Aromatic base

By using the curable compounds of the C5-6 aromatic ring and C9-30 fused aromatic ring system as the base material in semiconductor manufacturing, the problems of thermal setting and high absorbance of the base material in the prior art are solved, and high absorption is achieved in the existing technology. The planarization and etch selectivity of the aspect ratio resist pattern meet the requirements of high temperature stability and reflection characteristics.

CN111142328BActive Publication Date: 2024-11-05杜邦电子材料国际有限责任公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911057209.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-11-02
Filing Date
2019-10-31
Publication Date
2024-11-05
Estimated Expiration
2039-10-31

AI Technical Summary

Technical Problem

In the existing semiconductor manufacturing process, the underlying material is heat-set at high temperatures and has high absorbance, resulting in insufficient etch selectivity and reflection characteristics, and it is difficult to meet the planarization and stability requirements of high aspect ratio resist patterns.

Method used

Using curable compounds containing C5-6 aromatic rings and C9-30 fused aromatic ring systems aromatic cores as the base material, a planarization layer is formed on the substrate by spin coating process and cured at high temperatures to provide low reflectivity and Etching selectivity.

Benefits of technology

The formation of a stable bottom layer at high temperature is achieved, the planarization and etch selectivity of the resist pattern are improved, the demand for high aspect ratio patterns is met, and the stability is maintained in the subsequent silicon oxynitride CVD process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002255444540000021
    Figure BDA0002255444540000021
  • Figure BDA0002255444540000022
    Figure BDA0002255444540000022
  • Figure BDA0002255444540000031
    Figure BDA0002255444540000031
Patent Text Reader

Abstract

Compounds having three or more alkynyl moieties substituted with aromatic moieties having one or more of certain substituents can be used to form bottom layers useful in semiconductor manufacturing processes.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates generally to the field of manufacturing electronic devices, and more particularly to the field of materials used as substrates in semiconductor manufacturing.

[0002] It is well known in photolithography that if the resist pattern is too high (high aspect ratio), the resist pattern may collapse due to the surface tension from the developer used. Multilayer resist processes (such as three-layer and four-layer processes) have been designed, which can solve this problem of pattern collapse when high aspect ratio is desired. Such multilayer processes use a resist top layer, one or more intermediate layers, and a bottom layer (or bottom layer) (or underlayer). In such multilayer resist processes, the top photoresist layer is imaged and developed in a typical manner to provide the resist pattern. The pattern is then typically transferred to one or more intermediate layers by etching. Each intermediate layer is selected so that different etching processes are used, such as different plasma etchings. Finally, the pattern is typically transferred to the bottom layer by etching. Such intermediate layer can be made of a variety of materials, but the bottom material is typically made of high carbon content materials. The bottom material is selected to provide desired anti-reflection properties, planarization properties, and etching selectivity.

[0003] Existing technologies for bottom layers include chemical vapor deposition (CVD) carbon and solution-processed high carbon content polymers. CVD materials have several significant limitations, including high cost of ownership, inability to form a planarization layer on the topography on the substrate, and high absorbance at 633nm for pattern alignment. For these reasons, the industry has turned to solution-processed high carbon content materials as bottom layers. The ideal bottom layer needs to meet the following characteristics: able to be cast onto the substrate by a spin coating process; heat-set when heated, with low outgassing and sublimation; soluble in common processing solvents with good equipment compatibility; have appropriate n and k values ​​to work in conjunction with the currently used silicon hard mask and bottom anti-reflective (BARC) layer to give the low reflectivity necessary for photoresist imaging, and be thermally stable up to >400°C so as not to be damaged during the subsequent silicon oxynitride (SiON) CVD process.

[0004] It is well known that materials with relatively low molecular weight have relatively low viscosity and flow into features in the substrate such as vias and trenches to provide a planarizing layer. The underlayer material must be capable of planarization with relatively low outgassing up to 400°C. For use as a high carbon content underlayer, any composition must be heat set when heated. U.S. Patent No. 9,581,905 B2 discloses a compound having the formula

[0005]

[0006] Wherein R1, R2 and R3 are each independently represented by the formula RA -C≡CR B -, where R A In particular, it may be an aryl group substituted with at least one of a hydroxyl group and an aryl group, and R B is a single bond or an aromatic group, wherein such compounds can be used to form a bottom layer in semiconductor device manufacturing. Such compounds solidify at relatively high temperatures. There is still a need for the following materials: they solidify at relatively low temperatures and can be used to form a bottom layer in semiconductor manufacturing processes.

[0007] The present invention provides a method, which comprises: (a) providing an electronic device substrate; (b) coating a coating composition layer comprising one or more curable compounds on the surface of the electronic device substrate, wherein the one or more curable compounds comprise a 5-6 Aromatic ring and C 9-30 The aromatic nucleus of the fused aromatic ring system and three or more substituents having the formula (1)

[0008]

[0009] wherein at least two substituents having formula (1) are attached to the aromatic core; and wherein Ar 1 is an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Z is a substituent selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x is an integer from 1 to 4; and * represents an attachment point to the aromatic core; (c) curing the layer of the curable compound to form a bottom layer; (d) coating a photoresist layer on the bottom layer; (e) exposing the photoresist layer to actinic radiation through a mask; (f) developing the exposed photoresist layer to form a resist pattern; and (g) transferring the pattern to the bottom layer to expose a portion of the electronic device substrate.

[0010] The present invention also provides an electronic device comprising an electronic device substrate, the electronic device substrate having a polymer layer on a surface of the electronic device substrate, the polymer comprising one or more curable compounds as polymerized units, wherein the one or more curable compounds comprises a 5-6 Aromatic ring and C 9-30 The aromatic nucleus of the fused aromatic ring system and three or more substituents having the formula (1)

[0011]

[0012] wherein at least two substituents having formula (1) are attached to the aromatic core; and wherein Ar 1 is an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Z is a substituent selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x is an integer from 1 to 4; and * represents the point of attachment to the aromatic core.

[0013] The present invention further provides a compound having formula (2)

[0014]

[0015] Among them, Ar c is an aromatic nucleus having 5 to 30 carbon atoms; Ar 1 ,Ar 2 , and Ar 3 Each is independently an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Y is a covalent chemical single bond, a divalent linking group, or a trivalent linking group; Z 1 and Z 2 are independently selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x1 = 1 to 4; x2 = 1 to 4; y1 = 2 to 4; each y2 = 0 to 4; y1 + each y2 ≥ 3; w = 0 to 2; and z is equal to 0 to 2; wherein when Y is a covalent chemical single bond or a divalent linking group, z = 1; and when Y is a trivalent linking group, z = 2; provided that when w = 0, Ar c and each Ar 1 Neither is phenyl.

[0016] Still further, the present invention provides a method comprising: (a) providing an electronic device substrate; (b) coating a coating composition layer comprising one or more curable compounds having formula (2) on a surface of the electronic device substrate.

[0017]

[0018] Among them, Ar c is an aromatic nucleus having 5 to 30 carbon atoms; Ar 1 ,Ar 2 , and Ar 3 Each is independently an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Y is a covalent chemical single bond, a divalent linking group, or a trivalent linking group; Z 1 and Z 2 are independently selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1; x1=1 to 4; x2=1 to 4; y1=2 to 4; each y2=0 to 4; y1+each y2≥3; w=0 to 2; and z equals 0 to 2; wherein when Y is a covalent chemical single bond or a divalent linking group, z=1; and when Y is a trivalent linking group, z=2; (c) curing the layer of the curable compound to form a bottom layer; (d) coating a photoresist layer on the bottom layer; (e) exposing the photoresist layer to actinic radiation through a mask; (f) developing the exposed photoresist layer to form a resist pattern; and (g) transferring the pattern to the bottom layer to expose a portion of the electronic device substrate.

[0019] The present invention also provides a method for filling gaps (or holes), the method comprising: (a) providing a semiconductor substrate having a relief image on the surface of the substrate, the relief image comprising a plurality of gaps to be filled; (b) applying a coating of one or more compounds having formula (2) on the relief image; and (c) heating the coating at a temperature sufficient to cure the coating.

[0020] It will be understood that when an element is referred to as being "on" another element, it can be directly adjacent to the other element or intervening elements may be present therebetween. Conversely, when an element is referred to as being "directly on" another element, there are no intervening elements present. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0021] It will also be understood that, although the terms first, second, third, etc. can be used to describe different elements, components, regions, layers and / or parts in this article, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish an element, component, region, layer or part from another element, component, region, layer or part. Therefore, the first element, component, region, layer or part discussed below can be referred to as the second element, component, region, layer or part without departing from the teaching content of the present invention.

[0022] As used throughout this specification, unless the context clearly indicates otherwise, the following abbreviations shall have the following meanings: °C = degrees Celsius; g = gram; mg = milligram; L = liter; mL = milliliter; nm = nanometer; μm = micron = micrometer; mm = millimeter; sec. = second; min. = minute; hr. = hour; DI = deionized; and Da = Dalton. Unless otherwise stated, "wt%" refers to the weight percentage based on the total weight of the reference composition. Unless otherwise stated, all amounts are wt% and all ratios are molar ratios. All numerical ranges are inclusive and can be combined in any order, except that it is obvious that this numerical range is limited to add up to 100%. The articles "a / an" and "the" refer to the singular and plural. Unless otherwise stated, "alkyl" refers to straight chain, branched and cyclic alkyl. As used herein, "alkyl" refers to an alkane group, and includes alkane monovalent groups, divalent groups (alkylene), and higher valent groups. "Halogen" refers to fluorine, chlorine, bromine and iodine. Unless otherwise stated, "alkyl" includes "heteroalkyl". The term "heteroalkyl" refers to an alkyl group that replaces one or more carbon atoms in the group with one or more heteroatoms (such as nitrogen, oxygen, sulfur, phosphorus), for example, as in an ether or thioether. In a preferred embodiment, "alkyl" does not include "heteroalkyl". If the number of carbons is not indicated for any alkyl or heteroalkyl, 1-12 carbons are expected.

[0023] "Aryl" includes aromatic carbocyclic rings and aromatic heterocyclic rings. The term "aryl" refers to an aromatic group and includes monovalent groups, divalent groups (arylene groups), and higher valent groups. Preferably, the aryl moiety is an aromatic carbocyclic ring. "Substituted aryl" refers to any aryl moiety whose one or more hydrogens are replaced by one or more substituents selected from the group consisting of halogen, C 1-6 -alkyl, halo-C 1-6 -alkyl, C 1-6 -alkoxy, halo-C 1-6 -alkoxy, phenyl, and phenoxy, preferably selected from halogen, C 1-6 -alkyl, halo-C 1-4 -alkyl, C 1-6 -alkoxy, halo-C 1-4 -alkoxy, and phenyl, and is more preferably selected from halogen, C 1-6 -alkyl, C 1-6-alkoxy, phenyl and phenoxy. Preferably, the substituted aryl has 1 to 3 substituents, and more preferably 1 or 2 substituents. As used herein, the term "polymer" includes oligomers. The term "oligomer" refers to dimers, trimers, tetramers and other polymer materials that can be further cured. The term "curing" means increasing the total molecular weight of the resin of the present invention or removing the group that enhances solubility from the oligomer of the present invention, or any process that increases the total molecular weight and removes the group that enhances solubility, such as polymerization or condensation. "Curable" refers to any material that can be cured under certain conditions. As used herein, "gap" refers to any hole on a semiconductor substrate that is intended to be filled with a composition that fills the gap.

[0024] An aromatic bottom layer is formed in the manufacture of an electronic device according to the following method, the method comprising: (a) providing an electronic device substrate; (b) coating a coating composition layer comprising one or more curable compounds on the surface of the electronic device substrate, wherein the one or more curable compounds comprises a 5-6 Aromatic ring and C 9-30 The aromatic nucleus of the fused aromatic ring system and three or more substituents having the formula (1)

[0025]

[0026] wherein at least two substituents having formula (1) are attached to the aromatic core; and wherein Ar 1 is an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Z is selected from OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1; x is an integer from 1 to 4; and * represents an attachment point to the aromatic core; (c) curing the layer of the curable compound to form a bottom layer; (d) coating a photoresist layer on the bottom layer; (e) exposing the photoresist layer to actinic radiation through a mask; (f) developing the exposed photoresist layer to form a resist pattern; and (g) transferring the pattern to the bottom layer to expose a portion of the electronic device substrate. Next, the substrate is patterned and the patterned bottom layer is removed. In a preferred embodiment, the photoresist layer is directly coated on the bottom layer. In an alternative preferred embodiment, before step (d), a layer of one or more of a silicon-containing composition, an organic anti-reflective composition (BARC), and a combination thereof is directly coated on the bottom layer to form an intermediate layer, and the photoresist layer is directly coated on the intermediate layer. When a silicon-containing intermediate layer is used, the pattern is transferred to the silicon-containing intermediate layer after step (f) and before step (g).

[0027] A wide variety of electronic device substrates can be used in the present invention, such as: packaging substrates, such as multi-chip modules; flat panel display substrates; integrated circuit substrates; substrates for light emitting diodes (LEDs) including organic light emitting diodes (OLEDs); semiconductor wafers; polycrystalline silicon substrates; etc., where semiconductor wafers are preferred. Such substrates are typically composed of one or more of silicon, polycrystalline silicon, silicon oxide, silicon nitride, silicon oxynitride, silicon germanium, gallium arsenide, aluminum, sapphire, tungsten, titanium, titanium-tungsten, nickel, copper and gold. Suitable substrates can be in the form of wafers, such as those used to manufacture integrated circuits, optical sensors, flat panel displays, integrated optical circuits, and LEDs. As used herein, the term "semiconductor wafer" is intended to cover "semiconductor substrates", "semiconductor devices" and various packages for various interconnect levels, including single-chip wafers, multi-chip wafers, packages for various levels, or other components requiring solder connections. Such substrates can be of any suitable size. The preferred wafer substrate diameter is 200 mm to 300 mm, although wafers with smaller and larger diameters can be appropriately used according to the present invention. As used herein, the term "semiconductor substrate" includes any substrate having one or more semiconductor layers or structures, which may optionally include active or operable portions of a semiconductor device. A semiconductor device refers to a semiconductor substrate on which at least one microelectronic device has been or is being mass-produced.

[0028] Optionally, an adhesion promoter layer can be applied to the substrate surface, after which the coating composition of the present invention is deposited and subsequently cured to form a bottom layer. If an adhesion promoter is desired, any suitable adhesion promoter for polymer films can be used, such as silanes, preferably organosilanes such as trimethoxyvinylsilane, triethoxyvinylsilane, hexamethyldisilazane, or aminosilane coupling agents such as γ-aminopropyltriethoxysilane. Particularly suitable adhesion promoters include those sold under the names of AP 3000, AP 8000, and AP 9000S available from Dow Electronic Materials (Marlborough, Massachusetts).

[0029] The coating composition useful in the present invention comprises one or more curable compounds, wherein the one or more curable compounds comprises a 5-6 Aromatic ring and C 9-30 The aromatic nucleus of the fused aromatic ring system and three or more substituents having the formula (1)

[0030]

[0031] wherein at least two substituents having formula (1) are attached to the aromatic core; and wherein Ar 1 is an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Z is selected from OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 -alkyl, C 2-10 -unsaturated hydrocarbon group, and C 5-30 -aryl; each R 2 Selected from H, C 1-10 -alkyl, C 2-10- Unsaturated hydrocarbon group, C 5-30 -Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x is an integer from 1 to 4; and * represents the point of attachment to the aromatic core. Preferably, each Z is independently selected from OR 1 , protected hydroxyl, carboxyl (C(=O)OH), protected carboxyl, SH, fluorine, and NHR 2 More preferably, each Z is independently selected from hydroxyl (OH), protected hydroxyl, OCH2C≡CH, C(=O)OH, protected carboxyl, and NHR 2, and more preferably selected from OH, protected hydroxyl, OCH2C≡CH, carboxyl, and protected carboxyl, and still more preferably selected from OH and protected hydroxyl. Each R 1 Independently selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl, and more preferably selected from H, C 1-10 -alkyl, C 2-10 -Alkenyl, C 2-10 -alkynyl, and C 5-30 In a preferred embodiment, R 1 is H. Preferably, R 2 Selected from H, C 1-10 -alkyl, C 2-10 -unsaturated hydrocarbon group, and C 5-30 -aryl, and more preferably selected from H, C 1-10 -alkyl, C 2-10 -Alkenyl and C 2-10 As used herein, the term "aromatic core" refers to a single aromatic ring or a fused aromatic ring system to which at least two moieties of formula (1) are attached. The aromatic core may be optionally substituted with one or more substituents selected from the group consisting of: C 1-20 - aliphatic or alicyclic moiety and C 5-30 - an aromatic moiety. Preferably, the aromatic nucleus is selected from pyridine, benzene, naphthalene, quinoline, isoquinoline, carbazole, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, more preferably selected from benzene, naphthalene, carbazole, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, and more preferably selected from benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, In formula (1), preferably, each Ar 1 independently selected from pyridine, benzene, naphthalene, quinoline, isoquinoline, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, more preferably selected from benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, and even more preferably selected from benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, and phenalene. Preferably, x=1 or 2, and more preferably x=1. The curable compound of the present invention has at least three moieties of formula (1), wherein at least two substituents of formula (1) are directly attached to the aromatic core. The curable compound of the present invention may have any suitable number of moieties of formula (1), such as 3 to 10, preferably 3 to 8, more preferably 3 to 6, and even more preferably 3 or 4. It is further preferred that the curable compound of the present invention has 2 to 4 moieties of formula (1) directly attached to the aromatic core.

[0032] In one embodiment, preferred curable compounds useful in the coating compositions of the present invention are those having formula (2)

[0033]

[0034] Among them, Ar c is an aromatic nucleus having 5 to 30 carbon atoms; Ar 1 ,Ar 2 , and Ar 3 Each is independently an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Y is a covalent chemical single bond, a divalent linking group, or a trivalent linking group; Z 1 and Z 2 Independently selected from OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x1 = 1 to 4; x2 = 1 to 4; y1 = 2 to 4; each y2 = 0 to 4; y1 + each y2 ≥ 3; w = 0 to 2; and z is equal to 0 to 2; wherein when Y is a covalent chemical single bond or a divalent linking group, z = 1; and when Y is a trivalent linking group, z = 2. Preferably, Ar c is an aromatic nucleus having 5 to 25 carbon atoms, and more preferably 5 to 20 carbon atoms. c Suitable aromatic nuclei include, but are not limited to, pyridine, benzene, naphthalene, quinoline, isoquinoline, carbazole, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, preferably benzene, naphthalene, carbazole, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, and more preferably benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, Preferably, Ar 1 Selected from benzene, pyridine, naphthalene, quinoline, isoquinoline, anthracene, phenanthrene, pyrene, coronene, triphenylene, More preferably, Ar 1 ,Ar 2 , and Ar 3 Each independently selected from pyridine, benzene, naphthalene, quinoline, isoquinoline, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, more preferably selected from benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenanthene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, and more preferably selected from benzene, naphthalene, anthracene, phenanthrene, pyrene, coronene, triphenylene, Further preferably, Ar c Selected from pyridine, benzene, naphthalene, quinoline, isoquinoline, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenalene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene, and Ar 1 ,Ar 2 , and Ar 3 Each independently selected from pyridine, benzene, naphthalene, quinoline, isoquinoline, anthracene, phenanthrene, pyrene, coronene, triphenylene, Preferably, Z 1 and Z 2 Each independently selected from OR 1 , protected hydroxyl, carboxyl (C(=O)OH), protected carboxyl, SH, fluorine, NHR 2 , more preferably selected from hydroxyl (OH), protected hydroxyl, OCH2C≡CH, C(=O)OH, protected carboxyl, and NHR 2 , and more preferably selected from OH, protected hydroxyl, OCH2C≡CH, carboxyl, and protected carboxyl, and still more preferably selected from OH and protected hydroxyl. Each R 1 Independently selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl, and more preferably selected from H, C 1-10-alkyl, C 2-10 -Alkenyl, C 2-10 -alkynyl, and C 5-30 In a preferred embodiment, R 1 is H. Preferably, R 2 Selected from H, C 1-10 -alkyl, C 2-10 -unsaturated hydrocarbon group, and C 5-30 -aryl, and more preferably selected from H, C 1-10 -alkyl, C 2-10 -Alkenyl and C 2-10 Preferably, each Z 1 are the same. It is also preferred that each Z 2 are the same. It is further preferred that Z 1 =Z 2 Preferably, x1 and x2 are each independently selected from 1 to 3, more preferably independently 1 or 2, and even more preferably each 1. Preferably, each y2=0 to 2. Preferably, y1+each y2=3 to 8, more preferably 3 to 6, and even more preferably 3 or 4. Preferably, w=0 to 1. In a preferred embodiment, when w=0, Ar c and each Ar 1 In one preferred embodiment, Y is a covalent single bond. In another preferred embodiment, Y is a divalent or trivalent linking group. For Y, exemplary linking groups include, but are not limited to, O, S, N (R 3 ) r 、S(=O)2、CR 4 R 5 , bis-imide moiety, bis-etherimide moiety, bis-ketoimide moiety, bis-benzoxazole moiety, bis-benzimidazole moiety, and bis-benzothiazole moiety, wherein r = 0 or 1, and preferably the linking group of Y is O, N (R 3 ) w , and CR 4 R 5 . R 3 It is **-C(=O)-C 5-30 -aryl or **-S(=O)2-C 5-30 -aryl, where ** is the point of attachment to N. R 4 and R 5 Independently selected from H, C 1-10 -alkyl and C 5-10 -aryl, and R 4 and R 5 Together with the carbon to which they are attached, they may form a 5- or 6-membered ring, which may be fused to one or more aromatic rings. 4 R 5When a suitable linking group is a fluorenyl moiety having the following formula (A)

[0035]

[0036] Where * indicates the c and Ar 2 For Y, suitable bis-imide moiety linking groups are shown by formula (B) and formula (C), wherein Y 1 Is a covalent single bond or C 5-30 -arylene, where * represents the c and Ar 2 Suitable bis-etherimide and bis-ketimide moieties are those of formula (C) wherein Y 1 =O or -C(=O)-, respectively, and wherein * represents the same as Ar c and Ar 2 Suitable bis-benzoxazole, bis-benzimidazole, and bis-benzothiazole moieties are those of formula (D) wherein G = O, NH, and S, respectively, and wherein Y 2 Is a covalent single bond or C 5-30 -arylene, and wherein * represents c and Ar 2 attachment point.

[0037]

[0038] For Z and Z in equations (1) and (2), 1 and Z 2 , a protected carboxyl group is any group that can be cleaved under certain conditions to produce a carboxyl group. Such protected carboxyl groups can be cleaved by heat, acid, base or a combination thereof, preferably by heat, acid or a combination thereof, and more preferably by heat. Exemplary protected carboxyl groups include esters, such as benzyl esters and esters having a quaternary carbon directly bonded to the alkoxy oxygen of the ester group. Preferably, the protected carboxyl group is an ester having a quaternary carbon directly bonded to the alkoxy oxygen of the ester group, and more preferably the ester has the formula YC(O)-O-CR'R"R'", wherein Y is an organic residue, and R', R" and R'"' are each independently selected from C 1-10 Preferred protected carboxyl groups include: tert-butyl esters; 1-alkylcyclopentyl esters such as 1-methylcyclopentyl ester and 1-ethylcyclopentyl ester; 2,3-dimethyl-2-butyl ester; 3-methyl-3-pentyl ester; 2,3,3-trimethyl-3-butyl ester; 1,2-dimethylcyclopentyl ester; 2,3,4-trimethyl-3-pentyl ester; 2,2,3,4,4-pentamethyl-3-pentyl ester; and adamantyl esters such as hydroxyadamantyl ester and C 1-12Alkyl adamantyl esters. Each of the above-mentioned protected carboxyl groups can be cleaved by one or more of heat, acid or base. Preferably, heat, acid or a combination of heat and acid, and more preferably the protected carboxyl group is cleaved by heat. For example, these protected carboxyl groups can be cleaved at a pH of ≤4 and preferably ≤1. Such protected carboxyl groups can be cleaved at room temperature when exposed to a pH of 1 to 4. When pH<1, such protected carboxyl groups are typically heated to about 90°C to 110°C, and preferably to about 100°C. Alternatively, when the protected carboxyl group is an ester having a quaternary carbon directly bonded to the alkoxy oxygen of the ester group, the protected carboxyl group can be cleaved by heating to a suitable temperature, such as ≥125°C, preferably 125°C to 250°C, and more preferably 150°C to 250°C. Such protected carboxyl groups and conditions for their use are well known in the art, such as US Pat. No. 6,136,501, which discloses a variety of ester groups having a quaternary carbon bonded directly to the alkoxy oxygen of the ester group.

[0039] For Z and Z in equations (1) and (2), 1 and Z 2 , a suitable protected hydroxyl group is any group that can be cleaved under certain conditions to produce a hydroxyl group. Such protected hydroxyls can be cleaved by heat, acid, base, or a combination thereof. Exemplary protected hydroxyls include: ethers, such as methoxymethyl ether, tetrahydropyranyl ether, tert-butyl ether, allyl ether, benzyl ether, tert-butyldimethylsilyl ether, tert-butyldiphenylsilyl ether, acetone compounds, and benzylidene acetals; esters, such as pivalate and benzoate; and carbonates, such as tert-butyl carbonate. Each of the above-mentioned protected hydroxyls can be cleaved under acidic or alkaline conditions, and preferably under acidic conditions. More preferably, the protected hydroxyl group is cleaved using an acid or a combination of acid and heat. For example, these protected hydroxyls can be cleaved at a pH of ≤4 and preferably ≤1. Such protected hydroxyls can be cleaved at room temperature when exposed to a pH of 1 to 4. When pH<1, such protected hydroxyls are typically heated to about 90°C to 110°C, and preferably to about 100°C. Such protected hydroxyl groups and conditions for their use are well known in the art.

[0040] For Z and Z in equations (1) and (2), 1 and Z 2, a suitable protected thiol group is any group that can be cleaved under certain conditions to produce a thiol group. Such protected thiol groups can be cleaved by heat, acid, base or a combination thereof. Exemplary protected thiol groups include: thioethers, such as methoxymethyl thioether, tetrahydropyranyl thioether, tert-butyl thioether, allyl thioether, benzyl thioether, tert-butyldimethylsilyl thioether, tert-butyldiphenylsilyl thioether, thioacetone compounds, and benzylidene thioacetals; thioesters, such as pivalic acid thioesters and benzoic acid thioesters; and thiocarbonates, such as tert-butyl thiocarbonate. Each of the above-mentioned protected thiol groups can be cleaved under acidic or alkaline conditions, and preferably under acidic conditions. More preferably, the protected thiol group is cleaved using an acid or a combination of acid and heat. For example, these protected thiol groups can be cleaved at a pH of ≤4 and preferably ≤1. Such thiol groups can be cleaved at room temperature when exposed to a pH of 1 to 4. Such protected thiol groups are typically heated to about 90° C. to 110° C., and preferably to about 100° C. when pH < 1. Such protected thiol groups and conditions for their use are well known in the art.

[0041] In addition to the one or more curable compounds described above, the coating composition of the present invention may optionally include, and preferably includes, one or more organic solvents. Suitable organic solvents are any organic solvents that dissolve one or more curable compounds, and are preferably organic solvents that are routinely used to make electronic devices. Organic solvents can be used alone or a mixture of organic solvents can be used. Suitable organic solvents include, but are not limited to, ketones such as cyclohexanone and methyl-2-n-pentyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol methyl ether (PGME), propylene glycol ethyl ether (PGEE), ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether, anisole; esters such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl lactate (EL), methyl hydroxyisobutyrate (HBM), ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate; lactones such as γ-butyrolactone; and any combination of the foregoing. Preferred solvents are PGME, PGEE, PGMEA, EL, HBM, and combinations thereof.

[0042] The coating composition of the present invention may also include one or more coating additives typically used for such coatings, such as curing agents, crosslinking agents, surface leveling agents, etc. The selection of such optional additives and their amounts are completely within the capabilities of those skilled in the art. Curing agents are typically present in an amount of 0 to 20 wt% based on total solids, and preferably 0 to 3 wt%. Crosslinking agents are typically used in an amount of 0 to 30 wt% based on total solids, and preferably 3 to 10 wt%. Surface leveling agents are typically used in an amount of 0 to 5 wt% based on total solids, and preferably 0 to 1 wt%. The selection of such optional additives and their usage amounts are within the capabilities of those skilled in the art.

[0043] A curing agent may optionally be used in the coating composition to aid in the curing of the deposited curable compound. A curing agent is any component that causes the curable compound to cure on the substrate surface. Preferred curing agents are acids and thermal acid generators. Suitable acids include, but are not limited to: aryl sulfonic acids, such as p-toluenesulfonic acid; alkyl sulfonic acids, such as methanesulfonic acid, ethanesulfonic acid, and propanesulfonic acid; perfluoroalkyl sulfonic acids, such as trifluoromethanesulfonic acid; and perfluoroaryl sulfonic acids. A thermal acid generator is any compound that releases an acid when exposed to heat. Thermal acid generators are well known in the art and are typically commercially available as from King Industries, Norwalk, Connecticut. Exemplary thermal acid generators include, but are not limited to, amine-terminated strong acids, such as amine-terminated sulfonic acids, such as amine-terminated dodecylbenzenesulfonic acid. It will also be appreciated by those skilled in the art that certain photoacid generators are capable of releasing an acid when heated and can be used as thermal acid generators.

[0044] Any suitable crosslinking agent may be used in the composition of the present invention, provided that such crosslinking agent has at least 2, and preferably at least 3, moieties that are capable of reacting with the aromatic resin reaction product of the present invention under suitable conditions (e.g., under acidic conditions). Exemplary crosslinking agents include, but are not limited to, novolac resins, epoxy-containing compounds, melamine compounds, guanamine compounds, isocyanate-containing compounds, benzocyclobutene, and the like, and preferably, among the foregoing, 2 or more, preferably 3 or more, and more preferably 4, selected from hydroxymethyl, C1-C 10 Alkoxymethyl, and C2-C 10 Any of the substituents of the acyloxymethyl group. Examples of suitable crosslinking agents are those shown by formulas (3) and (4).

[0045]

[0046] Such cross-linking agents are well known in the art and are commercially available from a variety of sources.

[0047] The coating compositions of the present invention may optionally include one or more surface leveling agents (or surfactants). Although any suitable surfactant may be used, such surfactants are typically nonionic. Exemplary nonionic surfactants are those containing alkyleneoxy linkages (such as ethyleneoxy, propyleneoxy, or a combination of ethyleneoxy and propyleneoxy linkages).

[0048] The coating composition of the present invention can be applied to the electronic device substrate by any suitable means such as spin coating, slot die coating, scraping, curtain coating, roller coating, spray coating, dip coating, etc. Preferred is spin coating. In a typical spin coating method, the composition of the present invention is applied to a substrate rotating at a speed of 500 to 4000 rpm for a period of 15 to 90 seconds to obtain a desired coating composition layer on the electronic device substrate. It will be appreciated by those skilled in the art that the height of the coating composition layer can be adjusted by changing the rotation speed.

[0049] After the coating composition layer is applied to the substrate, it is optionally baked at a relatively low temperature to remove any organic solvents and other relatively volatile components from the layer. Typically, the substrate is baked at a temperature of 80° C. to 150° C., although other suitable temperatures can be used. The baking time is typically 10 seconds to 10 minutes, and preferably 30 seconds to 5 minutes, although longer or shorter times can be used. When the substrate is a wafer, this baking step can be performed by heating the wafer on a hot plate. After the solvent is removed, a layer, film or coating of the curable compound on the substrate surface is obtained.

[0050] The curable compound layer is then fully cured to form an aromatic bottom layer so that the film is not mixed with a coating applied subsequently (such as a photoresist layer or other layer directly coated on the aromatic bottom layer). The bottom layer can be cured in an oxygen-containing atmosphere (such as air) or in an inert atmosphere (such as nitrogen) and preferably in an oxygen-containing atmosphere. The curing conditions used are those that are sufficient to cure the film so that it is not mixed with an organic layer (such as a photoresist layer) applied subsequently, while still maintaining the anti-reflection properties (n and k values) and etching selectivity of the desired bottom layer film. This curing step is preferably carried out on a hot plate device, although oven curing can be used to obtain equivalent results. Typically, this curing is carried out by heating the bottom layer at a curing temperature of ≥150°C, preferably ≥170°C, and more preferably ≥200°C. The selected curing temperature should be sufficient to cure the aromatic bottom layer. The suitable temperature range for curing the aromatic bottom layer is 150°C to 400°C, preferably 170°C to 350°C, and more preferably 200°C to 250°C. This curing step may take from 10 seconds to 10 minutes, preferably from 1 to 3 minutes, and more preferably from 1 to 2 minutes, although other suitable times may be used.

[0051] If the curing step is performed in such a way that the rapid release of solvents and curing byproducts does not allow the quality of the underlying film to be damaged, an initial baking step may not be necessary. For example, a ramp-up bake that starts at a relatively low temperature and then gradually increases to a temperature of ≥200°C may produce acceptable results. In some cases, it may be preferred to have a two-stage curing process, where the first stage is a lower baking temperature of less than 150°C and the second stage is a higher baking temperature of ≥200°C. The two-stage curing process promotes uniform filling and planarization of pre-existing substrate surface topography, such as the filling of trenches and vias.

[0052] After curing the bottom layer, one or more processing layers, such as a photoresist, a silicon-containing layer, a hard mask layer, a bottom anti-reflective coating (or BARC) layer, etc., can be applied to the cured bottom layer. For example, the photoresist can be applied (such as by spin coating) directly on the surface of the silicon-containing layer or other intermediate layer directly on the resin bottom layer, or alternatively, the photoresist can be applied directly to the cured bottom layer. A wide variety of photoresists can be suitably used, such as those used for 193 nm lithography, such as those available from Dow Electronic Materials (Marlborough, MA) under the trade name Epic TM Those sold under the brand name of . Suitable photoresists can be positive developing or negative developing resists. After coating, the photoresist layer is then imaged (exposed) using patterned actinic radiation, and the exposed photoresist layer is then developed using a suitable developer to provide a patterned photoresist layer. Next, the pattern is transferred from the photoresist layer to the bottom layer by a suitable etching technique. Typically, the photoresist is also removed during this etching step. Next, the pattern is transferred to the substrate and the bottom layer is removed by a suitable etching technique known in the art (such as by plasma etching). After the patterned substrate, the bottom layer is removed using conventional techniques. The electronic device substrate is then processed according to conventional means.

[0053] The cured bottom layer can be used as the bottom layer of a multilayer resist process. In this process, a coating composition layer is applied to a substrate and cured as described above. Next, one or more intermediate layers are applied to the aromatic bottom layer. For example, a silicon-containing layer or a hard mask layer is directly applied to the aromatic bottom layer. An exemplary silicon-containing layer such as silicon-BARC can be deposited on the bottom layer by spin coating and subsequently cured, or an inorganic silicon layer such as SiON or SiO2 can be deposited on the bottom layer by chemical vapor deposition (CVD). Any suitable hard mask can be used and can be deposited on the bottom layer by any suitable technique, and cured (when appropriate). Optionally, an organic BARC layer can be directly placed on a silicon-containing layer or a hard mask layer, and appropriately cured. Next, a photoresist (such as those used in 193nm lithography) is directly coated on the silicon-containing layer (in a three-layer process) or directly coated on the organic BARC layer (in a four-layer process). The photoresist layer is then imaged (exposed) using patterned actinic radiation, and the exposed photoresist layer is then developed using an appropriate developer to provide a patterned photoresist layer. Next, the pattern is transferred from the photoresist layer to the layer directly below it by an appropriate etching technique known in the art (such as by plasma etching), resulting in a patterned silicon-containing layer in a three-layer process and a patterned organic BARC layer in a four-layer process. If a four-layer process is used, the pattern is then transferred from the organic BARC layer to the silicon-containing layer or hard mask layer using an appropriate pattern transfer technique (such as plasma etching). After the silicon-containing layer or hard mask layer is patterned, the aromatic bottom layer is then patterned using an appropriate etching technique (such as O2 or CF4 plasma). During the etching of the aromatic bottom layer, any remaining patterned photoresist layer and organic BARC layer are removed. Next, the pattern is transferred to the substrate, such as by an appropriate etching technique, which also removes any remaining silicon-containing layer or hard mask layer, and any remaining patterned aromatic bottom layer is subsequently removed to provide a patterned substrate.

[0054] The cured bottom layer of the present invention can also be used for self-aligned double patterning process. In this process, the coating composition layer of the present invention is coated on the substrate as by spin coating. Any remaining organic solvent is removed and the coating composition layer is cured to form a cured bottom layer. A suitable intermediate layer such as a silicon-containing layer is coated on the cured bottom layer. Then a suitable photoresist layer is coated on the intermediate layer as by spin coating. Then the photoresist layer is imaged (exposed) using patterned actinic radiation, and then the exposed photoresist layer is developed using a suitable developer to provide a patterned photoresist layer. Next, the pattern is transferred from the photoresist layer to the intermediate layer and the cured bottom layer by a suitable etching technique to expose a part of the substrate. Typically, the photoresist is also removed during this etching step. Next, a conformal silicon-containing layer is placed on the exposed portion of the patterned cured bottom layer and the substrate. Such silicon-containing layers are typically inorganic silicon layers conventionally deposited by CVD, such as SiON or SiO2. Such conformal coating produces a silicon-containing layer on the exposed portion of the substrate surface and on top of the underlying pattern, i.e., such silicon-containing layer substantially covers the sides and top of the patterned underlying layer. Next, the silicon-containing layer is partially etched (trimmed) to expose the top surface of the patterned polyarylene resin underlying layer and a portion of the substrate. After this partial etching step, the pattern on the substrate comprises a plurality of features, each of which comprises a line or column of the cured underlying layer, wherein the silicon-containing layer is directly adjacent to the side of each cured underlying feature. Next, the cured underlying layer is removed, such as by etching, to expose the substrate surface below the cured underlying pattern, and to provide a patterned silicon-containing layer on the substrate surface, wherein such patterned silicon-containing layer is double (i.e., twice as many lines and / or columns) compared to the patterned cured underlying layer.

[0055] The coating composition of the present invention can also be used to form a planarization layer, a gap filling layer, and a protective layer in the manufacture of integrated circuits. When used as such a planarization layer, a gap filling layer or a protective layer, one or more intervening material layers (such as a silicon-containing layer, other aromatic resin layers, hard mask layers, etc.) are typically present between the cured layer of the coating composition of the present invention and any photoresist layer. Typically, such planarization layers, gap filling layers, and protective layers are finally patterned. The gap filling process according to the present invention includes: (a) providing a semiconductor substrate having a relief image on the surface of the substrate, the relief image comprising a plurality of gaps to be filled; (b) applying a gap filling composition on the relief image, wherein the gap filling composition comprises: (i) one or more curable compounds, the one or more curable compounds comprising selected from C 5-6 Aromatic ring and C 9-30 The aromatic nucleus of the fused aromatic ring system and three or more substituents having the formula (1)

[0056]

[0057] wherein at least two substituents having formula (1) are attached to the aromatic core; and wherein Ar 1 is an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Z is a substituent selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x is an integer from 1 to 4; and * represents a point of attachment to the aromatic core; and (ii) one or more organic solvents; and (c) heating the gap-filling composition at a temperature to cure the one or more curable compounds. The composition of the present invention substantially fills, preferably fills, and more preferably completely fills a plurality of gaps in a semiconductor substrate.

[0058] The compounds of the present invention have good gap-filling properties. Films formed from the compounds of the present invention have good planarization, solvent resistance, and reduced defect formation compared to the compounds disclosed in US Pat. No. 9,581,905.

[0059] Example 1. 1,3,5-tribromobenzene (2.36g), cuprous iodide (0.21g) and triethylamine (3.42g) were added to 20g of 1,4-dioxane at room temperature. The reaction mixture was purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.53g) was added to the reaction mixture, and the mixture was heated to 70 ° C. 4-ethynylphenyl acetate (4.81g) was dissolved in degassed 1,4-dioxane (14g), and then the solution was slowly added to the reaction mixture by a feed funnel. After completion of the addition, the reaction mixture was stirred overnight at 70 ° C under nitrogen. After the reaction was completed, the reaction mixture was cooled to room temperature, filtered, and the solvent was evaporated. The residue was purified by column chromatography to obtain 3.5g (84% yield) of 1,3,5-tris((4-acetoxyphenyl)ethynyl)benzene (compound I1) as a light yellow solid. The reaction is shown in the following reaction scheme.

[0060] Reaction Scheme 1

[0061]

[0062] Example 2. 1,3,5-tribromobenzene (2.36g), cuprous iodide (0.21g) and triethylamine (3.42g) are added to 20g of 1,4-dioxane at room temperature. The reaction mixture is purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.53g) is added to the reaction mixture, and the mixture is heated to 70°C. 4-ethynylphenyl acetate (4.81g) is dissolved in degassed 1,4-dioxane (14g), and then the solution is slowly added to the reaction mixture by a feed funnel. After completion of the addition, the reaction mixture is stirred overnight at 70°C under nitrogen. After the reaction is complete, the reaction mixture is cooled to room temperature, filtered, and the solvent is evaporated. The residue is purified by column chromatography to obtain a light yellow solid. The solid obtained is then dissolved in THF (35g) under nitrogen. Lithium hydroxide monohydrate (0.94g) and water (8g) are added, and the reaction mixture is stirred at 60°C for 1 hour. The reaction mixture is then diluted with ethyl acetate, and then treated with hydrochloric acid until the pH of the water layer is 1. The organic phase is separated and the aqueous phase is extracted with ethyl acetate. The organic layers are combined and washed with water. The solvent is removed under vacuum to obtain 2.6g (81% yield) of 1,3,5-tris ((4-hydroxyphenyl) ethynyl) benzene (compound I2) as a light yellow solid. The reaction is shown in the following reaction scheme.

[0063] Reaction Scheme 2

[0064]

[0065] Example 3.4-iodophenyl acetate (24.75g), cuprous iodide (0.17g) and triethylamine (27.32g) are added to 22.82g of 1,4-dioxane at room temperature. The reaction mixture is purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.63g) is added to the reaction mixture, and the mixture is heated to 70°C. Then a solution of 1,3,5-triethynylbenzene (4.5g) in degassed 1,4-dioxane (20g) is slowly added to the reaction mixture via a syringe pump. After completion of the addition, the reaction mixture is stirred overnight at 70°C under nitrogen. After completion of the reaction, the reaction mixture is cooled to room temperature, and the solvent is evaporated. The residue is diluted with ethyl acetate and filtered to remove solids. The solution is evaporated, and the residue is purified by column chromatography to obtain a light yellow solid. The solid obtained is then dissolved in THF (38g) under nitrogen. Lithium hydroxide monohydrate (3.81g) and water (16g) are added, and the mixture is stirred at 60°C for 1 hour. The mixture is then cooled to room temperature, and the solvent is removed. The residue is diluted with ethyl acetate and water, and then treated with hydrochloric acid until the pH of the water layer is 1. The organic phase is separated and the aqueous phase is extracted with ethyl acetate. The organic layers are merged and washed with water. The solvent is removed under vacuum, and the residue is purified by column chromatography to obtain 7.7g (61% yield) of 1,3,5-tris ((4-hydroxyphenyl) ethynyl) benzene (compound I2) in a light yellow solid. The reaction is shown in the following reaction scheme.

[0066] Reaction Scheme 3

[0067]

[0068] Example 4. 1,3,5-tribromobenzene (3.12g), cuprous iodide (0.29g) and triethylamine (4.55g) were added to 22g of 1,4-dioxane at room temperature. The reaction mixture was purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.70g) was added to the reaction mixture, and the mixture was heated to 70 ° C. 1-ethynyl-4-methoxybenzene (5.28g) was dissolved in degassed 1,4-dioxane (20g), and then the solution was slowly added to the reaction mixture by a feed funnel. After completion of the addition, the reaction mixture was stirred overnight at 70 ° C under nitrogen. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the solvent was evaporated. The residue was purified by column chromatography to obtain 4.0g (85% yield) of 1,3,5-tris((4-methoxyphenyl)ethynyl)benzene (compound I3) as a light yellow solid. The reaction is shown in the following reaction scheme.

[0069] Reaction Scheme 4

[0070]

[0071] Example 5. 1,3,5-tribromobenzene (3.12g), cuprous iodide (0.29g) and triethylamine (4.55g) are added to 22g of 1,4-dioxane at room temperature. The reaction mixture is purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.70g) is added to the reaction mixture, and the mixture is heated to 70 ° C. 4-ethynylaniline (4.68g) is dissolved in degassed 1,4-dioxane (20g), and then the solution is slowly added to the reaction mixture by a feed funnel. After completion of the addition, the reaction mixture is stirred overnight at 70 ° C under nitrogen. After the reaction is completed, the reaction mixture is cooled to room temperature, filtered, and the solvent is evaporated. The residue is purified by column chromatography to obtain 1.5g (36% yield) of 1,3,5-tris((4-aminophenyl)ethynyl)benzene (compound I4) as a yellow solid. The reaction is shown in the following reaction scheme.

[0072] Reaction Scheme 5

[0073]

[0074] Example 6. 1,3,5-tribromobenzene (15.0g) is added to 40.0g of 1,4-dioxane at room temperature to produce a clear solution. Triethylamine (14.5g) and cuprous iodide (0.91g) are added to the reaction mixture. The reaction mixture is purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (1.00g) is added to the reaction mixture. Next, 22.9g of 4-fluorophenylacetylene is slowly added to the reaction mixture via a feed funnel. After completion of the addition, the reaction mixture is stirred at 55°C under nitrogen for 24 hours. The reaction mixture is filtered and the solvent is evaporated. The residue is dissolved in heptane and filtered through a silica plug. After filtration, the solvent is removed to produce 1,3,5-tri((4-fluorophenyl)ethynyl)benzene (Compound I5) as a light yellow solid (8.0g) (39% yield). The reaction is shown in the following reaction scheme.

[0075] Reaction Scheme 6

[0076]

[0077] Example 7.5,5'-oxybis(1,3-dibromobenzene) (3.61g), cuprous iodide (0.21g) and triethylamine (3.42g) are added to 20g of 1,4-dioxane at room temperature. The reaction mixture is purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.53g) is added to the reaction mixture, and the mixture is heated to 70°C. 4-ethynylphenyl acetate (4.81g) is dissolved in degassed 1,4-dioxane (17g), and then the solution is slowly added to the reaction mixture by a feed funnel. After completion of the addition, the reaction mixture is stirred overnight at 70°C under nitrogen. After the reaction is complete, the reaction mixture is cooled to room temperature, filtered, and the solvent is evaporated. The residue is purified by chromatography to obtain a light yellow solid. The solid obtained is then dissolved in THF (40g) under nitrogen. Lithium hydroxide monohydrate (1.26g) and water (10g) are added, and the mixture is stirred at 60°C for 1 hour. The reaction mixture is then diluted with ethyl acetate, and then treated with hydrochloric acid until the pH of the water layer is 1. The organic phase is separated and the aqueous phase is extracted with ethyl acetate. The organic layers are merged and washed with water. The solvent is removed under vacuum, and the residue is purified by column chromatography to obtain 3.1g (65% yield) of 5,5'-oxybis(1,3-bis((4-hydroxyphenyl)ethynyl)benzene) (compound I6) as a light yellow solid. The reaction is shown in the following reaction scheme.

[0078] Reaction Scheme 7

[0079]

[0080] Example 8.9,9-bis(6-(3,5-dibromophenoxy)naphthalene-2-yl)-9H-fluorene (6.85 g), cuprous iodide (0.21 g) and triethylamine (3.42 g) were added to 25 g of 1,4-dioxane at room temperature. The reaction mixture was purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.53 g) was added to the reaction mixture, and the mixture was heated to 70 ° C. 4-ethynylphenyl acetate (4.81 g) was dissolved in degassed 1,4-dioxane (22 g), and the solution was then slowly added to the reaction mixture through an addition funnel. After the addition was completed, the reaction mixture was stirred overnight at 70 ° C under nitrogen. After the reaction was completed, the reaction mixture was cooled to room temperature, filtered, and the solvent was evaporated. The residue was purified by chromatography to obtain a light yellow solid. The solid obtained was then dissolved in THF (40 g) under nitrogen. Lithium hydroxide monohydrate (1.26g) and water (10g) are added, and the mixture is stirred at 60°C for 1 hour.Then the reaction mixture is diluted with ethyl acetate, and then treated with hydrochloric acid until the pH of the water layer is 1. The organic phase is separated and the aqueous phase is extracted with ethyl acetate. The organic layers are merged and washed with water. The solvent is removed under vacuum, and the residue is purified by column chromatography to obtain 4.7g (59% yield) of 9,9-bis-(6-(3,5-bis-((4-hydroxyphenyl)ethynyl)phenoxy)naphthalene-2-yl)-9H-fluorene (compound I7) in a light yellow solid. The reaction is shown in the following reaction scheme.

[0081] Reaction Scheme 8

[0082]

[0083] Example 9.1,3,5-triethynylbenzene (2.83g), cuprous iodide (0.17g) and triethylamine (4.10g) are added to 20g of 1,4-dioxane at room temperature. The reaction mixture is purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.32g) is added to the reaction mixture, and the mixture is heated to 70°C. 2-((6-ethynylnaphthalene-2-yl)oxy)tetrahydro-2H-pyran (6.81g) is dissolved in degassed 1,4-dioxane (13g), and then the solution is slowly added to the reaction mixture by a feed funnel. After completion of the addition, the reaction mixture is stirred overnight at 70°C under nitrogen. After the reaction is complete, the reaction mixture is cooled to room temperature, filtered, and the solvent is evaporated. The residue is purified by chromatography to obtain a white solid. The solid obtained is then dispersed in MeOH (54g) under nitrogen. 12N HCl (4.5g) and water (54g) were added, and the mixture was refluxed at 60°C overnight. The reaction mixture was then cooled to room temperature, and the solvent was removed under vacuum. The residue was diluted with ethyl acetate, and the organic phase was separated and the aqueous phase was extracted with ethyl acetate. The organic layers were merged and washed with water. The solvent was removed under vacuum, and the residue was purified by column chromatography to obtain 1.1g (21% yield) of 1,3,5-tris((2-hydroxynaphthyl-6-ethynyl)benzene (compound I8) as a white solid. The reaction is shown in the following reaction scheme.

[0084] Reaction Scheme 9

[0085]

[0086] Compound I2 (6.0 g) was stirred in 46 g of anhydrous DMF for 15 minutes at room temperature. The mixture was heated to 30 ° C and then 10.34 g of K2CO3 was added. The reaction was then heated to 50 ° C and 8.63 g of bromopropyne (80% in toluene) solution was added dropwise via an addition funnel. The reaction mixture was heated at 50 ° C for 24 hours. The reaction was then cooled to room temperature and filtered to remove most of K2CO3. Organic matter was precipitated into 2L water and stirred at room temperature for 0.5 hour. The precipitated polymer was collected by filtration and solid (17.8 g) was obtained after drying for 1 day at 35 ° C under vacuum.

[0087] Reaction Scheme 10

[0088]

[0089] Comparative Example 1.1,3,5-tri(4-bromophenyl)benzene (4.05g), cuprous iodide (0.21g) and triethylamine (3.42g) are added to 20g of 1,4-dioxane at room temperature. The reaction mixture is purged with nitrogen for 1 hour. Bis(triphenylphosphine)palladium chloride (II) (0.53g) is added to the reaction mixture, and the mixture is heated to 70°C. 4-ethynylphenyl acetate (4.81g) is dissolved in degassed 1,4-dioxane (14g), and then the solution is slowly added to the reaction mixture by a feed funnel. After completion of the addition, the reaction mixture is stirred overnight at 70°C under nitrogen. After the reaction is complete, the reaction mixture is cooled to room temperature, filtered, and the solvent is evaporated. The residue is purified by chromatography to obtain a light yellow solid. The solid obtained is then dissolved in THF (35g) under nitrogen. Lithium hydroxide monohydrate (0.94g) and water (8g) are added, and the mixture is stirred at 60°C for 1 hour. The reaction mixture is then diluted with ethyl acetate, and then treated with hydrochloric acid until the pH of the water layer is 1. The organic phase is separated and the aqueous phase is extracted with ethyl acetate. The organic layers are merged and washed with water. The solvent is removed under vacuum, and the residue is purified by column chromatography to obtain 2.2g (44% yield) of 1,3,5-tris ((4-(4-hydroxyphenyl)ethynyl)phenyl)benzene (comparison 1) in a light yellow solid. The reaction is shown in the following reaction scheme.

[0090] Reaction Scheme 11

[0091]

[0092] Example 10. Solubility was assessed by mixing the compound of the present invention with each of PGME and PGMEA at 5% solids. Visual inspection and use of a turbidity meter (Orbeco-Hellige Company) to check these mixtures. If the turbidity value is less than 1, the compound is rated as soluble ("S"), and if the turbidity value is greater than 1, it is rated as insoluble ("NS"). The results are reported in Table 1. As can be seen from these data, the compound of the present invention and the comparative compound are soluble in each of PGME and PGMEA.

[0093] Table 1

[0094]

[0095] Example 11.The thermal stability of the compounds of the present invention was evaluated using a thermogravimetric analyzer (TGA) Q500 from TA-Instruments under the following conditions: ramping to 700°C at 10°C / min under N2; and ramping to 700°C at 10°C / min under air. The temperature at which the material loses 5% of its weight (“Td 5% ”) are reported in Table 2.

[0096] Table 2

[0097]

[0098] Example 12. Resistance to solvent stripping was measured as an indicator of film crosslinking. Compositions of the compounds of the invention and comparative compound 1 at 4.5% solids in a mixture of PGMEA and benzyl benzoate were prepared. Each composition was spin coated on an 8" (200 mm) silicon wafer using an ACT-8 Clean Track (Tokyo Electron Co.) at a rate of 1500 rpm and then baked for 60 seconds at the temperatures reported in Table 3 to form a film. The film was prepared using an OptiProbe from Therma-Wave Corporation. TM Measure the initial film thickness. Next, commercial remover OK73 (PGME / PGMEA=70 / 30) was applied to each film for 90 seconds, followed by a stripping post-baking step at 105°C for 60 seconds. The thickness of each film after stripping post-baking was measured again to determine the amount of film thickness loss. The difference in film thickness before and after contact with the remover is reported in Table 3 as a percentage of the remaining film thickness. As can be seen from the data, after contact with the release agent, the film formed by the compound of the present invention retains more than 99% of its thickness, whereas the film formed by comparative compound 1 retains only 12% of the film thickness (i.e., it loses 88% of its thickness).

[0099] Table 3

[0100] Item Number Compound % Remaining Film 1 I2 >99(230℃) 2 I6 >99(230℃) 3 I9 >99(300℃) 4 Comparison 1 12(230℃)

[0101] Example 13.Compositions of the compounds of the present invention and comparative compound 1 at 4.5% solids in a mixture of PGMEA and benzyl benzoate were prepared. Each composition was spin-coated on an 8" (200 mm) silicon wafer at a rate of 1500 rpm using an ACT-8 Clean Track (Tokyo Electron Co.), and then baked for 60 seconds at the temperature determined in Table 4 to form a cured film. The optical constants were measured at 193 nm by a Vacuum Ultra-Violet Variable Angle Ellipsometer (VUV-VASE, from Woollam Co.), and are reported in Table 4.

[0102] Table 4

[0103]

[0104] Example 14. The compounds of the present invention were evaluated to determine their gap filling properties. A gap filling template was created at CNSE Nano-FAB (Albany, NY). The template had a SiO2 film thickness of 100 nm and various spacings and patterns. Before coating the sample with the composition of the present invention, the template sample was baked at 150°C for 60 seconds as a dehydration bake. Each coating composition (4.5% solids in a mixture of PGMEA, benzyl benzoate and PolyFox PF656) was coated on the template sample using an ACT-8Clean Track (Tokyo Electron) spin coater and a rotation rate of 1500rpm+ / -200rpm. The target film thickness after curing was 100nm, and the composition dilution was adjusted accordingly to approximately obtain the target film thickness after curing. The film was cured by placing the wafer on a hot plate at a temperature determined in Table 5 for 60 seconds. Cross-sectional scanning electron microscope (SEM) images of the coated sample were collected using a Hitachi S4800 SEM (from Hitachi High Technologies). The planarization quality of the film is obtained from the SEM image using Hitachi offline CD measurement software or CDM software by measuring the thickness difference (ΔFT) between the dense grooves and the open area of ​​the film. Films with ΔFT <20nm are considered to have "good" planarization and films with ΔFT>20nm are considered to have "poor" planarization. Gap filling is evaluated by visually inspecting the SEM image to observe whether there are any voids or bubbles in the groove pattern. Films without voids in the groove pattern are considered to have "good" gap filling and films with voids in the groove pattern are considered to have "poor" gap filling. These results are reported in Table 5.

[0105] Table 5

[0106] Sample No. Compound (Temperature) Flattening Gap Filling 1 I2(240℃) good good 2 I6(240℃) good good 3 I8(300℃) good good 4 I9(300℃) good good 5 Comparison 1 (300°C) Difference good

[0107] Example 15. Compositions of the compounds of the invention and comparative compound 1 at 4.5% solids in PGMEA were prepared. Each composition was spin coated on an 8" (200 mm) silicon wafer using an ACT-8 Clean Track (Tokyo Electron) at a rate of 1500 rpm and then baked for 60 seconds at the temperature reported in Table 6 to form a cured film. The coating quality was evaluated by visual inspection of the film and the results are reported in Table 6.

[0108] Table 6

[0109] Item Number Compound (Temperature) Coating quality 1 I2(240℃) good 2 I9(300℃) good 3 Comparison 1 (300°C) Difference

[0110] Example 16. Each bottom layer solution (4.5% solid in a mixture of PGMEA and benzyl benzoate) was spin-coated on a 200mm silicon wafer at 1500rpm using ACT-8Clean Track, with a target film thickness of 100nm after curing. The original silicon wafer was inverted on the top of the coated wafer with three (2mm) spacers on the edge. The wafer stack was baked for 60 seconds on a hot plate (wherein the coated wafer was at the bottom) at a temperature determined in Table 7. The haze of the top wafer was checked (which indicated sublimation) and defects were checked using an SP2 defect tool (from KLA-Tencor Corporation, Inc., USA) with a sensitivity of 500nm. As can be seen from the data in Table 7, Comparative Compound 1 gives significantly higher defect counts and defect densities than Compound I2 of the present invention.

[0111] Table 7

[0112]

Claims

1. A method for manufacturing an electronic device, comprising: (a) providing an electronic device substrate; (b) coating a coating composition layer comprising one or more curable compounds on the surface of the electronic device substrate, wherein the one or more curable compounds comprises a 5-6 Aromatic ring and C 9-30 The aromatic nucleus of the fused aromatic ring system and three or more substituents having the formula (1) wherein at least two substituents having formula (1) are attached to the aromatic core; and wherein Ar 1 is an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Z is a substituent selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x is an integer from 1 to 4; and * represents an attachment point to the aromatic core or an attachment point to a curable compound other than the aromatic core; (c) curing the layer of the curable compound to form an underlying layer; (d) coating a photoresist layer on the underlying layer; (e) exposing the photoresist layer to actinic radiation through a mask; (f) developing the exposed photoresist layer to form a resist pattern; and (g) transferring the pattern to the bottom layer to expose a portion of the electronic device substrate.

2. The method of claim 1, further comprising the steps of patterning the substrate; and then removing the patterned bottom layer.

3. The method of claim 1, further comprising the step of coating one or more of a silicon-containing layer, an organic anti-reflective coating, and a combination thereof on the base layer before step (d).

4. The method of claim 3, further comprising the step of transferring the pattern onto one or more of the silicon-containing layer, the organic anti-reflective coating, and combinations thereof, after step (f) and before step (g).

5. The method of claim 1, wherein each Z is independently selected from OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SH, fluorine, and NHR 2 .

6. The method of claim 1, wherein the aromatic nucleus is selected from pyridine, benzene, naphthalene, quinoline, isoquinoline, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenacene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene.

7. The method of claim 1, wherein each Ar 1 independently selected from pyridine, benzene, naphthalene, quinoline, isoquinoline, anthracene, phenanthrene, pyrene, coronene, triphenylene, phenacene, benz[a]anthracene, dibenzo[a,h]anthracene, and benzo[a]pyrene.

8. The method of claim 1, wherein the coating composition further comprises one or more of an organic solvent, a curing agent, and a surface leveling agent.

9. An electronic device comprising an electronic device substrate, the electronic device substrate having a polymer layer on a surface of the electronic device substrate, the polymer consisting of one or more curable compounds as polymerized units, wherein the one or more curable compounds comprises a 5-6 Aromatic ring and C 9-30 The aromatic nucleus of the fused aromatic ring system and three or more substituents having the formula (1) wherein at least two substituents having formula (1) are attached to the aromatic core; and wherein Ar 1 is an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Z is a substituent selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x is an integer from 1 to 4; and * represents an attachment point to the aromatic core or an attachment point to a curable compound other than the aromatic core.

10. A method for manufacturing an electronic device, comprising: (a) providing an electronic device substrate; (b) coating a coating composition layer comprising one or more curable compounds having formula (2) on the surface of the electronic device substrate Among them, Ar c is an aromatic nucleus having 5 to 30 carbon atoms; Ar 1 ,Ar 2 , and Ar 3 Each is independently an aromatic ring or fused aromatic ring system having 5 to 30 carbon atoms; Y is a covalent chemical single bond, a divalent linking group, or a trivalent linking group; Z 1 and Z 2 are independently selected from the group consisting of: OR 1 , protected hydroxyl, carboxyl, protected carboxyl, SR 1 , protected thiol group, -OC(=O)-C 1-6 -Alkyl, halogen, and NHR 2 ; Each R 1 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon groups, and C 5-30 Aryl; each R 2 Selected from H, C 1-10 Alkyl, C 2-10 Unsaturated hydrocarbon group, C 5-30 Aryl, C(=O)-R 1 , and S(=O)2-R 1 ; x1=1 to 4; x2=1 to 4; y1=2 to 4; each y2=0 to 4; y1+each y2≥3; w=0 to 2; and z is equal to 0 to 2; wherein z=1 when Y is a covalent chemical single bond or a divalent linking group; and z=2 when Y is a trivalent linking group; (c) curing the layer of the curable compound to form a bottom layer; (d) coating a photoresist layer on the bottom layer; (e) exposing the photoresist layer to actinic radiation through a mask; (f) developing the exposed photoresist layer to form a resist pattern; and (g) transferring the pattern to the bottom layer to expose a portion of the electronic device substrate.