Lithium ion secondary battery, lithium ion capacitor, and method for manufacturing the same

By forming an active material layer on the surface of the negative electrode collector of lithium-ion batteries and capacitors and doping it with lithium, the aperture ratio and discharge capacity ratio are controlled, which solves the problem of poor cycle characteristics and achieves high energy density and good cycling of batteries and capacitors. characteristic.

CN112042029BActive Publication Date: 2024-10-18MUSASHI ENERGY SOLUTIONS CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN201980026814.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-04-18
Publication Date
2024-10-18
Estimated Expiration
2039-04-18

AI Technical Summary

Technical Problem

Existing lithium-ion secondary batteries and lithium-ion capacitors suffer from poor cycle characteristics, making it difficult to simultaneously improve cycle characteristics and energy density.

Method used

By forming a negative active material layer on the surface of the negative electrode current collector and doping it with lithium, the aperture ratio of the negative electrode current collector is controlled to be above 0% and below 0.1%, and a specific discharge capacity ratio formula is used to define the performance of the battery to ensure The discharge capacity ratio of the battery within a specific voltage range is above 0.05 and below 0.2, achieving the stacked structure of the electrode and the composition of the electrolyte.

Benefits of technology

A manufacturing method for lithium-ion secondary batteries and lithium-ion capacitors with good cycle characteristics and high energy density has been realized, and the cycle durability and energy density of the batteries have been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004761774140000261
    Figure GDA0004761774140000261
  • Figure GDA0004761774140000271
    Figure GDA0004761774140000271
  • Figure GDA0004761774140000321
    Figure GDA0004761774140000321
Patent Text Reader

Abstract

A lithium-ion secondary battery comprises an electrode unit and an electrolyte. The negative electrode comprises a negative electrode collector and a negative electrode active material layer formed on the surface of the negative electrode collector. The negative electrode is doped with lithium. The aperture ratio of the negative electrode collector is greater than 0% and less than 0.1%. The discharge capacity ratio X defined by formula (1) is greater than 0 and less than or equal to 0.9. Formula (1) X = C1 / C2. C1 in formula (1) is the discharge capacity of a single cell when charging and discharging the single cell voltage between 2.0V and 4.3V. C2 in formula (1) is the discharge capacity of the negative electrode when charging and discharging the negative electrode between 0V vs.Li / Li+ and 3V vs.Li / Li+.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This international application claims the benefit of Japanese Patent Application No. 2018-80711 and Japanese Patent Application No. 2018-163231 filed in the Japan Patent Office on April 19, 2018, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to a lithium ion secondary battery, a lithium ion capacitor, and methods of manufacturing the same. Background Art

[0004] In recent years, the miniaturization and lightness of electronic devices have attracted attention. Along with the miniaturization and lightness of electronic devices, there is also an increasing demand for miniaturization and lightness of batteries used as power sources for driving electronic devices.

[0005] In order to meet the demand for miniaturization and lightness of batteries, non-aqueous electrolyte secondary batteries have been developed. As non-aqueous electrolyte secondary batteries, for example, lithium ion secondary batteries can be cited. In addition, as a power storage device for applications requiring high energy density characteristics and high output characteristics, lithium ion capacitors are known.

[0006] In the above-mentioned batteries and capacitors, a process of pre-doping an electrode active material with an alkali metal is adopted for various purposes. The process of pre-doping an electrode active material with an alkali metal is called pre-doping.

[0007] For example, lithium is pre-doped in lithium ion capacitors to reduce the negative electrode potential and increase energy density. The pre-doping method in this case is a method of pre-doping the negative electrode active material in a single cell mainly using a current collector having through holes (see, for example, Patent Document 1).

[0008] In addition, in lithium-ion secondary batteries, pre-doping is performed to reduce the irreversible capacity of the negative electrode. As a method of pre-doping in this case, in addition to the above method, a method of pre-doping the negative electrode active material before assembling the battery is also known (for example, see Patent Documents 2 and 3).

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2007-67105

[0012] Patent Document 2: Japanese Patent Application Laid-Open No. 7-235330

[0013] Patent Document 3: Japanese Patent Application Laid-Open No. 9-293499 Summary of the invention

[0014] Problem that the invention aims to solve

[0015] The lithium ion secondary batteries described in Patent Documents 2 to 4 have a problem of poor cycle characteristics. In addition, cycle characteristics and energy density are generally in a trade-off relationship, and therefore it is difficult to improve both.

[0016] One aspect of the present disclosure is to preferably provide a lithium ion secondary battery and a lithium ion capacitor having excellent cycle characteristics and high energy density, and methods for producing the same.

[0017] Technical solutions to the problem

[0018] One embodiment of the present disclosure relates to a lithium-ion secondary battery, which has an electrode unit and an electrolyte, the electrode unit includes a positive electrode and a negative electrode, the negative electrode has a negative electrode collector and a negative electrode active material layer formed on the surface of the negative electrode collector, and the negative electrode is doped with lithium, the aperture ratio of the negative electrode collector is greater than 0% and less than 0.1%, and the discharge capacity ratio X defined by the following formula (1) is greater than 0 and less than or equal to 0.9.

[0019] Formula (1) X = C1 / C2

[0020] C1 in the above formula (1) is the discharge capacity of the single cell when charging and discharging between the single cell voltage of 2.0 V and 4.3 V. C2 in the above formula (1) is the discharge capacity of the negative electrode when charging and discharging between 0 V vs. Li / Li+ and 3 V vs. Li / Li+. The single cell voltage represents the potential difference between the positive electrode and the negative electrode.

[0021] A lithium ion secondary battery according to one embodiment of the present disclosure has good cycle characteristics and high energy density.

[0022] Another embodiment of the present disclosure relates to a method for manufacturing a lithium-ion secondary battery, wherein the lithium-ion secondary battery has an electrode battery, and the method for manufacturing the lithium-ion secondary battery comprises: doping lithium into a negative electrode, wherein the negative electrode has a negative electrode collector and a negative electrode active material layer formed on the surface of the negative electrode collector; stacking a positive electrode and the negative electrode doped with lithium to form the electrode battery, and the aperture ratio of the negative electrode collector is greater than 0% and less than 0.1%, and the discharge capacity ratio X defined by the following formula (1) is greater than 0 and less than or equal to 0.9.

[0023] Formula (1) X = C1 / C2

[0024] C1 in the above formula (1) is the discharge capacity of the single cell when charging and discharging between the single cell voltage of 2.0 V and 4.3 V. C2 in the above formula (1) is the discharge capacity of the negative electrode when charging and discharging between 0 V vs. Li / Li+ and 3 V vs. Li / Li+. The units of C1 and C2 are mAh or Ah.

[0025] According to a method for manufacturing a lithium ion secondary battery which is another aspect of the present disclosure, a lithium ion secondary battery having excellent cycle characteristics and high energy density can be manufactured.

[0026] Another embodiment of the present disclosure relates to a lithium ion capacitor comprising an electrode unit and an electrolyte, wherein the electrode unit includes a positive electrode and a negative electrode, wherein the negative electrode includes a negative electrode collector and a negative electrode active material layer formed on the surface of the negative electrode collector, and the negative electrode is doped with lithium, the aperture ratio of the negative electrode collector is greater than 0% and less than 0.1%, and the discharge capacity ratio X defined by the following formula (3) is greater than 0.05 and less than 0.2.

[0027] Formula (3) X = C1 / C2

[0028] C1 in the above formula (3) is the discharge capacity of the single cell when charging and discharging between the single cell voltage of 2.2 V and 3.8 V. C2 in the above formula (3) is the discharge capacity of the negative electrode when charging and discharging between 0 V vs. Li / Li+ and 3 V vs. Li / Li+. The units of C1 and C2 are mAh or Ah.

[0029] A lithium ion capacitor according to another aspect of the present disclosure has good cycle characteristics and high energy density.

[0030] Another embodiment of the present disclosure relates to a method for manufacturing a lithium ion capacitor, the lithium ion capacitor comprising an electrode unit and an electrolyte, the electrode unit comprising a negative electrode and an electrode different from the negative electrode, the negative electrode comprising a negative electrode collector and a negative electrode active material layer formed on a surface of the negative electrode collector, the method comprising: doping the negative electrode with lithium; and stacking the negative electrode doped with lithium and the electrode different from the negative electrode to form the electrode unit, wherein the aperture ratio of the negative electrode collector is greater than 0% and less than 0.1%, and the discharge capacity ratio X defined by the following formula (3) is greater than 0.005 and less than 0.2.

[0031] Formula (3) X = C1 / C2

[0032] C1 in the above formula (3) is the discharge capacity of the single cell when charging and discharging between the single cell voltage of 2.2 V and 3.8 V. C2 in the above formula (3) is the discharge capacity of the negative electrode when charging and discharging between 0 V vs. Li / Li+ and 3 V vs. Li / Li+. The units of C1 and C2 are mAh or Ah.

[0033] According to a method for manufacturing a lithium ion capacitor according to another aspect of the present disclosure, a lithium ion capacitor having good cycle characteristics and high energy density can be manufactured. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is an explanatory diagram showing the structure of an electrode manufacturing apparatus.

[0035] Figure 2A is a plan view showing a part of a strip-shaped electrode and a partial structure of a strip-shaped pre-doped negative electrode for an electricity storage device; Figure 2B yes Figure 2A Cross-sectional view at section IIB-IIB of .

[0036] Description of Reference Numerals

[0037] 1…electrode manufacturing device; 3, 5…electrolyte tank; 7…cleaning tank; 9, 11, 13, 15, 17, 19, 21, 23, 25, 27, 29, 31, 33, 35, 37, 39, 41, 43, 45…conveying roller;

[0038] 47 ... supply roller; 49 ... winding roller; 51 ... counter electrode unit; 53 ... porous insulating member;

[0039] 55 ... support platform; 57 ... circulation filter unit; 61 ... DC power supply; 63 ... blower;

[0040] 67, 68 ... support rods; 69 ... partition; 70 ... support rods; 71 ... space; 73 ... electrode;

[0041] 75…negative electrode for power storage device; 81…filter; 83…pump; 85…pipeline;

[0042] 93 ... negative electrode current collector; 95 ... negative electrode active material layer DETAILED DESCRIPTION

[0043] Exemplary embodiments of the present disclosure are described with reference to the accompanying drawings.

[0044] 1. Power storage device

[0045] (1-1) Overall structure of power storage device

[0046] The power storage device disclosed in the present invention comprises an electrode unit and an electrolyte. The electrode unit comprises a positive electrode and a negative electrode. The negative electrode comprises a negative electrode collector and a negative electrode active material layer. The negative electrode active material layer is formed on the surface of the negative electrode collector. The negative electrode is doped with lithium.

[0047] In this specification, the "positive electrode" refers to the electrode on the side where current flows out during discharge and flows in during charge. In this specification, the "negative electrode" refers to the electrode on the side where current flows in during discharge and flows out during charge.

[0048] In this specification, "doped with lithium" refers to a state in which lithium is occluded, intercalated, adsorbed, supported, alloyed, or embedded in various forms such as metals, ions, compounds, etc. As "doping", for example, the phenomenon of at least one of lithium and anions being doped into the positive electrode active material, and the phenomenon of lithium ions being doped into the negative electrode active material, etc. can be cited. "Dedoping" refers to deintercalation and release. As "dedoping", for example, the phenomenon of lithium ions or anions being deintercalated from the positive electrode active material, and the phenomenon of lithium ions being deintercalated from the negative electrode active material, etc. can be cited.

[0049] As a method of pre-doping lithium into the negative electrode, for example, a method of doping lithium by electrically connecting the negative electrode and a lithium electrode using a motor manufacturing device can be mentioned. The lithium electrode contains metal lithium and the like.

[0050] For example, the power storage device of the present disclosure can be manufactured in the following manner. A positive electrode active material layer is formed on the surface of a positive electrode current collector to manufacture a positive electrode. A negative electrode active material layer is formed on the surface of a negative electrode current collector to manufacture a negative electrode. Lithium is doped into the negative electrode. For example, a doping unit can be used to dope lithium into the negative electrode. The doping unit includes, for example, a doping tank, a transfer unit, a counter electrode unit, a connecting unit, and a porous insulating component.

[0051] The doping tank contains a solution containing lithium ions. The transport unit transports the electrode along a path passing through the doping tank. The counter electrode unit is housed in the doping tank. The connecting unit electrically connects the electrode and the counter electrode unit. The porous insulating component is arranged between the electrode and the counter electrode unit and does not contact the electrode.

[0052] Next, the positive electrode, the first separator, the negative electrode, and the second separator are stacked in this order to form a stack. The stack is, for example, a stack formed by stacking three or more constituent units, wherein the constituent unit includes a positive electrode, a first separator, a negative electrode, and a second separator. The stack is in the form of, for example, a plate, a sheet, or a wound form. The stack corresponds to an electrode unit.

[0053] Next, the electrode unit is sealed in an outer container. The outer container may be in the form of a square, a cylinder, a laminate, or the like. The outer container may be a film or a can. Then, the outer container is filled with an electrolyte. The above steps are used to produce a power storage device.

[0054] In the case of a lithium-ion secondary battery, in order to improve the energy density and cycle characteristics in a balanced manner, the doping ratio of lithium doped into the negative electrode active material layer is preferably 5% or more and 95% or less relative to the discharge capacity C2 of the negative electrode, and further preferably 15% or more and 90% or less, more preferably 25% or more and 80% or less, and particularly preferably 25% or more and 75% or less. The doping ratio of lithium doped into the negative electrode active material layer is 5% or more and 95% or less relative to the discharge capacity C2 of the negative electrode, thereby making the lithium-ion secondary battery have good cycle characteristics and high energy density. The doping ratio of lithium doped into the negative electrode active material layer refers to the ratio of the amount of lithium doped into the negative electrode active material layer relative to the discharge capacity C2 of the negative electrode. The doping amount of lithium doped into the negative electrode active material layer refers to the value obtained by dividing the capacity of the current used to dope lithium by the mass of the negative electrode active material. The unit of the doping amount of lithium doped into the negative electrode active material layer is mAh / g.

[0055] In the case of a lithium ion capacitor, the doping ratio of lithium doped into the negative electrode active material layer is preferably 30% or more and 95% or less of the negative electrode discharge capacity C2. In this case, the negative electrode capacity and cycle durability are improved. The negative electrode discharge capacity C2 is the discharge capacity of the negative electrode when the negative electrode is charged and discharged between 0V vs. Li / Li+ and 3V vs. Li / Li+.

[0056] The discharge capacity C2 of the negative electrode is the discharge capacity of the negative electrode when the negative electrode is charged and discharged between 0 V vs. Li / Li+ and 3 V vs. Li / Li+.

[0057] The power storage device of the present disclosure may have a configuration basically similar to that of a power storage device described in Japanese Patent Application Laid-Open No. 2004-266091, for example.

[0058] (1-2) Specific Examples of Power Storage Devices

[0059] Specific examples of the power storage device disclosed in the present invention include lithium ion capacitors, lithium ion secondary batteries, etc. In the present specification, a lithium ion secondary battery is a power storage device in which the positive electrode and the negative electrode are non-polarizable electrodes and contain lithium ions. In the present specification, a lithium ion capacitor is a power storage device in which the positive electrode is a polarizable electrode and the negative electrode is a non-polarizable electrode and contains lithium ions.

[0060] (1-3) Current Collector

[0061] The term "current collector" in this specification refers to both a positive electrode current collector and a negative electrode current collector. The positive electrode includes a positive electrode current collector for receiving and distributing electricity. The negative electrode includes a negative electrode current collector for receiving and distributing electricity.

[0062] (1-4) Positive electrode collector

[0063] As the material of the positive electrode current collector, for example, aluminum, stainless steel, etc. can be cited. As the material of the positive electrode current collector, aluminum is preferred. The thickness of the positive electrode current collector is not particularly limited, but is preferably in the range of 1 μm to 50 μm, more preferably in the range of 5 μm to 40 μm, and particularly preferably in the range of 10 μm to 40 μm.

[0064] The opening ratio of the positive electrode current collector (hereinafter referred to as the positive electrode current collector opening ratio) is preferably 0% or more and 0.1% or less, and more preferably 0%. Here, the positive electrode current collector opening ratio can be calculated by the following formula (4).

[0065] Formula (4)

[0066] Positive electrode collector opening ratio (%) = [1-(mass of positive electrode collector / true specific gravity of positive electrode collector) / (apparent volume of positive electrode collector)] × 100

[0067] In the above formula (4), the "true specific gravity of the positive electrode collector" refers to the mass per unit volume of the positive electrode collector without holes, which is the mass per unit volume of the material constituting the positive electrode collector. The "apparent volume of the positive electrode collector" refers to the volume of the positive electrode collector assuming that the positive electrode collector has no holes. The "apparent volume of the positive electrode collector" is the volume calculated based on the longitudinal dimension, transverse dimension and thickness dimension of the positive electrode collector measured respectively. By making the opening rate of the positive electrode collector greater than 0% and less than 0.1%, it is easy to apply the positive active material layer to the positive electrode collector.

[0068] (1-5) Positive electrode active material

[0069] As the positive electrode active material of the lithium ion secondary battery, a substance that can be reversibly doped and dedoped with at least one anion is used. Examples of anions include lithium and tetrafluoroborate. Examples of positive electrode active materials include transition metal oxides such as cobalt oxide, nickel oxide, manganese oxide, and vanadium oxide; sulfur-based active materials such as sulfur and metal sulfides. Both the positive electrode active material and the negative electrode active material may be composed of a single substance or a mixture of two or more substances. The specific surface area of ​​lithium cobalt oxide is preferably 0.1 m 2 / g or more and 30m 2 / g or less.

[0070] As the positive electrode material of the lithium ion capacitor, a material having a large specific surface area, such as activated carbon and polyacene-based organic semiconductor, is preferred.

[0071] The activated carbon is in the form of powder, for example. In addition, from the viewpoint of the packing density of the activated carbon, the volume average diameter (D50) of the activated carbon is preferably greater than 3 μm and less than 30 μm. When the specific surface area and the volume average diameter (D50) of the activated carbon are within the above range, the energy density of the storage device is further improved. The value of the volume average diameter (D50) described herein is a value calculated by a laser diffraction / scattering method. The specific surface area of ​​the activated carbon is preferably 1900 m 2 / g and above 3000m 2 / g or less, more preferably 1950m 2 / g and above 2800m 2 / g or less.

[0072] The polyacene-based organic semiconductor is a heat-treated product of an aromatic condensation polymer. The polyacene-based organic semiconductor has a polyacene-based skeleton structure. In the polyacene-based skeleton structure, the atomic number ratio of hydrogen atoms to carbon atoms is greater than 0.05 and less than 0.50. The atomic number ratio of hydrogen atoms to carbon atoms is a value obtained by dividing the number of hydrogen atoms by the number of carbon atoms.

[0073] (1-6) Positive Electrode Active Material Layer

[0074] The positive electrode active material layer is formed by attaching the positive electrode active material to the positive electrode current collector. Examples of the method for attaching the positive electrode active material include coating, printing, injection, spraying, vapor deposition, and compression bonding.

[0075] The thickness of the positive electrode active material layer is preferably 10 μm or more and 250 μm or less, more preferably 25 μm or more and 200 μm or less, and particularly preferably 50 μm or more and 280 μm or less.

[0076] In the case where a positive electrode active material layer is formed on both surfaces of the positive electrode, the thickness of the positive electrode active material layer refers to the sum of the thicknesses of the positive electrode active material layers formed on the two surfaces of the positive electrode. In the case where a positive electrode active material layer is formed on only one surface of the positive electrode, the thickness of the positive electrode active material layer refers to the thickness of the positive electrode active material layer formed on one surface of the positive electrode. When the thickness of the positive electrode active material layer is within the above range, the positive electrode capacity can be increased and the impedance can be reduced.

[0077] The density of the positive electrode active material layer is preferably 0.1 g / cm 3 Above and 5g / cm 3 Below, more preferably 1g / cm 3 Above and 4.5g / cm 3 Below, especially preferably 2g / cm3 Above 4g / cm 3 When the density of the positive electrode active material layer is within the above range, the energy density of the power storage device increases, and the cycle characteristics of the power storage device improves.

[0078] The density of the positive electrode active material layer can be measured by the following method. The positive electrode is obtained by decomposing the storage device. The obtained positive electrode is cleaned with diethyl carbonate and vacuum dried at 100°C. The mass of the positive electrode active material layer and the outer volume of the positive electrode active material are measured. The density of the positive electrode active material layer is calculated by dividing the mass of the positive electrode active material layer by the outer volume of the positive electrode active material layer. The "outer volume of the positive electrode active material layer" mentioned here refers to the volume calculated based on the longitudinal dimension, transverse dimension and thickness dimension of the positive electrode active material layer, which are measured respectively.

[0079] In addition, as a method for setting the thickness and density of the positive electrode active material layer within the above range, a method such as roller pressing the positive electrode active material layer can be cited. In addition, when roller pressing is performed, the thickness and density of the positive electrode active material layer are the thickness and density after roller pressing, respectively. The roller pressing conditions are not particularly limited. Generally, the roller temperature is 10°C or more and 50°C or less, the line pressure is 0.1t / c or more and 10t / cm or less, and the conveying speed is 0.01m / min or more and 10m / min or less.

[0080] The weight per unit area of ​​the positive electrode active material layer is preferably 10 g / m 2 Above and 1000g / m 2 Below, more preferably 20g / m 2 Above and 800 / m 2 Below. When the positive electrode active material layer is formed on both surfaces of the positive electrode, the unit area weight of the positive electrode active material layer is the sum of the unit area weights of the positive electrode active material layers formed on the two surfaces of the positive electrode. When the positive electrode active material layer is formed on only one surface of the positive electrode, the unit area weight of the positive electrode active material layer is the unit area weight of the positive electrode active material layer formed on one surface of the positive electrode.

[0081] When the weight per unit area of ​​the positive electrode active material layer is within the above range, the energy density of the power storage device increases and the cycle characteristics of the power storage device improves.

[0082] The weight per unit area of ​​the positive electrode active material layer can be measured by the following method. The positive electrode is obtained by decomposing the storage device. The obtained positive electrode is cleaned with diethyl carbonate and vacuum dried at 100°C. A measurement sample with a specified area is cut from the positive electrode and its mass is measured. The positive electrode active material layer is then peeled off from the positive electrode collector in the measurement sample, and the mass of the remaining positive electrode collector is measured. The mass of the positive electrode active material layer is calculated by subtracting the mass of the remaining positive electrode collector from the mass of the measurement sample. The weight per unit area of ​​the positive electrode active material layer is calculated by dividing the mass of the positive electrode active material layer by the area of ​​the measurement sample.

[0083] (1-7) Negative electrode collector

[0084] As the negative electrode current collector, stainless steel, copper, nickel, etc. can be used. The thickness of the negative electrode current collector is not particularly limited. The thickness of the negative electrode current collector is usually 1 μm or more and 50 μm or less, and particularly preferably 5 μm or more and 20 μm or less.

[0085] The opening ratio of the negative electrode collector (hereinafter referred to as the negative electrode collector opening ratio) is 0% or more and 0.1% or less. The negative electrode collector opening ratio is preferably 0% or more and 0.05% or less, and more preferably 0%. When the negative electrode collector does not have a through hole, the negative electrode collector opening ratio is 0%. The negative electrode collector opening ratio described herein can be calculated by the following formula (4).

[0086] Formula (4)

[0087] Negative electrode collector opening ratio (%) = [1-(mass of negative electrode collector / true specific gravity of negative electrode collector) / (apparent volume of negative electrode collector)] × 100

[0088] In the above formula (4), the "true specific gravity of the negative electrode collector" refers to the mass per unit volume of the negative electrode collector without holes, which is the mass per unit volume of the material constituting the negative electrode collector. The "apparent volume of the negative electrode collector" refers to the volume of the negative electrode collector assuming that the negative electrode collector has no holes. The "apparent volume of the negative electrode collector" is the volume calculated based on the longitudinal dimension, transverse dimension and thickness dimension of the negative electrode collector measured respectively.

[0089] The upper limit of the negative electrode collector aperture ratio is preferably 0.05%, and particularly preferably 0%. When the negative electrode collector aperture ratio is within the above range, the electrode strength of the negative electrode collector can be maintained even if the thickness of the negative electrode collector is small. As a result, the negative electrode collector can be prevented from breaking when manufacturing electrodes and batteries. In addition, when the negative electrode collector aperture ratio is within the above range, the impedance of the negative electrode can be reduced.

[0090] (1-8) Negative Electrode Active Material

[0091] As the negative electrode active material of the lithium ion secondary battery, a material capable of reversibly doping and de-doping lithium can be used. As the negative electrode active material, for example, silicon-based materials, carbon-based materials, silicon-carbon composite materials, etc. can be mentioned. As the silicon-based materials, for example, Si, SiO, SiOC, etc. can be mentioned. As the carbon-based materials, for example, graphite-based particles, etc. can be mentioned. As the graphite-based particles, for example, graphite-based composite particles, polyacene-based organic semiconductors (PAS), etc. can be mentioned. As the silicon-carbon composite material, a silicon-carbon composite material obtained by coating a carbon-based material on a silicon-based material can be mentioned. In addition, the content rate of silicon in the silicon-carbon composite material is preferably 5% by mass or more and 99% by mass or less, more preferably 20% by mass or more and 90% by mass or less.

[0092] As the silicon-based materials, in addition to, for example, elemental silicon, silicon oxides, silicon alloys, etc. can be mentioned, the silicon materials described in Japanese Unexamined Patent Application Publication No. 2004-185810 can also be used. As the above-mentioned silicon oxide, a silicon oxide represented by the compositional formula SiOx (0 < x < 2, preferably 0.1 ≤ x ≤ 1) is preferred. As the above-mentioned silicon alloy, an alloy of silicon and at least one transition metal selected from titanium, zirconium, nickel, copper, iron, and molybdenum is preferred. The silicides of these transition metals have a high electron conductivity and high strength, so they are preferably used. In addition, since the active material contains these transition metals, the transition metals present on the surface of the active material are oxidized to form oxides having hydroxyl groups on the surface, so the adhesive force with the binder is better, and thus it is also preferred in this regard. As the silicon alloy, a silicon-nickel alloy or a silicon-titanium alloy is more preferably used, and a silicon-titanium alloy is particularly preferably used. The content ratio of silicon in the silicon alloy is preferably 10 mol% or more, more preferably 20 to 70 mol%, relative to all the metal elements in the alloy. The active material containing silicon atoms can be any of single crystal, polycrystal, and amorphous.

[0093] The graphite-based composite particles include core particles and a graphitized substance covering the surface of the core particles. As the core particles, for example, graphite, hardly graphitizable carbon, natural graphite, etc. can be mentioned. As the graphitized substance, for example, graphitized substances derived from tar, pitch, etc. can be mentioned.

[0094] The particle size at which the cumulative value of the particle size distribution of the graphite-based particles corresponds to 50%, that is, the volume average diameter (D50), is preferably 1.0 μm or more and 35 μm or less, more preferably 2 μm or more and 30 μm or less. When the volume average diameter (D50) of the graphite-based particles is 1.0 μm or more, it is easy to manufacture the graphite-based particles. In addition, when the volume average diameter (D50) of the graphite-based particles is 1.0 μm or more, gas is not easily generated during charging. As a result, the durability of the power storage device is improved. The volume average diameter (D50) of the graphite-based particles is a value calculated by the laser diffraction / scattering method.

[0095] The polyacene-based organic semiconductor is a heat-treated product of an aromatic condensation polymer. The polyacene-based organic semiconductor has a polyacene-based skeleton structure. In the polyacene-based skeleton structure, the atomic number ratio of hydrogen atoms to carbon atoms is greater than 0.05 and less than 0.50. The atomic number ratio of hydrogen atoms to carbon atoms is a value obtained by dividing the number of hydrogen atoms by the number of carbon atoms.

[0096] The silicon-carbon composite material is a composite of a silicon-based material and a carbon-based material. Examples of the silicon-carbon composite material include a silicon-based material coated with the carbon-based material.

[0097] The aromatic condensation polymer is a condensate of an aromatic hydrocarbon compound and an aldehyde. Examples of the aromatic hydrocarbon compound include phenol, cresol, and xylenol. Examples of the aldehyde include formaldehyde, acetaldehyde, and furfural.

[0098] The specific surface area of ​​the negative electrode active material is preferably 0.1 m 2 / g and above and 200m 2 / g or less, more preferably 0.5m 2 / g or more and 50m 2 / g or less. When the specific surface area of ​​the negative electrode active material is 0.1m 2 When the specific surface area of ​​the negative electrode active material is 200 m 2 When the MgO2O3 content is less than 1.17 g / cm2, the irreversible capacity of the produced power storage device during charging becomes small, and gas is less likely to be generated during charging. As a result, the durability of the power storage device is improved.

[0099] Examples of materials for the negative electrode of the lithium ion capacitor include carbon materials and silicon materials. Examples of carbon materials include graphite composite particles and polyacene organic semiconductors (PAS). Examples of silicon materials include Si, SiO, and SiOC.

[0100] The graphite composite particles include core particles and a graphitized material covering the surface of the core particles. Examples of the core particles include graphite, non-graphitizable carbon, and natural graphite. Examples of the graphitized material include graphitized materials derived from tar and asphalt.

[0101] The polyacene-based organic semiconductor is a heat-treated product of an aromatic condensation polymer. The polyacene-based organic semiconductor has a polyacene-based skeleton structure. In the polyacene-based skeleton structure, the atomic number ratio of hydrogen atoms to carbon atoms is greater than 0.05 and less than 0.50. The atomic number ratio of hydrogen atoms to carbon atoms is a value obtained by dividing the number of hydrogen atoms by the number of carbon atoms.

[0102] (1-9) Negative Electrode Active Material Layer

[0103] The negative electrode active material layer is formed by attaching the negative electrode active material to the surface of the negative electrode current collector. Examples of the method for attaching the negative electrode active material include coating, printing, injection, spraying, vapor deposition, and compression bonding.

[0104] When the negative electrode is used to manufacture an electrode for a lithium ion secondary battery, the density of the negative electrode active material layer is preferably 1.50 g / cm 3 Above and 2.00g / cm 3 Below, more preferably 1.60g / cm 3 Above and 1.90g / cm 3 the following.

[0105] The negative electrode active material layer preferably contains a silicon-based material or a silicon-carbon composite material. The content of the silicon-based material or the silicon-carbon composite material in the negative electrode active material layer is preferably 5% by mass or more and 99% by mass or less, and further preferably 20% by mass or more and 90% by mass or less, and more preferably 30% by mass or more and 80% by mass or less. When the content of the silicon-based material in the negative electrode active material layer is within the above range, the negative electrode capacity is further increased.

[0106] The weight per unit area of ​​the negative electrode active material layer is preferably 5 g / m 2 Above and 500g / m 2 Below, more preferably 20g / m 2 Above and 400g / m 2 Below, more preferably 30g / m 2 Above and 300g / m 2 the following.

[0107] In the case where negative electrode active material layers are formed on both surfaces of the negative electrode, the weight per unit area of ​​the negative electrode active material layers refers to the sum of the weight per unit area of ​​the negative electrode active material layers formed on both surfaces of the negative electrode. In the case where negative electrode active material layers are formed on only one surface of the negative electrode, the weight per unit area of ​​the negative electrode active material layers refers to the weight per unit area of ​​the negative electrode active material layers formed on one surface of the negative electrode.

[0108] When the weight per unit area of ​​the negative electrode active material layer is within the above range, the negative electrode capacity and the cycle characteristics of the storage device are improved. When the content of the silicon-based material in the negative electrode active material layer is 5% by mass or more and 99% by mass or less, and the weight per unit area of ​​the negative electrode active material layer is within the above range, the negative electrode capacity and the cycle characteristics of the storage device are further improved. In addition, the weight per unit area of ​​the negative electrode active material layer can be measured by the same method as the weight per unit area of ​​the positive electrode active material layer.

[0109] The thickness of the negative electrode active material layer is preferably 3 μm or more and 300 μm or less, more preferably 10 μm or more and 250 μm or less, and more preferably 25 μm or more and 200 μm or less.

[0110] In the case where negative electrode active material layers are formed on both surfaces of the negative electrode, the thickness of the negative electrode active material layer refers to the sum of the thicknesses of the negative electrode active material layers formed on both surfaces of the negative electrode. In the case where a negative electrode active material layer is formed on only one surface of the negative electrode, the thickness of the negative electrode active material layer refers to the thickness of the negative electrode active material layer formed on one surface of the negative electrode.

[0111] When the thickness of the negative electrode active material layer is within the above range, the negative electrode capacity and the cycle characteristics of the storage device are improved. When the content of the silicon-based material in the negative electrode active material layer is 5 mass % or more and 99 mass % or less, and the thickness of the negative electrode active material layer is within the above range, the negative electrode capacity and the cycle characteristics of the storage device are further improved.

[0112] In addition, as a method for setting the thickness and density of the negative electrode active material layer within the above range, a method such as roller pressing the negative electrode active material layer can be cited. In addition, when roller pressing is performed, the thickness and density of the negative electrode active material layer are the thickness and density after roller pressing, respectively. The roller pressing conditions are not particularly limited. Generally, the roller temperature is 10°C or more and 50°C or less, the line pressure is 0.1t / c or more and 10t / cm or less, and the conveying speed is 0.01m / min or more and 10m / min or less.

[0113] (1-10) Manufacturing of positive and negative electrodes

[0114] The positive electrode having the positive electrode active material layer and the negative electrode having the negative electrode active material layer as described above can be produced by a known production method.

[0115] For example, the positive electrode can be manufactured as follows: A positive electrode active material, a binder, and a solvent are mixed to prepare a positive electrode slurry. The positive electrode slurry may further contain a conductive material or a thickener as required.

[0116] The positive electrode having the positive electrode active material layer can be manufactured by coating the positive electrode slurry on the positive electrode collector. In addition, the positive electrode slurry can be formed into a sheet and the sheet-shaped molded product can be attached to the positive electrode collector.

[0117] For example, the negative electrode can be manufactured in the following manner: A negative electrode active material, a binder, and a solvent are mixed to prepare a negative electrode slurry. The negative electrode slurry may further contain a conductive material or a thickener as required.

[0118] The negative electrode having the negative electrode active material layer can be manufactured by coating the negative electrode slurry on the negative electrode current collector. In addition, the negative electrode slurry can be formed into a sheet and the sheet-shaped product can be attached to the negative electrode current collector.

[0119] As the binder contained in the positive electrode slurry or the negative electrode slurry, for example, a rubber-based binder, a fluorine-containing resin, and an acrylic resin can be cited. As the rubber-based binder, for example, SBR can be cited. As the fluorine-containing resin, for example, a fluorine-containing resin obtained by seed polymerization of polytetrafluoroethylene, polyvinylidene fluoride, etc. with an acrylic resin can be cited.

[0120] Examples of the solvent contained in the positive electrode slurry or the negative electrode slurry include water, organic solvents, etc. Examples of the conductive material contained in the positive electrode slurry or the negative electrode slurry include acetylene black, Ketjen black, graphite, metal powder, etc. Examples of the thickener contained in the positive electrode slurry or the negative electrode slurry include carboxymethyl cellulose (CMC), etc.

[0121] The amount of binder and conductive material added to the positive electrode slurry or the negative electrode slurry can be appropriately adjusted according to the conductivity of the active material used, the shape of the electrode to be produced, etc. In general, the amount of binder and conductive material added is preferably 2% by mass or more and 20% by mass or less relative to the active material, and particularly preferably 2% by mass or more and 10% by mass or less. In addition, the active material refers to the positive electrode active material or the negative electrode active material.

[0122] (1-11) Diaphragm

[0123] As a material of the separator of the power storage device of the present disclosure, a separator having an air permeability in the range of 1 sec to 200 sec is preferred. The air permeability is a value measured by a method in accordance with JISP 8117.

[0124] As the separator, for example, nonwoven fabrics and microporous films made of polyethylene, polypropylene, polyester, cellulose, polyolefin, cellulose / rayon, etc. can be appropriately selected and used. As the separator, nonwoven fabrics made of polyethylene, polypropylene, or cellulose / rayon are particularly preferred.

[0125] The thickness of the separator is, for example, 5 μm to 20 μm, preferably 5 μm to 15 μm. When the thickness of the separator is 5 μm or more, short circuit is less likely to occur. When the thickness of the separator is 20 μm or less, impedance is reduced.

[0126] (1-12) Electrolytes

[0127] In the power storage device of the present disclosure, as the electrolyte, for example, an electrolytic solution, a solid electrolyte, or a gel electrolyte can be used.

[0128] As the electrolyte, for example, an aprotic organic solvent electrolyte solution of a lithium salt can be used. The electrolyte contains, for example, an aprotic organic solvent. As the aprotic organic solvent, for example, cyclic carbonates, chain carbonates, etc. can be listed. As cyclic carbonates, for example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, etc. can be listed. As chain carbonates, for example, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, etc. can be listed. The electrolyte can be a mixed solvent formed by mixing two or more of the above substances.

[0129] Aprotic organic solvents may also contain organic solvents other than cyclic carbonates and chain carbonates. As organic solvents other than cyclic carbonates and chain carbonates, for example, cyclic ethers, chain carboxylates, chain ethers, etc. may be cited. As cyclic ethers, for example, gamma-butyrolactone, etc. may be cited. As chain carboxylates, for example, ethyl propionate, etc. may be cited. As chain ethers, for example, dimethoxyethane, etc. may be cited.

[0130] The electrolyte solution contains lithium salts, etc. Examples of lithium salts include LiClO4, LiAsF6, LiBF4, LiPF6, LiN(C2F5SO2)2, and LiN(CF3SO2)2.

[0131] As the lithium salt, LiPF6 is particularly preferred. LiPF6 has high ion conductivity and low impedance. The concentration of the lithium salt in the electrolyte is preferably 0.1 mol / L or more, more preferably 0.5 mol / L or more and 5 mol / L or less. When the concentration of the lithium salt in the electrolyte is within the above range, the internal impedance of the power storage device can be reduced.

[0132] Specific examples of the solid electrolyte include inorganic solid electrolyte materials, sulfide solid electrolyte materials, solid polymer materials, etc. Furthermore, the electrolyte solution may be swollen in the solid electrolytes described above.

[0133] Specific examples of the gel electrolyte include polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, etc. In addition, an organic solvent as a plasticizer may be added to the gel electrolyte described above to adjust the hardness of the gel electrolyte, and the electrolyte solution may be swollen in the gel electrolyte described above.

[0134] (1-13) Discharge capacity ratio X of lithium ion secondary battery

[0135] The discharge capacity ratio X of the lithium ion secondary battery is defined by the following formula (1).

[0136] Formula (1) X = C1 / C2

[0137] C1 in formula (1) is the discharge capacity of the single cell when charging and discharging the single cell voltage is between 2.0V and 4.3V.

[0138] C2 in formula (1) is the discharge capacity of the negative electrode during charge and discharge between 0 V vs. Li / Li+ and 3 V vs. Li / Li+. The units of C1 and C2 are mAh or Ah.

[0139] C1 in the above formula (1) is measured, for example, by the following method. A lithium-ion secondary battery is charged with a constant current-constant voltage in the following manner: first, the lithium-ion secondary battery is charged with a constant current until it reaches 4.3 V, wherein the constant current is a current that can discharge for 10±1 hours so that the voltage of the single cell changes from 4.3 V to 2.0 V, and then the battery is charged with a constant voltage of 4.3 V until the current decreases to 1 / 10 of the above constant current, and from this state, the lithium-ion secondary battery is discharged with a constant current equal to the above constant current until it reaches 2.0 V, and the discharge capacity of the single cell in the above case is taken as C1.

[0140] C2 in the above formula (1) is measured, for example, by the following method. In a single cell in which metal lithium is configured as a counter electrode of the negative electrode, constant current-constant voltage charging is performed in the following manner: first, charging is performed at a constant current until the cell voltage reaches 0 V, wherein the constant current is a current that can discharge for 10±1 hours so that the cell voltage changes from 0 V to 3.0 V, and then charging is performed at a constant voltage of 0 V until the current decreases to 1 / 10 of the above constant current, and from this state, constant current discharge is performed at a current equal to the above constant current until the cell voltage reaches 3.0 V, and the discharge capacity of the negative electrode in the above case is taken as C2.

[0141] The negative electrode to be measured may be a sample obtained from the electrode state before the single cell is produced, or may be a sample obtained after the single cell is disassembled.

[0142] Alternatively, C2 may be calculated by cutting off a portion of the negative electrode to be tested, measuring the discharge capacity, and calculating the discharge capacity per unit area and then multiplying the result by the negative electrode area in the cell.

[0143] When the power storage device disclosed in the present invention is a lithium ion secondary battery, the discharge capacity ratio X of the lithium ion secondary battery is greater than 0 and less than or equal to 0.9, and is preferably greater than 0.25 and less than 0.8, more preferably greater than 0.3 and less than 0.7, and particularly preferably greater than 0.35 and less than 0.55. By making the discharge capacity ratio X within the above range, the cycle characteristics of the lithium ion secondary battery are good and the energy density is large. In order to improve the energy density of the lithium ion secondary battery, the discharge capacity ratio X is further preferably greater than 0.5 and less than 0.9, more preferably greater than 0.6 and less than 0.88, and particularly preferably greater than 0.7 and less than 0.85. When the discharge capacity ratio X is within the above range, the energy density of the lithium ion secondary battery is further improved. In order to improve the cycle characteristics of the lithium ion secondary battery, the discharge capacity ratio X is further preferably greater than 0.1 and less than 0.6, more preferably greater than 0.2 and less than 0.6, and particularly preferably greater than 0.2 and less than 0.5. When the discharge capacity ratio X is within the above range, the cycle characteristics of the lithium ion secondary battery are further improved.

[0144] (1-14) Discharge capacity ratio Y of lithium-ion secondary battery

[0145] The discharge capacity ratio X of the lithium ion secondary battery is defined by the following formula (2).

[0146] Formula (2)Y=C3 / C2

[0147] C2 in the above formula (2) is the same as the discharge capacity C2 of the negative electrode in formula (1). C3 in the above formula (2) is the discharge capacity C3 of the negative electrode taken out from the cell when the cell voltage is 4.3V.

[0148] C3 in the above formula (2) is measured, for example, by the following method: In a single cell in which metal lithium is arranged as a negative electrode counter electrode, constant current discharge is performed until the voltage reaches 3.0 V, and the discharge capacity of the negative electrode in this case is defined as C3.

[0149] Alternatively, C3 may be calculated by cutting off a portion of the negative electrode to measure the discharge capacity, calculating the discharge capacity per unit area, and then multiplying the result by the negative electrode area in the cell.

[0150] When the power storage device of the present disclosure is a lithium ion secondary battery, the discharge capacity ratio Y of the lithium ion secondary battery is preferably 0.7 or more and 1.0 or less. When the discharge capacity ratio Y is within the above range, the lithium ion secondary battery has good cycle characteristics and high energy density.

[0151] In the manufacturing conditions of the power storage device, the discharge capacity ratio X increases as the weight per unit area of ​​the negative electrode active material increases.

[0152] (1-15) Discharge capacity ratio X of lithium ion capacitor

[0153] The discharge capacity ratio X of the lithium ion capacitor is defined by the following formula (3).

[0154] Formula (3) X = C1 / C2

[0155] C1 in the above formula (3) is the discharge capacity of the single cell when charging and discharging the single cell voltage between 2.2 V and 3.8 V. C2 in the above formula (3) is the discharge capacity of the negative electrode when charging and discharging the negative electrode between 0 V vs. Li / Li+ and 3 V vs. Li / Li+. The unit of C1 and C2 is mAh / g.

[0156] When the power storage device of the present disclosure is a lithium ion capacitor, the discharge capacity ratio X of the lithium ion capacitor is greater than 0.005 and less than 0.2. By making the discharge capacity ratio X greater than 0.005 and less than 0.2, the cycle characteristics of the lithium ion capacitor are good and the energy density of the lithium ion capacitor is large. In addition, the discharge capacity ratio X is further preferably greater than 0.007 and 0.18, and more preferably greater than 0.008 and less than 0.15. When the discharge capacity ratio X is within the above range, the cycle characteristics of the lithium ion capacitor are further improved, and the energy density of the lithium ion capacitor is further improved.

[0157] In the manufacturing conditions of the power storage device, the discharge capacity ratio X increases as the weight per unit area of ​​the negative electrode active material increases.

[0158] 2. Method for manufacturing negative electrode for power storage device

[0159] (2-1) Structure of the electrode manufacturing device 1

[0160] You can use, for example Figure 1 The electrode manufacturing apparatus 1 shown is used to manufacture a negative electrode provided in an electricity storage device (hereinafter referred to as a negative electrode for an electricity storage device).

[0161] Reference Figure 1 The structure of the electrode manufacturing device 1 is described. The electrode manufacturing device 1 has: electrolyte tanks 3, 5; a cleaning tank 7; conveying rollers 9, 11, 13, 15, 17, 19, 21, 23, 25, 27, 29, 31, 33, 35, 37, 39, 41, 43, 45 (hereinafter collectively referred to as a conveying roller group); a supply roller 47; a winding roller 49; an electrode unit 51; a porous insulating member 53; a support table 55; a circulation filter unit 57; two DC power supplies 61; and a blower 63.

[0162] The electrolyte tank 3 is a square tank with an upper opening. The bottom surface of the electrolyte tank 3 has a substantially U-shaped cross-section. The electrolyte tank 3 contains a separator 69 , four counter electrode units 51 , four porous insulating members 53 , and a conveying roller 17 .

[0163] The partition 69 is supported by a support rod 67 that passes through the upper end of the partition 69. The support rod 67 is fixed to a wall or the like that is not shown. The portion of the partition 69 other than the upper end is located in the electrolyte tank 3. The partition 69 extends in the up-down direction and divides the interior of the electrolyte tank 3 into two spaces. The conveying roller 17 is mounted on the lower end of the partition 69. The partition 69 and the conveying roller 17 are fixed by a support rod 68 that passes through the partition 69 and the conveying roller 17. In addition, a portion near the lower end of the partition 69 is cut off so as not to contact the conveying roller 17. There is a space between the conveying roller 17 and the bottom surface of the electrolyte tank 3.

[0164] The four electrode units 51 are supported by support rods 70 that penetrate the upper ends of the four electrode units 51, and the four electrode units 51 extend in the up-down direction. The support rods 70 are fixed to a wall or the like that is not shown. The portion of the electrode unit 51 other than the upper end is in the electrolyte tank 3. Two of the four electrode units 51 are arranged to sandwich the partition 69 from both sides. The remaining two electrode units 51 are arranged along the inner side surface of the electrolyte tank 3.

[0165] There is a space 71 between the counter electrode unit 51 disposed on the separator 69 side and the counter electrode unit 51 disposed along the inner side surface of the electrolyte tank 3. The counter electrode unit 51 is connected to the positive electrode of the DC power supply 61. The detailed structure of the counter electrode unit 51 will be described later.

[0166] A porous insulating member 53 is attached to the surface of each counter electrode unit 51 on the side of the space 71. The detailed structure of the porous insulating member 53 will be described later.

[0167] The cleaning tank 7 has basically the same structure as the electrolyte tank 3. However, the counter electrode unit 51 and the porous insulating member 53 are not present in the cleaning tank 7.

[0168] The electrolytic solution tank 5 has basically the same structure as the electrolytic solution tank 3. However, the electrolytic solution tank 5 does not include the conveying roller 17, but includes a conveying roller 27.

[0169] The conveying roller group conveys the electrode 73 described later along a predetermined path. The path is a path that starts from the supply roller 47 and passes through the electrolyte tank 3, the electrolyte tank 5, and the cleaning tank 7 in order to reach the winding roller 49.

[0170] The portion of the path that passes through the electrolyte tank 3 is the following path: first, it moves downward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 3 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53, then the moving direction is changed to an upward direction by the conveying roller 17, and finally, it moves upward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 3 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53.

[0171] In addition, the portion of the above-mentioned path that passes through the electrolyte tank 5 is the following path: first, it moves downward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 5 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53, then, the moving direction is changed to an upward direction by the conveying roller 27, and finally, it moves upward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 5 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53.

[0172] In addition, the portion of the above-mentioned path passing through the cleaning tank 7 is the following path: first, it moves downward between the inner side surface of the cleaning tank 7 and the partition 69, then the moving direction is changed to an upward direction by the conveying roller 37, and finally, it moves upward between the inner side surface of the cleaning tank 7 and the partition 69.

[0173] The conveying rollers 15, 21, 25, 29 in the conveying roller group are formed of a conductive material. In addition, the conveying rollers 15, 21, 25, 29 are connected to the negative electrode of the DC power supply 61. The conveying roller 13 pushes the electrode 73 in the direction of the conveying roller 15. The conveying roller 19 pushes the electrode 73 in the direction of the conveying roller 21. The conveying roller 23 pushes the electrode 73 in the direction of the conveying roller 25. The conveying roller 31 pushes the electrode 73 in the direction of the conveying roller 29. The conveying roller group corresponds to the conveying unit. The conveying rollers 15, 21, 25, 29 are conductive conveying rollers, corresponding to the connecting unit.

[0174] The conveying rollers 13, 19, 23, 31 are formed of elastomer except for the bearing portion. That is, the conveying rollers 13, 19, 23, 31 are formed of elastomer including their surfaces. Elastomer is an example of an elastic body. Therefore, the conveying rollers 13, 19, 23, 31 can be elastically deformed.

[0175] The elastomer may be natural rubber or synthetic rubber. Examples of the elastomer include EPDM, EPR, SBR, NBR, isoprene rubber, butadiene rubber, acrylic rubber, chloroprene rubber, silicone rubber, urethane rubber, and fluororubber.

[0176] The electrode 73 is wound around the outer periphery of the supply roller 47. That is, the supply roller 47 holds the electrode 73 in a wound state. The conveying roller group pulls out the electrode 73 held by the supply roller 47 and conveys it.

[0177] The winding roll 49 winds up and stores the negative electrode 75 for the power storage device conveyed by the conveying roll group. The negative electrode 75 for the power storage device is a negative electrode produced by doping the electrode 73 with lithium in the electrolytic solution tanks 3 and 5 .

[0178] Furthermore, as a method of lithium doping, lithium may be doped into an active material in an ionic state, a method of forming a lithium alloy, or a method of consuming lithium ions in the form of a SEI (Solid Electrolyte Interface) film.

[0179] As described above, the electrode unit 51 is accommodated in the electrolyte tank 3, 5. The electrode unit 51 has a plate-like shape. The electrode unit 51 has a structure in which a conductive substrate and a lithium-containing plate are stacked. As the material of the conductive substrate, copper, stainless steel, nickel, etc. can be cited, for example. The form of the lithium-containing plate is not particularly limited, and for example, a lithium plate, a lithium alloy plate, etc. can be cited. The thickness of the lithium-containing plate can be, for example, 0.03 mm or more and 3 mm or less.

[0180] The porous insulating member 53 has a plate-like shape. The porous insulating member 53 is mounted on the surface of the counter electrode unit 51. The plate-like shape of the porous insulating member 53 refers to the shape when the porous insulating member 53 is mounted on the surface of the counter electrode unit 51. The porous insulating member 53 may be a member that maintains a predetermined shape itself, or may be a member that can be easily deformed, such as a mesh.

[0181] The porous insulating member 53 does not contact the electrode 73 conveyed by the conveying roller group. The shortest distance from the surface of the porous insulating member 53 to the electrode 73 is preferably in the range of 0.5 mm to 100 mm, and more preferably in the range of 1 mm to 10 mm. The shortest distance refers to the distance between the point on the surface of the porous insulating member 53 closest to the electrode 73 and the electrode 73.

[0182] The porous insulating member 53 is porous, so that a doping solution described later can pass through the porous insulating member 53. Thus, the counter electrode unit 51 can come into contact with the doping solution.

[0183] As the porous insulating member 53, for example, a mesh made of resin can be mentioned. As the resin, for example, polyethylene, polypropylene, nylon, polyetheretherketone, polytetrafluoroethylene, etc. can be mentioned.

[0184] The mesh size of the sieve can be appropriately set, and the mesh size of the sieve can be set, for example, to be greater than 0.1 μm and less than 10 mm, preferably greater than 0.1 mm and less than 5 mm. The thickness of the sieve can be appropriately set. The thickness of the sieve can be set, for example, to be greater than 1 μm and less than 10 mm, preferably greater than 30 μm and less than 1 mm. The opening rate of the sieve can be appropriately set. The opening rate of the sieve can be set, for example, to be greater than 5% and less than 95%, preferably greater than 50% and less than 95%.

[0185] The porous insulating member 53 may be formed entirely of an insulating material, or may include a layer having insulating properties in part.

[0186] The support stand 55 supports the electrolyte tanks 3 and 5 and the cleaning tank 7 from below. The height of the support stand 55 can be changed. If the support stand 55 is lowered while the positions of the partition 69, the counter electrode unit 51, and the porous insulating member 53 in the vertical direction are maintained, the electrolyte tanks 3 and 5 can be moved downward relative to the partition 69, the counter electrode unit 51, and the porous insulating member 53. In addition, if the support stand 55 is raised, the electrolyte tanks 3 and 5 can be moved upward relative to the partition 69, the counter electrode unit 51, and the porous insulating member 53.

[0187] The circulation filtering unit 57 is respectively disposed on the electrolyte tanks 3 and 5. The circulation filtering unit 57 includes a filter 81, a pump 83, and a pipeline 85.

[0188] In the circulation filtration unit 57 provided in the electrolyte tank 3, the pipeline 85 is a circulation pipeline which starts from the electrolyte tank 3 and then passes through the pump 83 and the filter 81 in sequence and returns to the electrolyte tank 3. The driving force of the pump 83 is used to circulate the doping solution in the electrolyte tank 3 in the pipeline 85 and the filter 81 and returns to the electrolyte tank 3 again. At this time, foreign matter in the doping solution is filtered by the filter 81. Examples of foreign matter include foreign matter precipitated from the doping solution and foreign matter generated by the electrode 73. In addition, for the sake of convenience, Figure 1 The doping solution is omitted in the figure.

[0189] In the circulation filtration unit 57 provided in the electrolyte tank 5, the pipeline 85 is a circulation pipeline starting from the electrolyte tank 5, passing through the pump 83 and the filter 81 in sequence, and returning to the electrolyte tank 5. The driving force of the pump 83 is used to circulate the doping solution in the electrolyte tank 5 in the pipeline 85 and the filter 81, and then returns to the electrolyte tank 5 again. The circulation filtration unit 57 provided in the electrolyte tank 5 also has the same effect as the circulation filtration unit 57 provided in the electrolyte tank 3.

[0190] The material of the filter 81 may be, for example, a resin such as polypropylene or polytetrafluoroethylene. The pore size of the filter 81 may be set appropriately. The pore size of the filter 81 is, for example, not less than 30 μm and not more than 50 μm.

[0191] The negative terminal of one of the two DC power supplies 61 (hereinafter referred to as one DC power supply 61) is connected to the conveying rollers 15 and 21, respectively. In addition, the positive terminal of the DC power supply 61 on one side is connected to a total of four counter electrode units 51. These four counter electrode units 51 are the counter electrode units 51 in the electrolyte tank 3. The electrode 73 is in contact with the conductive conveying rollers 15 and 21. In addition, the electrode 73 and the counter electrode unit 51 in the electrolyte tank 3 are in the doping solution as the electrolyte. Therefore, the electrode 73 and the counter electrode unit 51 in the electrolyte tank 3 are electrically connected.

[0192] The negative terminal of the other of the two DC power supplies 61 (hereinafter referred to as the other DC power supply 61) is connected to the conveying rollers 25 and 29, respectively. In addition, the positive terminal of the other DC power supply 61 is connected to a total of four counter electrode units 51. These four counter electrode units 51 are the counter electrode units 51 in the electrolyte tank 5. The electrode 73 is in contact with the conductive conveying rollers 25 and 29. In addition, the electrode 73 and the counter electrode unit 51 in the electrolyte tank 5 are in the doping solution as the electrolyte. Therefore, the electrode 73 and the counter electrode unit 51 in the electrolyte tank 5 are electrically connected.

[0193] The blower 63 blows gas toward the negative electrode 75 for the storage device coming out of the cleaning tank 7 to vaporize the cleaning liquid, thereby drying the negative electrode 75 for the storage device. The gas used is preferably a gas that is inert to the active material doped with lithium. Examples of such gases include helium, neon, argon, and dehumidified air from which water has been removed.

[0194] (2-2) Structure of the electrode 73

[0195] Reference Figure 2A as well as Figure 2B The structure of the electrode 73 is described below. The electrode 73 is a long strip-shaped component. Figure 2BAs shown, the electrode 73 includes a negative electrode current collector 93 and a negative electrode active material layer 95. The negative electrode active material layer 95 is formed on both surfaces of the negative electrode current collector 93. The negative electrode active material layer 95 in the electrode 73 is not yet doped with lithium.

[0196] The negative electrode active material layer 95 can be formed by applying the negative electrode slurry onto the negative electrode collector 93 . Alternatively, the negative electrode slurry can be formed into a sheet and the sheet can be attached to the negative electrode collector 93 .

[0197] (2-3) Method for doping negative electrode for power storage device

[0198] The electrode 73 is wound around the supply roll 47. The electrolyte tanks 3 and 5 contain a doping solution. The doping solution contains lithium ions and a solvent. Examples of the solvent include organic solvents. As the organic solvent, an aprotic organic solvent is preferred.

[0199] As aprotic organic solvent, for example, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, 1-fluoroethylene carbonate, γ-butyrolactone, acetonitrile, dimethoxyethane, tetrahydrofuran, dioxolane, methylene dichloride, sulfolane, diethylene glycol dimethyl ether (diglyme), diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether (triglyme), triethylene glycol methyl butyl ether, tetraethylene glycol dimethyl ether (tetraglyme), and ionic liquids etc. can be enumerated. As ionic liquid, for example, quaternized imidazolium salt, quaternized pyridinium salt, quaternized pyrrolidinium salt, quaternized piperidinium salt etc. can be enumerated. The above-mentioned organic solvent can be composed of a single component, or it can be a mixed solvent of more than two components.

[0200] The lithium ions contained in the above-mentioned doping solution are ions constituting lithium salts. Examples of the anion portion constituting the lithium salt include PF6 - PF3(C2F5)3 - PF3(CF3)3 - Phosphorus anions with fluorine groups, such as BF4 - 、BF2(CF)2 - 、BF3(CF3) - 、B(CN)4 - Boron anions with fluorine or cyanide groups, such as N(FSO2)2 - 、N(CF3SO2)2 - 、N(C2F5SO2)2 - Sulfonyl imide anions with fluorine groups, such as CF3SO3 - Such as organic sulfonic acid anions having a fluorine group.

[0201] The concentration of the lithium salt in the doping solution is preferably 0.1 mol / L or more, more preferably 0.5 mol / L or more and 5 mol / L or less. When the concentration of the lithium salt in the doping solution is within the above range, lithium doping can be performed efficiently.

[0202] The doping solution may further contain additives such as vinylene carbonate, vinyl ethylene carbonate, 1-fluoroethylene carbonate, 1-(trifluoromethyl)ethylene carbonate, anhydrous succinic acid, anhydrous maleic acid, propane sultone, diethyl sulfone, and the like.

[0203] In addition, a cleaning liquid is contained in the cleaning tank 7. The cleaning liquid preferably contains, for example, an aprotic solvent. Examples of the aprotic solvent include, for example, at least one selected from carbonate solvents, ester solvents, ether solvents, hydrocarbon solvents, ketone solvents, nitrile solvents, sulfur-containing solvents, and amide solvents.

[0204] The cleaning liquid may be substantially composed of an aprotic solvent, or may contain other components in addition to the aprotic solvent. The boiling point of the aprotic solvent is preferably 30° C. or higher and 200° C. or lower, more preferably 40° C. or higher and 150° C. or lower, and more preferably 50° C. or higher and 120° C. or lower. By setting the boiling point to 30° C. or higher, excessive evaporation of the cleaning liquid in the cleaning tank 7 can be suppressed. By setting the boiling point to 200° C. or lower, the cleaning liquid can be easily removed from the negative electrode 75 for the power storage device after cleaning.

[0205] The composition of the doping solution contained in the electrolyte tank 3 is preferably different from that of the doping solution contained in the electrolyte tank 5. When the composition of the doping solution contained in the electrolyte tank 3 is different from that of the doping solution contained in the electrolyte tank 5, a higher quality negative electrode 75 for a power storage device can be efficiently manufactured.

[0206] Examples of the different compositions of the doping solutions in the electrolyte tanks 3 and 5 include a case where the concentration of the SEI film forming component in the doping solution contained in the electrolyte tank 3 is higher than the concentration of the SEI film forming component in the doping solution contained in the electrolyte tank 5 .

[0207] Next, the electrode 73 is pulled out from the supply roller 47 by the conveying roller group and conveyed along the above-mentioned path. When the electrode 73 passes through the electrolyte tanks 3 and 5 , lithium is doped into the active material included in the negative electrode active material layer 95 .

[0208] The lithium doping step described above corresponds to the doping step. The current density of the first doping step performed in the electrolyte tank 3 is preferably different from the current density of the second doping step performed in the electrolyte tank 5. In this case, a higher quality negative electrode 75 for a power storage device can be efficiently manufactured.

[0209] As a form in which the current density of the first doping step is different from the current density of the second doping step, for example, the current density in the first doping step is higher or lower than the current density in the second doping step, etc. The difference between the current density in the first doping step and the current density in the second doping step corresponds to the difference between the conditions for doping lithium into the active material in the first doping step and the conditions for doping lithium into the active material in the second doping step.

[0210] In addition, when the electrode unit 51 contained in the electrolyte tank 3, 5 has a conductive substrate and a lithium-containing plate arranged on the conductive substrate, the mass of lithium contained in the lithium-containing plate contained in the electrolyte tank 3 may be different from the mass of lithium contained in the lithium-containing plate contained in the electrolyte tank 5.

[0211] As a form in which the masses of lithium contained in the lithium-containing plates contained in the electrolyte tanks 3 and 5 are different from each other, for example, the mass of lithium contained in the lithium-containing plates contained in the electrolyte tank 3 is greater than or less than the mass of lithium contained in the lithium-containing plates contained in the electrolyte tank 5. The mass of lithium contained in the lithium-containing plates contained in the electrolyte tank 3 is different from the mass of lithium contained in the lithium-containing plates contained in the electrolyte tank 5, which corresponds to the difference between the conditions for doping lithium into the active material in the first doping step and the conditions for doping lithium into the active material in the second doping step.

[0212] By doping the negative electrode active material with lithium, the electrode 73 is formed into a negative electrode 75 for a storage device. The negative electrode 75 for a storage device is transported by a transport roller group and cleaned in a cleaning tank 7. Finally, the negative electrode 75 for a storage device is wound on a winding roller 49. The negative electrode 75 for a storage device has the same structure as the electrode 73 except that lithium is doped in the negative electrode active material.

[0213] The electrode manufacturing apparatus 1 is particularly suitable for manufacturing a negative electrode for an electric storage device included in a lithium ion capacitor or a lithium ion secondary battery.

[0214] The doping ratio of lithium doped into the negative electrode active material layer is preferably 5% or more and 95% or less of the discharge capacity C2 of the negative electrode. In this case, the negative electrode capacity and cycle durability are improved. The discharge capacity C2 of the negative electrode is the discharge capacity of the negative electrode when the negative electrode is charged and discharged between 0V vs. Li / Li+ and 3V vs. Li / Li+.

[0215] 3. Battery manufacturing method

[0216] The method for producing a battery disclosed herein is a method for producing a battery including a positive electrode, a negative electrode, and an electrolyte, and includes a step of producing a negative electrode for an electricity storage device by using the above-mentioned "2. Method for producing a negative electrode for an electricity storage device".

[0217] The basic structure of the positive electrode constituting the battery may be a common structure. As the positive electrode active material, in addition to the positive electrode active materials already exemplified, an organic active material such as a nitroxide radical compound or oxygen may be used.

[0218] The electrolyte constituting the battery is usually in the form of a liquid electrolyte. The basic composition of the electrolyte is the same as that of the above-mentioned doping solution. In addition, the concentration of lithium ions and the concentration of lithium salts in the electrolyte are preferably 0.1 mol / L or more, more preferably 0.5 mol / L or more and 5.0 mol / L or less. The electrolyte may have a gel-like or solid form to prevent leakage.

[0219] The battery may have a separator between the positive electrode and the negative electrode for preventing the positive electrode from physically contacting the negative electrode. Examples of the separator include nonwoven fabrics or porous films made of cellulose / rayon, polyethylene, polypropylene, polyamide, polyester, polyimide, and the like.

[0220] As a battery structure, for example, the following stacked unit can be cited, which is formed by stacking more than three plate-shaped constituent units to form a stacked body and sealing the stacked body in an outer film, wherein the constituent unit includes a positive electrode and a negative electrode, and a separator between the positive electrode and the negative electrode.

[0221] The battery can be manufactured, for example, by forming a basic structure including at least a negative electrode and a positive electrode, and injecting an electrolyte into the basic structure.

[0222] 4. Manufacturing method of capacitor

[0223] The method for producing a capacitor disclosed herein is a method for producing a capacitor including a positive electrode, a negative electrode, and an electrolyte, and includes the step of producing a negative electrode for an electric storage device by using the above-mentioned "2. Method for producing a negative electrode for an electric storage device".

[0224] The basic structure of the positive electrode constituting the capacitor may be a common structure. As the positive electrode active material, activated carbon is preferably used.

[0225] The electrolyte constituting the capacitor is usually in the form of a liquid electrolyte. The basic composition of the electrolyte is the same as that of the above-mentioned doping solution. In addition, the concentration of lithium ions and the concentration of lithium salts in the electrolyte are preferably 0.1 mol / L or more, more preferably 0.5 mol / L or more and 5.0 mol / L or less. The electrolyte may have a gel or solid form to prevent leakage.

[0226] The capacitor may have a separator between the positive electrode and the negative electrode to prevent the positive electrode from physically contacting the negative electrode. Examples of the separator include nonwoven fabrics or porous films made of cellulose rayon, polyethylene, polypropylene, polyamide, polyester, polyimide, and the like.

[0227] As the structure of the capacitor, for example, the following stacked unit can be listed, which is formed by stacking more than three plate-shaped constituent units to form a stacked body and sealing the stacked body in an outer film, wherein the constituent unit includes a positive electrode and a negative electrode, and a separator between the positive electrode and the negative electrode.

[0228] In addition, as the structure of the capacitor, for example, the following wound unit can also be listed, which is formed by winding a strip-shaped constituent unit to form a stack, and storing the stack in a square or cylindrical container, wherein the constituent unit includes a positive electrode and a negative electrode, and a separator between the positive electrode and the negative electrode.

[0229] The capacitor can be manufactured, for example, by forming a basic structure including at least a negative electrode and a positive electrode, and injecting an electrolyte into the basic structure.

[0230] In the case of a lithium ion capacitor, the density of the negative electrode active material layer is preferably 0.50 g / cm 3 Above and 1.50g / cm 3 Below, especially preferably 0.70g / cm 3 Above and 1.20g / cm 3 the following.

[0231] 5. Examples 1 to 6 and Comparative Examples 1 to 3

[0232] (5-1) Production of Negative Electrode for Power Storage Device of Example 1

[0233] A negative electrode slurry was prepared by mixing 31 parts by mass of SiO, 62 parts by mass of artificial graphite, 4 parts by mass of acetylene black powder, 2 parts by mass of SBR binder, 1 part by mass of carboxymethyl cellulose, and 85 parts by mass of ion exchange water in a planetary mixer. Acetylene black corresponds to a conductive agent.

[0234] A long strip-shaped negative electrode current collector was prepared. The dimensions of the negative electrode current collector were: width 150 mm, length 500 m, thickness 8 μm. The surface roughness Ra of the negative electrode current collector was 0.1 μm. The negative electrode current collector was made of copper foil.

[0235] like Figure 2B As shown, the negative electrode slurry is applied to both surfaces of the negative electrode collector 93 using a comma scraper, thereby forming negative electrode active material layers 95 on both surfaces of the negative electrode collector 93, and drying under reduced pressure at 120°C for 12 hours. Thus, the electrode 73 as the negative electrode is obtained. Next, the electrode is pressed using a roller press to obtain a negative electrode 75 for a storage device. The total unit area weight of the negative electrode active material layer 95 formed on both surfaces of the negative electrode is 130 g / m 2. In addition, the thickness of the negative electrode active material layer 95 formed on both surfaces of the negative electrode is 87μm in total. The negative electrode active material layer 95 is formed along the length direction of the negative electrode collector 93. The negative electrode active material layer 95 is formed at the central part of the negative electrode collector 93 in the width direction, and the width of the negative electrode active material layer 95 is 120mm. The negative electrode active material layer unformed portion at both ends of the negative electrode collector 93 in the width direction is 15mm respectively. The negative electrode active material layer unformed portion is a portion where the negative electrode active material layer 95 is not formed.

[0236] (Measurement of the charge capacity, discharge capacity, and irreversible capacity per unit area of ​​the negative electrode)

[0237] From the prepared electrode 73, a piece of 1.5 cm×2.0 cm (area 3.0 cm 2 ) for measurement. Prepare a sample with a longitudinal and lateral size of 1.5 cm × 2.0 cm (area 3.0 cm 2 ) and 200μm thick metal lithium was used as the counter electrode of the sample. In addition, a non-woven fabric made of polyethylene with a thickness of 50μm was prepared as a separator. Counter electrodes were arranged on both surfaces of the sample with a separator between them, and a metal lithium plate was provided as a reference electrode. A mixed solution containing 1.4M LiPF6 and ethylene carbonate, 1-fluoroethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:2:7 was used as an electrolyte, and a coin-type single cell for negative electrode evaluation was prepared with the above configuration.

[0238] The coin-type battery prepared is charged with constant current-constant voltage in the following manner. First, the coin-type battery prepared is charged with a charging current of 4mA until it reaches 0V, and then charged with a constant voltage of 0V until the charging current decreases to 0.4mA. The charging capacity obtained is divided by the area of ​​the measurement sample to calculate the charging capacity per unit area. Next, a constant current discharge is performed with a discharge current of 4mA until the battery voltage reaches 3.0V, and the discharge capacity obtained is divided by the area of ​​the measurement sample to calculate the discharge capacity per unit area. In addition, the discharge capacity per unit area calculated here is the same as the discharge capacity per unit area calculated when calculating the discharge capacity C2 of the negative electrode described later. In addition, the difference between the charge capacity and the discharge capacity per unit area is calculated as the irreversible capacity. The results are shown in Table 1.

[0239] Next, the counter electrode unit is made in the following manner. First, a long copper plate with a thickness of 2 mm is prepared. A lithium metal plate is pasted to the copper plate. The dimensions of the lithium metal plate are: width 120 mm, length 800 mm, thickness 1 mm. The lithium metal plate is pasted along the length direction of the copper plate. The copper plate with the lithium metal plate pasted as above is used as the counter electrode unit 51. Eight identical counter electrode units 51 are manufactured.

[0240] Prepare Figure 1 The electrode manufacturing device 1 shown in the figure is provided with an electrode 73 and a counter electrode unit 51. Then, an electrolyte is supplied into the electrode manufacturing device 1. The electrolyte is a solution containing 1.4M LiPF6. The solvent of the electrolyte is a mixed solvent containing ethylene carbonate, 1-fluoroethylene carbonate, and ethyl methyl carbonate in a volume ratio of 1:2:7.

[0241] Next, the electrode 73 and the counter electrode unit 51 provided on the electrode manufacturing apparatus 1 were connected to a DC power supply with a current and voltage monitor, and the electrode 73 was transported at a speed of 0.1 m / min while a current of 5 A was supplied. The power supply time was set to a time for the lithium doping ratio per unit area to reach 26% of the discharge capacity per unit area calculated above.

[0242] In this step, the negative electrode active material in negative electrode active material layer 95 is doped with lithium, so that electrode 73 is formed as negative electrode 75 for power storage device. The negative electrodes for power storage devices in this embodiment and embodiments 2 to 6 and comparative examples 1 to 3 described later are negative electrodes for lithium ion secondary batteries.

[0243] After the negative electrode 75 for an electric storage device was passed through the cleaning tank 7, the negative electrode 75 for an electric storage device was wound. DMC (dimethyl carbonate) was contained in the cleaning tank 7 at 25° C. In the above manner, the negative electrode 75 for an electric storage device was manufactured.

[0244] Table 1 shows the negative electrode collector aperture ratio, the thickness of the negative electrode collector, the unit weight of the negative electrode active material layer, the thickness of the negative electrode active material layer, the charge capacity per unit area of ​​the negative electrode, the discharge capacity, the irreversible capacity, and the doping ratio of lithium doped into the negative electrode active material layer of the negative electrode 75 for the power storage device of Example 1. In addition, Table 1 also shows the above-mentioned numerical values ​​of Examples 2 to 6 and Comparative Examples 1 to 3 described later.

[0245]

Table 1

[0246]

[0247] (5-2) Production of Negative Electrodes for Power Storage Devices of Examples 2 to 6 and Comparative Examples 1 to 3

[0248] The negative electrodes for storage devices of Examples 2 to 6 and Comparative Examples 1 to 3 were manufactured and evaluated in the same manner as Example 1, except that the weight per unit area of ​​the negative electrode active material layer, the thickness of the negative electrode active material layer, and the doping ratio of lithium into the negative electrode active material layer shown in Table 1 were different.

[0249] (5-3) Evaluation of negative electrodes for power storage devices

[0250] The evaluation was performed when the negative electrode for the power storage device of Example 1 was used as the negative electrode of the lithium ion secondary battery. Specifically, the single cell discharge capacity C1, the negative electrode discharge capacity C2, the discharge capacity ratio X, the negative electrode discharge capacity C3, the discharge capacity ratio Y, the weight energy density, and the capacity retention rate (%) after 200 cycles were measured. The results of the measurement are shown in Table 2.

[0251]

Table 2

[0252]

[0253] The measurement methods of the initial capacity and the capacity retention rate after 200 cycles are as follows.

[0254] (5-4) Preparation of single cell for evaluation

[0255] A positive electrode slurry was prepared by fully mixing 93 parts by mass of lithium nickel-manganese-cobalt oxide, 3 parts by mass of acetylene black powder, 4 parts by mass of polyvinylidene fluoride binder, and 62 parts by mass of N-methylpyrrolidone in a planetary mixer.

[0256] A long strip-shaped positive electrode current collector was prepared. The dimensions of the positive electrode current collector were: 150 mm in width, 500 m in length, and 15 μm in thickness. The positive electrode current collector was made of aluminum foil.

[0257] The positive electrode slurry was applied to both surfaces of the positive electrode collector using a comma scraper, thereby forming a positive electrode active material layer on both surfaces of the positive electrode collector, and dried under reduced pressure at 120°C for 12 hours. Next, the electrode was pressed using a roller press to obtain a positive electrode. The total unit area weight of the positive electrode active material layer formed on both surfaces of the positive electrode was 440 g / m 2 , with a total thickness of 163 μm. The positive electrode active material layer is formed along the length direction of the positive electrode collector. The positive electrode active material layer is formed at the central portion of the positive electrode collector in the width direction, and the width of the positive electrode active material layer is 120 mm. The positive electrode active material layer-unformed portions at both ends of the positive electrode collector in the width direction are 15 mm respectively. The positive electrode active material layer-unformed portion is a portion where the positive electrode active material layer is not formed.

[0258] Thirty pieces of negative electrodes with a size of 10.0 cm × 12.9 cm (excluding the terminal welding portion) were cut from the negative electrode for the power storage device prepared in (5-1) above. In addition, 29 pieces of positive electrodes with a size of 9.7 cm × 12.6 cm (excluding the terminal welding portion) were cut from the positive electrode prepared above. The positive electrode collector was composed of aluminum foil.

[0259] Then, the positive electrode and the negative electrode were alternately stacked through a 16 μm thick polyethylene nonwoven fabric, thereby producing an electrode unit consisting of a laminate. At this time, the positive electrode and the negative electrode were aligned so that the coating portion of the positive electrode overlapped with the coating portion of the negative electrode and the terminal welding portion of the positive electrode collector and the terminal welding portion of the negative electrode collector were on opposite sides of each other. In this state, the separator, the negative electrode, the separator, and the positive electrode were stacked in this order, and the four sides of the stack were fixed with tape to produce an electrode unit. And the negative electrode was arranged at the outermost part of the electrode unit.

[0260] A rectangular aluminum positive electrode power supply tab with a sealing film pre-heat-fused to the sealing portion was stacked and welded to the terminal welding portion of each of the 28 positive electrodes of the manufactured electrode unit. On the other hand, a rectangular nickel negative electrode power supply tab with a sealing film pre-heat-fused to the sealing portion was stacked and welded to the terminal welding portion of each of the 29 negative electrodes of the electrode stack unit, thereby manufacturing an evaluation single cell.

[0261] The following first laminate film and second laminate film are prepared as laminate films for accommodating electrode units, wherein the first laminate film and the second laminate film are subjected to deep drawing so that the central portion is large enough to accommodate a single cell element for evaluation. The first laminate film and the second laminate film each have a structure formed by stacking a polypropylene layer, an aluminum layer, and a nylon layer. Next, the electrode unit is arranged in the central portion of the second laminate film so that the positive electrode terminal and the negative electrode terminal each protrude to the outside of the second laminate film. Then, the second laminate film is overlapped in such a manner as to clamp the electrode unit. Thereafter, three sides of the first laminate film and the second laminate film (including two sides protruding from the positive electrode terminal and the negative electrode terminal) are welded. As a result, a laminate film bag with only one side open is formed. The electrode unit is contained in the laminate film bag.

[0262] Next, the laminated film bag was vacuum impregnated with an electrolyte. The electrolyte was a mixed solution containing 1.4M LiPF6 and ethylene carbonate, 1-fluoroethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:2:7. Next, the remaining open side of the laminated film bag was welded. The evaluation single cell was made through the above process.

[0263] (5-5) Production of Evaluation Cells of Examples 2 to 6 and Comparative Examples 1 to 3

[0264] The negative electrode prepared in (5-2) was used as the negative electrode of Examples 2 to 6 and Comparative Examples 1 to 3, and evaluation cells were prepared in the same manner as in Example 1. However, the values ​​of the weight per unit area of ​​the positive electrode active material layer shown in Table 2 were different.

[0265] (5-6) Evaluation using evaluation cells

[0266] (Initial evaluation)

[0267] The evaluation cell was charged with a constant current-constant voltage as follows: the evaluation cell was charged at a constant current of 2.5 A until the cell voltage reached 4.3 V, and then charged at a constant voltage of 4.3 V until the current decreased to 0.25 A. Next, the cell was discharged at a constant current of 2.5 A until the cell voltage reached 2.0 V. The above charge and discharge were repeated twice, and the discharge capacity of the second discharge was measured. The measured value was taken as the initial discharge capacity C1.

[0268] Furthermore, the weight energy density (Wh / kg) of the cell was calculated based on the following formula (5) from the initial discharge capacity, the cell weight, and the average voltage during discharge.

[0269] Formula (5)

[0270] Gravimetric energy density (Wh / kg) = (initial discharge capacity × average cell voltage during discharge) / cell weight

[0271] (Calculation of C2 and C3)

[0272] The prepared evaluation cell was charged at a constant current of 2.5 A until the cell voltage reached 4.3 V. The charged evaluation cell was disassembled and the negative electrode was taken out. Then, the negative electrode was immersed in a container containing dehydrated ethyl methyl carbonate in an argon-substituted glove box and washed at 25° C. for 10 minutes while stirring with a stirrer. After repeating this washing three times, a drying treatment was performed at 25° C. for 1 hour.

[0273] Then, a piece of 1.5 cm × 2.0 cm (area 3.0 cm) was cut from the dried negative electrode. 2 ) for measurement. Prepare a sample with a vertical dimension of 1.5 cm × 2.0 cm (area 3.0 cm 2) and a metal lithium with a thickness of 200μm was used as the counter electrode of the sample. In addition, a polyethylene nonwoven fabric with a thickness of 50μm was prepared as a separator. Counter electrodes were arranged on both surfaces of the sample with a separator between them, and a metal lithium plate was provided as a reference electrode. The following mixed solution was used as an electrolyte: containing 1.4M LiPF6, and containing ethylene carbonate, 1-fluoroethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:2:7, thereby making a coin-type single cell for negative electrode evaluation having the above structure.

[0274] The coin-type cell thus prepared was discharged at a constant current of 4 mA until the cell voltage reached 3.0 V, and the obtained discharge capacity was divided by the area of ​​the measurement sample to calculate the discharge capacity per unit area.

[0275] And the discharge capacity C3 of the negative electrode is calculated based on the following formula (5).

[0276] Formula (5)

[0277] C3 = discharge capacity per unit area × negative electrode area in a single cell

[0278] Next, constant current-constant voltage charging was performed as follows: first, charging was performed at a charging current of 4 mA until the voltage reached 0 V, and then charging was performed at a voltage of 0 V until the charging current decreased to 0.4 mA. Next, constant current discharge was performed at a discharge current of 4 mA until the cell voltage reached 3.0 V, and the discharge capacity obtained was divided by the area of ​​the measurement sample to calculate the discharge capacity per unit area. The discharge capacity C2 of the negative electrode was calculated based on the following formula (6).

[0279] Formula (6)

[0280] C2 = discharge capacity per unit area × negative electrode area in the single cell

[0281] And, the discharge capacity ratio Y defined by the following formula (2) is calculated.

[0282] Formula (2)Y=C3 / C2

[0283] (Capacity retention after 200 cycles)

[0284] Next, the evaluation cell was charged at a constant current of 25 A until the cell voltage reached 4.3 V. Then, the cell was discharged at a constant current of 25 A until the cell voltage reached 2.0 V. The above cycle was repeated 200 times.

[0285] Next, the evaluation cell was charged with a constant current-constant voltage as follows: first, the evaluation cell was charged at a constant current of 2.5A until the cell voltage reached 4.3V. Then, a constant voltage of 4.3V was applied for charging until the charging current decreased to 0.25A. Thereafter, the cell was discharged at a constant current of 2.5A until the cell voltage reached 2.0V. The above charge and discharge were repeated twice, and the discharge capacity of the second discharge was measured. The measured value was taken as the discharge capacity after 200 cycles. The capacity retention rate (%) after 200 cycles was calculated based on the following formula (7).

[0286] Formula (7)

[0287] Capacity retention after 200 cycles (%) = (discharge capacity after 200 cycles / initial discharge capacity) × 100

[0288] In the evaluation cells of each embodiment, the initial cell discharge capacity is high and the weight energy density is large, and the capacity retention rate after 200 cycles is high. In addition, the capacity retention rate after 200 cycles of the evaluation cells of Examples 2, 3, and 6 is particularly high. In addition, the weight energy density of the evaluation cells of Examples 1 and 5 is particularly high. However, the initial cell discharge capacity of the negative electrode for the storage device of Comparative Examples 1 to 3 is low, the weight energy density is small, and the capacity retention rate after 200 cycles is low.

[0289] 6. Examples 7 to 11 and Comparative Examples 4 to 6

[0290] (6-1) Production of Negative Electrode for Power Storage Device of Example 7

[0291] Prepare a long strip-shaped negative electrode collector. The dimensions of the negative electrode collector are: width 150 mm, length 100 m, thickness 8 μm. The surface roughness Ra of the negative electrode collector is 0.1 μm. The negative electrode collector is made of copper foil. Figure 2B As shown, negative electrode active material layers 95 are formed on both surfaces of the negative electrode collector 93, respectively, to obtain the electrode 73. The thickness of the negative electrode active material layer 95 is 80 μm. The negative electrode active material layer 95 is formed along the length direction of the negative electrode collector 93. The negative electrode active material layer 95 is formed at the center of the negative electrode collector 93 in the width direction, and the width of the negative electrode active material layer 95 is 120 mm. The negative electrode active material layer unformed portions at both ends of the negative electrode collector 93 in the width direction are 15 mm respectively. The negative electrode active material layer unformed portion is a portion where the negative electrode active material layer 95 is not formed.

[0292] Negative electrode active material layer 95 contains graphite, carboxymethyl cellulose, acetylene black, a binder, and a dispersant at a mass ratio of 88:3:5:3:1. Graphite corresponds to the negative electrode active material and to the carbon-based material. Acetylene black corresponds to the conductive agent.

[0293] Next, a lithium electrode was manufactured as follows. First, a long copper plate with a thickness of 2 mm was prepared. A lithium metal plate was pasted onto the copper plate. The lithium metal plate was 120 mm in width × 800 mm in length and 1 mm in thickness. The lithium metal plate was pasted along the length direction of the copper plate. The copper plate with the lithium metal plate pasted thereon was used as a counter electrode unit 51. Eight identical counter electrode units 51 were manufactured.

[0294] Prepare Figure 1 The electrode manufacturing device 1 shown in the figure is provided with an electrode 73 and a counter electrode unit 51. Then, an electrolyte is supplied into the electrode manufacturing device 1. The electrolyte is a solution containing 1.2M LiPF6. The solvent of the electrolyte is a mixed solvent containing ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a volume ratio of 3:4:3.

[0295] Next, the electrode 73 and the electrode unit 51 provided on the electrode manufacturing device 1 are connected to a DC power supply with a current and voltage monitor, and the electrode 73 is conveyed at a speed of 0.16 m / min and a current of 40 A is connected at the same time. Taking into account the irreversible capacity, the power-on time is set to a time in which the doping ratio of lithium doped into the negative electrode active material layer reaches 70% of the discharge capacity C2 of the negative electrode. In addition, the irreversible capacity is estimated in advance by measuring the discharge capacity of the negative electrode after lithium doping. Through this process, lithium is doped into the negative electrode active material in the negative electrode active material layer 95, so that the electrode 73 is formed into a negative electrode 75 for a storage device. In addition, the negative electrode for the storage device in this embodiment and the later-described embodiments 7 to 11 and comparative examples 4 to 6 is a negative electrode for a lithium ion capacitor.

[0296] After passing the negative electrode 75 for an electric storage device through the cleaning tank 7 containing DMC (dimethyl carbonate) at 25° C., the negative electrode 75 for an electric storage device was wound. In the above manner, the negative electrode 75 for an electric storage device was manufactured.

[0297] (6-2) Production of Positive Electrode for Power Storage Device of Example 7

[0298] A long strip-shaped positive electrode current collector was prepared. The dimensions of the positive electrode current collector were: width 150 mm, length 100 m, thickness 8 μm. The positive electrode current collector was made of aluminum foil. The thickness of the positive electrode current collector was 12 μm. The positive electrode current collector had an opening ratio of 0%.

[0299] A positive electrode primer layer is formed on both surfaces of the positive electrode current collector. A positive electrode active material layer is formed on the positive electrode primer layer. The thickness of the positive electrode active material layer is 144 μm. The positive electrode active material layer is formed along the length direction of the negative electrode current collector 93. The positive electrode active material layer contains activated carbon, acetylene black, a binder and a dispersant in a mass ratio of 88:5:3:3. The positive electrode for the storage device is obtained through the above process.

[0300] The negative electrode collector aperture ratio, the thickness of the negative electrode collector, the discharge capacity C2 of the negative electrode, the discharge capacity C1 of the positive electrode, the discharge capacity ratio X, the doping ratio of lithium doped into the negative electrode active material layer, and the weight per unit area of ​​the negative electrode active material of the negative electrode 75 for the power storage device of Example 7 are shown in Table 3. In addition, the above-mentioned numerical values ​​in Examples 7 to 11 and Comparative Examples 4 to 6 described later are also shown in Table 3. The evaluation method is as follows.

[0301]

Table 3

[0302]

[0303] (Measurement of the discharge capacity C2 of the negative electrode)

[0304] The discharge capacity C2 of the negative electrode is the discharge capacity of the negative electrode when the negative electrode is charged and discharged between 0V vs. Li / Li+ and 3V vs. Li / Li+. Specifically, the discharge capacity C2 of the negative electrode is measured in the following manner. A discharge capacity measurement sample having a diameter of 16 mm is cut from the negative electrode for the storage device prepared in (6-1) above. A metallic lithium having a longitudinal dimension and a lateral dimension of 16 mm and a thickness of 200 μm is prepared as the counter electrode of the sample. In addition, a polyethylene nonwoven fabric having a thickness of 50 μm is prepared as a separator. Counter electrodes are arranged on both surfaces of the sample with a separator between them, and a metallic lithium plate is provided as a reference electrode. A mixed solution containing 1.4 M LiPF6 and containing ethylene carbonate, 1-fluoroethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:2:7 is used as the electrolyte, thereby producing a coin-type single cell having the above structure.

[0305] The coin-type battery was charged with a constant current-constant voltage in the following manner: first, the coin-type battery was charged with a charging current of 4 mA until the voltage reached 0 V, and then, the battery was charged with a voltage of 0 V until the charging current decreased to 0.4 mA. Next, the battery was discharged with a discharge current of 4 mA until the battery voltage reached 3.0 V, and the discharge capacity obtained was divided by the mass of the negative electrode active material to calculate the discharge capacity C2 per unit mass of the negative electrode active material.

[0306] In addition, the discharge capacity C1 of the positive electrode is the discharge capacity of the positive electrode when charging and discharging between the single cell voltage of 2.2V and 3.8V. Specifically, the discharge capacity C1 of the positive electrode is measured in the following manner. A discharge capacity measurement sample having a diameter of 15mm is cut from the positive electrode for the storage device prepared in the above (6-2). And, a discharge capacity measurement sample having a diameter of 16mm is cut from the negative electrode for the storage device prepared in the above (6-1). Then, the positive electrode and the counter electrode are arranged in a manner of separating the separators. A polyethylene nonwoven fabric with a thickness of 50μm is used as a separator. And, a mixed solution containing 1.2M LiPF6 and containing ethylene carbonate, 1-fluoroethyl carbonate, and ethyl methyl carbonate in a volume ratio of 3:4:3 is used as an electrolyte, thereby preparing a coin-type single cell having the above structure.

[0307] The coin-type single cell prepared was charged with constant current-constant voltage in the following manner: first, it was charged at a constant current of 4 mA until the cell voltage reached 3.8 V, and then it was charged at a constant voltage of 0 V until the charging current decreased to 0.4 mA. Next, it was discharged at a constant current of 4 mA until the cell voltage reached 2.2 V. The above charge and discharge were repeated twice, and the discharge capacity of the second discharge was measured. The measured value was divided by the mass of the negative electrode active material, which was used as the discharge capacity C1 of the positive electrode per unit mass of the negative electrode active material.

[0308] The discharge capacity ratio X is a value defined by the following formula (3): The unit of C1 and C2 described here is mAh / g.

[0309] Formula (3) X = C1 / C2

[0310] The doping ratio (%) of lithium doping into the negative electrode active material layer is the ratio of the doping amount of lithium doped into the negative electrode active material layer to the discharge capacity C2 of the negative electrode. The unit of the doping amount of lithium is mAh / g.

[0311] (6-3) Production of Negative Electrode for Power Storage Device of Example 8

[0312] The negative electrode for a power storage device of Example 8 was produced in basically the same manner as in Example 7. However, Example 8 was different from Example 7 in that the doping ratio of lithium in the negative electrode active material layer was 40%.

[0313] (6-4) Production of Negative Electrodes for Power Storage Devices of Examples 9 to 11

[0314] Negative electrodes for power storage devices of Examples 9 to 11 were produced basically in the same manner as in Example 7. However, the type of negative electrode active material, the discharge capacity C2 of the negative electrode, the discharge capacity ratio X, and the weight per unit area of ​​the negative electrode active material were different.

[0315] (6-5) Production of Negative Electrode for Power Storage Device of Comparative Example 4

[0316] The negative electrode for a power storage device of Comparative Example 3 was produced in basically the same manner as in Example 7. However, the discharge capacity C1 of the positive electrode, the discharge capacity ratio X, and the weight per unit area of ​​the negative electrode active material layer were different.

[0317] (6-6) Production of Negative Electrode for Power Storage Device of Comparative Example 5

[0318] The negative electrode for the storage device of Comparative Example 5 was manufactured in basically the same manner as Example 7. However, the aperture ratio of the negative electrode collector was different. In Comparative Example 5, the negative electrode collector had a plurality of through holes. The average pore size of the plurality of through holes was 90 μm. The average value of the spacing between the through holes was 147 μm. In Comparative Example 5, due to the high aperture ratio of the negative electrode collector, the electrode was broken during the formation of the negative electrode active material layer.

[0319] (6-7) Production of Negative Electrode for Power Storage Device of Comparative Example 6

[0320] A negative electrode for an electric storage device of Comparative Example 6 was produced in basically the same manner as in Comparative Example 5. However, Comparative Example 6 was different from Comparative Example 5 in that the thickness of the negative electrode current collector was 10 μm.

[0321] (6-8) Evaluation of negative electrodes for power storage devices

[0322] When the negative electrodes for power storage devices of Examples 7 to 11 and Comparative Examples 4 to 6 were used in lithium ion capacitors, the negative electrodes for power storage devices of Examples 7 to 11 and Comparative Examples 4 to 6 were evaluated. Specifically, the initial capacity, initial impedance, capacity retention rate (%) after 100,000 cycles, and the presence or absence of Li precipitation were evaluated. The results are shown in Table 3 above. The evaluation method is as follows.

[0323] (Production of single cell for evaluation)

[0324] Cut 15 pieces of negative electrode, each with a size of 10.0 cm × 13.0 cm (excluding the terminal welding part). In addition, cut 14 pieces of positive electrode, each with a size of 9.7 cm × 12.5 cm (excluding the terminal welding part). The positive electrode collector is composed of aluminum foil. The thickness of the positive electrode collector is 12 μm. The positive electrode collector opening rate is 0%.

[0325] A positive electrode primer layer is formed on both surfaces of the positive electrode current collector. A positive electrode active material layer is formed on the positive electrode primer layer. The thickness of the positive electrode active material layer is 144 μm. The positive electrode active material layer is formed along the length direction of the negative electrode current collector 93.

[0326] Then, the positive electrode and the negative electrode were alternately stacked through a separator formed of a polyethylene nonwoven fabric with a thickness of 35 μm, thereby producing an electrode stack unit. At this time, the terminal welding part of the positive electrode collector and the terminal welding part of the negative electrode collector were on opposite sides to each other. In addition, the negative electrode was arranged on the outermost side of the electrode stack unit.

[0327] Next, separators were placed at the top and bottom of the electrode stack, and the four sides of the electrode stack were fixed with tape. Then, the terminal welding parts of the 14 positive electrode collectors were ultrasonically welded to the aluminum positive terminal. And the terminal welding parts of the 15 negative electrode collectors were resistance welded to the nickel negative terminal.

[0328] Next, the electrode stacking unit is placed inside the laminate film, the opening is covered with another laminate film, and three sides are welded. Then, the electrolyte is vacuum impregnated into the laminate film, and then the remaining side of the opened laminate film is welded. The electrolyte is a mixture containing 1.2M LiPF6 and ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a volume ratio of 3:4:3. Through the above process, a single cell for evaluation is made.

[0329] (Initial evaluation)

[0330] The evaluation cell produced was charged with a constant current-constant voltage for 30 minutes in the following manner. First, the evaluation cell was charged with a constant current of 7A until the cell voltage reached 3.8V. Then a constant voltage of 3.8V was applied for charging. Then the cell was discharged at a constant current of 7A until the cell voltage reached 2.2V. The cycle test of the above cycle was repeated, and the discharge capacity of the second discharge was measured. The value obtained by dividing the measured value by the sum of the areas of the positive active material layer and the negative active material layer is taken as the initial discharge capacity of the active material per unit area. In addition, the value obtained by dividing the voltage difference between the voltage immediately before the start of the second discharge and the voltage 3 seconds after the start of the discharge by the discharge current was measured. The measured value is set as the initial impedance. The initial impedance is the DC internal impedance of the cell.

[0331] (Capacity retention after 100,000 cycles)

[0332] Next, the evaluation cell was charged at a constant current of 70 A until the cell voltage reached 3.8 V. Then, the cell was discharged at a constant current of 70 A until the cell voltage reached 2.2 V, and the above cycle was repeated 100,000 times.

[0333] Then, the evaluation cell was charged with a constant current-constant voltage for 30 minutes as follows: first, the evaluation cell was charged with a constant current of 7A until the cell voltage reached 3.8V. Then, charging was performed with a constant voltage of 3.8V. Next, discharge was performed with a constant current of 7A until the cell voltage reached 2.2V. The above cycle test was repeated, and the cell capacity of the second discharge was set to the discharge capacity after 100,000 cycles. The capacity retention rate (%) after 100,000 cycles was calculated based on the following formula (8).

[0334] Formula (8)

[0335] Capacity retention rate after 100,000 cycles (%) = (discharge capacity after 100,000 cycles / initial discharge capacity) × 100

[0336] (Li precipitation evaluation)

[0337] After the above 100,000 cycles of charge and discharge, the evaluation cell was disassembled and the negative electrode for the power storage device was taken out. The area of ​​the region where lithium metal was deposited in each of the negative electrodes for the power storage device taken out (hereinafter referred to as lithium deposition area) was measured.

[0338] The case where the negative electrode for a power storage device had no lithium deposition area of ​​5% or less was evaluated as "A", and the case where the negative electrode for a power storage device had lithium deposition area of ​​5% or more was evaluated as "B".

[0339] The lithium deposition area (%) was calculated by the following formula (9).

[0340] Formula (9)

[0341] Lithium deposition area (%) = (lithium deposition area of ​​negative electrode for power storage device) / (total area of ​​negative electrode for power storage device) × 100

[0342] The evaluation results are shown in Table 4.

[0343]

Table 4

[0344]

[0345] The negative electrodes for power storage devices of Examples 7 to 11 had high initial capacities and low initial impedances, high capacity retention rates after 100,000 cycles, and no Li precipitation occurred.

[0346] In contrast, the negative electrode for a power storage device of Comparative Example 4 had a low capacity retention rate after 100,000 cycles, and Li precipitation was confirmed. The negative electrode for a power storage device of Comparative Example 5 had an electrode break during the formation of the negative electrode active material layer, and thus could not be evaluated as a single cell. In addition, the negative electrode for a power storage device of Comparative Example 6 had a high initial impedance.

[0347] 7. Other Implementation Methods

[0348] As mentioned above, although embodiment of this disclosure was described, this disclosure is not limited to the said embodiment, Various deformation|transformation can be carried out.

[0349] (1) The functions of one constituent element in each of the above-mentioned embodiments may be shared by multiple constituent elements, or the functions of multiple constituent elements may be performed by one constituent element. In addition, a part of the configuration of each of the above-mentioned embodiments may be omitted. In addition, at least a part of the configuration of each of the above-mentioned embodiments may be added to the configuration of the other embodiments, or at least a part of the configuration of each of the above-mentioned embodiments may be replaced with the configuration of the other embodiments, etc. In addition, all the modes included in the technical ideas determined by the statements recorded in the claims are embodiments of the present disclosure.

[0350] (2) In addition to the above-described power storage device, the present disclosure can be implemented in various forms such as a system in which the power storage device is a constituent element.

Claims

1. A lithium ion secondary battery, comprising an electrode unit and an electrolyte, wherein the electrode unit includes a positive electrode and a negative electrode, wherein the negative electrode includes a negative electrode collector and a negative electrode active material layer formed on the surface of the negative electrode collector, wherein the positive electrode includes a positive electrode collector and a positive electrode active material layer formed on the surface of the positive electrode collector, and wherein the negative electrode is doped with lithium, wherein the lithium ion secondary battery is characterized in that: The opening ratio of the negative electrode current collector represented by the following formula (4) is 0% or more and 0.1% or less, The density of the positive electrode active material layer is 2 g / cm 3 Above 4g / cm 3 the following, The negative electrode active material layer has a unit area weight of 5 g / m 2 Above and 500g / m 2 the following, The thickness of the negative electrode active material layer is greater than or equal to 3 μm and less than or equal to 300 μm. The discharge capacity ratio X defined by the following formula (1) is greater than 0 and less than or equal to 0.9, where Formula (1) X = C1 / C2 C1 in the formula (1) is the discharge capacity of the single cell when the single cell voltage is charged and discharged between 2.0V and 4.3V, and C2 in the formula (1) is the discharge capacity of the negative electrode when the single cell voltage is charged and discharged between 0V vs. Li / Li+ and 3V vs. Li / Li+. The doping ratio of lithium doped into the negative electrode active material layer is 20% or more and 69% or less relative to C2, Formula (4) Negative electrode collector opening ratio (%) = [1-(mass of negative electrode collector / true specific gravity of negative electrode collector) / (apparent volume of negative electrode collector)] × 100, The true specific gravity of the negative electrode collector in the formula (4) refers to the mass per unit volume of the material constituting the negative electrode collector; the apparent volume of the negative electrode collector in the formula (4) refers to the volume of the negative electrode collector assuming that the negative electrode collector has no holes.

2. The lithium ion secondary battery according to claim 1, characterized in that: The discharge capacity ratio Y defined by the following formula (2) is 0.7 or more and 1 or less, wherein Formula (2)Y=C3 / C2 C2 in the formula (2) is the same as the discharge capacity C2 of the negative electrode in the formula (1), and C3 in the formula (2) is the discharge capacity C3 when the following negative electrode is discharged, and the negative electrode is a negative electrode taken out from a single cell that has been charged with a constant current-constant voltage at a single cell voltage of 4.3V.

3. The lithium ion secondary battery according to claim 1 or 2, characterized in that: The negative electrode active material layer contains a silicon-based material. The content of the silicon-based material in the negative electrode active material layer is 5 mass % or more and 99 mass % or less.

4. A lithium ion capacitor comprising an electrode unit and an electrolyte, wherein the electrode unit includes a positive electrode and a negative electrode, the negative electrode includes a negative electrode collector and a negative electrode active material layer formed on the surface of the negative electrode collector, the positive electrode includes a positive electrode collector and a positive electrode active material layer formed on the surface of the positive electrode collector, and the negative electrode is doped with lithium, wherein the lithium ion capacitor is characterized in that an aperture ratio of the negative electrode collector represented by the following formula (4) is greater than or equal to 0% and less than or equal to 0.1%, The density of the positive electrode active material layer is 2 g / cm 3 Above 4g / cm 3 the following, The discharge capacity ratio X defined by the following formula (3) is 0.005 or more and 0.2 or less, wherein Formula (3) X = C1 / C2 C1 in the formula (3) is the discharge capacity of the single cell when the single cell voltage is charged and discharged between 2.2V and 3.8V, and C2 in the formula (3) is the discharge capacity of the negative electrode when the single cell voltage is charged and discharged between 0V vs. Li / Li+ and 3V vs. Li / Li+. Formula (4) Negative electrode collector opening ratio (%) = [1-(mass of negative electrode collector / true specific gravity of negative electrode collector) / (apparent volume of negative electrode collector)] × 100, The true specific gravity of the negative electrode collector in the formula (4) refers to the mass per unit volume of the material constituting the negative electrode collector; the apparent volume of the negative electrode collector in the formula (4) refers to the volume of the negative electrode collector assuming that the negative electrode collector has no holes.

5. The lithium ion capacitor according to claim 4, characterized in that: The negative electrode active material layer contains a silicon-based material. The content of the silicon-based material in the negative electrode active material layer is 30 mass % or more and 99 mass % or less.

6. The lithium ion capacitor according to claim 4, characterized in that: The negative electrode active material layer contains a carbon-based material. The content of the carbon-based material in the negative electrode active material layer is 80 mass % or more and 99 mass % or less.

7. The lithium ion capacitor according to claim 6, characterized in that The carbon-based material is graphite-based particles.

8. The lithium ion capacitor according to any one of claims 5 to 7, characterized in that The doping ratio of lithium doped into the negative electrode active material layer is greater than or equal to 30% and less than or equal to 95% of C2.

Citation Information

Patent Citations

  • Manufacture of nonaqueous electrolyte secondary battery

    JP1995235330A

  • Nonaqueous electrolyte secondary battery and manufacture thereof

    JP1997293499A

  • Electrode material for lithium secondary battery, electrode structural body with the electrode material, secondary battery with the electrode structure, manufacturing method of the electrode material, manufacturing method of the electrode structural body, and manufacturing method of the secondary battery

    JP2004185810A

  • Wound type lithium ion capacitor

    JP2007067105A

  • Method and device for measuring position in existing pipe, and method for regenerating existing pipe

    JP2018080711A