Method for preparing capacitor hole of semiconductor memory
Through the combination of pitch doubling technology and multi-layer structure, the problem of uneven size and holes in semiconductor memory capacitor holes in small-size preparation is solved, shrinkage and uniformity in the 30nm and below process are achieved, and the density and density of the device are improved. Accuracy.
Patent Information
- Application Number
- CN201810654407.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-06-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2038-06-22
AI Technical Summary
It is difficult to prepare semiconductor memory capacitor holes smaller than 30nm with the existing technology, and there are problems of uneven size and sidewall feature size holes, which limits the size reduction and density increase of integrated circuits.
Using pitch multiplication technology, a multi-layer structure is formed on the semiconductor substrate, including an ashesable hard mask layer and a diamond-like film layer, for multi-directional etching and pattern transfer, and a spacer sacrificial layer and a filling mask layer are used for pattern correction. and shrink to form evenly spaced capacitor holes.
It achieves pattern shrinkage and uniformity of capacitor holes in the 30nm and below processes, improves the accuracy and density of the device structure, solves the problem of uneven size and hole size, and improves the preparation quality of capacitor holes.
Smart Images

Figure CN110634733B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor device manufacturing, and in particular relates to a method for preparing a semiconductor memory capacitor hole. Background Art
[0002] Dynamic Random Access Memory (DRAM) is a commonly used semiconductor memory device in computers, which consists of many repeated storage units. Each storage unit usually includes a capacitor and a transistor; the gate of the transistor is connected to the word line, the drain / source of the transistor is connected to the bit line, and the source / drain of the transistor is connected to the capacitor; the voltage signal on the word line can control the opening or closing of the transistor, and then read the data information stored in the capacitor through the bit line, or write the data information into the capacitor through the bit line for storage.
[0003] As the semiconductor industry has grown, the size of integrated circuits has continued to decrease due to a number of factors, including the need for increased portability, computing power, storage capacity, and energy efficiency in modern electronic devices. To aid in this size reduction, methods continue to be developed to reduce the size of component features of integrated circuits, examples of which include capacitors, electrical contacts, interconnects, and other electrical devices. The trend toward reduced feature size is particularly evident in memory circuits or devices, such as dynamic random access memory (DRAM) or static random access memory (SRAM).
[0004] There is an increasing demand for ever-decreasing feature sizes, and correspondingly, increasing requirements are placed on the techniques used to form the features. In addition, the concept of pitch can be used to describe the size of these features, and the pitch is the distance between the same points in two adjacent features. Currently, some photoresist materials only respond to certain wavelengths. A common wavelength range that can be used is the ultraviolet (UV) range. Because many photoresist materials selectively respond to specific wavelengths, each photolithography technique has a minimum pitch. However, below the minimum pitch, a particular photolithography technique cannot reliably form features. This minimum pitch is usually determined by the wavelength of light that can be used with the technique. Therefore, the minimum pitch of the photolithography technique may limit the reduction of feature size. Therefore, there is a need to reduce the size of integrated circuits and increase the operational density of arrays of electrical devices on computer chips. There is a need to provide improved methods for forming smaller features, improved methods for increasing feature density, methods that will produce more efficient arrays, and technologies that will provide more compact arrays without compromising feature resolution.
[0005] Therefore, it is necessary to provide a method for preparing a semiconductor memory capacitor hole to solve the above problems in the prior art. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a semiconductor memory capacitor hole, which is used to solve the problems in the prior art that miniaturized semiconductor structures are difficult to prepare, have uneven sizes and inaccurate graphics, and have holes of different sidewall feature sizes.
[0007] To achieve the above-mentioned and other related purposes, the present invention provides a method for preparing a semiconductor memory capacitor hole structure, comprising the following steps:
[0008] 1) providing a semiconductor substrate, and sequentially forming a capacitor support sacrificial structure layer, a hard mask consumption layer, a double pattern integration layer, a first pattern migration layer and a first mask layer on the semiconductor substrate, wherein the first mask layer comprises at least one of an ashing hard mask layer (AHM) and a diamond-like carbon film layer (DLC);
[0009] 2) forming a first pattern layer arranged along a first direction on the first mask layer, wherein the first pattern layer comprises a plurality of first pattern units arranged in parallel and at intervals;
[0010] 3) transferring the pattern on the first pattern layer to the first pattern migration layer via the first mask layer to form a second pattern layer, wherein the second pattern layer includes a plurality of second pattern units arranged in parallel and at intervals;
[0011] 4) forming a first spacer sacrificial layer on the top, sidewalls and the surface of the double pattern integration layer between the second pattern units, forming a first gap groove on the surface of the first spacer sacrificial layer between adjacent second pattern units, and forming a first filling mask layer on the surface of the first spacer sacrificial layer, wherein the first filling mask layer covers the first spacer sacrificial layer and fills the first gap groove;
[0012] 5) removing the first lateral portion of the first spacer sacrificial layer located at the top of the second pattern unit, the first filling mask layer and a portion of the first filling mask layer located in the first gap groove, wherein a size defining unit and a pattern auxiliary unit located between the size defining units are formed between adjacent second pattern units, the first longitudinal portion of the first spacer sacrificial layer located on the sidewall of the second pattern unit forms the size defining unit, and the second lateral portion of the first spacer sacrificial layer located on the double pattern integration layer and the remaining first filling mask layer located on the second lateral portion form the pattern auxiliary unit;
[0013] 6) forming an etch stop layer, a second pattern migration layer and a second mask layer in sequence on the structure obtained in step 5);
[0014] 7) forming a third pattern layer arranged along a second direction on the second mask layer, wherein the third pattern layer comprises a plurality of third pattern units arranged in parallel and spaced apart, wherein the second direction and the first direction have an intersection angle;
[0015] 8) transferring the pattern on the third pattern layer to the second pattern migration layer via the second mask layer to form a fourth pattern layer, wherein the fourth pattern layer includes a plurality of fourth pattern units arranged in parallel and at intervals;
[0016] 9) forming a second spacer sacrificial layer on the top and sidewalls of the four pattern units and on the surface of the etch stop layer between the fourth pattern units, and forming a second gap groove on the surface of the second spacer sacrificial layer between adjacent fourth pattern units, and forming a second filling mask layer on the surface of the second spacer sacrificial layer, wherein the second filling mask layer covers the second spacer sacrificial layer and fills the second gap groove;
[0017] 10) planarizing the structure obtained in step 9) until the top surface of the second sacrificial spacer layer is exposed, and the remaining second filling mask layer between the second longitudinal portions of the second sacrificial spacer layer on the sidewalls of the fourth pattern unit is retained;
[0018] 11) etching and removing the third transverse portion and the second longitudinal portion of the second spacer sacrificial layer located at the top of the fourth pattern unit to expose the etch stop layer and obtain a fifth pattern layer, wherein the fifth pattern layer comprises a plurality of fifth pattern units arranged in parallel and spaced apart, wherein the fourth pattern unit located on the etch stop layer, the fourth transverse portion of the second spacer sacrificial layer located on the surface of the etch stop layer, and the remaining second filling mask layer located on the fourth transverse portion constitute a stacked layer forming the fifth pattern unit;
[0019] 12) using the fifth pattern unit as a mask, selectively etching away the etch stop layer and the dimension defining unit, so as to transfer the pattern on the fifth pattern layer to the second pattern layer, so as to form a pattern transfer layer on the double pattern integration layer, wherein the pattern transfer layer comprises a plurality of first spacing multiplication units arranged in parallel and spaced apart along the first direction, and a plurality of second spacing multiplication units arranged in parallel and spaced apart along the second direction and connected to the first spacing multiplication units, wherein the first spacing multiplication unit is composed of the second pattern unit and the pattern auxiliary unit, and the second spacing multiplication unit is formed by transferring the fifth pattern unit; and
[0020] 13) Transferring the pattern on the pattern transfer layer to the hard mask consuming layer via the double pattern integration layer to obtain a patterned hard mask consuming layer, and etching the capacitor support sacrificial structure layer based on the patterned hard mask consuming layer to form a plurality of semiconductor memory capacitor holes evenly spaced in the capacitor support sacrificial structure layer.
[0021] As a preferred solution of the present invention, in step 1), the double-pattern integration layer includes a first pad layer, a second pad layer, a third pad layer and a fourth pad layer from bottom to top.
[0022] As a preferred embodiment of the present invention, the material of the first pad layer includes any one of silicon oxide and tetraethyl orthosilicate (TEOS), and the thickness of the first pad layer is between 100nm and 500nm; the material of the second pad layer includes any one of amorphous silicon, silicon oxynitride and silicon nitride, and the thickness of the second pad layer is between 100nm and 800nm; the material of the third pad layer includes any one of silicon oxide and tetraethyl orthosilicate layer, and the thickness of the third pad layer is between 100nm and 500nm; the material of the fourth pad layer includes any one of amorphous silicon, silicon oxynitride and silicon nitride, and the thickness of the fourth pad layer is between 50nm and 200nm.
[0023] As a preferred solution of the present invention, before step 13) transferring the pattern on the pattern transfer layer to the hard mask consumption layer, the step further includes: transferring the pattern on the pattern transfer layer to the double pattern integration layer, and the specific steps include:
[0024] 13-1) etching the fourth pad layer using the pattern transfer layer as a mask to obtain a first intermediate pattern transfer layer, and retaining the pattern transfer layer remaining after etching;
[0025] 13-2) depositing a pattern-optimized sacrificial layer on the surface of the structure obtained in step 13-1), wherein the pattern-optimized sacrificial layer fills the gap between the first intermediate pattern transfer layer and the remaining pattern transfer layer and covers the remaining pattern transfer layer;
[0026] 13-3) planarizing the pattern optimization sacrificial layer to the remaining pattern transfer layer, and removing the remaining pattern transfer layer, wherein the pattern optimization sacrificial layer is converted into a second intermediate pattern transfer layer;
[0027] 13-4) removing the second intermediate pattern transfer layer, and etching the third pad layer based on the first intermediate pattern transfer layer obtained by etching in step 13-1) to obtain a third intermediate pattern transfer layer, and adjusting the size of the pattern in the first direction and the second direction during etching the third pad layer; and
[0028] 13-5) etching the second cushion layer to obtain a fourth intermediate pattern transfer layer, and etching the first cushion layer using the fourth intermediate pattern transfer layer obtained by etching as a mask to obtain a fifth intermediate pattern transfer layer, so as to transfer the pattern on the pattern transfer layer to the first cushion layer.
[0029] As a preferred embodiment of the present invention, in step 1), the first pattern migration layer includes a bottom pattern transfer layer and an upper pattern transfer layer located on the bottom pattern transfer layer, wherein the bottom pattern transfer layer includes at least one of a silicon oxide layer and a tetraethyl orthosilicate (TEOS) layer, and the upper pattern transfer layer includes a silicon-rich photoresist layer; and in step 3), the pattern on the first pattern layer is transferred to the bottom pattern migration layer to form the second pattern layer.
[0030] As a preferred solution of the present invention, step 3) includes: etching the first mask layer to transfer the pattern on the first pattern layer to the first mask layer, wherein the process parameters for etching the first mask layer include: the etching gas includes at least one of O2, AR, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V; step 3) also includes: etching the upper pattern transfer layer and the bottom pattern transfer layer The process parameters for etching the upper pattern transfer layer include: the etching gas includes at least one of N2, O2 and HE; the process parameters for etching the bottom pattern transfer layer include: the etching gas includes at least CH4 and CHF3, and the ratio of CH4 to CHF3 is between 3:1 and 1:1, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V.
[0031] As a preferred solution of the present invention, step 4) further includes: depositing a planarization auxiliary layer on the surface of the first filling mask layer.
[0032] As a preferred solution of the present invention, the planarization auxiliary layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like carbon film layer (DLC); the thickness of the planarization auxiliary layer is between 20nm and 100nm.
[0033] As a preferred embodiment of the present invention, in step 5), planarizing the structure obtained in step 4) to the second pattern layer includes: etching the planarization auxiliary layer, etching the first filling mask layer, and etching the first lateral portion of the first spacing sacrificial layer at the top of the second pattern unit, wherein the process parameters for etching the planarization auxiliary layer include: the etching gas includes at least one of O2, AR, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V; etching the first filling mask layer The process parameters of the layer include: the etching gas includes at least CH4 and CHF3, and the ratio of CH4 to CHF3 is between 3:1 and 1:1, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V; the process parameters for etching the first spacing sacrificial layer at the top of the second pattern unit include: the etching gas includes at least one of CHF3, CH4 and SF6, the etching pressure is between 5mT and 30mT, the source power is between 300W and 600W, and the bias voltage is between 50V and 250V.
[0034] As a preferred embodiment of the present invention, step 6) also includes: forming a stress relief layer between the etch stop layer and the second graphic migration layer; and etching the stress relief layer simultaneously during the process of etching and removing the second longitudinal portion of the second spacing sacrificial layer in step 11).
[0035] As a preferred solution of the present invention, step 8) includes: etching the second mask layer to transfer the pattern of the third pattern layer to the second mask layer, and the process parameters for etching the second mask layer include: the etching gas includes at least one of O2, AR, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V; step 8) also includes: etching the second graphic migration layer to transfer the pattern of the third pattern layer to the second graphic migration layer, and the process parameters for etching the second graphic migration layer include: the etching gas includes at least one of N2, O2 and HE.
[0036] As a preferred solution of the present invention, in step 10), planarizing the structure obtained in step 9) to the second spacer sacrificial layer includes: etching the second filling mask layer, and the process parameters for etching the second filling mask layer include: the etching gas includes at least one of O2, AR, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V.
[0037] As a preferred solution of the present invention, in step 11), the process parameters for etching and removing the third lateral portion and the second longitudinal portion of the second spacing sacrificial layer include: the etching gas includes at least one of O2, CH4 and CHF3, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V.
[0038] As a preferred solution of the present invention, the pattern transfer layer formed includes at least one of a grid-shaped pattern transfer layer and a diamond-shaped pattern transfer layer.
[0039] As a preferred solution of the present invention, in step 1), the capacitor supporting sacrificial structure layer includes an etch barrier layer located on the semiconductor substrate and at least one dielectric sacrificial layer and at least one supporting layer located on the etch barrier layer; step 13) includes: etching the supporting layer, the dielectric sacrificial layer and the etch barrier layer based on the patterned hard mask consumable layer, and removing the patterned hard mask consumable layer remaining after etching, so as to etch on the semiconductor substrate a plurality of semiconductor memory capacitor holes evenly spaced and arranged in the capacitor supporting sacrificial structure layer.
[0040] As a preferred solution of the present invention, the support layer, the dielectric sacrificial layer and the etching stop layer are etched by pulse radio frequency etching, wherein the etching cycle of the pulse radio frequency etching includes one pulse on and one pulse off, etching is performed when the pulse is on, and by-products are discharged when the pulse is off, and the pulse on time accounts for 70% to 90% of the etching cycle of the pulse radio frequency etching.
[0041] As a preferred embodiment of the present invention, the dielectric layer includes a first dielectric sacrificial layer, a second dielectric sacrificial layer and a third dielectric sacrificial layer, the supporting layer includes a first supporting layer and a second supporting layer, and the first dielectric sacrificial layer, the second dielectric sacrificial layer, the first supporting layer, the third dielectric sacrificial layer and the second supporting layer are stacked in sequence from bottom to top.
[0042] As a preferred embodiment of the present invention, the etch stop layer includes a silicon nitride layer, and the thickness of the etch stop layer is between 10nm and 80nm; the material of the first dielectric layer includes at least one of phosphorus-doped silicon oxide (PSG), boron-phosphorus-doped oxide (BPSG) and fluorine-doped silicon oxide glass (FSG), and the thickness of the first dielectric layer is between 100nm and 600nm; the hardness of the second dielectric layer is greater than the hardness of the first dielectric layer, the material of the second dielectric layer includes TEOS, and the thickness of the second dielectric layer is between 300nm and 1000nm; the material of the third dielectric layer includes at least one of silicon oxide and TEOS, and the thickness of the third dielectric layer is between 300nm and 1000nm; the material of the first supporting layer includes silicon nitride, and the thickness of the first supporting layer is between 10nm and 80nm; the material of the second supporting layer includes silicon nitride, and the thickness of the second supporting layer is between 50nm and 200nm.
[0043] As a preferred solution of the present invention, it is characterized in that, in step 6), the second mask layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC); in step 9), the second filling mask layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC).
[0044] As described above, the method for preparing a semiconductor memory capacitor hole of the present invention has the following beneficial effects:
[0045] In the preparation of the semiconductor structure layer based on pitch multiplication of the present invention, sidewall layers (spacer) are formed in two directions to double the pattern. Based on this pitch doubling technology, pattern miniaturization can be achieved in a process of 30nm and below. Furthermore, the present invention controls the dimensions of the two directions in the preparation process to achieve good uniformity of the pitch doubling pattern, further improves the definition of the feature size in the device structure, solves the problem of large and small holes, and improves the double pattern integration layer in the etching process to perform pattern correction in the preparation process to improve the pattern accuracy. In addition, the present invention also improves the structural layer to achieve a better selection ratio, improve the capacitor size defects, and improve the yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 Shown is a process flow chart of the memory capacitor hole preparation process of the present invention.
[0047] Figure 2 It is a schematic diagram showing the structure of providing a semiconductor substrate in the preparation of the memory capacitor hole of the present invention.
[0048] Figure 3It is a schematic structural diagram showing a hard mask consumption layer, a first pattern migration layer and a first mask layer formed on a semiconductor substrate in the preparation of a memory capacitor hole according to the present invention.
[0049] Figure 4 Displayed as Figure 3 A structural schematic diagram of a double pattern integration layer is also formed on this basis.
[0050] Figure 5 It is a schematic structural diagram of forming a first pattern layer in the preparation of a memory capacitor hole according to the present invention.
[0051] Figure 6 Display as Figure 5 A top view of Figure 5 Display as Figure 6 Cross-sectional view at position A-A'.
[0052] Figure 7 It is a schematic structural diagram of forming a second pattern layer in the preparation of the memory capacitor hole of the present invention.
[0053] Figure 8 It is a schematic structural diagram of forming a first spacer sacrificial layer in the preparation of a memory capacitor hole according to the present invention.
[0054] Fig. 9 It is a schematic structural diagram of forming a first filling mask layer in the preparation of the memory capacitor hole of the present invention.
[0055] Fig.10 It is a schematic diagram showing the structure of forming a planarization auxiliary layer in the preparation of the memory capacitor hole of the present invention.
[0056] Fig.11 It is a schematic diagram of the structure of planarization to the second pattern layer in the preparation of the memory capacitor hole of the present invention.
[0057] Fig.12 It shows a schematic diagram of the structure of forming an etch stop layer, a stress relief layer, a second graphic migration layer and a second mask layer in the preparation of the memory capacitor hole of the present invention.
[0058] Fig.13 It is a schematic structural diagram of the first direction of forming the third pattern layer in the preparation of the memory capacitor hole of the present invention.
[0059] Fig.14 It is a schematic structural diagram showing the second direction of forming the third pattern layer in the preparation of the memory capacitor hole of the present invention.
[0060] Fig.15 It is a top view of the third pattern layer formed in the preparation of the memory capacitor hole of the present invention, wherein: Fig.13 Display as Fig.15 The cross-sectional view along the A-A' direction, Fig.14Display as Fig.15 Cross-sectional view along the BB' direction.
[0061] Fig.16 It is a schematic structural diagram showing the second direction of forming the fourth pattern layer in the preparation of the memory capacitor hole of the present invention.
[0062] Fig.17 It is a schematic structural diagram of the first direction of forming the fourth pattern layer in the preparation of the memory capacitor hole of the present invention.
[0063] Fig.18 It is a top view of the fourth pattern layer formed in the preparation of the memory capacitor hole of the present invention, wherein: Fig.16 Display as Fig.18 Cross-sectional view along the B-B' direction, Fig.17 Display as Fig.18 Cross-sectional view along the A-A' direction.
[0064] Fig.19 It is a schematic structural diagram of forming a second spacer sacrificial layer in the preparation of the memory capacitor hole of the present invention.
[0065] Fig. 20 It is a schematic structural diagram of the second direction of forming the second filling mask layer in the preparation of the memory capacitor hole of the present invention.
[0066] Fig.21 It is a schematic structural diagram of the first direction of forming a second filling mask layer in the preparation of the memory capacitor hole of the present invention.
[0067] Fig. 22 It is a top view of forming a second filling mask layer in the preparation of the memory capacitor hole of the present invention, wherein: Fig. 20 Display as Fig. 22 Cross-sectional view along the B-B' direction, Fig.21 Display as Fig. 22 Cross-sectional view along the A-A' direction.
[0068] Fig.23 It is a schematic diagram showing the structure of the second spacer sacrificial layer that is planarized during the preparation of the memory capacitor hole of the present invention.
[0069] Fig.24 It is a schematic structural diagram of forming a fifth pattern layer in the preparation of the memory capacitor hole of the present invention.
[0070] Fig.25 It shows a schematic diagram of the second direction structure of the relief layer pattern transfer layer formed in the preparation of the memory capacitor hole of the present invention.
[0071] Fig.26 It shows a schematic diagram of the first direction structure of the relief layer pattern transfer layer formed in the preparation of the memory capacitor hole of the present invention.
[0072] Fig. 27 It shows a top view of a mitigation layer pattern transfer layer formed in the preparation of a memory capacitor hole of the present invention, wherein: Fig.25 Display as Fig. 27 Cross-sectional view along the B-B' direction, Fig.26 Display as Fig. 27 Cross-sectional view along the A-A' direction.
[0073] Fig.28 It is a schematic diagram showing the second direction structure of forming a mesh pattern transfer layer in the preparation of the memory capacitor hole of the present invention.
[0074] Fig.29 It is a schematic diagram showing the first direction structure of forming a mesh pattern transfer layer in the preparation of the memory capacitor hole of the present invention.
[0075] Fig.30 It is a top view of a mesh pattern transfer layer formed in the preparation of a memory capacitor hole of the present invention, wherein: Fig.28 Display as Fig.30 Cross-sectional view along the B-B' direction, Fig.29 Display as Fig.30 Cross-sectional view along the A-A' direction.
[0076] Fig.31 It is a schematic diagram showing the second direction structure of the first intermediate pattern transfer layer formed by preparing the memory capacitor hole of the present invention.
[0077] Fig.32 It is a schematic diagram showing the structure of the first direction of the first intermediate pattern transfer layer formed by preparing the memory capacitor hole of the present invention.
[0078] Fig.33 It is a schematic diagram showing the structure of a pattern-optimized sacrificial layer formed in the preparation of a memory capacitor hole according to the present invention.
[0079] Fig.34 It is a schematic diagram showing the structure of the second intermediate pattern transfer layer formed by planarization in the preparation of the memory capacitor hole of the present invention.
[0080] Fig.35 It is a schematic structural diagram showing the removal of the remaining mesh pattern transfer layer in the preparation of the memory capacitor hole of the present invention.
[0081] Fig.36 It is a schematic structural diagram of forming a third intermediate pattern transfer layer in the preparation of the memory capacitor hole of the present invention.
[0082] Fig.37 It is a schematic diagram showing the structure of the fourth intermediate pattern transfer layer in the second direction formed by preparing the memory capacitor hole of the present invention.
[0083] Fig.38It is a schematic diagram showing the structure of the first direction of the fourth intermediate pattern transfer layer formed by preparing the memory capacitor hole of the present invention.
[0084] Fig.39 It is a top view of forming a fourth intermediate pattern transfer layer in the preparation of the memory capacitor hole of the present invention, wherein: Fig.37 Display as Fig.39 Cross-sectional view along the B-B' direction, Fig.38 Display as Fig.39 Cross-sectional view along the A-A' direction.
[0085] Fig.40 It is a schematic diagram showing the structure of the fifth intermediate pattern transfer layer in the second direction formed by preparing the memory capacitor hole of the present invention.
[0086] Fig.41 It is a schematic diagram showing the structure of the first direction of the fifth intermediate pattern transfer layer formed by preparing the memory capacitor hole of the present invention.
[0087] Fig.42 It is a top view of the fifth intermediate pattern transfer layer formed in the preparation of the memory capacitor hole of the present invention, wherein: Fig.40 Display as Fig.42 Cross-sectional view along the B-B' direction, Fig.41 Display as Fig.42 Cross-sectional view along the A-A' direction.
[0088] Fig.43 It is a schematic diagram of the second direction structure of the patterned hard mask consumption layer formed by preparing the memory capacitor hole of the present invention.
[0089] Fig.44 It is a schematic diagram showing the structure of the first direction of the patterned hard mask consumption layer formed by preparing the memory capacitor hole of the present invention.
[0090] Fig.45 It is a top view of a patterned hard mask consumption layer formed in the preparation of a memory capacitor hole of the present invention, wherein: Fig.43 Display as Fig.45 Cross-sectional view along the B-B' direction, Fig.44 Display as Fig.45 Cross-sectional view along the A-A' direction.
[0091] Fig.46 The diagram shows the method of etching the capacitor support sacrificial layer to form the memory capacitor hole for the memory capacitor hole preparation of the present invention.
[0092] Fig.47 A diagram showing the removal of the remaining patterned hard mask sacrificial layer during the preparation of the memory capacitor hole according to the present invention.
[0093] Fig.48It shows a top view of a memory capacitor hole formed in the preparation of the memory capacitor hole of the present invention, wherein: Fig.47 Display as Fig.48 Cross-sectional view along the A-A' direction.
[0094] Component number description
[0095] 100 Semiconductor substrate
[0096] 101 Hard Mask Consumption Layer
[0097] 102 Double pattern integration layer
[0098] 102a First cushion layer
[0099] 102b Second cushion
[0100] 102c Third cushion
[0101] 102d Fourth cushion
[0102] 103 First Graphic Migration Layer
[0103] 103a Bottom Graphics Transfer Layer
[0104] 103b Upper Graphics Transfer Layer
[0105] 104 First mask layer
[0106] 105 First pattern layer
[0107] 105a First pattern unit
[0108] 106 Second pattern layer
[0109] 106a Second pattern unit
[0110] 107 first spacer sacrificial layer
[0111] 107a First gap groove
[0112] 107b first transverse portion
[0113] 107c First longitudinal portion
[0114] 107d Second transverse portion
[0115] 108 first filling mask layer
[0116] 109 Planarization auxiliary layer
[0117] 110 Size-limited units
[0118] 111 Pattern auxiliary unit
[0119] 112 Etch stop layer
[0120] 113 Stress relief layer
[0121] 114 Second Graphic Migration Layer
[0122] 115 Second mask layer
[0123] 116 Third pattern layer
[0124] 116a The third pattern unit
[0125] 117 Fourth pattern layer
[0126] 117a Fourth pattern unit
[0127] 118 second spacer sacrificial layer
[0128] 118a Second gap groove
[0129] 118b Third transverse portion
[0130] 118c Second longitudinal portion
[0131] 118d Fourth transverse portion
[0132] 119 second filling mask layer
[0133] 120 Fifth Pattern Layer
[0134] 120a Fifth pattern unit
[0135] 121 Mitigation layer Graphic transfer layer
[0136] 121a Mitigation layer pattern transfer unit
[0137] 122 Graphics transfer layer
[0138] 122a First spacing multiplication unit
[0139] 122b Second spacing multiplication unit
[0140] 123 First intermediate graphics transfer layer
[0141] 123a First direction first intermediate pattern transfer layer unit
[0142] 123b Second direction first intermediate pattern transfer layer unit
[0143] 124 Graphics Optimization Sacrificial Layer
[0144] 125 Second intermediate graphic transfer layer
[0145] 125b Second direction second intermediate pattern transfer layer unit
[0146] 126 Third intermediate graphics transfer layer
[0147] 126b Second direction third intermediate pattern transfer layer unit
[0148] 127 Fourth intermediate graphic transfer layer
[0149] 127a First direction fourth intermediate pattern transfer layer unit
[0150] 127b The fourth intermediate pattern transfer layer unit in the second direction
[0151] 128 Fifth intermediate graphics transfer layer
[0152] 128a First direction fifth intermediate pattern transfer layer unit
[0153] 128b The fifth intermediate pattern transfer layer unit in the second direction
[0154] 129 Patterned Hard Mask Consumption Layer
[0155] 129a Polysilicon cell patterned in the first direction
[0156] 129b Second direction patterned polysilicon unit
[0157] 300 Capacitor support sacrificial structure layer
[0158] 301 Etching stop layer
[0159] 302 first dielectric sacrificial layer
[0160] 303 Second dielectric sacrificial layer
[0161] 304 First support layer
[0162] 305 Third dielectric sacrificial layer
[0163] 306 Second support layer
[0164] 307 semiconductor device layer
[0165] 307a Semiconductor memory capacitor hole
[0166] 308 first pattern mask replication layer
[0167] S1~S13 Step 1)~Step 13) DETAILED DESCRIPTION
[0168] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0169] See also Figures 1 to 48 It should be noted that the illustrations provided in this embodiment are only schematic illustrations of the basic concept of the present invention. Although the illustrations only show components related to the present invention and are not drawn according to the number, shape and size of components in actual implementation, the form, quantity and proportion of each component in actual implementation may be changed arbitrarily, and the component layout may also be more complicated.
[0170] like Figures 1 to 48 As shown, the present invention provides a method for preparing a semiconductor memory capacitor hole, comprising the following steps:
[0171] First, if Figure 1 S1 and Figures 2 to 4 As shown, step 1) is performed to provide a semiconductor substrate 100, and a capacitor support sacrificial layer 300, a hard mask consumption layer 101, a double pattern integration layer 102, a first graphic migration layer 103 and a first mask layer 104 are sequentially formed on the semiconductor substrate 100, wherein the first mask layer 104 includes at least one of an ashable hard mask layer (AHM) and a diamond-like carbon film layer (DLC).
[0172] Specifically, the present invention provides a step for forming a semiconductor memory capacitor hole based on a pitch doubling technology. During the preparation process, a semiconductor substrate 100 and a graphic layer (a patterned hard mask consumable layer 129) are formed by patterning the hard mask consumable layer 101 based on the pitch doubling technology. The pitch doubling technology of the present invention is a technology for achieving capacitor pattern miniaturization and deep hole formation in a 30nm and below process by using the pitch doubling technology. The semiconductor substrate 100 can be a single-layer semiconductor material layer, such as a silicon material layer, or a stacked material layer formed by stacking multiple material layers. For example, it can be a material layer that constitutes a semiconductor device structure. In addition, the graphic layer that patterns the hard mask consumable layer 101 can be used as a semiconductor mask layer. The semiconductor substrate 100 can be further etched based on the patterned hard mask consumable layer to transfer the pattern to the semiconductor substrate 100 to obtain a desired structure, such as a capacitor of 30nm and below. The hard mask consumable layer 101 can be selected from a polysilicon layer. In addition, the concept of “pitch” can be used to describe the characteristic size of a semiconductor, where the pitch is the distance between the same points in two adjacent features, wherein pitch multiplication is a multiple increase in the number of pitches at a fixed interval.
[0173] As an example, Figure 4 As shown, in step 1), the double-pattern integration layer 102 includes a first pad layer 102a, a second pad layer 102b, a third pad layer 102c and a fourth pad layer 102d from bottom to top.
[0174] Specifically, the present invention further forms a double pattern integration layer 102 before forming the first graphic migration layer 103, which is used for performing graphic modification during the preparation of the capacitor hole to obtain a more accurate graphic transfer. In addition, the double pattern integration layer 102 in this example includes a four-layer pad structure. Compared with other structures such as two-layer pads, the characteristic size of the graphic, such as the CD in the second direction, can be corrected on the bottom pad (such as A-si / Oxide). For example, in a preferred embodiment, a four-layer pad structure of A-si / Oxide / A-si / Oxide can be adopted, and the CD (characteristic size) in the Y direction in the subsequent process can be corrected in the bottom A-si / Oxide layer, so that the obtained graphic is more accurate.
[0175] As an example, the material of the first pad layer 102a includes any one of silicon oxide and tetraethyl orthosilicate (TEOS), which can be used as a hard mask, and the thickness of the first pad layer 102a is between 100nm and 500nm; the material of the second pad layer 102b includes any one of amorphous silicon (A-Si, Amorphous silicon), silicon oxynitride (Sion) and silicon nitride (Nitride), which can be used as a hard mask, and the thickness of the second pad layer 102b is between 100nm and 800nm; the material of the third pad layer 102c includes any one of silicon oxide and tetraethyl orthosilicate (TEOS), which can be used as a mask layer, and the thickness of the third pad layer 102c is between 100nm and 500nm; the material of the fourth pad layer 102d includes any one of amorphous silicon, silicon oxynitride and silicon nitride, which can be used as an etch stop layer, and the thickness of the fourth pad layer 102d is between 50nm and 200nm. In addition, the hard mask sacrificial layer 101 is formed by, for example, a chemical vapor deposition (CVD) process, and has a thickness between 300 nm and 1000 nm.
[0176] As an example, in step 1), the first graphic transfer layer 103 includes a bottom graphic transfer layer 103a and an upper graphic transfer layer 103b located on the bottom graphic transfer layer 103a.
[0177] As an example, the bottom pattern transfer layer 103a includes at least one of a silicon oxide layer and a tetraethyl orthosilicate (TEOS) layer as an oxide transfer layer, and in addition, the upper pattern transfer layer 103b (MLR, Multilayerphotoresist) includes a silicon-rich photoresist layer.
[0178] Specifically, the thickness of the bottom pattern transfer layer 103a is between 50nm and 100nm, and the upper pattern transfer layer (MLR, Multilayer photoresist) 103b can be used as a mask layer, and its thickness is between 20nm and 150nm. The present invention improves etching characteristics and optimizes pattern size through the structural design of two material layers as pattern transfer layers.
[0179] Specifically, in step 1), the first mask layer 104 includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC), and the thickness of the first mask layer 104 is between 50nm and 200nm. Specifically, in this example, AHM (Ashable hard mask) or DLC (Diamond like carbon) is used to replace the traditional Carbon as a mask layer, wherein AHM or DLC has a better selectivity than Carbon, and is more easily removed by O2 plasma, and the Profile is more ideal. Of course, in other examples, Carbon can also be selected. In addition, the first mask layer 104 can also be a stacked structure consisting of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC). Preferably, the ashable hard mask layer (AHM) is located on the diamond-like film layer (DLC), thereby further improving the stability during the device preparation process.
[0180] Then, if Figure 1 S2 and Figures 5-6 As shown, step 2) is performed to form a first pattern layer 105 arranged along a first direction on the first mask layer 104, and the first pattern layer 105 includes a plurality of first pattern units 105a arranged in parallel and at intervals.
[0181] Specifically, the present invention is based on the spacing multiplication technology, and etching is performed in at least two directions. For example, two directions are defined in a plane parallel to the semiconductor substrate 100, namely the first direction and the second direction. A certain degree of etching is first performed in one direction, and then deposition is performed on the etched structure layer, and the deposited structure and the previously formed material layer are etched in another direction, wherein the two directions can be the first direction and the second direction defined in this example, and the two directions can be perpendicular to each other, or can be other intersecting angles, such as 60°. In addition, the formation of the first pattern layer 105 can be obtained by first coating a photoresist layer (PR, Photo resist), and then exposing and developing. Of course, other methods known to ordinary technicians in this field can also be used. Preferably, the first pattern unit 105a is preferably arranged in parallel with equal sizes and equal spacing. Of course, it can also be selected and set according to actual needs.
[0182] Then, if Figure 1 S3 and Figure 7 As shown, step 3) is performed to transfer the pattern on the first pattern layer 105 to the first pattern migration layer 103 via the first mask layer 104 to form a second pattern layer 106, wherein the second pattern layer 106 includes a plurality of second pattern units 106a arranged in parallel and at intervals.
[0183] Specifically, in this step, the pattern formed in the first direction is transferred to the first pattern migration layer 103, thereby forming a second pattern layer 106, and the second pattern layer 106 is also the first pattern migration layer after patterning, wherein the second pattern layer 106 replicates the morphology of the first pattern layer 105. In addition, the pattern transfer process includes the step of etching the first mask layer 104, wherein the etching of the first mask layer 104 is preferably carried out by an ICP etching machine, and the etching process parameters include: the etching gas includes at least one of O2, AR, N2 and CH4, preferably selected from a combination of the above-mentioned etching gases O2, AR, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V.
[0184] As an example, Figure 7 As shown in , when the first pattern transfer layer 103 includes a bottom pattern transfer layer 103a and an upper pattern transfer layer 103b located on the bottom pattern transfer layer 103a, then in step 3), the pattern on the first pattern layer 105 is transferred to the bottom pattern transfer layer 103a to form the second pattern layer 106. In addition, preferably, the bottom pattern transfer layer 103a includes at least one of a silicon oxide layer and a tetraethyl orthosilicate (TEOS) layer, and the upper pattern transfer layer 103b includes a silicon-rich photoresist layer.
[0185] As an example, when the first graphic migration layer 103 includes a bottom graphic transfer layer 103a and an upper graphic transfer layer 103b, step 3) also includes: etching the upper graphic transfer layer 103b and the bottom graphic transfer layer 103a to transfer the pattern on the first pattern layer 105 to the bottom graphic transfer layer 103a, wherein the process parameters for etching the upper graphic transfer layer 103b include: the etching gas includes at least one of N2, O2 and HE; the process parameters for etching the bottom graphic transfer layer 103a include: the etching gas includes at least CH4 and CHF3, and of course can also include O2, the etching gas preferably contains O2, CH4 and CHF3, and the ratio of CH4 to CHF3 is between 3:1 and 1:1, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V.
[0186] Then, if Figure 1 S4 and Figures 8 to 10As shown, step 4) is performed to form a first spacing sacrificial layer 107 on the top, sidewall and surface of the double pattern integration layer 102 between the second pattern units 106a, and a first gap groove 107a is formed on the surface of the first spacing sacrificial layer 107 between adjacent second pattern units 106a, and a first filling mask layer 108 is formed on the surface of the first spacing sacrificial layer 107, the first filling mask layer 108 covers the first spacing sacrificial layer 107 and fills the first gap groove 107a formed by the first spacing sacrificial layer 107.
[0187] Specifically, in this step, a continuous first spacer sacrificial layer 107 is formed to define the subsequent characteristic size. The first spacer sacrificial layer 107 includes a first lateral portion 107b formed on the top of the second pattern unit 106, a first longitudinal portion 107c located on the side wall of the second pattern unit 106, and a second lateral portion 107d located on the double pattern integration layer 102. In the present invention, the first longitudinal portion 107c is subsequently etched away as the characteristic size CD of the device. Because the Nitride sidewalls (first longitudinal portion 107c) are all grown by Spacer, the thickness will be consistent, so the CD size is consistent, which solves the problem that in the sidewall process of the prior art, the structures on both sides of the deposited sidewalls form different CDs, that is, there are large and small holes with odd and even numbers of Spacer CDs.
[0188] In addition, the thickness of the deposited first spacer sacrificial layer 107 is between 10nm and 80nm. In this example, the thickness of the first spacer sacrificial layer 107 (sidewall Nitride) determines the CD size in the first direction (such as the X direction). In addition, a layer of the first filling mask layer 108 is deposited on the surface of the second spacer sacrificial layer 107. The thickness of the first filling mask layer 108 is between 20nm and 100nm. The material thereof may include at least one of silicon oxide and TEOS. Part of the first filling mask layer 108 is used as a mask layer for subsequent etching. Preferably, the first filling mask layer 108 fills the first gap 107a, which is beneficial to ensure etching accuracy and further beneficial to improve the uniformity of the capacitor hole size.
[0189] As an example, Fig.10 As shown, step 4) also includes: depositing a planarization auxiliary layer 109 on the surface of the first filling mask layer 108, and depositing the planarization auxiliary layer 109 is used to optimize the planarization effect of the subsequent step 5).
[0190] As an example, the planarization auxiliary layer 109 includes at least one of an ashing hard mask layer (AHM) and a diamond-like carbon film layer (DLC), which can be any one of the two, or a stacked structure layer composed of the two. As an example, the thickness of the planarization auxiliary layer 109 is between 20nm and 100nm.
[0191] Then, if Figure 1 S5 and Fig.11 As shown, step 5) is performed to remove the first lateral portion 107b of the first spacer sacrificial layer 107 located at the top of the second pattern unit 106a, the first filling mask layer 108, and a portion of the first filling mask layer 108 located in the first gap groove 107a, which is equivalent to planarizing the structure obtained in step 4) to the second pattern layer 106, wherein a size defining unit 110 and a pattern auxiliary unit 111 located between the size defining units 110 are formed between adjacent second pattern units 106a, wherein the first longitudinal portion 107c of the first spacer sacrificial layer 107 located on the side wall of the second pattern unit 106a forms the size defining unit 110, and the second lateral portion 107d of the first spacer sacrificial layer 107 located on the surface of the double pattern integration layer 102 and the remaining first filling mask layer 108a on the second lateral portion 107d form the pattern auxiliary unit 111;
[0192] Specifically, after the process of this step, a filler is formed between the second pattern units 106a on the second pattern layer 106, including the U-shaped second spacing sacrificial layer remaining after planarization and a portion of the first filling mask layer filled between the U-shaped openings, which are defined as a size defining unit 110 and a pattern auxiliary unit 111, wherein the size defining unit 110 is used to define the CD of the pattern and is removed in the subsequent process, and the second pattern unit 106a and the pattern auxiliary unit 111 therebetween serve as a mask pattern structure for subsequent first direction pattern etching.
[0193] As an example, in step 5), when the planarization auxiliary layer 109 exists, planarizing the structure obtained in step 4) to the second pattern layer 106 includes: etching the planarization auxiliary layer 109, etching the first filling mask layer 108, and etching the first lateral portion 107b of the first spacing sacrificial layer 107 at the top of the second pattern unit 106a, preferably using an ICP etching machine, wherein the process parameters for etching the planarization auxiliary layer 109 include: the etching gas includes at least one of O2, AR, N2 and CH4, preferably includes the above four etching gases, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V; the process parameters for etching the first filling mask layer 108 are as follows: The parameters include: the etching gas includes at least CH4 and CHF3, and of course can also include O2, preferably including three etching gases of O2, CH4 and CHF3, and the ratio of CH4 to CHF3 is between 3:1 and 1:1, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V; the process parameters for etching the first spacer sacrificial layer 107b at the top of the second pattern unit include: the etching gas includes at least one of CHF3, CH4 and SF6, preferably including the above three etching gases, the etching pressure is between 5mT and 30mT, the source power is between 300W and 600W, and the bias voltage is between 50V and 250V, so as to finally achieve a pattern with better surface flattening effect.
[0194] Then, if Figure 1 S6 and Fig.12 As shown, step 6) is performed to sequentially form an etching stop layer 112, a second pattern migration layer 114 and a second mask layer 115 on the structure obtained in step 5);
[0195] As an example, step 6) also includes: forming a stress relief layer 113 between the etch stop layer 112 and the second graphic migration layer 114 .
[0196] As an example, in step 6), the second mask layer 115 includes at least one of an ashable hard mask layer (AHM) and a diamond-like carbon film layer (DLC), and of course, it can also be a stacked structure consisting of the two.
[0197] Specifically, a material layer is deposited as a material layer for subsequent graphic etching in the second direction, and a layer of etching stop layer 112 is first deposited as an etching stop layer for subsequent etching, and its material includes silicon nitride, and its thickness is between 10nm and 80nm. In a preferred embodiment, the stress relief layer 113 for relieving the stress of the etching stop layer 112 is formed on the etching stop layer 112, and the material of the stress relief layer 113 includes at least one of silicon oxide and TEOS, and its thickness is between 50nm and 200nm. In addition, the material of the second graphic migration layer (MLR, Multilayerphotoresist) 114 is preferably a silicon-rich photoresist layer, and its thickness is between 20nm and 150nm, and the second mask layer 115 can be AHM (Ashable hard mask) or DLC (Diamond like carbon) or Carbon, and its thickness is between 50nm and 200nm.
[0198] Then, if Figure 1 S7 and Figures 13-15 As shown, step 7) is performed to form a third pattern layer 116 arranged along a second direction on the second mask layer 115, wherein the third pattern layer 116 includes a plurality of third pattern units 116a arranged in parallel and spaced apart, and the second direction and the first direction have an intersection angle;
[0199] Specifically, in this example, the graphic structure is defined in another direction, and the first pattern layer 116 can be obtained by first coating a photoresist layer (PR, Photo resist) and then exposing and developing. Of course, it can also be other methods known to ordinary technicians in this field. Preferably, the first pattern unit 116a is preferably arranged in parallel with equal size and equal spacing. Of course, it can also be selected and set according to actual needs. In addition, the second direction is selected according to actual needs. The second direction can be perpendicular to the first direction, and can be other angles of intersection, such as 60°.
[0200] Then, if Figure 1 S8 and Figures 16 to 18 As shown, step 8) is performed to transfer the pattern on the third pattern layer 116 to the second pattern migration layer 114 via the second mask layer 115 to form a fourth pattern layer 117, wherein the fourth pattern layer 117 includes a plurality of fourth pattern units 117a arranged in parallel and spaced apart;
[0201] As an example, step 8) includes: etching the second mask layer 115 to transfer the pattern of the third pattern layer 116 to the second mask layer 115, and the process parameters for etching the second mask layer 115 include: the etching gas includes at least one of O2, AR, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V. Preferably, the second mask layer 115 includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC).
[0202] Specifically, in this step, the pattern formed in the second direction is transferred to the second pattern migration layer 114, so as to form a fourth pattern layer 117, wherein the fourth pattern layer 117 replicates the morphology of the third pattern layer 116. In addition, the pattern transfer process includes the step of etching the first mask layer 104, wherein the second mask layer 115 is preferably etched using an ICP etching machine, and the etching process parameters include: the etching gas includes at least one of O2, AR, N2 and CH4, preferably a combination of the above etching gases, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V. Step 8) also includes: etching the second pattern migration layer 114 to transfer the pattern of the third pattern layer 116 to the second pattern migration layer 114 to form a fourth pattern layer 117, and the etching process parameters of the second pattern migration layer include: the etching gas includes at least one of N2, O2 and HE.
[0203] Then, if Figure 1 S9 and Figures 19 to 22 As shown, step 9) is performed to form a second spacing sacrificial layer 118 on the top, sidewalls of the four pattern units 117a and the surface of the etch stop layer 112 between the fourth pattern units 117a, and a second gap groove 118a is formed between the surfaces of the second spacing sacrificial layer 118 between adjacent fourth pattern units 117a, and a second filling mask layer 119 is formed on the surface of the second spacing sacrificial layer 118, and the second filling mask layer 119 covers the second spacing sacrificial layer 118 and fills the second spacing sacrificial layer 118 to form the second gap groove 118a.
[0204] As an example, in step 9), the second filling mask layer 119 includes at least one of an ashable hard mask layer (AHM) and a diamond-like carbon film layer (DLC), and the thickness of the second filling mask layer 119 is between 50 nm and 200 nm.
[0205] Specifically, in this step, a continuous second spacer sacrificial layer 118 is formed to define a subsequent feature size, and the second spacer sacrificial layer 118 includes a third lateral portion 118b formed on the top of the fourth pattern unit 117a, a second longitudinal portion 118c located on the side wall of the fourth pattern unit 117a, and a second longitudinal portion 118c located on the etch stop layer 112 (located on the stress relief layer 113 when the stress relief layer 113 is present, such as Fig.19 In the present invention, the second longitudinal portion 118c is subsequently etched away as the characteristic dimension CD of the device, because the second longitudinal portions 118c are all grown by Spacer, and the thickness will be consistent, so the CD size is consistent. In addition, the thickness of the deposited second sacrificial spacer layer 118 is between 10nm and 80nm. In this example, the thickness of the second sacrificial spacer layer 118 (at least one of sidewall silicon oxide or TEOS) determines the CD size in the second direction (such as the Y direction). In addition, in a preferred embodiment, the high selectivity of Oxide / Nitride is used in the graphic definition of the first direction and the second direction, so that the graphics are finer than other methods.
[0206] Then, if Figure 1 S10 and Fig.23 As shown, step 10) is performed to planarize the structure obtained in step 9) until the top surface of the second spacer sacrificial layer 118 is exposed, and the remaining second filling mask layer 119a between the second longitudinal portions 118c of the second spacer sacrificial layer 118 on the sidewalls of the fourth pattern unit 117a is retained;
[0207] Specifically, in this step, planarization is performed through an etching process to remove a portion of the second filling mask layer 119, exposing the third lateral portion 118b of the second spacing sacrificial layer 118 at the top of the fourth pattern unit 117a, for the next process to prepare a graphic structure in the second direction.
[0208] As an example, in step 10), planarizing the structure obtained in step 9) to the second spacer sacrificial layer 118 includes: etching the second filling mask layer 119, and the process parameters for etching the second filling mask layer 119 include: the etching gas includes at least one of O2, AR, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V.
[0209] Then, if Figure 1 S11 and Figures 24-27As shown, step 11) is performed to etch and remove the third lateral portion 118b of the second spacing sacrificial layer 118 located at the top of the fourth pattern unit 117a and the second longitudinal portion 118c of the second spacing sacrificial layer 118 located on the side wall of the fourth pattern unit 117a to expose the etch stop layer 112 and obtain the fifth pattern layer 120, wherein the fifth pattern layer 120 includes a plurality of fifth pattern units 120a arranged in parallel and spaced apart, wherein the fourth pattern unit 117a located on the etch stop layer 112, the fourth lateral portion 118d of the second spacing sacrificial layer 118 located on the surface of the etch stop layer and the remaining second filling mask layer 119a thereon form a stack to form the fifth pattern unit 120a.
[0210] As an example, when step 6) also includes forming a stress relief layer 113 between the etch stop layer 112 and the second graphic migration layer 114, the stress relief layer 113 is simultaneously etched during the process of etching and removing the second longitudinal portion 118c located at the second spacing sacrificial layer 118 in step 11) to form a relief layer graphic transfer layer 121.
[0211] Specifically, in this step, a pattern in the second direction is defined to ultimately form a capacitor hole structure, and the fifth pattern unit 120a is composed of a two-part structure, one part of which is the fourth pattern unit 117a, and the other part is the etched stacked structure, including the fourth transverse portion 118d of the second spacing sacrificial layer 118 and the remaining second filling mask layer 119a thereon. In addition, when the stress relief layer 113 is present, the material of the stress relief layer 113 is preferably the same as the material of the second spacing sacrificial layer 118, so that the stress relief layer is also etched while removing the second longitudinal portion 118c. At this time, the fifth pattern layer 120 formed includes a structural layer formed by etching the stress relief layer 113.
[0212] As an example, in step 11), the process parameters for etching and removing the third lateral portion 118b and the second longitudinal portion 118c of the second spacing sacrificial layer 118 include: the etching gas includes at least one of O2, CH4 and CHF3, and the etching gas preferably includes O2, CH4 and CHF3. The etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V.
[0213] In addition, if Figures 25-27As shown, when the stress relief layer 113 is present, and the stress relief layer 113 is etched simultaneously when the fifth pattern layer 120 is formed, that is, the stress relief layer 113 transfers the pattern on the fifth pattern layer 120 to form a relief layer graphic transfer layer 121, comprising a plurality of relief layer graphic transfer units 121a arranged in parallel and spaced apart. In a preferred embodiment, it also includes removing the fifth pattern layer 120 and retaining the relief layer graphic transfer layer 121. Fig.25 As shown, the mitigation layer pattern transfer layer 121 is used as a mask for subsequent etching process.
[0214] Then, if Figure 1 S12 and Figures 28-30 As shown, step 12) is performed, using the fifth pattern unit as a mask, selectively etching and removing the etching stop layer 112 and the dimension defining unit 110, so as to transfer the pattern on the fifth pattern layer 120 to the second pattern layer 106, so as to form a pattern transfer layer 122 on the double pattern integration layer 102, wherein the pattern transfer layer 122 includes a plurality of first spacing multiplication units 122a arranged in parallel and spaced apart along the first direction, and a plurality of second spacing multiplication units 122b arranged in parallel and spaced apart along the second direction and connected to the first spacing multiplication units, wherein the first spacing multiplication unit 122a is composed of the second pattern unit 106a and the pattern auxiliary unit 111, and the second spacing multiplication unit 122b is formed by transferring the fifth pattern unit 120a;
[0215] As an example, the pattern transfer layer 122 formed includes at least one of a grid-shaped pattern transfer layer and a diamond-shaped pattern transfer layer.
[0216] Specifically, in this step, the pattern in the first direction intersects with the pattern in the second direction. In a preferred embodiment, the material of the etch stop layer 112 is the same as the material of the first spacer sacrificial layer 107, which is conducive to the removal of the etch stop layer 112 and the size defining unit formed by the first spacer sacrificial layer 107, and finally forms Fig.28 and Fig.29The graphic transfer layer 122 shown obtains the pattern of the capacitor hole formed by subsequent etching. Further, in a preferred embodiment, the material of the second pattern layer 106 is preferably the same as the material of the first filling mask layer 108, which is beneficial to the implementation of the subsequent etching process, and is beneficial to improving the uniformity of the pattern morphology and improving the stability of the device performance. In addition, the graphic pattern in the graphic transfer layer 122 formed in this example is selected according to actual conditions, and can be a mesh pattern. For example, when the first direction and the second direction are perpendicular to each other, the pattern morphology in the graphic transfer layer 122 formed is a cross-grid shape, that is, a plurality of squares of uniform size and uniform array arrangement are formed. Of course, in other examples, it can be selected according to needs, such as forming a diamond-shaped pattern structure layer of uniform size.
[0217] Finally, if Figure 1 S13 and Figures 31 to 48 As shown, step 13) is performed to transfer the pattern on the pattern transfer layer 122 to the hard mask consuming layer 101 via the double pattern integration layer 102 to obtain a patterned hard mask consuming layer 129, and the capacitor supporting sacrificial structure layer 300 is etched based on the patterned hard mask consuming layer 129 to form a plurality of semiconductor memory capacitor holes 307a that are evenly spaced in the capacitor supporting sacrificial structure layer 300.
[0218] Specifically, the pattern on the pattern transfer layer 122 is transferred to the hard mask consumption layer 101, and the obtained patterned hard mask consumption layer 129 is used as a mask layer for subsequent etching process of capacitor holes, such as Figures 43-45 As shown. In the process of etching the hard mask consumption layer 101, a CCP machine is preferably used, and the exposed portion of the upper surface will be oxidized. In a preferred embodiment, at least one etching gas of AR / CF4 / O2 is first used to open the surface layer under the conditions of 5-30mt / HF, 200-500W / LF and 200-800W, and then at least one etching gas of HBR / NF3 / O2 is used to etch the hard mask consumption layer under the conditions of 30-200mt / HF, 100-800W / LF and 500-1500W. In addition, it is further preferred that in order to make the Profile more vertical, Pulse Etch is preferentially used for etching.
[0219] As an example, when the double pattern integration layer 102 exists, before transferring the pattern on the pattern transfer layer 122 to the hard mask consumption layer 101 in step 13), the step further includes: transferring the pattern on the pattern transfer layer 122 to the double pattern integration layer 102, and the specific steps include:
[0220] 13-1) Using the pattern transfer layer 122 as a mask, the fourth pad layer 102d is etched to obtain a first intermediate pattern transfer layer 123, and the pattern transfer layer remaining after etching is retained, such as Fig.31 and Fig.32 As shown, the fourth pad layer 102d is transformed into the first intermediate pattern transfer layer 123, and the pattern transfer layer 122 in two directions is transferred to form a first direction first intermediate pattern transfer unit 123a and a second direction first intermediate pattern transfer unit 123b;
[0221] 13-2) depositing a pattern-optimized sacrificial layer 124 on the surface of the structure obtained in step 13-1), wherein the pattern-optimized sacrificial layer 124 fills the gap between the first intermediate pattern transfer layer 123 and the remaining pattern on the pattern transfer layer 122 and covers the pattern transfer layer 122, such as Fig.33 As shown, the same effect is produced in the first direction and the second direction, and only the cross section in the second direction is used as an example;
[0222] 13-3) planarizing the graphic optimization sacrificial layer 124 to the remaining graphic transfer layer 122, and removing the remaining graphic transfer layer 122, wherein the graphic optimization sacrificial layer is converted into a second intermediate graphic transfer layer 125, including a second direction second intermediate graphic transfer unit 125b, such as Fig.34 and Fig.35 As shown, in the second direction, the pattern optimization sacrificial layer 124 is planarized to form a second intermediate pattern transfer layer 125, and then the remaining pattern transfer layer 122 is removed, and the fourth pad transfer layer 123 is retained, as shown in FIG. Fig.35 As shown, the same effect is produced in the first direction and the second direction, and only the cross section in the second direction is used as an example;
[0223] 13-4) removing the second intermediate pattern transfer layer 125, and etching the third pad layer 102c based on the first intermediate pattern transfer layer 123 obtained by etching in step 13-1), to obtain a third intermediate pattern transfer layer 126, including a second direction third intermediate pattern transfer unit 126b, and adjusting the size of the pattern in the first direction and the second direction during etching the third pad layer, such as Fig.36As shown, and in the process of etching the third pad layer 102c, the size of the pattern in the first direction and the second direction is adjusted. In one example, the role of the pattern optimization sacrificial layer here is as shown in the figure. If there is no pattern optimization sacrificial layer, the pattern transfer layer acts as a mask during direct etching. The material is the same and the etching morphology will be distorted. If the pattern transfer layer is not removed first, the oxide etching rate is fast and the underlying third pad layer will be damaged, so the morphology will be better. In addition, in this example, the CD size of the pattern obtained by the transfer in the first direction X is determined by the thickness of the side wall deposition of Nitride (Nitride at this time is the first spacer sacrificial layer 107), and here it can be determined by the CD in the transferred pattern (such as the CD at this time can be as shown in the figure below). Fig.35 The CD size of the pattern in the fourth pad transfer layer 123 is used to determine whether the required CD size meets the requirements. If it is too large or too small, the CD size can be corrected by adjusting the time of etching the third pad to achieve the correction of the size of the final pattern.
[0224] 13-5) Etching the second pad layer 102b to obtain a fourth intermediate pattern transfer layer 127, and etching the first pad layer 102a using the etched fourth intermediate pattern transfer layer 127 as a mask to obtain a fifth intermediate pattern transfer layer 128, so as to transfer the pattern on the pattern transfer layer 122 to the first pad layer 102a.
[0225] Specifically, in this step, the pattern on the pattern transfer layer 122 is transferred to the first cushion layer 102a, so as to transfer the pattern on the pattern transfer layer 122 to the pattern trimming mask layer 102. The present invention can obtain a pattern with precise morphology through the design of the pattern trimming mask layer of the above four cushion layers, wherein the pattern on the pattern transfer layer 122, the "up" here does not mean the position above or below in a strict sense, and so on. Ordinary technicians in this field can determine the meaning expressed based on the diagram and actual conditions.
[0226] As an example, Fig.46As shown, in step 1), the capacitor support sacrificial structure layer 300 includes an etch barrier layer 301 located on the semiconductor substrate 100 and at least one dielectric sacrificial layer (302, 303, 305) and at least one support layer (304, 306) located on the etch barrier layer 301; step 13) includes: etching the support layer (304, 306), the dielectric sacrificial layer (302, 303, 305) and the etch barrier layer 301 based on the patterned hard mask sacrificial layer 129, and removing the patterned hard mask sacrificial layer 129 remaining after etching, so as to etch on the semiconductor substrate 100 to form a plurality of semiconductor memory capacitor holes 307a that are evenly spaced and arranged in the capacitor support sacrificial layer 300.
[0227] Specifically, in this example, the capacitor supporting sacrificial structure layer 300 is etched to obtain a capacitor hole structure based on which the capacitor is subsequently prepared, wherein a semiconductor device layer 307 is formed, which includes a number of memory capacitor holes 307a. In addition, in a preferred embodiment, the semiconductor substrate 100 may have a plurality of capacitor contacts in a memory array structure, and the semiconductor substrate 100 may include a silicon substrate, a germanium substrate, a germanium silicon substrate, a silicon carbide substrate, etc. In this embodiment, the semiconductor substrate 100 may be a silicon substrate. In addition, the memory array structure also includes a transistor word line (Wordline) and a bit line (Bitline), and the capacitor contact is electrically connected to the transistor source in the memory array structure. The capacitor contact corresponds to the arrangement of the capacitor to be subsequently manufactured. In addition, the capacitor contacts are isolated by a spacer layer, and the material of the spacer layer may be silicon nitride (SiN), silicon oxide (SiO 2 ), aluminum oxide (Al 2 O 3 ) or a combination of any two or more thereof. In this embodiment, the material of the spacer layer is SiN.
[0228] As an example, the dielectric layer includes a first dielectric sacrificial layer 302, a second dielectric sacrificial layer 303 and a third dielectric sacrificial layer 305, and the supporting layer includes a first supporting layer 304 and a second supporting layer 306, wherein the first dielectric sacrificial layer 302, the second dielectric sacrificial layer 303, the first supporting layer 304, the third dielectric sacrificial layer 305 and the second supporting layer 306 are stacked in sequence from bottom to top.
[0229] As an example, the material of the etch stop layer 301 includes silicon nitride, and the thickness of the etch stop layer 301 is between 10nm and 80nm; the material of the first dielectric layer 302 includes at least one of phosphorus-doped silicon oxide (PSG), boron-phosphorus-doped oxide layer (BPSG) and fluorine-doped silicon oxide glass (FSG), and the thickness of the first dielectric sacrificial layer 302 is between 100nm and 600nm; preferably, the hardness of the second dielectric sacrificial layer 303 is greater than the hardness of the first dielectric sacrificial layer 302 to improve the stability of the subsequent capacitor structure, and the second dielectric sacrificial layer 303 is preferably greater than the hardness of the first dielectric sacrificial layer 302. The material of layer 303 includes TEOS, and the thickness of the second dielectric sacrificial layer 303 is between 300nm and 1000nm; the material of the third dielectric sacrificial layer 305 includes at least one of silicon oxide and TEOS, and the thickness of the third dielectric sacrificial layer 305 is between 300nm and 1000nm; the material of the first supporting layer 304 includes silicon nitride, and the thickness of the first supporting layer 304 is between 10nm and 80nm; the material of the second supporting layer 306 includes silicon nitride, and the thickness of the second supporting layer 306 is between 50nm and 200nm.
[0230] Specifically, this example provides a laminated material layer that can subsequently form a memory capacitor hole 307a, wherein a laminated dielectric sacrificial layer and a two-layer support layer structure are introduced. Due to the reduction in capacitor size and the increase in height, the capacitor is easily tilted to form a short circuit. Therefore, two layers of support layers (Nitride) are introduced and matched with the configuration of three layers of dielectric sacrificial layers, which can achieve the effect of fixing the capacitor and prevent the capacitor from shorting due to tilting. In addition, since the capacitor is deep hole etched, in order to reduce the occurrence of bottom Undercut, the first dielectric sacrificial layer is preferably made of relatively soft materials such as PSG / BPSG / FSG, and the hardness of the second dielectric sacrificial layer 303 is preferably greater than the hardness of the first dielectric sacrificial layer 302, and can be TEOS material or PSG / BPSG / FSG with a faster deposition speed than the first dielectric sacrificial layer 302. In addition, the third dielectric sacrificial layer 305 can be made of materials such as SiO2 or TEOS to achieve the required capacitor height.
[0231] In addition, in the process of etching the etch stop layer, the dielectric sacrificial layer and the supporting layer, it is preferred to use a CCP machine for etching. The etching process of the second supporting layer 306 includes: the etching gas includes at least one of C4F8, CHF3, CF4, and CH2F2 and the etching is carried out under the conditions of pressure 5-50mt / 2MHZ 1000-5000W / 27MHZ 50-300W / 60MHZ 200-1000W; the etching process of the third dielectric sacrificial layer 305 includes: the etching gas includes at least one of O2, C4F6, and NF3 and the etching is carried out under the conditions of pressure 5-30mt / 2MHZ 4000-8000W / 60MHZ 500~1500W is used for etching; the etching process of the first supporting layer 304 includes: the etching gas includes at least one of C4F6, O2, C4F8, NF3 and CH2F2 and the etching is carried out under the conditions of pressure 5~50mt / 2MHZ 1000~5000W / 27MHZ 100~500W / 60MHZ 200~800W; the etching process of the second dielectric sacrificial layer 303 includes: the etching gas includes at least one of C4F6, O2 and NF3 and the etching is carried out under the conditions of pressure 5~30mt 2MHZ 4000~8000W / 60MHZ 500~2000W; the etching process of the first dielectric sacrificial layer 302 includes: the etching gas includes at least one of C4F6, O2 and NF3 and the etching is carried out under the conditions of pressure 5~30mt 2MHZ 4000~8000W / 60MHZ The etching process of the etching stop layer 301 includes: the etching gas includes at least one of O2, CHF3, CH2F2 and the etching is performed under the conditions of pressure 5~50mt / 2MHZ 200~1000W / 27MHZ 50~300W / 60MHZ 200~1000W.
[0232] As an example, the support layer (304, 306), the dielectric sacrificial layer (302, 303, 305) and the etching stop layer 301 are etched by pulse radio frequency etching, wherein the etching cycle of the pulse radio frequency etching includes one pulse on and one pulse off, etching is performed when the pulse is on, and by-products are discharged when the pulse is off, and the pulse on time accounts for 70% to 90% of the etching cycle of the pulse radio frequency etching.
[0233] Specifically, since the etching depth is relatively deep, in order to make the Profile better, the Pulse Etch method is preferably used. Here, the RF on period in the Recipe setting is changed from 100% to 70%-90%, and the entire RF time is also increased in the same proportion to ensure that the RF on time is sufficient.
[0234] The present invention also provides a laminated structure in the process of preparing a semiconductor memory capacitor hole, see Figures 28-30 As shown, the stacked structure is preferably prepared by the process used in the semiconductor memory capacitor hole preparation process in this embodiment, including:
[0235] A semiconductor substrate 100;
[0236] The capacitor support sacrificial structure layer 300 comprises an etch stop layer 301 and at least one dielectric sacrificial layer (302, 303, 305) and at least one support layer (304, 306) located on the etch stop layer 301, and the etch stop layer 301 is located on the surface of the semiconductor substrate 100;
[0237] A hard mask consumption layer 101 is located on the surface of the capacitor support structure layer 300;
[0238] A double pattern integration layer 102 is located on the surface of the hard mask sacrificial layer 101; and
[0239] The pattern transfer layer 122 is located on the double pattern integration layer 102, and includes a plurality of first spacing multiplication units 122a arranged in parallel and spaced apart along a first direction, and a plurality of second spacing multiplication units 122b arranged in parallel and spaced apart along a second direction and connected to the first spacing multiplication units, wherein the second direction and the first direction have an intersection angle, and a first spacing is generated between adjacent first spacing multiplication units, and a second spacing is generated between adjacent second spacing multiplication units, and the first spacing and the second spacing are both defined by the thickness of individual spacing sacrificial layers.
[0240] As an example, the pattern transfer layer 122 formed includes at least one of a grid-shaped pattern transfer layer and a diamond-shaped pattern transfer layer.
[0241] Specifically, the graphic pattern in the graphic transfer layer 122 formed in this example is selected according to actual conditions, and can be a mesh pattern. For example, when the first direction and the second direction are perpendicular to each other, the pattern morphology in the graphic transfer layer 122 is a cross-grid shape, that is, a plurality of squares of uniform size and uniform array arrangement are formed. Of course, in other examples, it can be selected according to needs, such as forming a diamond-shaped pattern structure layer of uniform size.
[0242] As an example, the stacked structure in the preparation process of the semiconductor memory capacitor hole also includes a first graphic mask replication layer 308, which is used to form the first spacing multiplication unit 122a, the first graphic mask replication layer includes a plurality of first pattern units arranged in parallel and spaced apart and a plurality of second pattern units located between adjacent first pattern units, the second pattern unit includes a first bottom deposition layer and a first top deposition layer located on the first bottom deposition layer, and the spacing between adjacent first pattern units and the second pattern units is approximately the same as the thickness of the first bottom deposition layer.
[0243] Specifically, this example provides a first pattern mask replication layer 308 that can form the first pitch multiplication unit 122a. For details, see Fig.11 As shown, the first pattern unit in this example can be seen in Fig.11 The second pattern unit 106a in this example can be seen in Fig.11 The pattern auxiliary unit 111 in the figure, wherein the bottom deposition layer is equivalent to the second lateral portion 107d of the first spacer sacrificial layer in the figure, and the top deposition layer is equivalent to the remaining first filling mask layer 109a in the figure.
[0244] As an example, the stacked structure in the preparation process of the semiconductor memory capacitor hole also includes a second graphic mask replication layer 120. In this case, the second graphic mask replication layer can be the fifth pattern layer in the preparation process of the semiconductor memory in the embodiment of the present invention, which is used to form the second spacing multiplication unit. The second graphic mask replication layer includes a plurality of third pattern units arranged in parallel and spaced apart and a plurality of fourth pattern units located between adjacent third pattern units. The fourth pattern unit includes a second bottom deposition layer and a second top deposition layer located on the second bottom deposition layer, and the spacing between adjacent third pattern units and the fourth pattern unit is approximately the same as the thickness of the second bottom deposition layer.
[0245] Specifically, this example provides a pattern that can form the second spacing multiplication unit 122b. For details, see Fig.23 and Fig.24 As shown, the third pattern unit in this example is equivalent to the fourth pattern unit 117a in the figure, the fourth pattern unit in this example is equivalent to the fifth pattern unit 120a, wherein the second bottom deposition layer is equivalent to the fourth lateral portion 118d of the second spacing sacrificial layer in the figure, and the second top deposition layer is equivalent to the remaining second filling mask layer 119a.
[0246] As an example, the dielectric layer includes a first dielectric sacrificial layer 302, a second dielectric sacrificial layer 303 and a third dielectric sacrificial layer 305, and the supporting layer includes a first supporting layer 304 and a second supporting layer 306, wherein the first dielectric sacrificial layer 302, the second dielectric sacrificial layer 303, the first supporting layer 304, the third dielectric sacrificial layer 305 and the second supporting layer 306 are stacked in sequence from bottom to top.
[0247] As an example, the etch stop layer 301 includes a silicon nitride layer, and the thickness of the etch stop layer 301 is between 10nm and 80nm; the first dielectric sacrificial layer 302 includes at least one of a phosphorus-doped silicon oxide layer (PSG layer), a boron-phosphorus-doped oxide layer (BPSG layer) and a fluorine-doped silicon oxide glass layer (FSG layer), and the thickness of the first dielectric sacrificial layer 302 is between 100nm and 600nm; preferably, the hardness of the second dielectric sacrificial layer 303 is greater than the hardness of the first dielectric sacrificial layer 302, so as to improve the stability of the subsequent capacitor structure, and the first dielectric sacrificial layer 303 is preferably greater than the hardness of the first dielectric sacrificial layer 302. The second dielectric sacrificial layer 303 includes a TEOS layer, and the thickness of the second dielectric sacrificial layer 303 is between 300nm and 1000nm; the third dielectric sacrificial layer 305 includes at least one of a silicon oxide layer and a TEOS layer, and the thickness of the third dielectric sacrificial layer 305 is between 300nm and 1000nm; the first supporting layer 304 includes a silicon nitride layer, and the thickness of the first supporting layer 304 is between 10nm and 80nm; the second supporting layer 306 includes a silicon nitride layer, and the thickness of the second supporting layer 306 is between 50nm and 200nm.
[0248] Specifically, this example provides a laminated material layer that can subsequently form the capacitor support structure 307b and the memory capacitor hole 307a, wherein a laminated dielectric sacrificial layer and a two-layer support layer structure are introduced. Due to the reduction in capacitor size and the increase in height, the capacitor is easily tipped over to form a short circuit. Therefore, two layers of support layers (Nitride) are introduced and matched with the configuration of three layers of dielectric sacrificial layers, which can achieve the effect of fixing the capacitor and prevent the capacitor from tipping over and causing a short circuit. In addition, since the capacitor is deep hole etched, in order to reduce the occurrence of bottom Undercut, the first dielectric sacrificial layer is preferably made of relatively soft materials such as PSG / BPSG / FSG, and the hardness of the second dielectric sacrificial layer 303 is preferably greater than the hardness of the first dielectric sacrificial layer 302, and can be TEOS material or PSG / BPSG / FSG with a faster deposition speed than the first dielectric sacrificial layer 302. In addition, the third dielectric sacrificial layer 305 can be made of materials such as SiO2 or TEOS to achieve the required capacitor height.
[0249] As an example, the intersection angle includes 60°; the first spacing multiplication units 122a are arranged in parallel with equal spacing, and the second spacing multiplication units 122b are arranged in parallel with equal spacing; the width of the first spacing multiplication unit is equal to the width of the second spacing multiplication unit; the width of the first spacing is equal to the width of the second spacing.
[0250] As an example, the double pattern integration layer 102 in the stacked junction in the process of preparing the semiconductor memory capacitor hole is used to form the patterned hard mask consumption layer, see Figures 28-30 As shown, the double pattern integration layer 102 includes a first pad layer 102a, a second pad layer 102b, a third pad layer 102c and a fourth pad layer 102d from bottom to top. The present invention can correct the pattern in the etching process and obtain a pattern with precise morphology through the design of the above four pad layers.
[0251] As an example, the first pad layer 102a is selected from any one of a silicon oxide layer and a tetraethyl orthosilicate (TEOS) layer, the second pad layer 102b is selected from any one of an amorphous silicon layer, a silicon oxynitride layer and a silicon nitride layer, the third pad layer 102c is selected from any one of a silicon oxide layer and a tetraethyl orthosilicate (TEOS) layer, and the fourth pad layer 102d is selected from any one of an amorphous silicon layer, a silicon oxynitride layer and a silicon nitride layer.
[0252] As an example, the stacked structure in the preparation process of the semiconductor memory capacitor hole also includes a pattern transfer hard mask layer, which is used to transfer the pattern to form at least one of the first spacing multiplication unit 122a and the second spacing multiplication unit 122b, wherein the pattern transfer hard mask layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC).
[0253] Specifically, in a preferred embodiment, the pattern transfer hard mask layer includes a stacked structure of two material layers, including an ashable hard mask layer (AHM, Ashable hard mask carbon) and a diamond-like carbon film layer (DLC, Diamond like carbon) located on its upper surface, wherein the thickness of the ashable hard mask layer is between 50nm and 200nm, preferably between 100nm and 150nm, and the thickness of the diamond-like carbon film layer is between 200nm and 300nm, preferably between 120nm and 180nm; further preferably, the thickness of the diamond-like carbon film layer is greater than the thickness of the ashable hard mask layer. In this example, the mask layer is subjected to the above-mentioned structural improvement for etching to form the first pattern spacing multiplication unit, or for forming the second spacing multiplication unit, which has a better selectivity than carbon and other mask materials, so that the migrated pattern is more precise and easier to be removed by oxygen (O2).
[0254] like Fig.47 and Fig.48 As shown, as an example, the capacitor supporting sacrificial structure layer 300 has a plurality of semiconductor memory capacitor holes 307a arranged at uniform intervals; the present invention also provides a semiconductor memory capacitor hole structure, the semiconductor memory capacitor hole structure includes a stacked structure layer in the preparation process of the semiconductor memory capacitor hole as described in any of the above schemes and a semiconductor device layer 307 formed by etching the auxiliary structure layer based on the mesh pattern transfer layer, the semiconductor device layer is located on the semiconductor substrate, and the semiconductor device layer 307 includes a plurality of semiconductor memory capacitor holes 307a arranged at uniform intervals formed by etching.
[0255] In summary, the present invention provides a method for preparing a semiconductor memory capacitor hole, comprising: 1) providing a semiconductor substrate, and sequentially forming a capacitor support sacrificial structure layer, a hard mask consumption layer, a double pattern integration layer, a first graphic migration layer and a first mask layer on the semiconductor substrate, wherein the first mask layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC); 2) forming a first pattern layer arranged along a first direction on the first mask layer, wherein the first pattern layer includes a plurality of first pattern units arranged in parallel and spaced apart; 3) transferring the pattern on the first pattern layer to the first graphic migration layer via the first mask layer to form a second pattern layer, wherein the second pattern layer includes A plurality of second pattern units arranged in parallel and spaced relation; 4) forming a first spacing sacrificial layer on the top, sidewalls and surface of the double pattern integration layer between the second pattern units, and forming a first gap groove on the surface of the first spacing sacrificial layer between adjacent second pattern units, and forming a first filling mask layer on the surface of the first spacing sacrificial layer, wherein the first filling mask layer covers the first spacing sacrificial layer and fills the first gap groove formed by the first spacing sacrificial layer; 5) removing the first lateral portion of the first spacing sacrificial layer located at the top of the second pattern unit, the first filling mask layer and a portion of the first filling mask layer located in the first gap groove, wherein adjacent A size defining unit and a pattern auxiliary unit located between the size defining units are formed between the second pattern units, the first longitudinal portion of the first spacer sacrificial layer located on the side wall of the second pattern unit forms the size defining unit, the second lateral portion of the first spacer sacrificial layer located on the double pattern integration layer and the remaining first filling mask layer located on the second lateral portion form the pattern auxiliary unit; 6) forming an etching stop layer, a second graphic migration layer and a second mask layer in sequence on the structure obtained in step 5); 7) forming a third pattern layer arranged along a second direction on the second mask layer, the third pattern layer comprising a plurality of third pattern units arranged in parallel and spaced apart, wherein the second The direction has an intersection angle with the first direction; 8) transferring the pattern on the third pattern layer to the second pattern migration layer through the second mask layer to form a fourth pattern layer, wherein the fourth pattern layer includes a plurality of fourth pattern units arranged in parallel and spaced apart; 9) forming a second spacing sacrificial layer on the top, sidewalls and the surface of the etching stop layer between the four pattern units, and forming a second gap groove on the surface of the second spacing sacrificial layer between adjacent fourth pattern units, and forming a second filling mask layer on the surface of the second spacing sacrificial layer, wherein the second filling mask layer covers the second spacing sacrificial layer and fills the second gap groove formed by the second spacing sacrificial layer;10) planarizing the structure obtained in step 9) until the top surface of the second spacer sacrificial layer is exposed, and the remaining second filling mask layer between the second longitudinal portions of the second spacer sacrificial layer on the side wall of the fourth pattern unit is retained; 11) etching and removing the third lateral portion of the second spacer sacrificial layer located at the top of the fourth pattern unit and the second longitudinal portion of the second spacer sacrificial layer located on the side wall of the fourth pattern unit to expose the etch stop layer and obtain a fifth pattern layer, wherein the fifth pattern layer includes a plurality of fifth pattern units arranged in parallel and spaced apart, wherein the fourth pattern unit located on the etch stop layer, the fourth lateral portion of the second spacer sacrificial layer located on the surface of the etch stop layer, and the remaining second filling mask layer located on the fourth lateral portion form the fifth pattern unit; 12) using the fifth pattern unit as a mask, selectively etching and removing The etch stop layer and the size limiting unit are used to transfer the pattern on the fifth pattern layer to the second pattern layer to form a pattern transfer layer on the double pattern integration layer, wherein the pattern transfer layer includes a plurality of first spacing multiplication units arranged in parallel and spaced apart along the first direction and a plurality of second spacing multiplication units arranged in parallel and spaced apart along the second direction and connected to the first spacing multiplication unit, wherein the first spacing multiplication unit is composed of the second pattern unit and the pattern auxiliary unit, and the second spacing multiplication unit is formed by transferring the fifth pattern unit; and 13) transferring the pattern on the pattern transfer layer to the hard mask consuming layer via the double pattern integration layer to obtain a patterned hard mask consuming layer, and etching the capacitor support sacrificial structure layer based on the patterned hard mask consuming layer to form a plurality of semiconductor memory capacitor holes evenly spaced apart in the capacitor support structure layer. Through the above scheme, the semiconductor structure layer preparation based on pitch doubling of the present invention uses two directions to form sidewall layers (spacer) to double the pattern. Based on this pitch doubling technology, the pattern miniaturization can be achieved in the process of 30nm and below. Furthermore, the present invention controls the dimensions of the two directions in the preparation process to achieve good uniformity of the pitch doubling pattern. Further, the definition of the feature size in the device structure is improved to solve the problem of large and small holes. By improving the double pattern integration layer in the etching process, the pattern is corrected in the preparation process to improve the accuracy of the pattern. In addition, the present invention also improves the structural layer to achieve a better selection ratio, improve the capacitor size defects, and improve the yield. Therefore, the present invention effectively overcomes the various shortcomings of the prior art and has a high industrial utilization value. ;
[0256] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a semiconductor memory capacitor hole, characterized in that: The steps include: 1) providing a semiconductor substrate, and sequentially forming a capacitor support sacrificial structure layer, a hard mask consumption layer, a double pattern integration layer, a first pattern migration layer and a first mask layer on the semiconductor substrate, wherein the first mask layer comprises at least one of an ashing hard mask layer (AHM) and a diamond-like carbon film layer (DLC); 2) forming a first pattern layer arranged along a first direction on the first mask layer, wherein the first pattern layer comprises a plurality of first pattern units arranged in parallel and at intervals; 3) transferring the pattern on the first pattern layer to the first pattern migration layer via the first mask layer to form a second pattern layer, wherein the second pattern layer includes a plurality of second pattern units arranged in parallel and at intervals; 4) forming a first spacer sacrificial layer on the top, sidewalls and the surface of the double pattern integration layer between the second pattern units, forming a first gap groove on the surface of the first spacer sacrificial layer between adjacent second pattern units, and forming a first filling mask layer on the surface of the first spacer sacrificial layer, wherein the first filling mask layer covers the first spacer sacrificial layer and fills the first gap groove; 5) removing the first lateral portion of the first spacer sacrificial layer located at the top of the second pattern unit, the first filling mask layer and a portion of the first filling mask layer located in the first gap groove, wherein a size defining unit and a pattern auxiliary unit located between the size defining units are formed between adjacent second pattern units, the first longitudinal portion of the first spacer sacrificial layer located on the sidewall of the second pattern unit forms the size defining unit, and the second lateral portion of the first spacer sacrificial layer located on the double pattern integration layer and the remaining first filling mask layer located on the second lateral portion form the pattern auxiliary unit; 6) forming an etch stop layer, a second pattern migration layer and a second mask layer in sequence on the structure obtained in step 5); 7) forming a third pattern layer arranged along a second direction on the second mask layer, wherein the third pattern layer comprises a plurality of third pattern units arranged in parallel and spaced apart, wherein the second direction and the first direction have an intersection angle; 8) transferring the pattern on the third pattern layer to the second pattern migration layer via the second mask layer to form a fourth pattern layer, wherein the fourth pattern layer includes a plurality of fourth pattern units arranged in parallel and at intervals; 9) forming a second spacer sacrificial layer on the top and sidewalls of the four pattern units and on the surface of the etch stop layer between the fourth pattern units, and forming a second gap groove on the surface of the second spacer sacrificial layer between adjacent fourth pattern units, and forming a second filling mask layer on the surface of the second spacer sacrificial layer, wherein the second filling mask layer covers the second spacer sacrificial layer and fills the second gap groove; 10) planarizing the structure obtained in step 9) until the top surface of the second sacrificial spacer layer is exposed, and the remaining second filling mask layer between the second longitudinal portions of the second sacrificial spacer layer on the sidewalls of the fourth pattern unit is retained; 11) etching and removing the third transverse portion and the second longitudinal portion of the second spacer sacrificial layer located at the top of the fourth pattern unit to expose the etch stop layer and obtain a fifth pattern layer, wherein the fifth pattern layer comprises a plurality of fifth pattern units arranged in parallel and spaced apart, wherein the fourth pattern unit located on the etch stop layer, the fourth transverse portion of the second spacer sacrificial layer located on the surface of the etch stop layer, and the remaining second filling mask layer located on the fourth transverse portion constitute a stacked layer forming the fifth pattern unit; 12) using the fifth pattern unit as a mask, selectively etching away the etch stop layer and the dimension defining unit, so as to transfer the pattern on the fifth pattern layer to the second pattern layer, so as to form a pattern transfer layer on the double pattern integration layer, wherein the pattern transfer layer comprises a plurality of first spacing multiplication units arranged in parallel and spaced apart along the first direction, and a plurality of second spacing multiplication units arranged in parallel and spaced apart along the second direction and connected to the first spacing multiplication units, wherein the first spacing multiplication unit is composed of the second pattern unit and the pattern auxiliary unit, and the second spacing multiplication unit is formed by transferring the fifth pattern unit; and 13) Transferring the pattern of the pattern transfer layer to the hard mask consuming layer via the double pattern integration layer to obtain a patterned hard mask consuming layer, and etching the capacitor support sacrificial structure layer based on the patterned hard mask consuming layer to form a plurality of semiconductor memory capacitor holes evenly spaced in the capacitor support sacrificial structure layer.
2. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: In step 1), the double-pattern integration layer includes a first pad layer, a second pad layer, a third pad layer and a fourth pad layer from bottom to top.
3. The method for preparing a semiconductor memory capacitor hole according to claim 2, characterized in that: The material of the first pad layer includes any one of silicon oxide and tetraethyl orthosilicate, and the thickness of the first pad layer is between 100nm and 500nm; the material of the second pad layer includes any one of amorphous silicon, silicon oxynitride and silicon nitride, and the thickness of the second pad layer is between 100nm and 800nm; the material of the third pad layer includes any one of silicon oxide and tetraethyl orthosilicate, and the thickness of the third pad layer is between 100nm and 500nm; the material of the fourth pad layer includes any one of amorphous silicon, silicon oxynitride and silicon nitride, and the thickness of the fourth pad layer is between 50nm and 200nm.
4. The method for preparing a semiconductor memory capacitor hole according to claim 2, characterized in that: Before transferring the pattern on the pattern transfer layer to the hard mask consumption layer in step 13), the method further includes: transferring the pattern on the pattern transfer layer to the double pattern integration layer, and the specific steps include: 13-1) etching the fourth pad layer using the pattern transfer layer as a mask to obtain a first intermediate pattern transfer layer, and retaining the pattern transfer layer remaining after etching; 13-2) depositing a pattern-optimized sacrificial layer on the surface of the structure obtained in step 13-1), wherein the pattern-optimized sacrificial layer fills the gap between the first intermediate pattern transfer layer and the remaining pattern transfer layer and covers the remaining pattern transfer layer; 13-3) planarizing the pattern optimization sacrificial layer to the remaining pattern transfer layer, and removing the remaining pattern transfer layer, wherein the pattern optimization sacrificial layer is converted into a second intermediate pattern transfer layer; 13-4) removing the second intermediate pattern transfer layer, and etching the third pad layer based on the first intermediate pattern transfer layer obtained by etching in step 13-1) to obtain a third intermediate pattern transfer layer, and adjusting the size of the pattern in the first direction and the second direction during etching the third pad layer; and 13-5) etching the second cushion layer to obtain a fourth intermediate pattern transfer layer, and etching the first cushion layer using the fourth intermediate pattern transfer layer obtained by etching as a mask to obtain a fifth intermediate pattern transfer layer, so as to transfer the pattern on the pattern transfer layer to the first cushion layer.
5. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: In step 1), the first pattern transfer layer includes a bottom pattern transfer layer and an upper pattern transfer layer located on the bottom pattern transfer layer, wherein the bottom pattern transfer layer includes at least one of a silicon oxide layer and a tetraethyl orthosilicate (TEOS) layer, and the upper pattern transfer layer includes a silicon-rich photoresist layer; and in step 3), the pattern on the first pattern layer is transferred to the bottom pattern transfer layer to form the second pattern layer.
6. The method for preparing a semiconductor memory capacitor hole according to claim 5, characterized in that: Step 3) includes: etching the first mask layer to transfer the pattern on the first pattern layer to the first mask layer, wherein the process parameters for etching the first mask layer include: the etching gas includes at least one of O2, Ar, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V; Step 3) also includes: etching the upper pattern transfer layer and the bottom pattern transfer layer to transfer the pattern on the first pattern layer to the bottom pattern transfer layer, wherein the process parameters for etching the upper pattern transfer layer include: the etching gas includes at least one of N2, O2 and He; the process parameters for etching the bottom pattern transfer layer include: the etching gas includes at least CH4 and CHF3, and the ratio of CH4 to CHF3 is between 3:1 and 1:1, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V.
7. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: Step 4) also includes: depositing a planarization auxiliary layer on the surface of the first filling mask layer.
8. The method for preparing a semiconductor memory capacitor hole according to claim 7, characterized in that: The planarization auxiliary layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like carbon film layer (DLC); the thickness of the planarization auxiliary layer is between 20nm and 100nm.
9. The method for preparing a semiconductor memory capacitor hole according to claim 7, characterized in that: In step 5), planarizing the structure obtained in step 4) to the second pattern layer includes: etching the planarization auxiliary layer, etching the first filling mask layer, and etching the first lateral portion of the first spacing sacrificial layer at the top of the second pattern unit, wherein the process parameters for etching the planarization auxiliary layer include: the etching gas includes at least one of O2, Ar, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V; the process parameters for etching the first filling mask layer Including: the etching gas includes at least CH4 and CHF3, and the ratio of CH4 to CHF3 is between 3:1 and 1:1, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V; the process parameters for etching the first spacer sacrificial layer at the top of the second pattern unit include: the etching gas includes at least one of CHF3, CH4 and SF6, the etching pressure is between 5mT and 30mT, the source power is between 300W and 600W, and the bias voltage is between 50V and 250V.
10. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: Step 6) also includes: forming a stress relief layer between the etch stop layer and the second graphic migration layer; and step 11) simultaneously etches the stress relief layer during the process of etching and removing the second longitudinal portion of the second spacing sacrificial layer.
11. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: Step 8) includes: etching the second mask layer to transfer the pattern of the third pattern layer to the second mask layer, and the process parameters for etching the second mask layer include: the etching gas includes at least one of O2, Ar, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V; Step 8) also includes: etching the second graphic migration layer to transfer the pattern of the third pattern layer to the second graphic migration layer, and the process parameters for etching the second graphic migration layer include: the etching gas includes at least one of N2, O2 and He.
12. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: In step 10), planarizing the structure obtained in step 9) to the second spacer sacrificial layer includes: etching the second filling mask layer, and the process parameters for etching the second filling mask layer include: the etching gas includes at least one of O2, Ar, N2 and CH4, the etching pressure is between 5mT and 20mT, the source power is between 200W and 600W, and the bias voltage is between 200V and 600V.
13. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: In step 11), the process parameters for etching and removing the third lateral portion and the second longitudinal portion of the second spacer sacrificial layer include: the etching gas includes at least one of O2, CH4 and CHF3, the etching pressure is between 1mT and 10mT, the source power is between 300W and 800W, and the bias voltage is between 10V and 100V.
14. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: In step 12), the pattern transfer layer formed includes at least one of a grid-shaped pattern transfer layer and a diamond-shaped pattern transfer layer.
15. The method for preparing a semiconductor memory capacitor hole according to claim 1, characterized in that: In step 1), the capacitor support sacrificial structure layer includes an etch stop layer located on the semiconductor substrate and at least one dielectric sacrificial layer and at least one support layer located on the etch stop layer; Step 13) includes: etching the support layer, the dielectric sacrificial layer and the etching stop layer based on the patterned hard mask consumable layer, and removing the patterned hard mask consumable layer remaining after etching, so as to etch on the semiconductor substrate to form a plurality of evenly spaced semiconductor memory capacitor holes located in the capacitor support sacrificial structure layer.
16. The method for preparing a semiconductor memory capacitor hole according to claim 15, characterized in that: The support layer, the dielectric sacrificial layer and the etching stop layer are etched by pulse radio frequency etching, wherein the etching cycle of the pulse radio frequency etching includes one pulse on and one pulse off, etching is performed when the pulse is on, and by-products are discharged when the pulse is off, and the pulse on time accounts for 70% to 90% of the etching cycle of the pulse radio frequency etching.
17. The method for preparing a semiconductor memory capacitor hole according to claim 15, characterized in that: The dielectric sacrificial layer includes a first dielectric sacrificial layer, a second dielectric sacrificial layer and a third dielectric sacrificial layer, and the supporting layer includes a first supporting layer and a second supporting layer, wherein the first dielectric sacrificial layer, the second dielectric sacrificial layer, the first supporting layer, the third dielectric sacrificial layer and the second supporting layer are stacked in sequence from bottom to top.
18. The method for preparing a semiconductor memory capacitor hole according to claim 17, characterized in that: The material of the etch stop layer includes silicon nitride, and the thickness of the etch stop layer is between 10nm and 80nm; the material of the first dielectric sacrificial layer includes at least one of phosphorus-doped silicon oxide (PSG), boron-phosphorus-doped oxide (BPSG) and fluorine-doped silicon oxide glass (FSG), and the thickness of the first dielectric sacrificial layer is between 100nm and 600nm; the hardness of the second dielectric sacrificial layer is greater than the hardness of the first dielectric sacrificial layer, the material of the second dielectric sacrificial layer includes TEOS, and the thickness of the second dielectric sacrificial layer is between 300nm and 1000nm; the material of the third dielectric sacrificial layer includes at least one of silicon oxide and TEOS, and the thickness of the third dielectric sacrificial layer is between 300nm and 1000nm; the material of the first supporting layer includes silicon nitride, and the thickness of the first supporting layer is between 10nm and 80nm; the material of the second supporting layer includes silicon nitride, and the thickness of the second supporting layer is between 50nm and 200nm.
19. The method for preparing a semiconductor memory capacitor hole according to any one of claims 1 to 18, characterized in that: In step 6), the second mask layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC); in step 9), the second filling mask layer includes at least one of an ashable hard mask layer (AHM) and a diamond-like film layer (DLC).