Positive electrode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

By adding sulfate ions to lithium transition metal oxides and optimizing their structures, the problems of charge-discharge cycle characteristics and charge transfer resistance in lithium transition metal oxides with high Ni ratios are solved, maintaining battery capacity and improving performance.

CN112005410BActive Publication Date: 2024-10-18PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201980022879.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-02-26
Publication Date
2024-10-18
Estimated Expiration
2039-02-26

AI Technical Summary

Technical Problem

When a lithium transition metal oxide with a Ni ratio of 91 mol% or more relative to the total moles of metal elements other than Li is used as the positive electrode active material, the charge-discharge cycle characteristics and charge transfer of the non-aqueous electrolyte secondary battery are reduced. The resistance increases, causing the battery capacity to decrease.

Method used

A lithium transition metal oxide containing Ni and Al is used as the positive electrode active material, and more than 0.02 mol% of sulfate ions are added to it to control the half-value width of the diffraction peak of the (208) plane of the X-ray diffraction pattern at 0.30°≤n ≤0.50° to optimize the arrangement of the lithium layer and the transition metal layer, improve ionic conductivity, and suppress charge transfer resistance and capacity reduction.

Benefits of technology

It effectively suppresses the decrease in charge and discharge cycle characteristics, reduces the increase in charge transfer resistance and the decrease in battery capacity, and improves the charge and discharge performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004946697120000171
    Figure GDA0004946697120000171
Patent Text Reader

Abstract

The positive electrode active material for a non-aqueous electrolyte secondary battery of the present embodiment is characterized in that it has a lithium transition metal oxide containing Ni and Al, the ratio of Ni in the aforementioned lithium transition metal oxide is greater than 91 mol% relative to the total molar number of metal elements other than Li, the aforementioned lithium transition metal oxide contains greater than 0.02 mol% of sulfate ions, and for the aforementioned lithium transition metal oxide, the half-value width n of the diffraction peak of the (208) plane of the X-ray diffraction pattern based on X-ray diffraction is 0.30°≤n≤0.50°.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material for a non-aqueous electrolyte secondary battery and a technology of a non-aqueous electrolyte secondary battery. Background Art

[0002] In recent years, as a secondary battery with high power and high energy density, a non-aqueous electrolyte secondary battery has been widely used, which includes a positive electrode, a negative electrode, and a non-aqueous electrolyte, and allows lithium ions or the like to move between the positive electrode and the negative electrode to perform charge and discharge.

[0003] As a positive electrode active material used in the positive electrode of a non-aqueous electrolyte secondary battery, for example, the following materials are known.

[0004] For example, Patent Document 1 discloses a positive electrode active material containing a lithium transition metal oxide represented by the general formula NiM(OH)2 (where M represents at least one element selected from transition metals other than Ni, alkaline earth metal elements, Al, Ga, In, and Si), and being monodisperse primary particles.

[0005] In addition, for example, Patent Document 2 discloses a positive electrode active material containing a lithium transition metal oxide represented by the general formula Li (1+δ) Mn x Ni y Co (1-x-y) O2, and δ, x, and y respectively satisfy the relationships of -0.15 < δ < 0.15, 0.1 < x ≤ 0.5, and 0.5 < x + y ≤ 1.0.

[0006] Prior Art Documents

[0007] Patent Documents

[0008] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2010-70431

[0009] Patent Document 2: Japanese Unexamined Patent Application Publication No. 2006-202702 Summary of the Invention

[0010] Problem that the invention aims to solve

[0011] However, if a lithium transition metal oxide in which the ratio of Ni is 91 mol% or more with respect to the total number of moles of metal elements other than Li is used as the positive electrode active material, high capacity of the non-aqueous electrolyte secondary battery can be achieved. On the contrary, there is a problem of deterioration of charge and discharge cycle characteristics. In addition, for the purpose of improving charge and discharge cycle characteristics, addition of metal elements other than Ni has been considered. However, merely by adding other metal elements, the charge transfer resistance during charge and discharge sometimes increases, and further the battery capacity sometimes decreases.

[0012] Therefore, the purpose of the present disclosure is to provide: when using a lithium transition metal oxide in which the ratio of Ni is 91 mol% or more relative to the total molar number of metal elements other than Li, a positive electrode active material for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery can suppress the reduction of charge and discharge cycle characteristics, and can suppress the increase of charge transfer resistance during charge and discharge and the reduction of battery capacity.

[0013] Solutions for solving problems

[0014] As one embodiment of the present invention, a positive electrode active material for a non-aqueous electrolyte secondary battery is characterized in that it has a lithium transition metal oxide containing Ni and Al, the ratio of Ni in the aforementioned lithium transition metal oxide is greater than 91 mol% relative to the total molar number of metal elements other than Li, the aforementioned lithium transition metal oxide contains greater than 0.02 mol% of sulfate ions, and for the aforementioned lithium transition metal oxide, the half-value width n of the diffraction peak of the (208) plane of the X-ray diffraction pattern based on X-ray diffraction is 0.30°≤n≤0.50°.

[0015] A nonaqueous electrolyte secondary battery as one embodiment of the present disclosure is characterized by including a positive electrode having the above-mentioned positive electrode active material for a nonaqueous electrolyte secondary battery.

[0016] Effects of the Invention

[0017] According to one embodiment of the present disclosure, it is possible to suppress a decrease in charge-discharge cycle characteristics, and to suppress an increase in charge transfer resistance and a decrease in battery capacity during charge and discharge. DETAILED DESCRIPTION

[0018] The positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present disclosure is characterized in that it has a lithium transition metal oxide containing Ni and Al, the ratio of Ni in the lithium transition metal oxide is 91 mol% or more relative to the total molar number of metal elements other than Li, the lithium transition metal oxide contains 0.02 mol% or more of sulfate ions, and the half-value width n of the diffraction peak of the (208) plane of the X-ray diffraction pattern based on X-ray diffraction of the lithium transition metal oxide is 0.30°≤n≤0.50°. The reason why the reduction in charge and discharge cycle characteristics, the increase in charge transfer resistance during charge and discharge, and the reduction in battery capacity are suppressed when using the positive electrode active material for a non-aqueous electrolyte secondary battery has not been fully clarified, but it is presumed as follows.

[0019] The lithium transition metal oxide containing Ni and Al is, for example, a layered structure having a transition metal layer, a Li layer, and an oxygen layer of Ni and Al, and the Li ions present in the Li layer are reversibly embedded / de-embedded, so that the charge and discharge reaction of the battery proceeds. Here, the half-value width of the diffraction peak of the (208) plane of the X-ray diffraction pattern based on X-ray diffraction is an index representing the fluctuation of the arrangement between the Li layer and the transition metal layer. When the value is within the above-specified range, a moderate fluctuation occurs in the arrangement between the Li layer and the transition metal layer, and the constraint of the Li ions of the Li layer is relaxed to a certain extent. Therefore, it is believed that during the charge and discharge reaction, the embedding / de-embedding of the Li ions of the Li layer becomes smooth, and the reduction of the charge and discharge cycle characteristics is suppressed. In addition, by including the above-specified amount of sulfate ions in the lithium transition metal oxide, the surface of the lithium transition metal oxide is modified, and the ion conductivity is specifically increased, so it is believed that the increase in charge transfer resistance can be suppressed, and the reduction in battery capacity can be suppressed.

[0020] An example of a nonaqueous electrolyte secondary battery using the positive electrode active material for a nonaqueous electrolyte secondary battery as one embodiment of the present disclosure will be described below.

[0021] As an example of an embodiment, a non-aqueous electrolyte secondary battery comprises: a positive electrode, a negative electrode and a non-aqueous electrolyte. It is suitable to provide a separator between the positive electrode and the negative electrode. Specifically, it has a structure in which a wound electrode body in which the positive electrode and the negative electrode are wound with a separator, and the non-aqueous electrolyte is accommodated in an outer shell. The electrode body is not limited to a wound electrode body, and other forms of electrode bodies such as a stacked electrode body in which the positive electrode and the negative electrode are stacked with a separator can also be applied. In addition, the form of the non-aqueous electrolyte secondary battery is not particularly limited, and examples thereof include cylindrical, square, coin-shaped, button-shaped, laminated, etc.

[0022] Hereinafter, the positive electrode, the negative electrode, the nonaqueous electrolyte, and the separator used in the nonaqueous electrolyte secondary battery as an example of the embodiment will be described in detail.

[0023] <Positive electrode>

[0024] The positive electrode is composed of, for example, a positive electrode current collector such as a metal foil, and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, or a thin film having the metal on the surface. The positive electrode active material layer may include, for example, a positive electrode active material, a binding material, a conductive material, and the like.

[0025] The positive electrode can be obtained, for example, by applying a positive electrode composite material slurry containing a positive electrode active material, a binder, a conductive material, etc. on a positive electrode collector and drying it to form a positive electrode active material layer on the positive electrode collector, and rolling the positive electrode active material layer.

[0026] The positive electrode active material contains a lithium transition metal oxide containing Ni and Al. The ratio of Ni in the lithium transition metal oxide is 91 mol% or more, preferably in the range of 91 mol% to 99 mol%, more preferably in the range of 91 mol% to 96 mol%, relative to the total number of moles of metal elements other than lithium. It should be noted that if the ratio of Ni is less than 91 mol%, it is difficult to achieve the original high capacity of the battery.

[0027] Al in the lithium transition metal oxide containing Ni and Al can be, for example, uniformly dispersed within the crystal structure of the lithium transition metal oxide containing Ni, or can exist in a part of the crystal structure. In addition, during the manufacturing stage of the lithium transition metal oxide, a part of Al contained within the crystal structure sometimes precipitates on the surface of the particles of the lithium transition metal oxide, but the precipitated Al is also the Al contained in the lithium transition metal oxide.

[0028] The lithium transition metal oxide containing Ni and Al can contain elements other than Al, and is represented by the following general formula, for example.

[0029] Li x Ni a Co b Al c M d O2(1)

[0030] In the above formula, a representing the ratio of Ni only needs to be a≥0.91, preferably 0.91≤a≤0.99, more preferably 0.91≤a≤0.96. In the above formula, in terms of suppressing the reduction of charge-discharge cycle characteristics, etc., b representing the ratio of Co is preferably b<0.06, more preferably 0.005≤b≤0.045. In the above formula, in terms of suppressing the reduction of charge-discharge cycle characteristics, etc., c representing the ratio of Al is preferably 0.03<c, more preferably 0.04≤c≤0.06.

[0031] M in the above formula is not particularly limited as long as it is an element other than Li, Ni, Al, and Co. For example, at least one element selected from Ti, Nb, Mn, Si, Mo, Zr, V, Fe, Mg, Cr, Cu, Sn, Ta, W, Na, K, Ba, Sr, Bi, Be, Zn, Ca, and B can be cited. Among them, in terms of suppressing the reduction of charge-discharge cycle characteristics, etc., M in the above formula is preferably at least one element selected from Ti, Nb, Mn, Si, and Mo. In the above formula, d representing the ratio of M is preferably 0≤d≤0.03, more preferably 0.005≤d≤0.025.

[0032] In the above formula, from the viewpoint of improvement of battery capacity and the like, x representing the ratio of Li preferably satisfies 0.95≤x≤1.10, and more preferably satisfies 0.97≤x≤1.03.

[0033] The lithium transition metal oxide containing Ni and Al contains sulfate ions. The sulfate ions include any form such as being attached to the particle surface of the lithium transition metal oxide in the form of a SO4 compound, being embedded in the secondary particles of the lithium transition metal oxide in the form of a SO4 compound, and being contained in the crystal structure of the lithium transition metal oxide containing Ni and Al.

[0034] Examples of SO4 compounds attached to the particle surface or embedded in secondary particles include Al2(SO4)3, Ti(SO4)2, MnSO4, Nb2(SO4)3, Si(SO4)2, Mo(SO4)3, Fe2(SO4)3, BaSO4, CaSO4, CuSO4, MgSO4, SrSO4, and ZnSO4.

[0035] In order to suppress the reduction of charge transfer resistance and battery capacity during charge and discharge, the sulfate ion content contained in the lithium transition metal oxide containing Ni and Al can be 0.02 mol% or more, preferably in the range of 0.02 mol% to 0.12 mol%, and more preferably in the range of 0.03 mol% to 0.1 mol%. Here, the sulfate ion content is measured as follows.

[0036] In pure water 50mL, add the lithium transition metal oxide 1g containing Ni and Al, obtain sample solution, the sample solution obtained is vibrated at room temperature for 24 hours.The sample solution after filtering and stirring, collects filtrate.The sulfate ion amount in the filtrate collected is measured by ion chromatography.In addition, the content of the element constituting the lithium transition metal oxide containing Ni and Al can be measured using inductively coupled plasma emission spectrometry analysis device (ICP-AES), electron probe microanalyzer (EPMA), energy dispersive X-ray analysis device (EDX) etc.

[0037] In the lithium transition metal oxide containing Ni and Al, in terms of suppressing the reduction of charge and discharge cycle characteristics, the half-value width n of the diffraction peak of the (208) plane of the X-ray diffraction pattern based on X-ray diffraction can be 0.30°≤n≤0.50°, preferably 0.30°≤n≤0.45°. When the half-value width n of the diffraction peak of the (208) plane is less than 0.30°, the Li ions of the Li layer are strongly constrained compared to the case where the above range is satisfied, and the charge and discharge cycle characteristics are reduced. In addition, when the half-value width n of the diffraction peak of the (208) plane exceeds 0.50°, the crystallinity of the Ni-containing Li transition metal oxide is reduced, the skeleton of the crystal structure becomes brittle, and the charge and discharge cycle characteristics are reduced compared to the case where the above range is satisfied.

[0038] The X-ray diffraction pattern was obtained by powder X-ray diffraction under the following conditions using a powder X-ray diffractometer (manufactured by Rigaku Corporation, trade name "RINT-TTR", radiation source Cu-Kα).

[0039] Measuring range: 15-120°

[0040] Scanning speed: 4° / min

[0041] Resolution range: 30-120°

[0042] Background; B-spline

[0043] Contour function; pseudo-Voigt function

[0044] Constraints: Li(3a)+Ni(3a)=1

[0045] Ni(3a)+Ni(3b)=y

[0046] ICSD No.; 98-009-4814

[0047] For example, in order to effectively suppress the reduction of charge and discharge cycle characteristics, the reduction of charge transfer resistance during charge and discharge, or the reduction of battery capacity, the content of the lithium transition metal oxide containing Ni and Al is preferably 90 mass % or more, preferably 99 mass % or more, relative to the total mass of the positive electrode active material for the non-aqueous electrolyte secondary battery.

[0048] In addition, the positive electrode active material for the non-aqueous electrolyte secondary battery of the present embodiment may contain other lithium transition metal oxides in addition to the lithium transition metal oxide containing Ni and Al. As other lithium transition metal oxides, for example, lithium transition metal oxides having a Ni content of 0 mol % to less than 91 mol % may be cited.

[0049] An example of a method for producing a lithium transition metal oxide containing Ni and Al will be described.

[0050] The method for producing a Ni-containing lithium transition metal oxide includes, for example, the following steps: a first step of mixing a Ni-containing compound, a Li compound, a SO 4 compound containing a metal element, and a non-SO 4 compound containing a metal element; and a second step of calcining the mixture.

[0051] The Ni-containing compound used in the first step may be a composite compound containing other elements such as Al and Co in addition to Ni, and examples thereof include oxides containing Ni, etc. The Li compound used in the first step is, for example, lithium carbonate, lithium hydroxide, etc.

[0052] The metal element-containing SO4 compound used in the first step is a SO4 compound containing metal elements such as Al, Ti, Nb, Mn, Si, Mo, Fe, Ba, Ca, Cu, Mg, Sr, and Zn, for example, Al2(SO4)3, Ti(SO4)2, MnSO4, Nb2(SO4)3, Si(SO4)2, Mo(SO4)3, Fe2(SO4)3, BaSO4, CaSO4, CuSO4, MgSO4, SrSO4, and ZnSO4.

[0053] The non-SO4 compound containing metal elements used in the first step is a compound containing the same element or a different element from the metal element contained in the above-mentioned SO4 compound, for example, hydroxides or oxides containing metal elements such as Al, Ti, Nb, Mn, Si, Mo, Fe, Ba, Ca, Cu, Mg, Sr, and Zn.

[0054] By adding both a metal element-containing SO4 compound and a metal element-containing non-SO4 compound, it is easy to control the half-value width n of the diffraction peak of the (208) plane in the final lithium transition metal oxide containing Ni and Al within the above-specified range. It should be noted that if only the amount of sulfate ions contained in the lithium transition metal oxide containing Ni and Al is controlled within the above-specified range, the Ni-containing compound, the Li compound, and the metal element-containing SO4 compound can be mixed and the mixture can be calcined. However, in the above case, it is difficult to control the half-value width n of the diffraction peak of the (208) plane in the final lithium transition metal oxide containing Ni and Al within the above-specified range.

[0055] The mixing ratio of the metal element-containing SO4 compound and the metal element-containing non-SO4 compound is preferably in the range of 1:9 to 7:3. If the ratio of the metal element-containing SO4 compound is reduced, the amount of sulfate ions contained in the final lithium transition metal oxide containing Ni and Al may not be controlled within the above-specified range. If the ratio of the metal element-containing SO4 compound is increased, the amount of Li present in the crystal structure of the final lithium transition metal oxide containing Ni and Al may decrease, which may sometimes cause a decrease in battery capacity.

[0056] In the second step, the mixture obtained in the first step is calcined at a predetermined temperature and time to obtain the lithium transition metal oxide containing Ni and Al of the present embodiment. The calcination of the mixture in the second step is preferably in the range of 500° C. to 900° C., for example. The calcination time is preferably 6 to 24 hours, for example. The calcination of the mixture obtained in the second step is preferably carried out in an oxygen flow.

[0057] Hereinafter, other materials contained in the positive electrode active material layer will be described.

[0058] Examples of the conductive material contained in the positive electrode active material layer include carbon black, acetylene black, Ketjen black, and carbon powders such as graphite. These may be used alone or in combination of two or more.

[0059] As the binding material contained in the positive electrode active material layer, for example, fluorine-based polymers, rubber-based polymers, etc. can be cited. As fluorine-based polymers, for example, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF) or their modified products, etc. can be cited, and as rubber-based polymers, for example, ethylene-propylene-isoprene copolymers, ethylene-propylene-butadiene copolymers, etc. can be cited. They can be used alone or in combination of two or more.

[0060] <Negative electrode>

[0061] The negative electrode includes, for example, a negative electrode current collector such as a metal foil, and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode current collector may include a foil of a metal such as copper that is stable within the potential range of the negative electrode, a thin film having the metal disposed on the surface, and the like. The negative electrode active material layer includes, for example, a negative electrode active material, a binder, a thickening material, and the like.

[0062] The negative electrode can be obtained, for example, by applying a negative electrode composite material slurry containing a negative electrode active material, a thickening material, and a binding material on a negative electrode current collector and drying the slurry to form a negative electrode active material layer on the negative electrode current collector, and rolling the negative electrode active material layer.

[0063] The negative electrode active material contained in the negative electrode active material layer is not particularly limited as long as it is a material that can absorb / release lithium ions. For example, carbon materials, metals that can form alloys with lithium, or alloy compounds containing the metals can be cited. As carbon materials, graphites such as natural graphite, difficult-graphitizing carbon, and artificial graphite, cokes, etc. can be used. As alloy compounds, substances containing at least one metal that can form alloys with lithium can be cited. As elements that can form alloys with lithium, silicon and tin are preferred. Silicon oxide, tin oxide, etc. formed by bonding them with oxygen can also be used. In addition, a mixture of the above-mentioned carbon materials with silicon and tin compounds can be used. In addition to the above, lithium titanate and the like whose potential for charging and discharging metallic lithium is higher than that of carbon materials can also be used.

[0064] As the binding material contained in the negative electrode active material layer, for example, fluorine-based polymers, rubber-based polymers, etc. can also be used in the same manner as in the case of the positive electrode, and styrene-butadiene copolymers (SBR) or their modified products can also be used. As the binding material contained in the negative electrode active material layer, fluorine-based resins, PAN, polyimide-based resins, acrylic resins, polyolefin-based resins, etc. can be used in the same manner as in the case of the positive electrode. When preparing the negative electrode composite material slurry with an aqueous solvent, it is preferred to use styrene-butadiene rubber (SBR), CMC or its salt, polyacrylic acid (PAA) or its salt (PAA-Na, PAA-K, etc., and salts that can be partially neutralized), polyvinyl alcohol (PVA), etc.

[0065] Examples of the thickener contained in the negative electrode active material layer include carboxymethyl cellulose (CMC), polyethylene oxide (PEO), etc. These may be used alone or in combination of two or more.

[0066] <Non-aqueous electrolytes>

[0067] The non-aqueous electrolyte includes: a non-aqueous solvent, and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous electrolyte is not limited to a liquid electrolyte (non-aqueous electrolyte solution), and can also be a solid electrolyte using a gel polymer or the like. Examples of non-aqueous solvents that can be used include esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen substituted product obtained by replacing at least a portion of the hydrogen of these solvents with a halogen atom such as fluorine.

[0068] Examples of the above esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, cyclic carboxylic acid esters such as γ-butyrolactone (GBL), γ-valerolactone (GVL), and chain carboxylic acid esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), ethyl propionate, etc.

[0069] Examples of the above ethers include cyclic ethers such as 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-epoxybutane, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, crown ethers, and chain ethers such as 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, etc.

[0070] As the above halogenated compounds, fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, fluorinated chain carboxylic acid esters such as fluoromethyl propionate (FMP), etc. are preferably used.

[0071] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylates, borate salts such as Li2B4O7, Li(B(C2O4)F2), LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1SO2) {l, m is an integer greater than 0} and other imide salts. The lithium salts may be used alone or in combination. Among them, LiPF6 is preferably used from the viewpoint of ion conductivity, electrochemical stability, etc. The concentration of the lithium salt is preferably 0.8 to 1.8 mol per 1 L of the non-aqueous solvent.

[0072] <Separator>

[0073] For example, a porous sheet having ion permeability and insulation can be used as the separator. Specific examples of the porous sheet include microporous films, woven fabrics, non-woven fabrics, etc. As the material of the separator, olefin resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator can be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin, and the surface of the separator can be coated with an aromatic polyamide resin, etc. A filler layer containing an inorganic filler can be formed at the interface between the separator and at least one of the positive electrode and the negative electrode. As an inorganic filler, for example, an oxide containing at least one of titanium (Ti), aluminum (Al), silicon (Si), and magnesium (Mg), a phosphate compound, or a surface thereof treated with a hydroxide, etc. can be cited. The filler layer can be formed, for example, by applying a slurry containing the filler to the surface of the positive electrode, the negative electrode, or the separator.

[0074] Example

[0075] Hereinafter, the present invention will be further described based on examples, but the present invention is not limited to these examples.

[0076] <Example 1>

[0077] [Preparation of positive electrode active material]

[0078] The composite oxide (Ni 0.92 Co 0.03 Al 0.05O2), LiOH, and a mixture of Ti(SO4)2 and Ti(OH)4 in a molar ratio of 3:7 are mixed so that the molar ratio becomes 100:101:1. The mixture is calcined at 700°C for 20 hours in an oxygen flow to obtain a lithium transition metal oxide. The amount of sulfate ions in the obtained lithium transition metal oxide is measured, and the result is 0.03 mol%. In addition, the ratios of Ni, Co, Al and Ti relative to the total molar number of Ni, Co, Al and Ti in the obtained lithium transition metal oxide are measured, and the results show that the ratio of Ni is 91 mol%, the ratio of Co is 3 mol%, the ratio of Al is 5 mol%, and the ratio of Ti is 1 mol%. In addition, the half-value width n of the diffraction peak of the (208) plane in the obtained lithium transition metal oxide is 0.44°. The determination method is as described above. The lithium transition metal oxide is used as the positive electrode active material of Example 1.

[0079] <Example 2>

[0080] A lithium transition metal oxide was prepared in the same manner as in Example 1 except that a mixture of Ti(SO4)2 and Ti(OH)4 was mixed at a molar ratio of 7:3. The amount of sulfate ions in the lithium transition metal oxide was 0.06 mol%, the ratio of Ni was 91 mol%, the ratio of Co was 3 mol%, the ratio of Al was 5 mol%, the ratio of Ti was 1 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.45°. The lithium transition metal oxide was used as the positive electrode active material of Example 2.

[0081] <Example 3>

[0082] The composite oxide (Ni 0.92 Co 0.03 Al 0.05 O2), LiOH, and a mixture of Al2(SO4)3 and Ti(OH)4 in a molar ratio of 3:7 were mixed so that the molar ratio was 100:101:1, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The amount of sulfate ions in the lithium transition metal oxide was 0.04 mol%, the ratio of Ni was 91 mol%, the ratio of Co was 3 mol%, the ratio of Al was 5.3 mol%, the ratio of Ti was 0.7 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.41°. The lithium transition metal oxide was used as the positive electrode active material of Example 3.

[0083] <Example 4>

[0084] A lithium transition metal oxide was prepared in the same manner as in Example 3 except that a mixture of Al2(SO4)3 and Ti(OH)4 was mixed at a molar ratio of 7:3. The amount of sulfate ions in the lithium transition metal oxide was 0.12 mol%, the ratio of Ni was 91 mol%, the ratio of Co was 3 mol%, the ratio of Al was 5.7 mol%, the ratio of Ti was 0.3 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.39°. The lithium transition metal oxide was used as the positive electrode active material of Example 4.

[0085] <Example 5>

[0086] The composite oxide (Ni 0.94 Co 0.015 Al 0.045 O2), LiOH, and a mixture of MnSO4 and Al(OH)3 in a molar ratio of 3:7 were mixed so that the molar ratio was 100:101:1.5, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The lithium transition metal oxide contained 0.03 mol% of sulfate ions, 92.5 mol% of Ni, 1.5 mol% of Co, 5 mol% of Al, 1 mol% of Mn, and a half-value width n of the diffraction peak of the (208) plane of 0.33°. The lithium transition metal oxide was used as the positive electrode active material of Example 5.

[0087] <Example 6>

[0088] A lithium transition metal oxide was prepared in the same manner as in Example 5 except that a mixture of MnSO4 and Al(OH)3 was mixed at a molar ratio of 7:3. The lithium transition metal oxide contained 0.07 mol% sulfate ions, 92.5 mol% Ni, 1.5 mol% Co, 5.5 mol% Al, 0.5 mol% Mn, and a half-value width n of the diffraction peak of the (208) plane of 0.37°. The lithium transition metal oxide was used as the positive electrode active material of Example 6.

[0089] <Example 7>

[0090] The composite oxide (Ni 0.94 Co 0.015 Al 0.045O2), LiOH, and a mixture of Al2(SO4)3 and LiNbO3 in a molar ratio of 3:7 were mixed so that the molar ratio was 100:101:1.5, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The lithium transition metal oxide contained 0.04 mol% of sulfate ions, 92.5 mol% of Ni, 1.5 mol% of Co, 5 mol% of Al, 1 mol% of Nb, and a half-value width n of the diffraction peak of the (208) plane of 0.37°. The lithium transition metal oxide was used as the positive electrode active material of Example 7.

[0091] <Example 8>

[0092] A lithium transition metal oxide was prepared in the same manner as in Example 7 except that a mixture of Al2(SO4)3 and LiNbO3 was mixed at a molar ratio of 7:3. The lithium transition metal oxide contained 0.12 mol% sulfate ions, 92.5 mol% Ni, 1.5 mol% Co, 5.5 mol% Al, 0.5 mol% Nb, and a half-value width n of the diffraction peak of the (208) plane of 0.41°. The lithium transition metal oxide was used as the positive electrode active material of Example 8.

[0093] <Example 9>

[0094] The composite oxide (Ni 0.945 Co 0.005 Al 0.050 O2), LiOH, and a mixture of Al2(SO4)3 and SiO2 in a molar ratio of 7:3 were mixed so that the molar ratio was 100:101:1, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The lithium transition metal oxide contained 0.05 mol% of sulfate ions, 93.5 mol% of Ni, 0.5 mol% of Co, 5.7 mol% of Al, 0.3 mol% of Si, and a half-value width n of the diffraction peak of the (208) plane of 0.34°. The lithium transition metal oxide was used as the positive electrode active material of Example 9.

[0095] <Example 10>

[0096] The composite oxide (Ni 0.955 Co 0.005 Al 0.04O2), LiOH, and a mixture of Al2(SO4)3 and Ti(OH)4 in a molar ratio of 1:9 were mixed so that the molar ratio was 100:101:3.5, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The amount of sulfate ions in the lithium transition metal oxide was 0.03 mol%, the ratio of Ni was 92 mol%, the ratio of Co was 0.5 mol%, the ratio of Al was 4.5 mol%, the ratio of Ti was 3 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.39°. The lithium transition metal oxide was used as the positive electrode active material of Example 10.

[0097] <Example 11>

[0098] Composite oxide containing Ni, Co and Al (Ni 0.94 Co 0.015 Al 0.045 O2), LiOH, and a mixture of Ti(SO4)2 and LiNbO3 in a molar ratio of 7:3 were mixed so that the molar ratio was 100:101:1.5, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The lithium transition metal oxide contained 0.05 mol% of sulfate ions, 93 mol% of Ni, 1.3 mol% of Co, 4.2 mol% of Al, 1 mol% of Ti, 0.5 mol% of Nb, and a half-value width n of the diffraction peak of the (208) plane of 0.34°. The lithium transition metal oxide was used as the positive electrode active material of Example 11.

[0099] <Example 12>

[0100] The composite oxide (Ni 0.94 Co 0.015 Al 0.045 O2), LiOH, and a mixture of Ti(SO4)2 and LiNbO3 in a molar ratio of 5:5 were mixed so that the molar ratio was 100:101:1, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The lithium transition metal oxide contained 0.04 mol% of sulfate ions, 93 mol% of Ni, 1.5 mol% of Co, 4.5 mol% of Al, 0.5 mol% of Ti, 0.5 mol% of Nb, and a half-value width n of the diffraction peak of the (208) plane of 0.37°. The lithium transition metal oxide was used as the positive electrode active material of Example 12.

[0101] <Example 13>

[0102] The composite oxide (Ni 0.955 Al0.045 O2), LiOH, and a mixture of Al2(SO4)3 and Li2MoO4 in a molar ratio of 2:8 were mixed so that the molar ratio was 100:101:0.6, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The amount of sulfate ions in the lithium transition metal oxide was 0.03 mol%, the ratio of Ni was 95 mol%, the ratio of Al was 4.5 mol%, the ratio of Mo was 0.5 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.34°. The lithium transition metal oxide was used as the positive electrode active material of Example 13.

[0103] <Example 14>

[0104] The composite oxide (Ni 0.94 Co 0.015 Al 0.045 O2), LiOH, and a mixture of Ti(SO4)2 and Li2MoO4 in a molar ratio of 5:5 were mixed so that the molar ratio was 100:101:1, and a lithium transition metal oxide was prepared in the same manner as in Example 1. The lithium transition metal oxide contained 0.04 mol% of sulfate ions, 93 mol% of Ni, 1.5 mol% of Co, 4.5 mol% of Al, 0.5 mol% of Ti, 0.5 mol% of Mo, and a half-value width n of the diffraction peak of the (208) plane of 0.35°. The lithium transition metal oxide was used as the positive electrode active material of Example 14.

[0105] <Comparative Example 1>

[0106] The composite oxide (Ni 0.92 Co 0.04 Al 0.04 O2), LiOH, and Ti(SO4)2 were mixed so that the molar ratio was 100:101:1, and a lithium transition metal oxide was prepared in the same manner as in Example 1 except that the amount of sulfate ions in the lithium transition metal oxide was 0.1 mol%, the ratio of Ni was 91 mol%, the ratio of Co was 4 mol%, the ratio of Al was 4 mol%, the ratio of Ti was 1 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.25°. The lithium transition metal oxide was used as the positive electrode active material of Comparative Example 1.

[0107] <Comparative Example 2>

[0108] The composite oxide (Ni 0.92 Co 0.03 Al 0.05O2), LiOH, and Al2(SO4)3 were mixed so that the molar ratio was 100:101:1, and a lithium transition metal oxide was prepared in the same manner as in Example 1 except that the amount of sulfate ions in the lithium transition metal oxide was 0.17 mol%, the ratio of Ni was 91 mol%, the ratio of Co was 3 mol%, the ratio of Al was 6 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.27°. The lithium transition metal oxide was used as the positive electrode active material of Comparative Example 2.

[0109] <Comparative Example 3>

[0110] The composite oxide (Ni 0.935 Co 0.015 Al 0.05 O2), LiOH, and MnSO4 were mixed so that the mass ratio was 100:101:1.5, and a lithium transition metal oxide was prepared in the same manner as in Example 1 except that the amount of sulfate ions in the lithium transition metal oxide was 0.13 mol%, the ratio of Ni was 92 mol%, the ratio of Co was 1.5 mol%, the ratio of Al was 5 mol%, the ratio of Mn was 1.5 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.28°. The lithium transition metal oxide was used as the positive electrode active material of Comparative Example 3.

[0111] <Comparative Example 4>

[0112] The composite oxide (Ni 0.93 Co 0.03 Al 0.04 O2), and LiOH were mixed so that the molar ratio was 100:101, and a lithium transition metal oxide was prepared in the same manner as in Example 1 except that the amount of sulfate ions in the lithium transition metal oxide was 0.01 mol%, the ratio of Ni was 93 mol%, the ratio of Co was 3 mol%, the ratio of Al was 4 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.23°. The lithium transition metal oxide was used as the positive electrode active material of Comparative Example 4.

[0113] <Comparative Example 5>

[0114] The composite oxide (Ni 0.935 Co 0.01 Al 0.055O2), LiOH, and Al were mixed so that the molar ratio was 100:101:1, and a lithium transition metal oxide was prepared in the same manner as in Example 1 except that the amount of sulfate ions in the lithium transition metal oxide was 0.01 mol%, the ratio of Ni was 92.5 mol%, the ratio of Co was 1 mol%, the ratio of Al was 6.5 mol%, and the half-value width n of the diffraction peak of the (208) plane was 0.28°. The lithium transition metal oxide was used as the positive electrode active material of Comparative Example 5.

[0115] [Production of positive electrode]

[0116] The positive electrode active material of Example 1 is mixed at a ratio of 91 parts by mass, acetylene black as a conductive material is mixed at a ratio of 7 parts by mass, and polyvinylidene fluoride as a binder is mixed at a ratio of 2 parts by mass. The mixture is kneaded with a mixer (TKHIVIS MIX, Primix Corporation) to prepare a positive electrode composite material slurry. Next, the positive electrode composite material slurry is applied to an aluminum foil having a thickness of 15 μm, and the coating is dried to form a positive electrode active material layer on the aluminum foil. This is used as the positive electrode of Example 1. The positive electrodes are also made in the same manner in other embodiments and comparative examples.

[0117] [Preparation of non-aqueous electrolyte]

[0118] Ethylene carbonate (EC), ethyl methyl carbonate (MEC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.

[0119] [Preparation of test battery]

[0120] The positive electrode of Example 1 and the negative electrode formed of lithium metal foil were stacked in a manner that they were opposed to each other with a separator interposed therebetween to produce an electrode body. Next, the electrode body and the nonaqueous electrolyte were inserted into an aluminum outer casing to produce a test cell. Test cells were also produced in the same manner for other Examples and Comparative Examples.

[0121] [Determination of Capacity Retention Rate in Charge and Discharge Cycle Characteristics]

[0122] At an ambient temperature of 25°C, the test batteries of each embodiment and each comparative example were charged at a constant current of 0.2C until the battery voltage reached 4.3V, then charged at a constant voltage of 4.3V until the current value reached 0.05mA, and discharged at a constant current of 0.2C until the battery voltage reached 2.5V. This charge and discharge cycle was repeated 20 times, and the capacity retention rate of the test batteries of each embodiment and each comparative example in the charge and discharge cycle was calculated according to the following formula. The higher the value, the more the reduction in the charge and discharge cycle characteristics is suppressed.

[0123] Capacity retention rate = (discharge capacity at the 20th cycle / discharge capacity at the 1st cycle) × 100

[0124] [Measurement of Charge Transfer Resistance]

[0125] After charging the test cells of each embodiment and each comparative example under the above charging conditions, AC impedance was measured in the range of 10 mHz to 100 kHz to prepare a Cole-Cole plot. The charge transfer resistance was calculated from the size of the approximate semicircle appearing in the obtained Cole-Cole plot.

[0126] Table 1 shows the results of the battery capacity (discharge capacity at the first cycle), charge transfer resistance, and capacity retention rate of the test batteries of each Example and each Comparative Example.

[0127] [Table 1]

[0128]

[0129] Examples 1 to 14 all show high capacity retention and battery capacity, and also show low charge transfer resistance. On the other hand, Comparative Examples 1 to 5 show low capacity retention, low battery capacity, or high charge transfer resistance. From this result, by using the following positive electrode active material, it is possible to suppress the reduction of charge and discharge cycle characteristics, and suppress the increase of charge transfer resistance during charge and discharge, and thus suppress the reduction of battery capacity, wherein the positive electrode active material has a lithium transition metal oxide containing Ni and Al, the ratio of Ni in the aforementioned lithium transition metal oxide is 91 mol% or more relative to the total molar number of metal elements other than Li, the aforementioned lithium transition metal oxide contains 0.02 mol% or more of sulfate ions, and the half-value width n of the diffraction peak of the (208) plane of the X-ray diffraction pattern of the aforementioned lithium transition metal oxide based on X-ray diffraction is 0.30°≤n≤0.50°.

Claims

1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium transition metal oxide containing Ni and Al, The ratio of Ni in the lithium transition metal oxide is 91 mol% or more relative to the total molar number of metal elements other than Li, The lithium transition metal oxide contains 0.02 mol% to 0.1 mol% of sulfate ions, For the lithium transition metal oxide, the half-value width n of the diffraction peak of the (208) plane of the X-ray diffraction pattern based on X-ray diffraction is 0.30°≤n≤0.50°, For the lithium transition metal oxide, a SO4 compound is attached to the surface of the lithium transition metal oxide particles, or a SO4 compound is embedded in the secondary particles of the lithium transition metal oxide. The SO4 compound is at least one of Al2(SO4)3, Ti(SO4)2, MnSO4, Nb2(SO4)3, Si(SO4)2, Mo(SO4)3, Fe2(SO4)3, BaSO4, CaSO4, CuSO4, MgSO4, SrSO4, and ZnSO4.

2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the SO4 compound is at least one of Al2(SO4)3, Ti(SO4)2, MnSO4, Nb2(SO4)3, Si(SO4)2, and Mo(SO4)3.

3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein the lithium transition metal oxide is represented by the following formula (1): Li x Ni a Co b Al c M d O2(1) in, M is at least one element selected from the group consisting of Ti, Nb, Mn, Si, Mo, Zr, V, Fe, Mg, Cr, Cu, Sn, Ta, W, Na, K, Ba, Sr, Bi, Be, Zn, Ca and B, 0.95≤x≤1.10, a≥0.91, 0.005≤b≤0.045, 0.03 <c,0≤d≤0.03。 4 . A non-aqueous electrolyte secondary battery comprising a positive electrode, wherein the positive electrode comprises the positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 .

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery

    JP2006202702A

  • Nickel-containing hydroxide, nickel-containing oxide, lithium-mixed nickel oxide and methods for manufacturing them

    JP2010070431A

  • Aluminum-coated nickel cobalt-containing composite hydroxide and method for manufacturing same, cathode active material for nonaqueous electrolyte secondary battery and method for manufacturing same, and nonaqueous electrolyte secondary battery

    CN107531510A

  • Composite positive active material, positive electrode including the same, and lithium battery including the positive electrode

    CN107689447A