Two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation and preparation method thereof
By introducing metal Nb into the P2 phase sodium ion battery cathode material, a two-phase structure is formed, which solves the problem of poor performance of existing materials at low temperatures, achieves high cycle stability and excellent high-rate performance, and is suitable for low-temperature working environments. .
Patent Information
- Application Number
- CN202010878886.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-08-27
AI Technical Summary
Existing P2-phase sodium-ion battery cathode materials have poor operating performance at low temperatures, especially insufficient discharge specific capacity and cycle stability at low temperatures, which limits their wide application.
A two-phase manganese-based P2 phase sodium ion battery cathode material is used. By introducing metal Nb, a two-phase structure of NaxAyNbzMn1-y-zO2 and NaNbO3 is formed, which enhances the structural stability and electronic conductivity of the material, and improves the cycle performance and high rate at low temperatures. performance.
It significantly improves the material's cycle stability and high-rate performance at low temperatures, avoids oxygen loss and structural collapse, improves electronic conductivity, and is suitable for low-temperature working environments.
Smart Images

Figure CN112103483B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a sodium ion battery positive electrode material and a preparation method thereof, in particular to a sodium ion battery positive electrode material with added metal material and a preparation method thereof, belonging to the technical field of battery positive electrode materials. Background Art
[0002] In the prior art, there are many types of positive electrode materials for sodium ion batteries. Among these materials, the polyanion-based type and the Prussian blue type have stable low-temperature performance. However, their low theoretical capacity limits their widespread application. The layered transition metal oxides of the P2 phase have become one of the research hotspots due to their controllable composition, easy synthesis, abundant raw materials, and high theoretical capacity. Compared with other positive electrode materials for sodium ion batteries, there are few studies on the operation of P2 phase sodium ion battery positive electrode materials at low temperatures. Therefore, the research and development of P2 phase sodium ion battery positive electrode materials with high discharge specific capacity and stable cycle performance under low temperature operation has important social significance and broad application prospects, and has become a technical problem that needs to be solved urgently. Summary of the invention
[0003] In order to solve the problems of the prior art, the purpose of the present invention is to overcome the shortcomings of the existing technology, and provide a two-phase manganese-based P2 phase sodium ion battery positive electrode material for low temperature operation and a preparation method thereof. Compared with other positive electrode materials for sodium ion batteries, the P2 phase sodium ion battery positive electrode material has a higher discharge specific capacity, but there is less research on operation at a low temperature of ≤0°C. Therefore, the present invention develops a P2 phase sodium ion battery positive electrode material with high cycle stability and high rate performance at low temperature, which has practical significance and broad application prospects. In addition, the present invention forms a two-phase structure by introducing metal Nb. The strong bond energy of the transition metal Nb-O stabilizes O during the charge and discharge process of the material, avoids the loss of O, enhances structural stability, and reduces structural collapse during the cycle. At the same time, Nb metal ions are prone to lose one 5s electron in the outer layer and four electrons in the sub-outer 4d orbit, which significantly improves the electronic conductivity of the material, so that the material exhibits good long-cycle stability and excellent high-rate performance.
[0004] In order to achieve the above object, the present invention adopts the following technical scheme:
[0005] A two-phase manganese-based P2-phase sodium ion battery cathode material for low temperature operation, the chemical formula of which is Na x A y Nb z Mn 1-y-z O2-NaNbO3, wherein A is any one or any two or more metal elements among Ni, Co, Fe, Mg, Zn, and Li, x is 0 to 0.85, y is 0 to 0.5, and z is 0 to 0.5; by introducing metal Nb, a two-phase structure is formed, namely Nax A y Nb z Mn 1-y-z O2 phase and NaNbO3 phase structure.
[0006] Preferably, in the chemical formula, x is 0.67, y is 0.32, and z is 0.04 to 0.1.
[0007] Preferably, the low temperature of the low temperature operation is ≤ 0° C. More preferably, the low temperature of the low temperature operation is ≤ -40° C.
[0008] A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation of the present invention adopts any one of the following methods:
[0009] Method 1: Using niobium oxide as the niobium source material, including the following steps:
[0010] a. Using manganese acetate as a manganese source material and acetate A as an A source material; weighing manganese acetate and acetate A and dissolving them in a solvent to obtain an acetate mixed solution, wherein A is any one metal element or any two or more metal elements selected from Ni, Co, Fe, Mg, Zn, and Li;
[0011] b. Weigh sodium carbonate as a sodium source material and prepare a sodium carbonate solution;
[0012] c. adding the sodium carbonate solution prepared in step b to the acetate mixed solution prepared in step a, stirring magnetically for at least 6 hours, and then washing. After washing, drying for at least 12 hours to obtain a precursor material;
[0013] d. Weigh anhydrous sodium carbonate and niobium oxide and the precursor material dried in step c, and evenly mix them by ball milling to obtain a mixed sintered material; then pre-sinter the mixed sintered material and sinter at high temperature, and then cool the sintered product to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material;
[0014] Method 2: Using niobium oxalate as the niobium source material, including the following steps:
[0015] 1) manganese acetate is used as a manganese source material and acetate A is used as an A source material; manganese acetate, acetate A and niobium oxalate are weighed, mixed and dissolved in a solvent to obtain a mixed salt solution; wherein A is any one metal element or any two or more metal elements selected from Ni, Co, Fe, Mg, Zn and Li;
[0016] 2) Weighing sodium citrate as a sodium source material and preparing a sodium citrate solution;
[0017] 3) adding the mixed salt solution prepared in step a to the sodium citrate solution prepared in step b, stirring and mixing in a water bath until a gel is formed, and then drying to obtain a precursor material;
[0018] 4) The precursor material dried in step c is used as a sintering material, and after ball milling, pre-sintering and high-temperature sintering are performed to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material.
[0019] Preferably, the molar ratio of manganese acetate, acetic acid A in step a of method one and anhydrous sodium carbonate in step d is (1-4):(1-2):1.
[0020] Preferably, in step d of the method 1, the mass ratio of the precursor material, anhydrous sodium carbonate and niobium salt dried in step c is 100:36:(15-25).
[0021] Preferably, in step d) of the method one or in step 4) of the method two, pre-sintering is carried out at a temperature not lower than 500°C for at least 12 hours, then the temperature is increased to the sintering temperature at a rate not lower than 5°C / min, and high-temperature sintering is carried out at a temperature not lower than 900°C for at least 10 hours, thereby obtaining a two-phase manganese-based P2 phase sodium ion battery positive electrode material.
[0022] Preferably, the solvent is deionized water.
[0023] Preferably, the molar ratio of manganese acetate, acetic acid A, niobium oxalate and sodium citrate in step a of method 2 is (1-4): (0.5-2): (0.0625-0.625): 1.
[0024] Compared with the prior art, the present invention has the following obvious outstanding substantial features and significant advantages:
[0025] 1. The present invention introduces metal Nb to form a two-phase structure; the strong bond energy of transition metal Nb-O stabilizes O in the material during the charge and discharge process, avoids the loss of O, enhances structural stability, and reduces structural collapse during cycling; the present invention significantly improves the electronic conductivity of the material, so that the material exhibits good long-cycle stability and excellent high-rate performance;
[0026] 2. The present invention can also adopt a simple and easy coprecipitation method and a sol-gel method, which has a high output rate and good repeatability and is suitable for popularization and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the comparative example of the present invention, Na 0.67 Ni 0.333 Mn 0.667 O2, battery cycling curve at -40℃, 0.5C.
[0028] Figure 2 The Na prepared in Example 1 of the present invention 0.67 Ni 0.323 Nb 0.04 Mn 0.64 O2-NaNbO3, battery cycling curve at -40℃, 0.5C.
[0029] Figure 3 The Na prepared in Example 2 of the present invention 0.67 Ni 0.323 Nb 0.07 Mn 0.64 O2-NaNbO3, battery cycling curve at -40℃, 0.5C.
[0030] Figure 4 The Na prepared in Example 3 of the present invention 0.67 Ni 0.323 Nb 0.10 Mn 0.64 O2-NaNbO3, battery cycling curve at -40℃, 0.5C.
[0031] Figure 5 The Na prepared in Comparative Example 2 of the present invention 0.67 Ni 0.323 Mn 0.64 O2, battery cycling curve at -40℃, 0.5C.
[0032] Figure 6 The Na prepared in Example 4 of the present invention 0.67 Ni 0.323 Nb 0.05 Mn 0.64 O2-NaNbO3, battery cycling curve at -40℃, 0.5C.
[0033] Figure 7 The Na prepared in Example 5 of the present invention 0.67 Ni 0.323 Nb 0.08 Mn 0.64 O2-NaNbO3, battery cycling curve at -40℃, 0.5C. DETAILED DESCRIPTION
[0034] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present invention are described in detail as follows:
[0035] Embodiment 1:
[0036] In this embodiment, a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation has a chemical formula of Na0.67 Ni 0.323 Nb 0.04 Mn 0.64 O2-NaNbO3, by introducing metal Nb, forms a two-phase structure, namely Na 0.67 Ni 0.323 Nb 0.04 Mn 0.64 O2 phase and NaNbO3 phase structure.
[0037] A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to this embodiment, using niobium salt as a niobium source material, comprises the following steps:
[0038] (1) Manganese acetate is used as a manganese source material, and acetate A is used as an A source material; 0.04 mol of manganese acetate, 0.02 mol of nickel acetate, and 0.1 mol of anhydrous sodium carbonate are weighed; manganese acetate and nickel acetate are dissolved in 60 ml of deionized water, and anhydrous sodium carbonate is dissolved in 50 ml of deionized water, and magnetic stirring is performed for 30 minutes. After the two solutions are clarified, anhydrous sodium carbonate is added dropwise to the acetate mixed solution, and stirring is continued for 6 hours; the mixed solution is washed with water and ethanol, dried for 12 hours, and ground into powder to obtain a precursor material;
[0039] (2) 1 g of the precursor material, 0.36 g of anhydrous sodium carbonate and 0.15 g of niobium oxide were weighed, mixed and ball-milled, and then placed in a muffle furnace for sintering. The pre-sintering was performed at 500° C. for 12 h, and then the temperature was raised to the sintering temperature at a rate of 5° C. / min, and the high-temperature sintering was performed at 900° C. for 10 h. The sintered product was then naturally cooled to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.323 Nb 0.04 Mn 0.64 O2-NaNbO3.
[0040] Embodiment 2:
[0041] This embodiment is basically the same as the first embodiment, except that:
[0042] In this embodiment, a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation has a chemical formula of Na 0.67 Ni 0.323 Nb 0.07 Mn 0.64 O2-NaNbO3, by introducing metal Nb, forms a two-phase structure, namely Na 0.67 Ni 0.323 Nb 0.07 Mn 0.64 O2 phase and NaNbO3 phase structure.
[0043] A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to this embodiment, using niobium salt as a niobium source material, comprises the following steps:
[0044] (1) Manganese acetate is used as a manganese source material, and acetate A is used as an A source material; 0.04 mol of manganese acetate, 0.02 mol of nickel acetate, and 0.1 mol of anhydrous sodium carbonate are weighed; manganese acetate and nickel acetate are dissolved in 60 ml of deionized water, and anhydrous sodium carbonate is dissolved in 50 ml of deionized water, and magnetic stirring is performed for 30 minutes. After the two solutions are clarified, anhydrous sodium carbonate is added dropwise to the acetate mixed solution, and stirring is continued for 6 hours; the mixed solution is washed with water and ethanol, dried for 12 hours, and ground into powder to obtain a precursor material;
[0045] (2) 1 g of the precursor material, 0.36 g of anhydrous sodium carbonate and 0.2 g of niobium oxide were weighed, mixed and ball-milled, and then placed in a muffle furnace for sintering. The pre-sintering was performed at 500° C. for 12 h, and then the temperature was raised to the sintering temperature at a rate of 5° C. / min, and the high-temperature sintering was performed at 900° C. for 10 h. The sintered product was then naturally cooled to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.323 Nb 0.07 Mn 0.64 O2-NaNbO3.
[0046] Embodiment three:
[0047] This embodiment is basically the same as the above embodiment, with the following features:
[0048] In this embodiment, a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation has a chemical formula of Na 0.67 Ni 0.323 Nb 0.1 Mn 0.64 O2-NaNbO3, by introducing metal Nb, forms a two-phase structure, namely Na 0.67 Ni 0.323 Nb 0.1 Mn 0.64 O2 phase and NaNbO3 phase structure.
[0049] A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to this embodiment, using niobium salt as a niobium source material, comprises the following steps:
[0050] (1) Manganese acetate is used as a manganese source material, and acetate A is used as an A source material; 0.04 mol of manganese acetate, 0.02 mol of nickel acetate, and 0.1 mol of anhydrous sodium carbonate are weighed; manganese acetate and nickel acetate are dissolved in 60 ml of deionized water, and anhydrous sodium carbonate is dissolved in 50 ml of deionized water, and magnetic stirring is performed for 30 minutes. After the two solutions are clarified, anhydrous sodium carbonate is added dropwise to the acetate mixed solution, and stirring is continued for 6 hours; the mixed solution is washed with water and ethanol, dried for 12 hours, and ground into powder to obtain a precursor material;
[0051] (2) 1 g of the precursor material, 0.36 g of anhydrous sodium carbonate and 0.25 g of niobium oxide were weighed, mixed and ball-milled, and then placed in a muffle furnace for sintering. The mixture was pre-sintered at 500 ° C for 12 h, and then heated to the sintering temperature at a rate of 5 ° C / min, and sintered at 900 ° C for 10 h. The sintered product was then naturally cooled to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.323 Nb 0.1 Mn 0.64 O2-NaNbO3.
[0052] Comparative Example 1:
[0053] A sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.33 Mn 0.67 O2.
[0054] A method for preparing a positive electrode material for a sodium ion battery of this comparative example comprises the following steps:
[0055] (1) Weigh 0.04 mol of manganese acetate, 0.02 mol of nickel acetate, and 0.1 mol of anhydrous sodium carbonate; dissolve manganese acetate and nickel acetate in 60 ml of deionized water, dissolve anhydrous sodium carbonate in 50 ml of deionized water, and stir magnetically for 30 min. After the two solutions are clarified, add anhydrous sodium carbonate dropwise into the acetate mixed solution, and continue stirring for 12 h; wash the mixed solution with water and ethanol, and dry it for 12 h; grind it carefully to obtain a dry sample;
[0056] Take 1g of dry sample, weigh 0.36g of anhydrous sodium carbonate, mix and grind, put into muffle furnace for sintering, pre-sinter at 500℃ for 12h, then heat to sintering temperature at 5℃ / min, sinter at 900℃ for 10h, and then cool the sintered product naturally to obtain the positive electrode material of sodium ion battery, the chemical formula of which is Na 0.67 Ni 0.33 Mn 0.67 O2.
[0057] Experimental test analysis:
[0058] The sodium ion battery positive electrode materials of the above embodiment and comparative example were used as samples for experimental testing and comparison. Figure 1-Figure 4 After constructing the two-phase structure, the electronic and ionic conductivity of the material at low temperature of -40°C was improved. Compared with the comparative example, when the Nb content in the main phase was 0.04, 0.07, and 0.1, the material showed excellent cycle performance. Figure 1 and Figure 2 , Figure 3 , Figure 4 From the comparison of the 0.5C cycle performance diagram, it can be seen that after 100 cycles, the capacity retention rate of Example 1 is 91.2%, and the capacity is 99.3 mAh / g; the capacity retention rate of Example 2 is 89.7%, and the capacity is 91.1 mAh / g; the capacity retention rate of Example 3 is 90.5%, and the capacity is 84.9 mAh / g, which are increased by 148.8%, 128%, and 112.8% over the comparative example.
[0059] In summary, by adding different contents of Nb to construct a two-phase structure, the rate and cycle performance of the material at low temperature are significantly improved. The material synthesis method is simple and highly repeatable.
[0060] Embodiment 4:
[0061] This embodiment is basically the same as the above embodiment, with the following features:
[0062] In this embodiment, a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation has a chemical formula of Na 0.67 Ni 0.323 Nb 0.05 Mn 0.64 O2-NaNbO3, by introducing metal Nb, forms a two-phase structure, namely Na 0.67 Ni 0.323 Nb 0.05 Mn 0.64 O2 phase and NaNbO3 phase structure.
[0063] A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to this embodiment, using niobium oxalate as a niobium source material, comprises the following steps:
[0064] 1) Weigh 0.04 mol manganese acetate, 0.02 mol nickel acetate, 0.0025 mol niobium oxalate and 0.025 mol sodium citrate as raw materials; dissolve manganese acetate, nickel acetate and niobium oxalate in 60 ml deionized water, and stir magnetically for 12 hours to obtain a mixed salt solution;
[0065] 2) Weighing sodium citrate as a sodium source material and preparing a sodium citrate solution;
[0066] 3) adding the mixed salt solution prepared in step a to the sodium citrate solution prepared in step b, stirring and mixing in a water bath at 30° C. until a gel is formed, and then drying to obtain a precursor material;
[0067] 4) The precursor material dried in step c is used as a sintering material, ball-milled, and then placed in a muffle furnace for sintering, pre-sintered at 500° C. for 12 h, then heated to the sintering temperature at a rate of 5° C. / min, and sintered at 900° C. for 10 h, and then the sintered product is naturally cooled to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.323 Nb 0.05 Mn 0.64 O2-NaNbO3.
[0068] Embodiment five:
[0069] This embodiment is basically the same as the above embodiment, with the following features:
[0070] In this embodiment, a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation has a chemical formula of Na 0.67 Ni 0.323 Nb 0.08 Mn 0.64 O2-NaNbO3, by introducing metal Nb, forms a two-phase structure, namely Na 0.67 Ni 0.323 Nb 0.08 Mn 0.64 O2 phase and NaNbO3 phase structure.
[0071] A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to this embodiment, using niobium oxalate as a niobium source material, comprises the following steps:
[0072] 1) Weigh 0.04 mol manganese acetate, 0.02 mol nickel acetate, 0.003 mol niobium oxalate and 0.025 mol sodium citrate as raw materials; dissolve manganese acetate, nickel acetate and niobium oxalate in 60 ml deionized water, and stir magnetically for 12 hours to obtain a mixed salt solution;
[0073] 2) Weighing sodium citrate as a sodium source material and preparing a sodium citrate solution;
[0074] 3) adding the mixed salt solution prepared in step a to the sodium citrate solution prepared in step b, stirring and mixing in a water bath at 30° C. until a gel is formed, and then drying to obtain a precursor material;
[0075] 4) The precursor material dried in step c is used as a sintering material, ball-milled, and then placed in a muffle furnace for sintering, pre-sintered at 500° C. for 12 h, then heated to the sintering temperature at a rate of 5° C. / min, and sintered at 900° C. for 10 h, and then the sintered product is naturally cooled to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.323 Nb 0.08 Mn 0.64 O2-NaNbO3.
[0076] Comparative Example 2:
[0077] A sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.33 Mn 0.67 O2.
[0078] A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to this embodiment, using niobium oxalate as a niobium source material, comprises the following steps:
[0079] 1) Weigh 0.04 mol manganese acetate, 0.02 mol nickel acetate and 0.067 mol sodium citrate as raw materials; dissolve manganese acetate, nickel acetate and niobium oxalate in 60 ml deionized water, and stir magnetically for 12 hours to obtain a mixed salt solution;
[0080] 2) Weighing sodium citrate as a sodium source material and preparing a sodium citrate solution;
[0081] 3) adding the mixed salt solution prepared in step a to the sodium citrate solution prepared in step b, stirring and mixing in a water bath at 30° C. until a gel is formed, and then drying to obtain a precursor material;
[0082] 4) The precursor material dried in step c is used as a sintering material, ball-milled, and then placed in a muffle furnace for sintering, pre-sintered at 500° C. for 12 h, then heated to the sintering temperature at a rate of 5° C. / min, and sintered at 900° C. for 10 h, and then the sintered product is naturally cooled to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material, the chemical formula of which is Na 0.67 Ni 0.33 Mn 0.67 O2.
[0083] Experimental test analysis:
[0084] The sodium ion battery positive electrode materials of the above embodiment and comparative example were used as samples for experimental testing and comparison. Figure 5-Figure 7After constructing the two-phase structure, the electronic and ionic conductivity of the material at low temperature of -40°C was improved. Compared with the comparative example, when the Nb content in the main phase was 0.05 and 0.08, the material showed excellent cycle performance. Figure 5 and Figure 6 , Figure 6 From the 0.5C cycle performance diagram, it can be seen that after 100 cycles, the capacity retention rate of Example 4 is 92.8%, and the capacity is 92 mAh / g. The capacity retention rate of Example 5 is 95.7%, and the capacity is 83.6 mAh / g, which are increased by 47.9% and 34.9% respectively compared with the comparative example.
[0085] The two-phase manganese-based P2-phase sodium ion battery positive electrode material prepared by the method of this embodiment is almost the same as the two-phase manganese-based P2-phase sodium ion battery positive electrode material prepared in Example 1. This embodiment adopts a simple and easy co-precipitation method and a sol-gel method, with high output rate and good repeatability, and is suitable for popularization and use.
[0086] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention of the present invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods. As long as they meet the purpose of the invention of the present invention and do not deviate from the technical principles and inventive concepts of the present invention, they belong to the protection scope of the present invention.
Claims
1. A method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation, characterized in that: The low temperature of the low temperature operation is ≤0°C, and any one of the following methods is used: Method 1: Using niobium oxide as the niobium source material, including the following steps: a. Manganese acetate is used as a manganese source material, and acetate A is used as a source material A; manganese acetate and acetate A are weighed and dissolved in a solvent to obtain an acetate mixed solution, wherein A is any one metal element or any two or more metal elements among Ni, Mg, Zn, and Li; b. Weigh sodium carbonate as a sodium source material and prepare a sodium carbonate solution; c. The sodium carbonate solution prepared in step b is added to the acetate mixed solution prepared in step a, magnetically stirred for at least 6 hours, and then washed, and after washing, dried for at least 12 hours to obtain a precursor material; d. Weighing anhydrous sodium carbonate and niobium oxide and the precursor material dried in step c, uniformly mixing by ball milling to obtain a mixed sintered material; then pre-sintering the mixed sintered material and sintering at high temperature, that is, pre-sintering at not less than 500 ° C for at least 12h, then heating to the sintering temperature at a rate of not less than 5 ° C / min, sintering at a high temperature of not less than 900 ° C for at least 10h, and then cooling the sintered product to obtain a two-phase manganese-based P2 phase sodium ion battery positive electrode material; Method 2: Using niobium oxalate as the niobium source material, including the following steps: 1) Manganese acetate is used as a manganese source material, and acetate A is used as an A source material; manganese acetate, acetate A, and niobium oxalate are weighed, mixed and dissolved in a solvent to obtain a mixed salt solution; wherein A is any one metal element or any two or more metal elements selected from Ni, Mg, Zn, and Li; 2) Weigh sodium citrate as a sodium source material and prepare a sodium citrate solution; 3) adding the mixed salt solution prepared in step a to the sodium citrate solution prepared in step b, stirring and mixing in a water bath until a gel is formed, and then drying to obtain a precursor material; 4) The precursor material dried in step c is used as a sintering material for pre-sintering and high-temperature sintering, that is, pre-sintering at a temperature not lower than 500° C. for at least 12 hours, then heating to the sintering temperature at a rate not lower than 5° C. / min, and high-temperature sintering at a temperature not lower than 900° C. for at least 10 hours, thereby obtaining a two-phase manganese-based P2 phase sodium ion battery positive electrode material; The two-phase manganese-based P2-phase sodium ion battery positive electrode material prepared by the method 1 and the method 2 has a chemical formula of Na x A y Nb z Mn 1-y-z O2-NaNbO3, wherein A is any one or any two or more metal elements among Ni, Mg, Zn, and Li, x is 0.67, y is 0.32, and z is 0.04 to 0.1; by introducing metal Nb, a two-phase structure is formed, namely Na x A y Nb z Mn 1-y-z O2 phase and NaNbO3 phase structure; The molar ratio of manganese acetate, acetic acid A in step a of the method 1 and anhydrous sodium carbonate in step d is (1-4): (1-2): 1; In step d of the method 1, the mass ratio of the precursor material, anhydrous sodium carbonate and niobium salt dried in step c is 100:36:(15-25); In step a of method 2, the molar ratio of manganese acetate, acetic acid A, niobium oxalate and sodium citrate is (1-4):(0.5-2):(0.0625-0.625):
1.
2. The method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to claim 1, characterized in that: The low temperature of the low temperature operation is ≤-40°C.
3. The method for preparing a two-phase manganese-based P2-phase sodium ion battery positive electrode material for low temperature operation according to claim 1, characterized in that: The solvent is deionized water.
Citation Information
Patent Citations
Hybrid-phase structure layered oxide material and preparation method and application thereof
CN109585795A