particularly limited as long as it is not the total number, but is preferably 1 to 5, and more preferably 1 to 2.

[0048] In addition, it is preferred that a group derived from a silicon compound (coupling agent) described in step (A) described later is present between the hydrocarbon-based linking group or the ether group and the end of the butadiene chain, and the group derived from the silicon compound (coupling agent) is preferably a silicon-containing linking group represented by the general formula (Si). The details of the silicon-containing linking group are described below.

[0049] The hydrocarbon-based linking group is preferably a group represented by the following general formula (C).

[0050] *aY-*b (C)

[0051] In the general formula (C),

[0052] Y is a polymethylene group having 1 to 20 carbon atoms which may have a substituent or an ether group.

[0053] One or more (preferably 1 to 5, more preferably 1 to 2) -CH2- in the polymethylene group may be independently replaced by -O-. However, the number of -CH2- replaced by -O- is not the total number of -CH2- constituting the polymethylene group.

[0054] Furthermore, the atom directly bonded to *a in the polymethylene group (that is, the atom directly bonded to the silicon atom in the polyorganosiloxane group) is preferably a carbon atom.

[0055] Y is preferably a polymethylene group having 1 to 20 carbon atoms which may have a substituent.

[0056] *a is a position bonding to a silicon atom in a polyorganosiloxane group.

[0057] *b is a position that bonds to a group derived from the silicon compound (coupling agent) described in step (A) (preferably *1 in the general formula (Si) described later) or a butadiene chain terminal.

[0058] Regarding the groups derived from the silicon compound (coupling agent) explained in step (A), these groups may be bonded to each other and exist continuously.

[0059] The group derived from the silicon compound (coupling agent) described in step (A) is preferably a silicon-containing linking group represented by the following general formula (Si).

[0060] *1-Q 1 -Si(R L1 )2-A 1 -Si(R L2 )2-Q 2 -*2 (Si)

[0061] In the general formula (Si),

[0062] Q 1 and Q 2 Each is independently a chemical single bond or -O-.

[0063] R L1 and R L2 Each independently represents a substituent, and multiple R L1 and R L2 They may be the same or different.

[0064] A 1 A chemical single bond, a polymethylene group with 1 to 20 carbon atoms ((CH2) k (k is an integer of 1 to 20.)), an arylene group having 6 to 20 carbon atoms, or a cycloalkylene group having 5 to 20 carbon atoms.

[0065] *1 is a position that bonds to *2 in other silicon-containing linking groups or a hydrocarbon-based linking group (preferably *b in the general formula (C)).

[0066] *2 is the position that bonds to *1 in other silicon-containing linking groups or to the end of the butadiene chain.

[0067] That is, in the modified butadiene rubber, the butadiene chain and the polyorganosiloxane group are preferably bonded in a form represented by the following formula. By using such a modified butadiene rubber, the processability of the composition of the present invention is improved.

[0068] (Silicon atom in the polyorganosiloxane group)-(hydrocarbon-based linking group or ether group)-(group derived from the silicon compound described in step (A)) x -(butadiene chain end)

[0069] In the above formula, x is an integer greater than or equal to 0, preferably 0 to 10, and more preferably 0 or 1. When x is 0, -(the group derived from the silicon compound described in step (A)) x - becomes a chemical single bond.

[0070] The above-mentioned "-(hydrocarbon-based linking group or ether group)-" is preferably "-(hydrocarbon-based linking group)-".

[0071] The hydrocarbon-based linking group is preferably a group represented by the above-mentioned general formula (C).

[0072] The group derived from the silicon compound described in the above step (A) is preferably a silicon-containing linking group represented by the above general formula (Si).

[0073] In the above formula, the bonding of the silicon atom in the polyorganosiloxane group with a group other than the hydrocarbon-based linking group is omitted. Similarly, the bonding of the butadiene chain terminal with a group other than the group derived from the silicon compound described in step (A) (or the hydrocarbon-based linking group) is omitted.

[0074] The content of the modified butadiene rubber in the diene rubber is 10 to 70% by mass, preferably 15 to 70% by mass, and more preferably 20 to 70% by mass.

[0075] Hereinafter, a method for producing the modified butadiene rubber will be described.

[0076] More specifically, a preferred embodiment of the method for producing a composition containing the modified butadiene rubber (hereinafter, also referred to as “composition S”) will be described.

[0077] (Preferred Aspects of the Method for Producing the Composition S Containing Modified Butadiene Rubber)

[0078] The method for producing the composition S containing the modified butadiene rubber is preferably a method for producing the composition S by mixing the following solution with the following silicon compound and polyorganosiloxane, for example,

[0079] The above solution is a solution containing a conjugated diene polymer chain having an active terminal obtained by polymerizing at least a conjugated diene monomer in an inert solvent using a polymerization initiator.

[0080] The silicon compound has six or more reaction sites capable of reacting with the active end of the conjugated diene polymer chain having an active end in one molecule, and the polyorganosiloxane has 3 to 200 functional groups capable of reacting with the active end of the conjugated diene polymer chain having an active end in one molecule.

[0081] ((Conjugated diene polymer chain with active terminal))

[0082] In the method for producing the composition S, first, at least a conjugated diene monomer is polymerized in an inert solvent using a polymerization initiator to obtain a solution containing a conjugated diene polymer chain having an active terminal.

[0083] The conjugated diene monomer is butadiene.

[0084] Examples of butadiene include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, and 2-chloro-1,3-butadiene. Among them, 1,3-butadiene is preferred.

[0085] These conjugated diene monomers can be used alone or in combination of two or more.

[0086] In addition to the conjugated diene monomer, an aromatic vinyl monomer may be used.

[0087] As the aromatic vinyl monomer, for example, styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-tert-butylstyrene, 5-tert-butyl-2-methylstyrene, vinylnaphthalene, dimethylaminomethylstyrene, dimethylaminoethylstyrene, etc. can be used.

[0088] Among them, styrene, α-methylstyrene, and 4-methylstyrene are preferred, and styrene is more preferred.

[0089] These aromatic vinyl monomers can be used alone or in combination of two or more.

[0090] The conjugated diene polymer chain having an active terminal is preferably a homopolymer chain of a conjugated diene monomer or a copolymer chain of a conjugated diene monomer and an aromatic vinyl monomer, and more preferably a homopolymer chain of a conjugated diene monomer.

[0091] The conjugated diene polymer chain preferably contains 50 to 100% by mass, more preferably 60 to 100% by mass, and further preferably 70 to 100% by mass of a conjugated diene monomer unit, and preferably contains 50 to 0% by mass, more preferably 40 to 0% by mass, and further preferably 30 to 0% by mass of an aromatic vinyl monomer unit.

[0092] Furthermore, other monomers than the conjugated diene monomer and the aromatic vinyl monomer may be used as necessary within a range not impairing the intended purpose.

[0093] As other monomers, for example, α,β-unsaturated nitriles such as acrylonitrile and methacrylonitrile; unsaturated carboxylic acids or anhydrides such as acrylic acid, methacrylic acid, and maleic anhydride; unsaturated carboxylic acid esters such as methyl methacrylate, ethyl acrylate, and butyl acrylate; non-conjugated dienes such as 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene; and the like.

[0094] The content of these monomers as monomer units in the conjugated diene polymer chain having an active terminal is preferably 10% by mass or less, more preferably 5% by mass or less.

[0095] The inert solvent used for the polymerization of the above-mentioned monomers can be used without particular limitation as long as it is an inert solvent commonly used in solution polymerization and does not inhibit the polymerization reaction.

[0096] Specific examples thereof include aliphatic hydrocarbons such as butane, pentane, hexane, and 2-butene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and cyclohexene; and aromatic hydrocarbons such as benzene, toluene, and xylene.

[0097] The amount of the inert solvent used is generally 1 to 50% by mass, preferably 10 to 40% by mass, based on the monomer concentration.

[0098] The polymerization initiator used for the polymerization of the above-mentioned monomers is not particularly limited as long as it is a polymerization initiator that can polymerize these monomers to obtain a polymer chain with an active end. For example, it is preferred to use an organic alkali metal compound, an organic alkaline earth metal compound, and a polymerization initiator using a lanthanide metal compound as a main catalyst.

[0099] Specific examples of organic alkali metal compounds include, for example, organic monolithium compounds such as n-butyllithium, sec-butyllithium, tert-butyllithium, hexyllithium, phenyllithium, and stilbene lithium; organic multivalent lithium compounds such as dilithium methane, 1,4-dilithium butane, 1,4-dilithium-2-ethylcyclohexane, 1,3,5-trilithium benzene, and 1,3,5-tri(lithium methyl)benzene; organic sodium compounds such as sodium naphthyl; organic potassium compounds such as potassium naphthyl; etc.

[0100] Examples of the organic alkaline earth metal compound include di-n-butylmagnesium, di-n-hexylmagnesium, diethoxycalcium, calcium distearate, di-tert-butoxystrontium, diethoxybarium, diisopropoxybarium, diethylmercaptobarium, di-tert-butoxybarium, diphenoxybarium, diethylaminobarium, barium distearate, and dicarbonylbarium.

[0101] Examples of polymerization initiators using lanthanide metal compounds as main catalysts include polymerization initiators using lanthanide metal salts formed from lanthanide metals such as lanthanum, cerium, praseodymium, neodymium, samarium and gadolinium, and carboxylic acids and phosphorus-containing organic acids as main catalysts, and polymerization initiators formed from lanthanide metal salts and co-catalysts such as alkylaluminum compounds, organic aluminum hydride compounds, and organic aluminum halide compounds.

[0102] Among these polymerization initiators, organic monolithium compounds and organic multivalent lithium compounds are preferred, organic monolithium compounds are more preferred, and n-butyllithium is further preferred.

[0103] The organic alkali metal compound may be used by reacting in advance with a secondary amine such as dibutylamine, dihexylamine, dibenzylamine, pyrrolidine, hexamethyleneimine, and heptamethyleneimine (preferably pyrrolidine, hexamethyleneimine, and heptamethyleneimine) to form an organic alkali metal amide compound.

[0104] These polymerization initiators can be used alone or in combination of two or more.

[0105] The amount of the polymerization initiator used may be determined depending on the desired molecular weight, and is generally in the range of 1 to 50 mmol, preferably 2 to 20 mmol, and more preferably 4 to 15 mmol per 1000 g of the monomer.

[0106] When the above monomers are polymerized, the polymerization temperature is usually in the range of -80 to +150°C, preferably 0 to 100°C, and more preferably 30 to 90°C.

[0107] The polymerization mode may be a batch mode or a continuous mode. However, when a conjugated diene monomer and an aromatic vinyl monomer are copolymerized, a batch mode is preferred from the viewpoint of facilitating control of the randomness of bonding between the conjugated diene monomer units and the aromatic vinyl monomer units.

[0108] When the conjugated diene polymer chain having an active terminal has a conjugated diene monomer unit and an aromatic vinyl monomer unit, the bonding pattern of the conjugated diene monomer unit and the aromatic vinyl monomer unit may be, for example, a block-shaped, cone-shaped, random bonding pattern, etc., and a random bonding pattern is preferred.

[0109] In order to adjust the vinyl bond content in the conjugated diene monomer unit in the conjugated diene polymer chain having an active terminal, it is preferred to add a polar compound to an inert organic solvent during polymerization.

[0110] Examples of the polar compound include ether compounds such as dibutyl ether and tetrahydrofuran; tertiary amines such as tetramethylethylenediamine; alkali metal alkoxides; phosphine compounds; and the like.

[0111] Among them, ether compounds and tertiary amines are preferred, tertiary amines are more preferred, and tetramethylethylenediamine is further preferred.

[0112] These polar compounds can be used alone or in combination of two or more.

[0113] The amount of the polar compound to be used may be determined depending on the intended vinyl bond content, and is generally in the range of 0.001 to 100 mol, preferably 0.005 to 50 mol, more preferably 0.01 to 30 mol, based on 1 mol of the polymerization initiator.

[0114] The peak top molecular weight of the conjugated diene polymer chain having an active terminal as detected by gel permeation chromatography (GPC) is preferably 200,000 or more and less than 300,000, more preferably 210,000 or more and less than 280,000, and further preferably 220,000 or more and less than 260,000.

[0115] The peak top molecular weight is detected by GPC and obtained as a polystyrene-converted molecular weight. In addition, when a plurality of conjugated diene polymer chains are confirmed to have peaks, the peak top molecular weight of the peak with the smallest molecular weight derived from the conjugated diene polymer chain detected by GPC is set as the peak top molecular weight of the conjugated diene polymer chain with an active terminal.

[0116] The molecular weight distribution represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the conjugated diene polymer chain having an active terminal is preferably 1.0 to 1.5, more preferably 1.0 to 1.4, and even more preferably 1.0 to 1.3.

[0117] ((Process (A)))

[0118] The method for producing the composition S comprises the following step (A): mixing the solution containing the conjugated diene polymer chain having an active end and a silicon compound having six or more reaction sites in one molecule that can react with the active end of the conjugated diene polymer chain having an active end (hereinafter also referred to as a "coupling agent").

[0119] The coupling agent used in step (A) is a silicon compound having 6 or more reaction sites capable of reacting with the active end of the conjugated diene polymer chain having an active end in one molecule, more preferably a silicon compound having 6 to 9 reaction sites capable of reacting with the active end of the conjugated diene polymer chain having an active end in one molecule, and even more preferably a silicon compound having 6 reaction sites capable of reacting with the active end of the conjugated diene polymer chain having an active end in one molecule. Specifically, a silicon compound represented by the following general formula (1) is particularly preferred.

[0120] The reactive site is not particularly limited as long as it can react with the active terminal of the conjugated diene polymer chain, and examples thereof include a halogen atom bonded to a silicon atom and an alkoxy group.

[0121] S L 1 3-A 1 -SiL 2 3 (1)

[0122] In the general formula (1), L 1 and L 2 Each independently represents a halogen atom or an alkoxy group having 1 to 20 carbon atoms, and a plurality of L 1 or L 2 Can be the same or different. 1 A chemical single bond, a polymethylene group with 1 to 20 carbon atoms ((CH2) k (k is an integer of 1 to 20.)), an arylene group having 6 to 20 carbon atoms, or a cycloalkylene group having 5 to 20 carbon atoms.

[0123] Among the silicon compounds represented by the above general formula (1), A 1 Preferably, it is a polymethylene group ((CH2) k (k is an integer of 1 to 20.)), wherein k is more preferably an integer of 1 to 10, and further preferably an integer of 1 to 6.

[0124] In the above general formula (1), L 1 and L 2 When all of L and L are halogen atoms, the silicon compound represented by the above general formula (1) is a halogenated silicon compound. 1 and L 2 On the other hand, in the above general formula (1), L 1 and L 2 When all of L and L are alkoxy groups having 1 to 20 carbon atoms, the silicon compound represented by the general formula (1) is an alkoxysilane compound. 1 and L 2An alkoxy group having 1 to 10 carbon atoms is preferred, an alkoxy group having 1 to 6 carbon atoms is more preferred, and a methoxy group or an ethoxy group is further preferred from the viewpoint of reactivity.

[0125] Specific examples of the silicon halide compound represented by the general formula (1) include hexachlorodisilane, bis(trichlorosilyl)methane, 1,2-bis(trichlorosilyl)ethane, 1,3-bis(trichlorosilyl)propane, 1,4-bis(trichlorosilyl)butane, 1,5-bis(trichlorosilyl)pentane, and 1,6-bis(trichlorosilyl)hexane. Among them, 1,6-bis(trichlorosilyl)hexane is preferred.

[0126] Specific examples of the alkoxysilane compound represented by the general formula (1) include hexamethoxydisilane, hexaethoxydisilane, bis(trimethoxysilyl)methane, bis(triethoxysilyl)methane, bis(trimethoxysilyl)ethane, bis(triethoxysilyl)ethane, bis(trimethoxysilyl)propane, bis(triethoxysilyl)propane, bis(trimethoxysilyl)butane, bis(triethoxysilyl) )butane, bis(trimethoxysilyl)pentane, bis(triethoxysilyl)pentane, bis(trimethoxysilyl)hexane, bis(triethoxysilyl)hexane, bis(trimethoxysilyl)benzene, bis(triethoxysilyl)benzene, bis(trimethoxysilyl)cyclohexane, bis(triethoxysilyl)cyclohexane, bis(3-trimethoxysilylpropyl)ethane, and bis(3-triethoxysilylpropyl)ethane. Among them, bis(trimethoxysilyl)hexane is preferred.

[0127] Other examples of the coupling agent include bis(3-triethoxysilylpropyl)methylamine and tris(trimethoxysilylmethyl)amine. These coupling agents can be used alone or in combination of two or more.

[0128] The amount of the coupling agent used is adjusted according to the coupling ratio range described below, but the molar amount of the coupling agent reactive site that reacts with the active terminal of the conjugated diene polymer chain is usually 0.1 to 0.35 mol, preferably 0.2 to 0.3 mol, per 1 mol of the polymerization initiator used in the polymerization reaction.

[0129] ((Process (B)))

[0130] The method for producing the composition S further comprises, in addition to the step (A), a step (B) of mixing the solution containing the conjugated diene polymer chain having an active terminal and a polyorganosiloxane having 3 to 200 functional groups in one molecule that can react with the active terminal of the conjugated diene polymer chain having an active terminal (hereinafter also referred to as a "modifier").

[0131] The modifier used in step (B) is a polyorganosiloxane having 3 to 200 functional groups capable of reacting with the active terminal of the conjugated diene polymer chain having an active terminal in one molecule. The number of functional groups in one polyorganosiloxane molecule is preferably 20 to 150, more preferably 30 to 120.

[0132] As the above-mentioned functional group, as long as it can react with the active end of the conjugated diene polymer chain, it is not particularly limited, and for example, epoxy, alkoxy, pyrrolidonyl, allyloxy, carbonyl, isocyanate, vinyl and halogen atoms etc. can be cited. Wherein, from the viewpoint of excellent affinity with silicon dioxide, epoxy, alkoxy and pyrrolidonyl are preferably considered. In addition, from the aspect of excellent processability of the composition of the present invention, epoxy or alkoxy are preferably considered, and epoxy is more preferably preferred.

[0133] Specifically, the polyorganosiloxane having 3 to 200 functional groups reactive with the active terminal of the conjugated diene polymer chain having an active terminal in one molecule is preferably a polyorganosiloxane represented by the following general formula (2).

[0134]

[0135] In the above general formula (2), R 1 ~R 8 Each independently represents an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms. 1 and X 4 is a functional group capable of reacting with the active terminal of the conjugated diene polymer chain having an active terminal, or an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, and X 1 and X 4 They can be the same or different. 2 Each independently represents a functional group capable of reacting with the active terminal of the conjugated diene polymer chain having an active terminal. 3 is a group containing 2 to 20 repeating units of alkylene glycol, X 3 A part of may be a group derived from a group containing 2 to 20 repeating units of an alkylene glycol. m is an integer of 3 to 200, n is an integer of 0 to 200, and k is an integer of 0 to 200.

[0136] As a component of R 1 ~R 8 , X 1 and X 4The alkyl group having 1 to 6 carbon atoms includes, for example, methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, and cyclohexyl. The aryl group having 6 to 12 carbon atoms includes, for example, phenyl and methylphenyl. Among them, methyl is preferred from the viewpoint of the ease of production of the polyorganosiloxane itself.

[0137] As a component X 1 , X 2 and X 4 The functional group capable of reacting with the active terminal of the conjugated diene polymer chain having an active terminal is preferably an alkoxy group having 1 to 5 carbon atoms, a hydrocarbon group containing a 2-pyrrolidone group, and a group having 4 to 12 carbon atoms containing an epoxy group.

[0138] Examples of the alkoxy group having 1 to 5 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, and a butoxy group. Among them, a methoxy group is preferred from the viewpoint of reactivity.

[0139] The hydrocarbon group containing a 2-pyrrolidone group is represented by, for example, the general formula (3).

[0140]

[0141] In the above general formula (3), j is an integer of 2 to 10, and is preferably 2.

[0142] The group having 4 to 12 carbon atoms and containing an epoxy group is represented by, for example, the general formula (4).

[0143] -Z 1 -Z 2 -E (4)

[0144] In the above general formula (4), Z 1 is an alkylene group or an alkylarylene group having 1 to 10 carbon atoms, and Z 2 is a methylene group, a sulfur atom, or an oxygen atom, and E is a hydrocarbon group having 2 to 10 carbon atoms and having an epoxy group. 2 is an oxygen atom, more preferably Z 2 is an oxygen atom, and E is a glycidyl group, and more preferably Z 1 is an alkylene group having 3 carbon atoms, Z 2 is an oxygen atom, and E is a glycidyl group.

[0145] In the polyorganosiloxane represented by the general formula (2), R 1 ~R 8 Among the above, an alkyl group having 1 to 6 carbon atoms is preferred as X 1 and X 4 Among the above, an alkyl group having 1 to 6 carbon atoms is preferred as X2 Among the above, a group having 4 to 12 carbon atoms and containing an epoxy group is preferred.

[0146] In the polyorganosiloxane represented by the general formula (2), X 3 , that is, a group containing 2 to 20 repeating units of alkylene glycol, for example, is represented by the following general formula (5).

[0147]

[0148] In the above general formula (5), t is an integer of 2 to 20, P is an alkylene group or an alkylarylene group having 2 to 10 carbon atoms, R is a hydrogen atom or a methyl group, and Q is an alkoxy group or an aryloxy group having 1 to 10 carbon atoms. Among them, it is preferred that t is an integer of 2 to 8, P is an alkylene group having 3 carbon atoms, R is a hydrogen atom, and Q is a methoxy group.

[0149] In the polyorganosiloxane represented by the general formula (2), m is an integer of 3-200, preferably an integer of 20-150, and more preferably an integer of 30-120.

[0150] In the polyorganosiloxane represented by the general formula (2), n is an integer of 0 to 200, preferably 0 to 150, more preferably 0 to 120. k is an integer of 0 to 200, preferably 0 to 150, more preferably 0 to 120. The total of m, n, and k is preferably 3 to 400, more preferably 3 to 300, and even more preferably 3 to 250.

[0151] The amount of the modifier used is adjusted according to the range of the coupling rate described below, but the molar amount of the functional group in the modifier capable of reacting with the active end of the conjugated diene polymer chain is usually 0.01 to 0.9 mol, preferably 0.05 to 0.8 mol, and more preferably 0.1 to 0.5 mol relative to 1 mol of the polymerization initiator used in the polymerization reaction.

[0152] These modifiers can be used alone or in combination of two or more.

[0153] In the method for producing the composition S, there is no particular limitation on the method for mixing a solution containing a conjugated diene polymer chain having an active terminal with a coupling agent and a modifier. From the viewpoint of good control of the coupling reaction and the modification reaction, a method of adding a coupling agent and a modifier to a solution containing a conjugated diene polymer chain having an active terminal is preferred. In this case, the coupling agent and the modifier are preferably dissolved in an inactive solvent and added to the polymerization system. The solution concentration is preferably in the range of 1 to 50% by mass.

[0154] The time for adding the coupling agent and the modifier to the solution containing the conjugated diene polymer chain with an active terminal is not particularly limited. It is preferred that the coupling agent and the modifier be added to the solution when the polymerization reaction is not completed and the solution containing the conjugated diene polymer chain with an active terminal still contains monomers. More specifically, the coupling agent and the modifier are added to the solution when the solution containing the conjugated diene polymer chain with an active terminal contains 100 ppm or more (more preferably 300 to 50,000 ppm) of monomers. By adding the coupling agent and the modifier in this way, the side reaction between the conjugated diene polymer chain with an active terminal and the impurities contained in the polymerization system can be suppressed, and the reaction can be well controlled.

[0155] As conditions for reacting the coupling agent and the modifier, the reaction temperature is usually in the range of 0 to 100° C., preferably 30 to 90° C., and the respective reaction times are usually in the range of 1 to 120 minutes, preferably 2 to 60 minutes.

[0156] In the method for producing composition S, the order of step (A) and step (B) is not particularly limited, and either step may be performed first or they may be performed simultaneously. However, step (A) is preferably performed before step (B).

[0157] In the method for producing the composition S, before and after step (A) and step (B), a known polymerization terminal modifier other than the coupling agent and the modifier that can react with the active terminal of the conjugated diene polymer chain can be added to the polymerization system within a range that does not impair the effects of the present invention.

[0158] In the method for producing the composition S, after reacting the coupling agent and the modifier with the conjugated diene polymer chain having an active terminal, if alcohol such as methanol or isopropanol or water is added to stop the reaction as necessary, a solution containing the composition S containing the modified butadiene rubber can be obtained.

[0159] Next, after adding an antioxidant, a crumbing agent, an antifouling agent, etc. to the polymerization solution as necessary, the solvent is separated by direct drying or stripping to recover the target composition S.

[0160] In the present invention, the composition S obtained in this way can be regarded as the above-mentioned modified butadiene rubber.

[0161] The area ratio of the peak portion having a peak top molecular weight 2.5 times or more of the peak top molecular weight of the minimum molecular weight peak detected by gel permeation chromatography (GPC) of the modified butadiene rubber to the total elution area (hereinafter also referred to as "coupling ratio") is preferably 25 to 35%.

[0162] Here, the "peak with the smallest molecular weight detected by GPC of the modified butadiene rubber" means "a peak derived from a polymer with the smallest molecular weight among the polymers contained in the modified butadiene rubber". If the coupling ratio is within the above range, the obtained composition S is less likely to flow and has excellent storage stability. In addition, the low heat build-up property of the tire finally obtained is more excellent.

[0163] The coupling ratio refers to the ratio (mass fraction) of structures in which three or more conjugated diene polymer chains are bonded via the remaining portion of the coupling agent and / or modifier after the reaction in the modified butadiene rubber, and can be measured by GPC (polystyrene conversion).

[0164] The weight average molecular weight of the modified butadiene rubber is preferably in the range of 200,000 to 800,000, more preferably 300,000 to 700,000, as a value measured by GPC in terms of polystyrene.

[0165] The molecular weight distribution of the modified butadiene rubber, represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is preferably from 1.1 to 5.0, and more preferably from 1.2 to 3.0.

[0166] The Mooney viscosity (ML) of the modified butadiene rubber 1+4 , 100°C) is preferably in the range of 30 to 75.

[0167] The vinyl bond content in the conjugated diene monomer unit portion of the modified butadiene rubber is preferably 50% by mass or less, more preferably 25% by mass or less.

[0168] 〈Silicon Dioxide〉

[0169] The silica contained in the composition of the present invention is not particularly limited, and any silica conventionally known to be compounded in rubber compositions for applications such as tires can be used.

[0170] Examples of the silica include wet silica, dry silica, fumed silica, diatomaceous earth, etc. As the silica, one type of silica may be used alone, or two or more types of silica may be used in combination.

[0171] The cetyltrimethylammonium bromide (CTAB) adsorption specific surface area of ​​the silica is not particularly limited, but is preferably 100 to 300 m2 for the reason that the effect of the present invention is more excellent. 2 / g, more preferably 150 to 250 m 2 / g.

[0172] In this specification, the CTAB adsorption specific surface area is a value obtained by measuring the amount of CTAB adsorbed on the surface of silica in accordance with JIS K6217-3:2001 "Part 3: Determination of specific surface area - CTAB adsorption method".

[0173] In the composition of the present invention, the content of silica is 20 to 100 parts by mass, preferably 30 to 90 parts by mass, and more preferably 50 to 80 parts by mass, based on 100 parts by mass of the diene rubber. This provides more excellent effects of the present invention.

[0174] 〈Solidified product (specific cured product)〉

[0175] The cured product contained in the composition of the present invention is a cured product obtained by curing a crosslinkable oligomer or polymer incompatible with the diene rubber, and has a JIS A hardness of 3 to 45 (hereinafter also referred to as a "specific cured product").

[0176] The phrase “incompatible with (the above-mentioned diene rubber)” does not mean that it is incompatible with all rubber components contained in the above-mentioned diene rubber, but means that the above-mentioned diene rubber and each specific component used in the above-mentioned crosslinkable oligomer or polymer are incompatible with each other.

[0177] That is, the crosslinkable oligomer or polymer only needs to be incompatible with the components actually contained in the diene rubber, and does not need to be incompatible with the rubber components not actually contained in the diene rubber (for example, the above-mentioned "other rubber components"). For example, in the case of the examples described later, since the diene rubber is composed of natural rubber and modified butadiene rubber, the crosslinkable polymer only needs to be incompatible with the natural rubber and the modified butadiene rubber.

[0178] The "cured product obtained by curing" refers to a cured product obtained by curing a crosslinkable oligomer or polymer before mixing and preparing the composition of the present invention.

[0179] The "JIS A hardness" refers to the durometer hardness specified in JIS K6253-3:2012, and is the hardness measured at a temperature of 25°C using a type A durometer.

[0180] 《Crosslinking oligomers or polymers》

[0181] The crosslinkable oligomer or polymer is not particularly limited as long as it is incompatible with the diene rubber and has crosslinkability.

[0182] The so-called "compatible" means that two (or more) different molecular chains are uniformly compatible at the molecular level (completely mixed at the molecular level). On the contrary, the so-called "incompatible" means that they are completely unmixable at the molecular level.

[0183] Examples of the crosslinkable oligomer or polymer include polyether-based, polyester-based, polyolefin-based, polycarbonate-based, aliphatic-based, saturated hydrocarbon-based, acrylic-based, plant-derived, or silicone-based polymers or copolymers.

[0184] Among them, from the viewpoints of thermal stability, flexibility of the molecular chain, hydrolysis resistance, and the like, the crosslinkable oligomer or polymer is preferably a polyether-based or siloxane-based polymer or copolymer.

[0185] Examples of the polyether-based polymer or copolymer include polyethylene glycol, polypropylene glycol (PPG), polyglycerol, ethylene oxide / propylene oxide copolymer, polytetramethylene ether glycol (PTMEG), and sorbitol-based polyols.

[0186] Examples of the siloxane-based polymer or copolymer include a main chain having -(Si(R 1 )(R 2 )O)-shown siloxane structure (wherein R 1 and R 2 Each independently represents an alkyl group having 1 to 4 carbon atoms or a phenyl group. )

[0187] The crosslinkable oligomer or polymer preferably has a silane functional group because a cured product can be easily formed by crosslinking between molecules.

[0188] The above-mentioned silane functional group is also called a so-called crosslinkable silyl group, and specific examples thereof include a hydrolyzable silyl group; a silanol group; a functional group in which the silanol group is substituted with an acetoxy derivative, an enoyloxy derivative, an oxime derivative, an amine derivative, etc.; and the like.

[0189] Specific examples of the hydrolyzable silyl group include an alkoxysilyl group, an alkenyloxysilyl group, an acyloxysilyl group, an aminosilyl group, an aminooxysilyl group, an oximesilyl group, and an amidesilyl group.

[0190] Among them, an alkoxysilyl group is preferred because a good balance between hydrolyzability and storage stability is achieved. Specifically, an alkoxysilyl group represented by the following formula (X) is more preferred, and a methoxysilyl group and an ethoxysilyl group are further preferred.

[0191]

[0192] In formula (X), R 1 represents an alkyl group having 1 to 4 carbon atoms, R 2represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and a represents an integer of 1 to 3. When a is 2 or 3, a plurality of R 1 They can be the same or different. When a is 1, multiple R 1 They may be the same or different, respectively.

[0193] The crosslinkable oligomer or polymer preferably has the silane functional group at least at the end of the main chain, and preferably has 1.5 or more silane functional groups when the main chain is linear, more preferably has 2 or more silane functional groups, while preferably has 3 or more silane functional groups when the main chain is branched.

[0194] The weight average molecular weight or number average molecular weight of the crosslinkable oligomer or polymer is preferably 300 to 30,000, more preferably 2,000 to 20,000 because the dispersibility of the obtained cured product in the diene rubber and the kneading processability of the rubber composition are improved.

[0195] Both the weight average molecular weight and the number average molecular weight are measured by gel permeation chromatography (GPC) and are converted to standard polystyrene.

[0196] The curing method for curing the crosslinkable oligomer or polymer is not particularly limited, and examples thereof include a method of curing using at least one catalyst selected from an acid catalyst, a base catalyst, a metal catalyst, and an amine catalyst.

[0197] Among them, the method of curing using an acid catalyst or a metal catalyst is preferred because of its high curing efficiency.

[0198] Specific examples of the acid catalyst include lactic acid, phthalic acid, lauryl acid, oleic acid, linoleic acid, linolenic acid, cycloalkane acid, octenic acid, octanoic acid (2-ethylhexanoic acid), formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, octanoic acid, capric acid, lauric acid, myristic acid, benzoic acid, oxalic acid, malic acid, and citric acid. These may be used alone or in combination of two or more.

[0199] As the acid catalyst, an acid that is liquid at room temperature is preferably used from the viewpoint of acidity and dispersibility, and specifically, lactic acid and formic acid are more preferably used.

[0200] Examples of the metal catalyst include organic metal compounds such as tin octylate and alkali metal alkoxides.

[0201] Specifically, there can be mentioned tin carboxylates such as dimethyltin dilaurate, dibutyltin dilaurate, dibutyltin maleate, dibutyltin diacetate, tin octoate, and tin cyclohexaneate; titanates such as tetrabutyl titanate and tetrapropyl titanate; organoaluminum compounds such as aluminum triacetylacetonate, triethyl aluminum acetylacetate, and diisopropoxyethyl aluminum acetylacetate; chelates such as zirconium tetraacetylacetonate and titanium tetraacetylacetonate; metal octanoates such as lead octanoate and bismuth octanoate; and the like.

[0202] As the metal catalyst, tin carboxylates are more preferably used from the viewpoint of acidity.

[0203] The hardness of the cured product is 3 to 45, preferably 3 to 20, and more preferably 3 to 15 in JIS A hardness.

[0204] Regarding the average particle size of the above-mentioned solidified material in the composition of the present invention prepared by mixing the above-mentioned solidified material, it is preferably a granular material with an average particle size of 5 to 250 μm, because the dispersibility in the above-mentioned diene rubber becomes good and the ice performance and wear resistance of the studless tire become better.

[0205] The average particle size of the cured product in the composition of the present invention refers to the maximum length of particles of the cured product observed by image analysis of a cross section of a vulcanized test specimen of the composition of the present invention using an electron microscope (magnification: about 500 to 2000 times), and is a value measured using any 10 or more particles and averaged.

[0206] In the composition of the present invention, the content of the cured product is 0.3 to 30 parts by mass, preferably 0.5 to 25 parts by mass, and more preferably 1 to 15 parts by mass, based on 100 parts by mass of the diene rubber, because the effects of the present invention are more excellent.

[0207] 〈Optional Ingredients〉

[0208] The composition of the present invention may further contain other components (optional components) as necessary within a range not impairing the effects and purposes thereof.

[0209] Examples of the optional components include carbon black, silane coupling agents, aromatic modified terpene resins, heat-expandable microcapsules, fillers, zinc oxide (zinc white), stearic acid, antioxidants, waxes, processing aids, oils, liquid polymers, thermosetting resins, vulcanizers (e.g., sulfur), vulcanization accelerators, and various additives generally used in rubber compositions.

[0210] 《Aromatic modified terpene resin》

[0211] The composition of the present invention may further contain an aromatic modified terpene resin.

[0212] Because the effects of the present invention are more excellent, the aromatic modified terpene resin preferably has a softening point of 60 to 150° C. Because the effects of the present invention are more excellent, the softening point is more preferably 100 to 140° C.

[0213] Here, the softening point is the Vicat softening point measured in accordance with JIS K7206:1999.

[0214] In the composition of the present invention, the content of the aromatic modified terpene resin is not particularly limited, but is preferably 2 to 20 parts by mass, more preferably 5 to 15 parts by mass, based on 100 parts by mass of the diene rubber, because the effects of the present invention are more excellent.

[0215] 《Thermal expandable microcapsules》

[0216] The composition of the present invention may further contain heat-expandable microcapsules.

[0217] The heat-expandable microcapsules are heat-expandable thermoplastic resin particles in which a liquid that is vaporized by heat to generate a gas is enclosed in a thermoplastic resin, and the particles are heated at a temperature above their expansion start temperature, usually at a temperature of 130 to 190° C. to expand them, thereby forming gas-enclosed thermoplastic resin particles in which a gas is enclosed in an outer shell formed of the thermoplastic resin.

[0218] In the above-mentioned thermoplastic resin, the expansion start temperature is preferably 100° C. or higher, more preferably 120° C. or higher, and the maximum expansion temperature is preferably 150° C. or higher, more preferably 160° C. or higher.

[0219] As the thermoplastic resin, for example, a polymer of (meth)acrylonitrile and a copolymer having a high (meth)acrylonitrile content are preferably used. As other monomers (comonomers) in the case of the copolymer, monomers such as vinyl halide, vinylidene halide, styrene monomers, (meth)acrylate monomers, vinyl acetate, butadiene, vinyl pyridine, and chloroprene are used.

[0220] The thermoplastic resin can be crosslinked by a crosslinking agent such as divinylbenzene, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, 1,3-butanediol di(meth)acrylate, allyl(meth)acrylate, 1,3,5-triacryloylhexahydro-1,3,5-triazine, and triallyl isocyanurate. The crosslinked form is preferably uncrosslinked, but may be partially crosslinked to the extent that the properties as a thermoplastic resin are not impaired.

[0221] Examples of the liquid that generates gas by vaporization using heat include hydrocarbons such as n-pentane, isopentane, neopentane, butane, isobutane, hexane, and petroleum ether; chlorinated hydrocarbons such as methyl chloride, dichloromethane, dichloroethylene, trichloroethane, and trichloroethylene; and the like.

[0222] The heat-expandable microcapsules are not particularly limited as long as they expand by heat to become gas-encapsulated thermoplastic resin heat-expandable microcapsules, and one type may be used alone or two or more types may be used in combination.

[0223] The particle size of the heat-expandable microcapsule before expansion is preferably 5 to 300 μm, more preferably 10 to 200 μm.

[0224] As the heat-expandable microcapsule, commercially available products can be used, and specific examples thereof include EXPANCEL 091DU-80 and EXPANCEL 092DU-120 manufactured by EXPANCEL Co., Ltd.; and Microsfea F-85 and Microsfea F-100 manufactured by Matsumoto Oil & Fats Co., Ltd.; and the like.

[0225] In the composition of the present invention, the content of the heat-expandable microcapsules is not particularly limited, but is preferably 0.5 to 20 parts by mass, more preferably 1 to 10 parts by mass, based on 100 parts by mass of the diene rubber.

[0226] Carbon Black

[0227] The composition of the present invention may further contain carbon black.

[0228] The carbon black is not particularly limited, and various grades of carbon black such as SAF-HS, SAF, ISAF-HS, ISAF, ISAF-LS, IISAF-HS, HAF-HS, HAF, HAF-LS, and FEF may be used.

[0229] The nitrogen adsorption specific surface area (N2SA) of the carbon black is not particularly limited, but is preferably 50 to 200 m2 for the reason that the effect of the present invention is more excellent. 2 / g, more preferably 70 to 150 m 2 / g.

[0230] The nitrogen adsorption specific surface area (N2SA) is a value obtained by measuring the amount of nitrogen adsorbed on the surface of carbon black in accordance with JIS K6217-2:2001 "Part 2: Determination of specific surface area - Nitrogen adsorption method - Single point method".

[0231] The content of the carbon black is not particularly limited, but is preferably 1 to 200 parts by mass, more preferably 10 to 100 parts by mass, based on 100 parts by mass of the diene rubber.

[0232] 《Silane coupling agent》

[0233] The composition of the present invention may further contain a silane coupling agent.

[0234] The silane coupling agent is not particularly limited as long as it is a silane compound having a hydrolyzable group and an organic functional group.

[0235] The hydrolyzable group is not particularly limited, and examples thereof include alkoxy, phenoxy, carboxyl, alkenyloxy, etc. Among them, alkoxy is preferred. When the hydrolyzable group is an alkoxy, the number of carbon atoms of the alkoxy is preferably 1 to 16, more preferably 1 to 4. Examples of the alkoxy having 1 to 4 carbon atoms include methoxy, ethoxy, propoxy, etc.

[0236] The organic functional group is not particularly limited, but is preferably a group capable of forming a chemical bond with an organic compound, and examples thereof include epoxy, vinyl, acryloyl, methacryloyl, amino, and mercapto groups, among which mercapto groups are preferred.

[0237] The silane coupling agents may be used alone or in combination of two or more.

[0238] The silane coupling agent is preferably a sulfur-containing silane coupling agent.

[0239] Specific examples of the silane coupling agent include bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)disulfide, mercaptopropyltrimethoxysilane, mercaptopropyltriethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl-tetrasulfide, trimethoxysilylpropyl-mercaptobenzothiazole tetrasulfide, triethoxysilylpropyl-methacrylate-monosulfide, and dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl-tetrasulfide. Any of these agents may be used alone or in combination of two or more.

[0240] In the composition of the present invention, the content of the silane coupling agent is not particularly limited, but is preferably 2 to 20% by mass, more preferably 5 to 15% by mass, relative to the content of the above-mentioned silica.

[0241] <Method for producing rubber composition for tire tread>

[0242] The method for producing the composition of the present invention is not particularly limited, and specific examples thereof include a method of kneading the above-mentioned components using a known method or apparatus (eg, a Banbury mixer, a kneader, a roll, etc.).

[0243] When the composition of the present invention contains sulfur or a vulcanization accelerator, it is preferred that the sulfur and components other than the vulcanization accelerator are first mixed at a high temperature (preferably 100 to 155° C.), and then the sulfur or the vulcanization accelerator is mixed after cooling.

[0244] The composition of the present invention can be vulcanized or crosslinked under conventionally known vulcanization or crosslinking conditions.

[0245] The composition of the present invention is excellent in on-ice performance, wet grip performance, low heat build-up and wear resistance and is therefore particularly suitable for studless tires.

[0246] [Pneumatic tires]

[0247] The pneumatic tire of the present invention is a pneumatic tire using the above-mentioned composition of the present invention. Among them, a pneumatic tire using the composition of the present invention for the tread is preferred.

[0248] Figure 1 FIG. 1 is a partial cross-sectional schematic diagram of a tire showing an example of an embodiment of a pneumatic tire of the present invention, but the pneumatic tire of the present invention is not limited to Figure 1 The form shown.

[0249] exist Figure 1 In the figure, reference numeral 1 denotes a bead portion, reference numeral 2 denotes a sidewall portion, and reference numeral 3 denotes a tire tread portion.

[0250] A carcass layer 4 in which fiber cords are embedded is mounted between the pair of left and right bead portions 1. The end of the carcass layer 4 is folded back around a bead core 5 and a bead filler 6 from the inside of the tire to the outside and rolled up.

[0251] In the tire tread portion 3 , a belt layer 7 is disposed outside the carcass layer 4 over the entire circumference of the tire.

[0252] A rim cushion 8 is disposed at a portion of the bead portion 1 that contacts the rim.

[0253] The tire tread portion 3 is formed from the above-mentioned composition of the present invention.

[0254] The pneumatic tire of the present invention can be manufactured, for example, by a conventionally known method. As the gas filled in the tire, in addition to normal air or air with an adjusted oxygen partial pressure, an inert gas such as nitrogen, argon, or helium can be used.

[0255] Example

[0256] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited thereto.

[0257] <Synthesis of modified butadiene rubber 1>

[0258] In an autoclave with a stirrer, 5670 g of cyclohexane, 700 g of 1,3-butadiene, and 0.17 mmol of tetramethylethylenediamine were added under a nitrogen atmosphere, and n-butyl lithium was added in an amount required to neutralize the impurities contained in cyclohexane and 1,3-butadiene that hindered polymerization. Furthermore, n-butyl lithium was added in an amount of 8.33 mmol used for the polymerization reaction, and polymerization was started at 50°C. After 20 minutes after the start of polymerization, 300 g of 1,3-butadiene was continuously added for 30 minutes. The highest temperature in the polymerization reaction was 80°C. After the continuous addition was completed, the polymerization reaction was further continued for 15 minutes, and after confirming that the polymerization conversion rate became in the range of 95% to 100%, a small amount of the polymerization solution was sampled. For the small amount of polymerization solution sampled, excess methanol was added to stop the reaction, and then air-dried to obtain the polymer as a sample for GPC analysis. Using this sample, the peak top molecular weight and molecular weight distribution of the polymer (corresponding to the conjugated diene polymer chain having an active terminal) were measured and the results were "230,000" and "1.04", respectively.

[0259] Immediately after sampling a small amount of the polymerization solution, 0.288 mmol (corresponding to 0.0345 times the mole of n-butyllithium used for polymerization) of 1,6-bis(trichlorosilyl)hexane was added to the polymerization solution in the form of a 40 wt% cyclohexane solution, and the mixture was reacted for 30 minutes.

[0260] Furthermore, 0.0382 mmol (corresponding to 0.00459 times the mole of n-butyllithium used for polymerization) of polyorganosiloxane A (the values ​​of m and k are average values) represented by the following formula (6) was added in the form of a 20 wt % xylene solution and reacted for 30 minutes.

[0261] Then, as a polymerization terminator, methanol was added in an amount equivalent to 2 times the molar amount of n-butyl lithium used. Thus, a solution containing modified butadiene rubber 1 was obtained. After adding 0.2 parts of 2,4-bis(n-octylthiomethyl)-6-methylphenol as an antioxidant to the solution for every 100 parts of rubber components, the solvent was removed by steam stripping, and vacuum dried at 60°C for 24 hours to obtain solid modified butadiene rubber 1 (composition S). Regarding the modified butadiene rubber 1 (composition S), the weight average molecular weight, molecular weight distribution, coupling rate, vinyl bond content and Mooney viscosity were measured, and the results were "510,000", "1.46", "28%, "11% by mass" and "46", respectively.

[0262]

[0263] <Synthesis of modified butadiene rubber 2>

[0264] 0.112 mol of 3-aminopropyltrimethoxysilane and 0.123 mol of methyl isopropyl ketone were stirred at room temperature for 2 days under a nitrogen atmosphere, and methanol and unreacted methyl isopropyl ketone were removed from the resulting reaction solution under vacuum to synthesize a ketiminesilane condensate having an average condensation degree of 2.4.

[0265] Cyclohexane, 9.215 mol of butadiene and 5.464 mol of 1,1,4,4-tetramethylethylenediamine were added to a 10 L autoclave reactor that had been substituted with nitrogen, and stirring was started. After the temperature of the contents in the reactor was set to 50°C, 4.856 mol of n-butyl lithium was added. After the polymerization addition rate reached 100%, a toluene solution of the ketimine silane condensate synthesized above was added and stirred for 1 hour, and 0.5 mL of methanol was further added and stirred for 30 minutes. A small amount of antioxidant (Ilganox 1520 manufactured by Chiba Spesialty Chemicals Co., Ltd.) was added to the resulting polymer solution, and the solvent was removed by concentrating under reduced pressure. The polymer was coagulated in methanol, washed, and dried to obtain a solid modified butadiene rubber 2.

[0266] 〈Synthesis of specific cured products〉

[0267] 0.1 parts by mass of lactic acid (acid catalyst) was added to 10 parts by mass of a paste product of hydrolyzable silyl-terminated polyoxypropylene glycol (polypropylene glycol having a hydrolyzable silyl group at a terminal) (MS polymer S810, manufactured by Kaneka Corporation) (crosslinking polymer).

[0268] Next, after sufficient stirring, the mixture was cured at room temperature for 2 days to synthesize a specific cured product.

[0269] The JIS A hardness of the obtained specific cured product 1 was 8. The average particle size of the specific cured product in the vulcanized rubber test piece described later was 38 μm.

[0270] <Preparation of rubber composition for tire tread>

[0271] The components shown in the following Table 1 were blended in the ratios (parts by mass) shown in the table.

[0272] Specifically, first, the components other than sulfur and a vulcanization accelerator among the components shown in the following Table 1 were heated to about 150° C. using a 1.7-liter closed Banbury mixer, mixed for 5 minutes, then discharged, and cooled to room temperature to obtain a masterbatch. Furthermore, sulfur and a vulcanization accelerator were mixed with the obtained masterbatch using the Banbury mixer to obtain a rubber composition for tire treads.

[0273] <evaluate>

[0274] 《Processability (viscosity)》

[0275] The obtained tire tread rubber composition was measured according to JIS K6300 using a Mooney viscometer and an L-type rotor (38.1 mm diameter, 5.5 mm thickness) at a preheating time of 1 minute, a rotor rotation time of 4 minutes, 100° C., and 2 rpm. The obtained results were expressed as an index when the value of Standard Example 1 was set to 100. The smaller the index, the smaller the viscosity and the better the molding processability. The index is preferably 115 or less.

[0276] Furthermore, the obtained rubber composition for tire tread was press-vulcanized in a predetermined mold at 170° C. for 10 minutes to prepare a vulcanized rubber test piece. Furthermore, the following evaluations were performed on the obtained vulcanized rubber test piece.

[0277] 《On-ice performance》

[0278] The vulcanized rubber test piece was attached to a flat cylindrical base rubber and tested using an inside drum type ice friction tester at a temperature of -1.5°C and a load of 5.5 kg / cm 3 , The friction coefficient on ice was measured under the condition of drum rotation speed: 25km / h.

[0279] The results are shown in Table 1 ("Ice Performance" column in Table 1). The results are expressed as an index when the coefficient of friction on ice of the standard example is set to 100. The larger the index, the greater the friction between rubber and ice, and the better the ice performance when the tire is made.

[0280] 《tanδ(0℃)》

[0281] About the vulcanized rubber test piece, tan δ (0°C) was measured under the conditions of tensile strain rate 10%±2%, frequency 20 Hz and temperature 0°C using a viscoelasticity spectrophotometer (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with JIS K6394:2007.

[0282] The results are shown in Table 1 ("tan δ (0°C)" column in Table 1). The results are expressed as an index with the tan δ (0°C) of the standard example being 100. The larger the index, the larger the tan δ (0°C), and the more excellent the wet grip performance when the tire is manufactured.

[0283] 《tanδ(60℃)》

[0284] The tan δ (60°C) of the vulcanized rubber test piece was measured in the same procedure as the above-mentioned tan δ (0°C) except that the measurement was performed at 60°C instead of at 0°C.

[0285] The results (the inverse of tan δ (60°C)) are shown in Table 1 (the "tan δ (60°C)" column in Table 1). The results are expressed as an index when the inverse of tan δ (60°C) of the standard example is 100. The larger the index, the smaller the tan δ (60°C), and the better the low heat build-up property when the tire is made.

[0286] 《Abrasion resistance》

[0287] The vulcanized rubber test piece was tested using a Lamborn abrasion tester (manufactured by Iwamoto Seisakusho Co., Ltd.) in accordance with JIS K6264-2:2005 at an applied force of 4.0 kg / cm 3 The wear test was conducted under the conditions of (=39N), sliding rate 30%, wear test time 4 minutes, and test temperature at room temperature, and the wear quality was measured. In addition, the index was calculated as follows. The results are shown in Table 1. The larger the index, the smaller the wear amount and the better the wear resistance.

[0288] Index = (wear mass of the test piece of the standard example / wear mass of each example) × 100

[0289]

[0290] The details of each component in Table 1 are as follows.

[0291] Natural rubber: TSR20 (natural rubber, Tg: -62°C)

[0292] Comparative butadiene rubber: NIPOL BR1220 (unmodified BR, manufactured by Nippon Zeon Co., Ltd.)

[0293] Modified butadiene rubber 1: Modified butadiene rubber 1 synthesized as described above

[0294] Modified butadiene rubber 2: Modified butadiene rubber 2 synthesized as described above

[0295] ·Carbon black: Sewage Fluid N339 (manufactured by Siberian Co., Ltd.)

[0296] ·Silica: ZEOSIL 1165MP (CTAB adsorption specific surface area: 159m 2 / g, manufactured by Roroman Co., Ltd.)

[0297] Silane coupling agent: Si69 (bis(3-triethoxysilylpropyl)tetrasulfide, manufactured by Ebonick Degussa Co., Ltd.)

[0298] ·Fragrance oil: Ekostor No. 4S (manufactured by Showa Seiko Oil Co., Ltd.)

[0299] · Specific cured product: The specific cured product synthesized as described above

[0300] ·Aromatic modified terpene resin: YSレジンTO-125 (softening point: 125±5℃, manufactured by YSスハラケミカル Co., Ltd.)

[0301] Thermally expandable microcapsules: Microspheres F100 (manufactured by Matsumoto Oil & Fats Co., Ltd.)

[0302] Sulfur: Jinhua ink-infused micro-powdered sulfur (sulfur content 95.24% by mass, manufactured by Tsurumi Chemical Industry Co., Ltd.)

[0303] ·Stearic acid: stearic acid (manufactured by NOF Corporation)

[0304] Zinc oxide: 3 types of zinc oxide (manufactured by Shodo Chemical Industry Co., Ltd.)

[0305] Vulcanization accelerator 1: Noxelara CZ-G (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)

[0306] Vulcanization accelerator 2: Soxhinolide DG (manufactured by Sumitomo Chemical Co., Ltd.)

[0307] As shown in Table 1, Examples 1 to 5 in which the modified butadiene rubber and the specific cured product were used in combination exhibited excellent performance on ice, wet grip performance, low heat build-up, and wear resistance.

[0308] When Example 2 is compared with Example 3, Example 2 containing the aromatic modified terpene resin exhibits more excellent wet grip performance.

[0309] When Examples 1 to 4 are compared, Examples 1 to 3 in which the silica content is 50 parts by mass or more exhibit more excellent performance on ice and wet grip performance.

[0310] Comparing Examples 1 to 4 with Example 5, Examples 1 to 4 using modified butadiene rubber 1 in which a polyorganosiloxane group is bonded to a butadiene chain via a hydrocarbon-based linking group (or a hydrocarbon-based linking group and a silicon-containing linking group) in the modified butadiene rubber exhibited more excellent processability.

[0311] On the other hand, in Standard Example 1 and Comparative Examples 1 to 5 in which the modified butadiene rubber and the specific cured product were not used in combination, and Comparative Example 6 in which the modified butadiene rubber and the specific cured product were used in combination but the silica content was less than 20 parts by mass, at least any one of the on-ice performance, wet grip performance, low heat build-up properties, and wear resistance was insufficient.

[0312] Explanation of symbols

[0313] 1: Bead

[0314] 2: Sidewall

[0315] 3: Tire tread

[0316] 4: Carcass layer

[0317] 5: Bead core

[0318] 6: Bead filler

[0319] 7: Belt

[0320] 8: Rim buffer.

Claims

1. A rubber composition for tire tread, comprising diene rubber, silica, and a cured product. The content of the silica is 20 to 100 parts by mass based on 100 parts by mass of the diene rubber, and the content of the cured product is 0.3 to 30 parts by mass based on 100 parts by mass of the diene rubber. The diene rubber contains natural rubber and modified butadiene rubber having a polyorganosiloxane group at the end, wherein the content of the natural rubber in the diene rubber is 30 to 90% by mass, and the content of the modified butadiene rubber in the diene rubber is 10 to 70% by mass. The butadiene chain of the modified butadiene rubber contains 100% by mass of butadiene monomer units. The cured product is a cured product obtained by curing a cross-linkable oligomer or polymer that is incompatible with the diene rubber, and the JIS A hardness of the cured product is 3 to 45. The polyorganosiloxane group is a group bonded to the end of a butadiene chain via a linking group or an ether group, wherein the linking group is formed by a divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent; in, A portion of the -CH2- that constitutes the linking group formed by the divalent hydrocarbon group having 1 to 20 carbon atoms that may have a substituent may be replaced by -O-; Furthermore, between the linking group formed by the divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent and the terminal of the butadiene chain, there exists a silicon-containing linking group represented by the following general formula (Si): *1-Q 1 -Si(R L1 )2-A 1 -Si(R L2 )2-Q 2 -*2(Si) In the general formula (Si), Q 1 and Q 2 Each is independently a chemical single bond or -O-; R L1 and R L2 Each independently represents a substituent, and multiple R L1 and R L2 Each may be the same, or may be different; A 1 A chemical single bond with 1 to 20 carbon atoms, namely (CH2) k , an arylene group having 6 to 20 carbon atoms, or a cycloalkylene group having 5 to 20 carbon atoms, wherein k is an integer of 1 to 20; *1 is the position that is bonded to *2 in other silicon-containing linking groups, or the position that is bonded to the linking group formed of the divalent hydrocarbon group having 1 to 20 carbon atoms which may have a substituent; *2 is a position that bonds to *1 in other silicon-containing linking groups, or a position that bonds to the terminal of the butadiene chain. 2 . The rubber composition for tire tread according to claim 1 , wherein the cured product is a particulate material having an average particle diameter of 5 to 250 μm. 3 . The rubber composition for a tire tread according to claim 1 , wherein the crosslinkable oligomer or polymer is a polyether-based or siloxane-based polymer or copolymer and has a silane functional group.

4. The rubber composition for tire tread according to claim 1 or 2, further comprising an aromatic modified terpene resin having a softening point of 60 to 150°C, The content of the aromatic modified terpene resin is 2 to 20 parts by mass based on 100 parts by mass of the diene rubber.

5. The rubber composition for tire tread according to claim 1 or 2, further comprising heat-expandable microcapsules, The content of the heat-expandable microcapsules is 0.5 to 20 parts by mass based on 100 parts by mass of the diene rubber. 6 . A pneumatic tire, wherein the rubber composition for a tire tread according to claim 1 is used for the tread.