High energy density all-solid-state battery and method for manufacturing the same
By alternately stacking electrode units in an all-solid-state battery and adding insulating members, the battery energy density and short circuit problems are solved, high energy density and stability are achieved, and the manufacturing process is simplified.
Patent Information
- Application Number
- CN201911220988.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-03
- Filing Date
- 2019-12-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-12-03
AI Technical Summary
The actual energy density and output of all-solid state batteries are lower than that of conventional lithium-ion batteries using liquid electrolytes, and due to the presence of the electrolyte membrane, the battery volume and weight increase, making it easy to short circuit.
By alternately stacking the first and second electrode units in an all-solid state battery and adding insulating members to the edge portions of the electrode current collector, the consumption of electrode current collector is reduced by a simple process, and the third electrode unit is located on the outermost side to reduce the excess electrode, pressing Conditions are optimized to prevent short circuits.
High energy density and stability are achieved, and the manufacturing process of all-solid-state batteries is simplified, which prevents or suppresses short circuits, and improves the overall performance of the battery.
Smart Images

Figure CN111883846B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an all-solid-state battery having high energy density and a method for manufacturing the same. Background Art
[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.
[0003] Generally, rechargeable secondary batteries are used not only in small electronic devices such as mobile phones, notebook computers, etc., but also in large vehicles such as hybrid electric vehicles, electric vehicles, etc.
[0004] Most conventional secondary batteries constitute batteries based on organic solvents (organic liquid electrolytes), and thus show limitations in improving stability and energy density.
[0005] On the other hand, an all-solid-state battery using an inorganic solid electrolyte is manufactured based on a technology that does not contain an organic solvent, thus enabling its battery to be manufactured in a safer and simpler form and is now attracting attention.
[0006] However, the actual energy density and output of all-solid-state batteries are lower than those of conventional lithium-ion batteries using liquid electrolytes. In all-solid-state batteries, since the electrolyte membrane including a solid electrolyte is located between the positive electrode and the negative electrode, the all-solid-state battery has a large volume and weight compared to conventional lithium-ion batteries, and thus has a lower energy density per unit volume and energy density per unit weight. If the thickness of the electrolyte membrane is reduced, a short circuit may occur between the positive electrode and the negative electrode.
[0007] The above information disclosed in this Background section is only for enhancement of understanding of the background of the present disclosure and therefore it may contain information that does not form the prior art that is already known to a person of ordinary skill in the art.
[0008] Related technical literature
[0009] Patent Literature
[0010] Korean registered patent No. 10-1750145 Summary of the invention
[0011] The present disclosure provides an all-solid-state battery that can have high stability and energy density while exerting the original function of the solid-state battery as a secondary battery.
[0012] The present disclosure also provides a method for manufacturing an all-solid-state battery, in which a short circuit occurring at an edge portion of a battery can be prevented or suppressed through a simple process, and the all-solid-state battery can be efficiently manufactured.
[0013] In one aspect, the present disclosure provides an all-solid-state battery, including a first unit, each first unit including a first electrode current collector and a first electrode active material layer formed on both surfaces of the first electrode current collector. The battery is also provided with a second unit, each second unit including a second electrode current collector, a second electrode active material layer formed on both surfaces of the second electrode current collector, and a solid electrolyte layer formed on the second electrode active material layer, wherein the first unit and the second unit are alternately stacked. The battery also includes an insulating member accommodated in a space between an edge portion of the first electrode active material layer and a side surface of the second unit.
[0014] In one form, the all-solid-state battery may further include third units, each of the third units including a third electrode current collector and a third electrode active material layer formed on one surface of the third electrode current collector, and the third units may be located at the outermost position of the all-solid-state battery.
[0015] In another form, the area of the first unit may be greater than or equal to the area of the second unit.
[0016] In still another form, the second unit may be placed on the central portion of the first electrode active material layer so that the first electrode active material layer and the solid electrolyte layer are stacked in contact with each other.
[0017] In yet another form, the area of the central portion of the first electrode active material layer may be greater than or equal to the area of the second unit.
[0018] In another form, the sum of the thickness of one insulating member and another insulating member adjacent thereto may be the same as the thickness of the second unit.
[0019] In another form, the insulating member may surround the side surface of the second unit and be formed of a transparent material.
[0020] In another form, the first unit may be configured such that one first electrode current collector having a thickness of 4 to 20 μm is interposed between a pair of first electrode active material layers.
[0021] In still another form, the second unit may be configured such that one second electrode current collector having a thickness of 5 to 20 μm is interposed between a pair of second electrode active material layers.
[0022] In yet another form, the first electrode active material layer may have a thickness of 50 to 300 μm, a mixed density of 1.2 to 3.5 g / cc, and a density of 10 to 45 mg / cm 2 load level and a brightness value of 30 to 80 in the CIELAB color space.
[0023] In another form, the second electrode active material layer may have a thickness of 50 to 300 μm, a mixed density of 2.5 to 5.0 g / cc, a loading level of 10 to 35 mg / cm 2 , and a brightness value of 40 to 90 in the CIELAB color space.
[0024] On the other hand, the present disclosure provides a method for manufacturing an all-solid-state battery, the method comprising: preparing a first unit, each first unit comprising a first electrode current collector, and a first electrode active material layer formed on both surfaces of the first electrode current collector. The method comprises forming an insulating member on the edge portion of the first electrode active material layer. The method comprises: preparing a second unit, each second unit comprising a second electrode current collector, a second electrode active material layer formed on both surfaces of the second electrode current collector, and a solid electrolyte layer formed on the second electrode active material layer. The method comprises obtaining a battery structure by alternately stacking the first unit and the second unit and pressing the battery structure.
[0025] In one form, the method may further include stacking third units on the outermost layer of the battery structure before pressing the battery structure, each third unit including a third electrode current collector and a third electrode active material layer formed on one surface of the third electrode current collector.
[0026] In another form, the battery structure may be configured such that the second unit is placed on the central portion of the first electrode active material layer, and thus the first electrode active material layer and the solid electrolyte layer are stacked in contact with each other.
[0027] In still another form, the sum of the thicknesses of one insulating member and another insulating member adjacent thereto may be the same as the thickness of the second unit.
[0028] In still another form, the insulating member may surround the side surface of the second unit and be formed of a transparent material.
[0029] In another form, the first unit and the second unit may not be pressed when the first unit and the second unit are prepared.
[0030] In another form, the battery structure may be pressed at a pressure of 250 MPa to 500 MPa.
[0031] Other aspects of the disclosure are discussed below.
[0032] Further areas of applicability will become apparent from the description provided herein.It should be understood that the description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order that the present disclosure may be readily understood, various forms thereof will now be described by way of example and with reference to the accompanying drawings, in which:
[0034] Figure 1 is a cross-sectional view schematically showing an all-solid-state battery according to the present disclosure;
[0035] Figure 2 is a cross-sectional view schematically showing a first unit according to the present disclosure;
[0036] Figure 3 is a cross-sectional view schematically showing a second unit according to the present disclosure;
[0037] Figure 4 is a perspective view schematically showing a central portion and an edge portion of a first unit according to the present disclosure;
[0038] Figure 5 is a cross-sectional view schematically showing a third unit according to the present disclosure;
[0039] Figure 6 is a flow chart showing a method for manufacturing an all-solid-state battery according to the present disclosure;
[0040] Fig. 7A and Figure 7B is a diagram showing observation results of a middle (10th) interface and a lowermost interface of a battery structure according to an example of the present disclosure after the battery structure is pressed at 200 MPa; and
[0041] Figure 7C and Fig.7D is a diagram showing observation results of a middle (10th) interface and a lowermost interface of a battery structure according to an example of the present disclosure after the battery structure was pressed at 300 MPa.
[0042] It should be understood that the drawings are not necessarily drawn to scale, presenting somewhat simplified representations of various features illustrating the basic principles of the present disclosure. The specific design features of the present disclosure disclosed herein, including, for example, specific dimensions, orientations, locations, and shapes will be determined in part by the specific intended application and use environment.
[0043] In the drawings, reference numbers refer to the same or equivalent parts of the present disclosure throughout the several figures of the drawing.
[0044] The drawings described herein are for illustration purposes only and are not intended to limit the scope of the present disclosure in any way. DETAILED DESCRIPTION
[0045] The following description is merely exemplary in nature and is not intended to limit the present disclosure, application, or uses. It should be understood that throughout the drawings, corresponding reference numerals indicate the same or corresponding parts and features.
[0046] Hereinafter, reference will be made in detail to various forms of the present disclosure, examples of which are shown in the accompanying drawings and described below. Although the present disclosure will be described in conjunction with the exemplary forms, it should be understood that this description is not intended to limit the present disclosure to the exemplary forms. On the contrary, the present disclosure is intended to cover not only the exemplary forms, but also various alternatives, modifications, equivalents and other forms within the spirit and scope of the present disclosure as defined by the appended claims.
[0047] In the following formal description, even if shown in different drawings, the same elements are also represented by the same reference numerals. In the accompanying drawings, for clarity, the size of the structure is enlarged compared to the actual size. In the following formal description, terms such as "first", "second", etc. can be used to describe various elements, but do not limit these elements. These terms are only used to distinguish an element from other elements. For example, in the spirit and scope of the present disclosure, the first element can be named as the second element, and similarly, the second element can be named as the first element. Unless singular expressions have significantly different contextual meanings, they can contain plural expressions.
[0048] In the following forms of description, terms such as "including", "having" and the like will be interpreted as indicating the presence or combination of features, numbers, steps, operations, elements or parts stated in the description, and do not exclude the presence of one or more other features, numbers, steps, operations, elements, parts or combinations thereof, or the possibility of adding them. In addition, it will be understood that when a part such as a layer, film, region or plate is referred to as being "above" another part, the part may be located "directly above" the other part or other parts may also be inserted between the two parts. In the same way, it will be understood that when a part such as a layer, film, region or plate is referred to as being "below" another part, the part may be located "directly below" the other part or other parts may also be inserted between the two parts.
[0049] All the numbers, values and / or expressions representing the amount of components, reaction conditions, polymer compositions and blends used in the specification are approximate values, which reflect the various uncertainties in the measurements generated when obtaining these values, and therefore, it should be understood that, unless otherwise stated, they should be modified with the term "about". In addition, it will be understood that if a numerical range is disclosed in the specification, the range includes all continuous values from the minimum value to the maximum value of the range unless otherwise stated. In addition, if such a range refers to an integer, the range includes all integers from the minimum integer to the maximum integer unless otherwise stated.
[0050] Figure 1 Schematically shows a cross-sectional view of an all-solid-state battery 1 according to the present disclosure. Figure 1 The all-solid-state battery 1 includes a first cell 10 , a second cell 20 , a third cell 30 located at the outermost position of the battery structure, and an insulating member 40 accommodated in a space between an edge portion of the first cell 10 and a side surface portion of the second cell 20 .
[0051] In the first electrode current collector 11 , the second electrode current collector 21 , and the third electrode current collector 31 included in the all-solid-state battery, each of the first electrode, the second electrode, and the third electrode may be a positive electrode or a negative electrode.
[0052] In particular, the first electrode and the third electrode may have the same polarity, and the second electrode may have a different polarity. For example, if the first electrode is a positive electrode, the second electrode may be a negative electrode, and the third electrode may be a positive electrode. In addition, if the first electrode is a negative electrode, the second electrode may be a positive electrode, and the third electrode may be a negative electrode. More specifically, the first electrode may be a negative electrode, the second electrode may be a positive electrode, and the third electrode may be a negative electrode.
[0053] Unit 1
[0054] Figure 2 2 is a cross-sectional view schematically showing the first unit 10. Figure 2 , the first unit 10 includes a first electrode current collector 11 and a first electrode active material layer 12 formed on each of both surfaces of the first electrode current collector 11 .
[0055] The first electrode may be a positive electrode or a negative electrode. If the first electrode is a negative electrode, the second electrode may be a positive electrode, and if the first electrode is a positive electrode, the second electrode may be a negative electrode, but is not limited thereto. Specifically, the first electrode may be a negative electrode.
[0056] The first electrode current collector 11 may be formed of any material having conductivity and current collecting function, but is not limited thereto. The material of the first electrode current collector 11 may be one selected from the group consisting of copper (Cu), copper (Cu) coated with carbon (C), and nickel (Ni). In addition, the first electrode current collector 11 may be formed, for example, as a nickel mesh, a copper foil, and the like.
[0057] The first electrode current collector 11 may have a thickness of about 4 to 20 μm. For example, the first electrode current collector 11 formed of copper (Cu) may have a thickness of 5 to 15 μm, the first electrode current collector 11 formed of copper (Cu) coated with carbon (C) may have a thickness of 7 to 20 μm. Or the first electrode current collector 11 formed of nickel (Ni) may have a thickness of 4 to 20 μm.
[0058] The first electrode active material layer 12 may include a first electrode active material, a solid electrolyte, a conductive material, a binder, and the like.
[0059] As the first electrode active material, a carbon material such as natural graphite, artificial graphite, graphite carbon fiber or resin-baked carbon, or an alloy material mixed with a solid electrolyte can be used. For example, the alloy material can be a lithium alloy (LiAl, LiZn, Li 3 Bi, Li 3 Cd, Li 3 Sb, Li 4 Si, Li 4.4 Pb, Li 4.4 Sn,Li 0.17 C, LiC 6 etc.) or metal oxides, such as lithium titanate (Li 4 Ti 5 O 12 ) or Zn.
[0060] The solid electrolyte may be responsible for conducting lithium ions in the first electrode active material layer 12, and may be an oxide-based solid electrolyte or a sulfide-based solid electrolyte. Specifically, a sulfide-based solid electrolyte having high lithium ion conductivity may be used.
[0061] Sulfide-based solid electrolytes can be Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -Li l , Li 2 SP 2 S 5 -LiC l , Li 2 SP 2 S 5 -LiBr, Li 2 SP 2 S 5 -Li 2 O. Li 2 SP 2 S 5 -Li 2 O-Li l , Li 2 S-SiS 2 , Li 2 S-SiS 2 -Li l , Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiC l , Li2 S-SiS 2 -B 2 S 3 -Li l , Li 2 S-SiS 2 -P 2 S 5 -Li l , Li 2 SB 2 S 3 , Li 2 SP 2 S 5 -Z m S n (where m and n are positive numbers, and Z is one selected from the group consisting of Ge, Zn and Ga), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (here, x and y are positive numbers, and M is one selected from the group consisting of P, Si, Ge, B, Al, Ga, and In), Li 10 G 2 S 12 wait.
[0062] The sulfide-based solid electrolyte may have an average particle size (D50) of 0.1 to 10 μm.
[0063] The lithium ion conductivity can be 1×10 -4 S / cm of sulfide-based solid electrolytes.
[0064] The conductive material may be carbon black, conductive graphite, ethylene black, graphene, or the like.
[0065] The binder of the first electrode active material layer 12 may be butadiene rubber (BR), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), etc., but is not limited thereto.
[0066] The first electrode active material layer 12 may have a thickness of 50-300 μm, a mixed density of 0.1-2.0 g / cc before pressing, a mixed density of 1.2-3.5 g / cc after pressing, and a viscosity of 10-45 mg / cm 2Load level, brightness value 30-80 in CIELAB color space.
[0067] In the present disclosure, the term “loading level” refers to the loading amount of a material constituting the first electrode active material layer 12 .
[0068] If each battery cell including a negative electrode, a positive electrode and a solid electrolyte is stacked as in a conventional method, the first electrode current collector or the second electrode current collector is stacked, and thus the two current collectors overlap each other. Therefore, the conventional laminate consumes a large amount of current collectors, thus resulting in a decrease in energy density. In contrast, a first electrode current collector 11 is inserted between a pair of first electrode active material layers 12, and thus, the amount of the first electrode current collector 11 consumed is reduced compared to the conventional process, and an all-solid-state battery manufactured by a simple process and having a high energy density can be obtained.
[0069] Unit 2
[0070] Figure 3 2 is a cross-sectional view schematically showing the second unit 20. Figure 3 The second unit 20 includes a second electrode current collector 21 , a second electrode active material layer 22 formed on both surfaces of the second electrode current collector 21 , and a solid electrolyte layer 23 formed on the second electrode active material layer 22 .
[0071] The second electrode may be a positive electrode or a negative electrode. If the second electrode is a positive electrode, the first electrode may be a negative electrode, and if the second electrode is a negative electrode, the first electrode may be a positive electrode, but is not limited thereto. Specifically, the second electrode may be a positive electrode.
[0072] The second electrode current collector 21 may be formed of any material having conductivity and a current collecting function, but is not limited thereto.
[0073] The material of the second electrode current collector 21 may be aluminum (Al) or aluminum (Al) coated with carbon (C). In addition, the second electrode current collector 21 may be formed as, for example, an aluminum foil.
[0074] The second electrode current collector 21 may have a thickness of about 5 to 20 μm. For example, the second electrode current collector 21 formed of aluminum (Al) may have a thickness of 5 to 15 μm, or the second electrode current collector 21 formed of aluminum (Al) coated with carbon (C) may have a thickness of 7 to 20 μm.
[0075] The second electrode active material layer 22 may include a second electrode active material, a solid electrolyte, a conductive material, a binder, and the like.
[0076] The second electrode active material may be an oxide active material or a sulfide active material.
[0077] The oxide active material can be a rock salt type active material (such as LiCoO 2 , LiMnO 2 , LiNiO 2 , LiVO 2 or Li 1+x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ), a spinel type active material (such as LiMn 2 O 4 or Li(Ni 0.5 Mn 1.5 )O 4 ), an inverse spinel type active material (such as LiNiVO 4 or LiCoVO 4 ), an olivine type active material (such as LiFePO 4 , LiMnPO 4 , LiCoPO 4 or LiNiPO 4 ), a silicon-containing active material (such as Li 2 FeSiO 4 or Li 2 MnSiO 4 ), a rock salt type active material in which a part of the transition metal is replaced by a different metal (such as LiNi 0.8 Co( 0.2-x )AlxO 2 (0 < x < 0.2)), a spinel type active material in which a part of the transition metal is replaced by a different metal (such as Li 1 +xMn 2-x-y M y O 4 (M is at least one of Al, Mg, Co, Fe, Ni or Zn, 0 < x + y < 2)) or lithium titanate (such as Li 4 Ti 5 O 12 ).
[0078] The sulfide active material can be Chevrel copper, iron sulfide, cobalt sulfide, nickel sulfide, etc.
[0079] The solid electrolyte can be an oxide-based solid electrolyte or a sulfide-based solid electrolyte, and is the same as or different from the solid electrolyte included in the first electrode active material layer 12.
[0080] The conductive material can be carbon black, conductive graphite, ethylene black, graphene, etc.
[0081] The binder may be butadiene rubber (BR), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), etc., and may be the same as or different from the binder contained in the first electrode active material layer 12 .
[0082] The second electrode active material layer 22 may have a thickness of 50-300 μm, a mixed density of 0.5-3.0 g / cc before pressing, a mixed density of 2.5-5.0 g / cc after pressing, and a viscosity of 10-35 mg / cm 2 The load level is 40-90 in the Lab color space.
[0083] The solid electrolyte layer 23 is provided on the second electrode active material layer 22 to allow lithium ions to move between the two electrodes.
[0084] The first electrode active material layer and the second electrode active material layer are respectively placed in contact with both surfaces of the solid electrolyte layer.
[0085] The solid electrolyte layer 23 may include an oxide-based solid electrolyte or a sulfide-based solid electrolyte. Here, the solid electrolyte may be the same as or different from the solid electrolyte included in the first electrode active material layer 12.
[0086] One second electrode current collector 21 is inserted between a pair of second electrode active material layers 22. Therefore, in the same manner as the first electrode current collector 11, the consumption of the positive electrode current collector is reduced compared to a conventional laminate. Therefore, an all-solid-state battery manufactured by a simple process and having a high energy density can be obtained.
[0087] Insulation components
[0088] Figure 4 is a perspective view schematically showing the first electrode active material layer 12 and the insulating member 40. Figure 1 and Figure 4 , the second unit 20 is placed on the center portion 121 of the first electrode active material layer 12 so that the first electrode active material layer 12 and the solid electrolyte layer 23 are in contact with each other. Here, the insulating member 40 is located at the edge portion 122 of the first electrode active material layer 12, and thus surrounds the side of the second unit 20. In addition, referring to Figure 1 In a state where a plurality of first units 10 and a plurality of second units 20 are stacked, a sum of thicknesses of one insulating member 40 and another insulating member 40 adjacent thereto is the same as the thickness of the second unit 20 .
[0089] The insulating member 40 may be formed of any material having an insulating function, but is not limited thereto.
[0090] The insulating member 40 may be formed of a transparent material and include one selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), polypropylene (PP), polyethylene (PE), and polycarbonate (PC). Since the insulating member 40 is formed of a transparent material, the insulating member 40 does not obstruct the field of view. Therefore, if a visual device for alignment is used when stacking the individual units, light can penetrate the insulating member 40 formed of a transparent material, and thus the alignment state of the individual units of the battery structure can be easily detected.
[0091] Unit 3
[0092] Figure 5 is a cross-sectional view schematically showing the third unit 30. Figure 5 , the third unit 30 includes a third electrode current collector 31 and a third electrode active material layer 32 formed on one surface of the third electrode current collector 31. The third electrode may be a positive electrode or a negative electrode. For example, if the first electrode is a negative electrode, the second electrode is a positive electrode, and the third electrode is a negative electrode. In addition, if the first electrode is a positive electrode, the second electrode is a negative electrode, and the third electrode is a positive electrode, but is not limited thereto. Specifically, the third electrode may be a negative electrode.
[0093] The third unit 30 is located at the outermost position of the all-solid-state battery 1 and is therefore directly pressed.
[0094] The material and thickness of the third electrode current collector 31 are the same as those of the first electrode current collector 11 .
[0095] The material, thickness, mixture density, loading level, and brightness value of the third electrode active material layer 32 are the same as those of the first electrode active material layer 12 .
[0096] If both the first unit 10 and the second unit 20 are stacked alternately, the excess electrode (the first electrode active material layer 12 or the solid electrolyte layer 23+the second electrode active material layer 22) remains at the outermost position of the all-solid-state battery 1. Therefore, the third unit 30 is arranged at the outermost position of the all-solid-state battery 1, so that the excess electrode can be reduced. Therefore, the material amount and volume of the all-solid-state battery 1 can be reduced, so that the energy density can be improved.
[0097] Figure 6 is a flow chart showing a method for manufacturing an all-solid-state battery 1 according to the present disclosure. Figure 6, the method includes: preparing first units 10, each of which includes a first electrode current collector 11 and a first electrode active material layer 12 (operation S10); forming an insulating member 40 at an edge portion 122 of the first electrode active material layer 12 (operation S20); preparing second units 20, each of which includes a second electrode current collector 21, a second electrode active material layer 22 and a solid electrolyte layer 23 (operation S30); stacking the first units 10 and the second units 20 (operation S40); preparing a battery structure by preparing a third unit 30 and stacking the third unit 30 on the outermost layer of the stacked first unit 10 and the second unit 20 (operation S50); and pressing the battery structure (operation S60).
[0098] When preparing the first unit 10 (operation S10), the first electrode active material layer 12 is formed on both surfaces of the first electrode current collector 11. The formation of the first electrode active material layer 12 on both surfaces of the first electrode current collector 11 is not limited to a specific method. For example, a slurry coating process, a spraying method, an aerosol deposition method, a cold spraying method, a sputtering method, a vapor deposition method, or a spraying method may be used, and in particular, a slurry coating process may be used.
[0099] The slurry coating process may be performed by preparing a slurry including a first electrode active material, coating both surfaces of the first electrode current collector 11 with the prepared slurry, and then drying the slurry. Such a slurry coating process on the first electrode current collector 11 may be performed by a dam type slurry coater method, a doctor blade method, a gravure transfer method, a reverse roll coater method, a die coating method, or the like.
[0100] The slurry including the first electrode active material may be prepared by a conventionally known method by mixing the first electrode active material, a solvent, and a solid electrolyte and a binder, if necessary.
[0101] The solvent used to prepare the slurry may use any solvent that does not have a negative impact on the performance of the first electrode active material, but is not limited thereto, and for example, a hydrocarbon-based organic solvent (e.g., heptane, toluene, or hexane), especially a hydrocarbon-based organic solvent having a low moisture content by dehydration. As the first electrode active material, a solid electrolyte and a binder that may be included in the slurry, the above-mentioned materials that may be included in the first electrode active material layer 12 may be used.
[0102] When forming the insulating member 40 (operation S20 ), the insulating member 40 is formed at the edge portion 122 of the first electrode active material layer 12 of the first cell 10 .
[0103] Since the insulating member 40 is formed of a transparent material, if a visual device for alignment is used when the respective cells are stacked, light may penetrate the insulating member 40 formed of the transparent material, and thus alignment of the cell structure may be achieved and the cell structure may be stabilized.
[0104] When preparing the second unit 20 (operation S30 ), the second electrode active material layer 22 is formed on both surfaces of the second electrode current collector 21 , and the solid electrolyte layer 23 is formed on the second electrode active material layer 22 .
[0105] The second electrode active material layer 22 is formed on both surfaces of the second electrode current collector 21, which may be the same as forming the first electrode active material layer 12 on both surfaces of the first electrode current collector 11, or a layer may be formed using a metal material that can oxidize and reduce lithium (Li) on both surfaces of the second electrode current collector 21. The metal material may include lithium (Li) or indium (Id).
[0106] Furthermore, a solid electrolyte layer 23 may be formed on the second electrode active material layer 22. The solid electrolyte layer 23 may have a thickness selected according to desired battery characteristics, and specifically, may have a thin thickness within a range in which a short circuit between the first electrode active material layer 12 and the second electrode active material layer 22 may be suppressed.
[0107] The solid electrolyte layer 23 may include a solid electrolyte and, if necessary, may include a binder. The solid electrolyte may be formed of a material of a solid electrolyte that may be included in the second electrode active material layer 22, and if the second electrode active material layer 22 includes a solid electrolyte, the solid electrolyte included in the solid electrolyte layer 23 and the solid electrolyte included in the second electrode active material layer 22 may be formed of the same material. The material of the binder may be the same as that of the binder included in the first electrode active material layer 12.
[0108] The formation of the solid electrolyte layer 23 on the second electrode active material layer 22 is not limited to a specific method. For example, a slurry coating process, a spraying method, an aerosol deposition method, a cold spraying method, a sputtering method, a vapor deposition method, or a spraying method may be used, and specifically, a slurry coating process may be used.
[0109] The slurry coating process is the same as the slurry coating process for forming the first electrode active material layer 12 on both surfaces of the first electrode current collector 11 .
[0110] In the stacking of the first unit 10 and the second unit 20 (operation S40), the prepared first unit 10 and the second unit 20 are stacked. In more detail, the second unit 20 is placed on the central portion 121 of the first electrode active material layer 12 of the first unit 10 so that the first electrode active material layer 12 and the solid electrolyte layer 23 are in contact with each other. Since the area of the first unit 10 is larger than that of the second unit 20, and the area of the central portion 121 of the first electrode active material layer 12 is greater than or equal to that of the second unit 20, the insulating member 40 accommodated in the space between the edge portion 122 of the first electrode active material layer 12 and the side of the second unit 20 is stacked to surround the side of the second unit 20.
[0111] In addition, in the conventional process, if each battery cell including a first electrode, a second electrode and a solid electrolyte is stacked, the first electrode current collector or the second electrode current collector is stacked so that the two current collectors overlap each other, and the consumption of the current collector increases, so it is difficult to obtain an all-solid-state battery with a high energy density. On the contrary, in the present disclosure, a first electrode current collector 11 with a thickness of 4 to 20 μm is inserted between a pair of first electrode active material layers 12 or a second electrode current collector 21 with a thickness of 4 to 20 μm is inserted between a pair of second electrode active material layers 22, and the consumption of the current collector is reduced compared to the conventional process, so that an all-solid-state battery manufactured by a simple process and having a high energy density can be obtained.
[0112] In addition, since the sum of the thicknesses of one insulating member 40 and another insulating member 40 adjacent thereto is the same as the thickness of the second unit 20, the insulating member 40 can prevent or suppress short circuits at the edge portions of the all-solid-state battery and at the same time align with the second unit 20 to stabilize the overall structure of the all-solid-state battery.
[0113] Here, the first unit 10 and the second unit 20 may be stacked in a jelly roll structure.
[0114] When preparing the battery structure (operation S50), the battery structure is prepared by stacking the third cells 30 on the outermost layer of the stacked first cells 10 and second cells 20, each of which includes a third electrode current collector 31 and a third electrode active material layer 32 formed on one surface of the third electrode current collector 31. If the third cell 30 is located at the outermost position of the battery structure, the third electrode active material layer 32 is not formed as the outermost layer, so the number of components is reduced, and the number of processing operations is also reduced.
[0115] In the pressing of the battery structure (operation S60 ), the prepared battery structure is pressed, thereby manufacturing an all-solid-state battery.
[0116] The pressing of the battery structure may be performed by surface pressing, ultra-high pressure isostatic pressing, 1-axis pressing, cold isostatic pressing (CIP) or hot pressing, and specifically by surface pressing or ultra-high pressure isostatic pressing.
[0117] In the conventional process, battery cells are pressed separately and then stacked, but in the present disclosure, the battery structure is prepared and then pressed at last, so the manufacturing process of the all-solid-state battery can be simplified.
[0118] When a battery structure in which the first unit and the second unit are alternately stacked 20 times is pressed at a pressure of 200 MPa, an interface defect occurs, but when the battery structure is pressed at a pressure of 300 MPa, no interface defects occur. Therefore, in order to manufacture an all-solid-state battery in which the battery according to the present disclosure works normally, the pressing conditions may be 250 MPa to 500 MPa. Hereinafter, the present disclosure will be described in more detail by the following examples. The following examples are only used to exemplarily describe the present disclosure and are not intended to limit the scope of the present disclosure.
[0119] Example
[0120] (Operation S10): A first electrode current collector using copper (Cu), copper (Cu) coated with carbon (C), or nickel (Ni) is formed to have a thickness of 5 to 15 μm, 7 to 20 μm, or 4 to 20 μm. A first electrode active material layer is formed on both surfaces of the first electrode current collector using a slurry including a graphite-based first electrode active material, a butyrate-based solvent, a sulfide-based solid electrolyte, and a rubber-based binder through a slurry coating process, thereby preparing a first unit. Here, the mixed density of the first electrode active material is 0.5 to 3.0 g / cc.
[0121] (Operation S20 ): A PI film is prepared as an insulating member and is placed at an edge portion of the first electrode active material layer.
[0122] (Operation S30): A second electrode current collector using aluminum (Al) or aluminum (Al) coated with carbon (C) is formed to have a thickness of 5 to 15 μm or 7 to 20 μm. A second electrode active material layer is formed on both surfaces of the second electrode current collector using a slurry comprising a 3-component second electrode active material (e.g., a nickel-cobalt-manganese (NCM)-based active material), a butyrate-based solvent, a sulfide-based solid electrolyte, and a rubber-based binder through a slurry coating process. Here, the mixed density of the second electrode active material is 0.1 to 2.0 g / cc. In addition, a solid electrolyte layer is formed on the second electrode active material layer using a slurry comprising a sulfide-based solid electrolyte and a rubber-based binder through a slurry coating process, thereby preparing a second unit.
[0123] (Operation S40): The first unit and the second unit are stacked. In more detail, the first unit and the second unit are stacked so that the second unit is placed on the center portion of the first electrode active material layer of the first unit, and thus the first electrode active material layer and the solid electrolyte layer are in contact with each other, and the insulating member is accommodated in the space between the edge portion of the first electrode active material layer and the side of the second unit.
[0124] (Operation S50): The same first electrode current collector as that used in operation S10 is used. In addition, a first electrode active material layer is formed on one surface of the first electrode current collector by the same process using the same slurry as that used in operation S10, thereby preparing a third unit. The third unit is stacked on the outermost layer of the structure obtained by operation S40, thereby manufacturing a battery structure.
[0125] (Operation S60 ): The battery structure is pressed so that the thickness of the first electrode active material layer and the second electrode active material layer is 50 to 300 μm.
[0126] Test Example 1 – Setting the Suppression Range
[0127] In order to manufacture the all-solid-state battery according to the above example, an improved pressing range was tested. Figures 7A to 7D The test results are shown.
[0128] Fig. 7A and Figure 7B is a diagram showing observation results of a middle (10th) interface and a lowest interface of a battery structure manufactured by alternately stacking a first unit and a second unit 20 times according to the above example after the battery structure was pressed at 200 MPa. Figure 7C and Fig.7D is a diagram showing the observation results of the middle (10th) interface and the lowermost interface of the battery structure manufactured by alternately stacking the first unit and the second unit 20 times according to the above example after the battery structure was pressed at 300 MPa.
[0129] Reference Fig. 7A and Figure 7B , it can be confirmed that in the all-solid-state battery manufactured by pressing the battery structure according to the above example at 200 MPa, interface defects occurred and only 76% of the actual battery performance was exhibited. On the other hand, reference Figure 7C and Fig.7D , it can be confirmed that in the all-solid-state battery made by pressing the battery structure according to the above example at 300 MPa, no interface defects occurred and 99% of the actual battery performance was exhibited.
[0130] From this, it can be understood that in order to manufacture an all-solid-state battery that can operate normally according to the example, a pressure of 300 MPa or more may be applied to a battery structure prepared by alternately stacking the first unit and the second unit 20 times.
[0131] It is obvious from the above description that compared with the conventional process of separately pressing battery cells corresponding to basic units and then stacking them, the present disclosure provides a process for manufacturing an all-solid-state battery, wherein a battery structure is prepared by stacking two or more units and then pressing them, thereby simplifying the process.
[0132] In addition, compared to a conventional battery structure in which two or more battery cells are stacked (each including a current collector, an electrode and a solid electrolyte layer), the present disclosure provides an all-solid-state battery formed by stacking cells and forming electrodes on both surfaces of the current collector, thereby reducing the number of consumed current collectors and the all-solid-state battery can have a high energy density.
[0133] Furthermore, the battery structure according to the present disclosure includes an insulating member, and thus it is possible to prevent or suppress a short circuit from occurring at an edge portion of the all-solid-state battery.
[0134] Furthermore, since the all-solid-state battery according to the present disclosure uses an insulating member formed of a transparent material, light from a visual device can penetrate the insulating member, so alignment of the battery structure can be achieved and the battery structure can be stabilized.
[0135] The present disclosure has been described in detail with reference to aspects of the present disclosure. However, it will be appreciated by those skilled in the art that changes may be made in these forms without departing from the principles and spirit of the present disclosure, the scope of which is defined by the appended claims and their equivalents.
[0136] While the present disclosure has been described in connection with what are presently considered to be practical exemplary forms, it should be understood that the disclosure is not limited to the forms disclosed, but on the contrary is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the present disclosure.
Claims
1. An all-solid-state battery, include: A plurality of first units, each of the plurality of first units comprising: a first electrode current collector, and a first electrode active material layer formed on both surfaces of the first electrode current collector; A plurality of second units, each of the plurality of second units comprising: the second electrode current collector, a second electrode active material layer formed on both surfaces of the second electrode current collector, and a solid electrolyte layer formed on the second electrode active material layer; wherein the plurality of first units and the plurality of second units are stacked alternately; wherein the first electrode active material layer and the second electrode active material layer abut on both surfaces of the solid electrolyte layer, respectively, and wherein an insulating member is accommodated in a space between an edge portion of the first electrode active material layer and a side surface of the second cell; wherein an area of at least one of the plurality of first units is greater than an area of at least one of the plurality of second units, and an area of a central portion of the first electrode active material layer is greater than or equal to an area of at least one of the plurality of second units; wherein the edge portion is an edge portion of a surface of the first electrode active material layer that is perpendicular to a stacking direction in which the plurality of first units and the plurality of second units are alternately stacked, and the side surface is a side surface of the second unit that is parallel to the stacking direction; wherein at least one of the plurality of first units is configured such that one first electrode current collector is interposed between a pair of first electrode active material layers; At least one of the plurality of second units is configured such that one second electrode current collector is interposed between a pair of second electrode active material layers.
2. The all-solid-state battery according to claim 1, further comprising: include: a plurality of third units, each of the plurality of third units comprising a third electrode current collector and a third electrode active material layer formed on one surface of the third electrode current collector, Wherein, each of the third units is located at the outermost position of the all-solid-state battery.
3. The all-solid-state battery according to claim 1, in, At least one of the plurality of second units is placed on a central portion of the first electrode active material layer so that the first electrode active material layer and the solid electrolyte layer are stacked in contact with each other.
4. The all-solid-state battery according to claim 1, in, A sum of thicknesses of the insulating member and another insulating member adjacent thereto is the same as a thickness of at least one of the plurality of second units.
5. The all-solid-state battery according to claim 1, in, The insulating member surrounds a side surface of at least one of the plurality of second units.
6. The all-solid-state battery according to claim 1, in, The insulating member is formed of a transparent material.
7. The all-solid-state battery according to claim 1, in, The first electrode current collector has a thickness of 4 to 20 μm.
8. The all-solid-state battery according to claim 1, in, The second electrode current collector has a thickness of 5 to 20 μm.
9. The all-solid-state battery according to claim 1, in, The first electrode active material layer has a thickness of 50 to 300 μm, a mixed density of 1.2 to 3.5 g / cc, and a 2 and lightness values from 30 to 80 in the CIELAB color space.
10. The all-solid-state battery according to claim 1, in, The second electrode active material layer has a thickness of 50 to 300 μm, a mixed density of 2.5 to 5.0 g / cc, and a 2 and lightness values from 40 to 90 in the CIELAB color space.
11. A method for manufacturing an all-solid-state battery, the method include: preparing at least one first unit, each of the first units comprising a first electrode current collector and a first electrode active material layer formed on both surfaces of the first electrode current collector; preparing at least one second unit, each of the second units including a second electrode current collector, a second electrode active material layer formed on both surfaces of the second electrode current collector, and a solid electrolyte layer formed on the second electrode active material layer; forming an insulating member in a space between an edge portion of the first electrode active material layer and a side surface of the second cell; Obtaining a battery structure by alternately stacking the first unit and the second unit; as well as pressing the battery structure; wherein the area of the first unit is greater than the area of the second unit, and the area of the central portion of the first electrode active material layer is greater than or equal to the area of the second unit; wherein the edge portion is an edge portion of a surface of the first electrode active material layer that is perpendicular to a stacking direction in which the first units and the second units are alternately stacked, and the side surface is a side surface of the second unit that is parallel to the stacking direction; wherein the at least one first unit is configured such that one first electrode current collector is inserted between a pair of first electrode active material layers; The at least one second unit is configured such that one second electrode current collector is interposed between a pair of second electrode active material layers.
12. The method according to claim 11, further comprising: include: Before pressing the battery structure, third units are stacked on the outermost layer of the battery structure, each of the third units including a third electrode current collector and a third electrode active material layer formed on one surface of the third electrode current collector.
13. The method according to claim 11, in, The battery structure is configured such that the second cell is placed on a central portion of the first electrode active material layer, and thus the first electrode active material layer and the solid electrolyte layer are stacked in contact with each other.
14. The method according to claim 11, in, A sum of thicknesses of the insulating member and another insulating member adjacent thereto is the same as a thickness of the second unit.
15. The method according to claim 11, in, The insulating member is stacked to surround a side surface of the second unit.
16. The method according to claim 11, in, The insulating member is formed of a transparent material.
17. The method according to claim 11, in, In preparing the first unit and preparing the second unit, the first unit and the second unit are not pressed.
18. The method according to claim 11, in, The battery structure is pressed at a pressure of 250 MPa to 500 MPa.