Sulfur-carbon composite and lithium secondary battery comprising the same

By introducing a conductive polymer-coated sulfur-carbon composite into a lithium-sulfur secondary battery, the problem of insufficient conductivity of sulfur-carbon composites is solved, and the lithium ion mobility and battery performance are improved.

CN112106236BActive Publication Date: 2024-11-29LG ENERGY SOLUTION LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN201980031792.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-09-10
Publication Date
2024-11-29
Estimated Expiration
2039-09-10

AI Technical Summary

Technical Problem

In the existing lithium-sulfur secondary batteries, due to insufficient conductivity of sulfur-carbon composites, it leads to difficulty in moving lithium ions, which affects battery performance.

Method used

Introducing a conductive polymer coating in the sulfur-carbon composite, polyaniline nanofibers are used as the conductive polymer to form a network-type coating to improve the conductivity and the mobile space of lithium ions.

Benefits of technology

Through the sulfur-carbon composite coated with conductive polymer, the conductivity and lithium-ion movement capacity of lithium-sulfur secondary batteries are improved, the battery life is extended and the energy density is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112106236B_ABST
    Figure CN112106236B_ABST
Patent Text Reader

Abstract

The present invention relates to a sulfur-carbon composite and a lithium secondary battery including the sulfur-carbon composite. More specifically, a network-like coating layer including a conductive polymer is formed on the surface of the sulfur-carbon composite, thereby enhancing the conductivity of the sulfur-carbon composite, and furthermore, lithium ions move freely, and therefore, when applied to a lithium secondary battery, the sulfur-carbon composite can enhance the performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2018-0112636 filed on September 20, 2018 and Korean Patent Application No. 10-2019-0111292 filed on September 9, 2019, which are hereby incorporated by reference in their entirety.

[0002] The present invention relates to a sulfur-carbon composite suitable for a positive electrode material for a lithium secondary battery and a lithium secondary battery comprising the sulfur-carbon composite. Background Art

[0003] Recently, with the rapid development of the fields of electronic devices and electric vehicles, the demand for secondary batteries is increasing. In particular, with the trend of miniaturization and lightness of portable electronic devices, the demand for secondary batteries with high energy density that can cope with this trend is growing.

[0004] Among secondary batteries, lithium-sulfur batteries are secondary batteries that use a sulfur compound having a sulfur-sulfur bond as a positive electrode active material, and use an alkali metal such as lithium, a carbon material in which metal ions such as lithium ions are intercalated and deintercalated, or silicon or tin that forms an alloy with lithium as a negative electrode active material. Specifically, during discharge as a reduction reaction, the oxidation number of sulfur decreases as the SS bond breaks, and during charging as an oxidation reaction, the SS bond is reformed as the oxidation number of sulfur increases. Through this redox reaction, electrical energy is stored and generated.

[0005] In particular, sulfur used as a positive electrode active material in a lithium-sulfur battery has a theoretical energy density of 1675 mAh / g, and thus its theoretical energy density is about 5 times that of a positive electrode active material used in a conventional lithium secondary battery, thereby enabling the battery to exhibit high power and high energy density. In addition, since sulfur has the advantages of being cheap and abundant in resources and thus easily available and environmentally friendly, sulfur has attracted attention not only as an energy source for portable electronic devices, but also as an energy source for medium-sized and large-sized devices such as electric vehicles.

[0006] Sulfur is an insulator and is therefore mainly used as a composite with carbon as a conductive material. The higher the sulfur content in the positive electrode, the higher the energy density, but the less the amount of conductive material. Therefore, there is a problem of electromotive force loss due to an increase in electrochemical overvoltage.

[0007] In order to solve this problem in lithium-sulfur secondary batteries, a technique has been proposed to coat a material capable of absorbing polysulfide on the positive electrode material or introduce it into a component such as a separator or a negative electrode within the battery. In addition, research results on coating a conductive polymer on a positive electrode material have been reported.

[0008] For example, Jun Jin et al. (SOLID STATE IONICS 262 (2014), pp. 170-173) disclosed a positive electrode for a lithium-sulfur secondary battery, which comprises a mesoporous sulfur-carbon composite coated with polyaniline as a conductive polymer.

[0009] In addition, Guo-Chun Li et al. (ADVANCED ENERGY MATERIALS, February 2012, pp. 1238-1245) also disclosed a positive electrode active material for a lithium-sulfur secondary battery, which comprises a sulfur-carbon black composite coated with polyaniline as a conductive polymer.

[0010] However, in the case of the sulfur-carbon composites proposed in these documents, there is a problem that since polyaniline is applied in the form of a thin film, the movement of lithium ions becomes difficult.

[0011] Therefore, there is an urgent need to develop a technology that allows smooth movement of lithium ions while improving the electrical conductivity of sulfur-carbon composites.

[0012] [Non-patent literature]

[0013] (Non-Patent Document 1) Jun Jin et al., SOLID STATE IONICS 262 (2014), pp. 170-173.

[0014] (Non-patent document 2) Guo-Chun Li et al., ADVANCED ENERGY MATERIALS, February 2012, pp. 1238-1245. Summary of the invention

[0015]

Technical issues

[0016] As a result of conducting various studies to solve the above problems, the present inventors have confirmed that, if a conductive polymer is introduced into a sulfur-carbon composite by coating in a form that allows lithium ions to pass through the surface of the sulfur-carbon composite while using polyaniline nanofibers as the conductive polymer, the conductivity of the sulfur-carbon composite is improved. In addition, the present inventors have confirmed that the sulfur-carbon composite coated with polyaniline nanofibers has an improved adsorption rate for polysulfide and lithium ions smoothly move between the coated polyaniline nanofibers, thereby improving battery performance.

[0017] Therefore, one embodiment of the present invention provides a sulfur-carbon composite in which a conductive polymer coating is formed in a form that enables movement of lithium ions.

[0018] Another embodiment of the present invention provides a lithium secondary battery including a sulfur-carbon composite having a conductive polymer coating layer having a form that enables movement of lithium ions.

[0019]

Technical solution

[0020] In order to achieve the above object, one embodiment of the present invention provides a sulfur-carbon composite comprising a network-type conductive polymer coating.

[0021] The conductive polymer may be at least one selected from the group consisting of polyaniline, polypyrrole, polythiophene, poly(3,4-ethylenedioxythiophene), polyacetylene, polydiacetylene, poly(thiophenevinylene), polyfluorene, and derivatives thereof.

[0022] The conductive polymer may be in the form of at least one selected from the group consisting of nanofibers, nanowires, nanorods, and nanotubes.

[0023] The sulfur-carbon composite may include sulfur particles including at least one carbon particle therein and carbon particles located on a portion or the entire surface of the sulfur particles.

[0024] The weight ratio of sulfur to carbon may be from 6:4 to 9:1.

[0025] The conductive polymer may be included in an amount of 0.1 wt % to 10 wt % based on the total weight of the sulfur-carbon composite including the conductive polymer coating layer.

[0026] In addition, in the sulfur-carbon composite, the sulfur may be selected from sulfur (S8), Li2S n (n is a real number satisfying n ≥ 1), organic sulfur compounds and carbon-sulfur polymers [(C2S x ) n , wherein x is a real number from 2 to 50 and n is a real number satisfying n≥2].

[0027] The carbon may be selected from graphite, graphene, carbon black, carbon fiber, carbon nanofiber, carbon nanotube, carbon nanowire, carbon nanoring, carbon cloth and fullerene (C 60 ) in the group consisting of any one of the following.

[0028] The carbon black may be selected from the group consisting of Super P, Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black.

[0029] Another embodiment of the present invention further provides a positive electrode, comprising the sulfur-carbon composite.

[0030] The present invention also provides a lithium secondary battery comprising the sulfur-carbon composite.

[0031]

Beneficial Effects

[0032] According to the sulfur-carbon composite of the present invention, since a conductive polymer coating is introduced to absorb polysulfide dissolved from the positive electrode when applied to a lithium-sulfur secondary battery, the phenomenon of shortening the life caused by polysulfide dissolving in the electrolyte and moving to the negative electrode can be prevented.

[0033] Furthermore, when polysulfides are adsorbed on the sulfur-carbon composite, they form a conductive structure together with carbon, thereby improving the utilization of sulfur.

[0034] Furthermore, in the sulfur-carbon composite, a conductive polymer coating may be introduced to improve the electrical conductivity.

[0035] Furthermore, in the sulfur-carbon composite having the conductive polymer coating layer, since the conductive polymer coating layer is formed of the conductive polymer nanofiber, a space in which lithium ions can move can be ensured, and thus the lithium ions can move smoothly.

[0036] Furthermore, when the sulfur-carbon composite including the conductive polymer coating layer formed of the conductive polymer nanofibers is applied to a positive electrode of a lithium-sulfur secondary battery, the performance of the lithium-sulfur secondary battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematic diagram of a sulfur-carbon composite comprising a conductive polymer coating according to the present invention.

[0038] Figure 2 Graph showing the correlation between potential and current when a charging voltage is applied to an electrolyte solution containing aniline and an electrolyte solution not containing aniline according to Comparative Example 2.

[0039] Figure 3a and Figure 3b Scanning electron microscope (SEM) images of the polyaniline nanofibers synthesized in Preparation Example 1 and the polyaniline nanofiber coating formed on the surfaces of the sulfur-carbon composite prepared in Example 1, respectively.

[0040] Figure 4 It is a graph showing first discharge curves as evaluation results of coin-type batteries of lithium-sulfur secondary batteries prepared in Example 1 and Comparative Examples 1 and 2, respectively.

[0041] Figure 5 Graphs showing cycle-discharge capacity curves of lithium-sulfur secondary batteries prepared in Example 1 and Comparative Examples 1 and 2, respectively. DETAILED DESCRIPTION

[0042] Hereinafter, the present invention will be described in more detail to help understanding of the present invention.

[0043] The terms and words used in this specification and claims should not be interpreted as limited to common terms or dictionary terms, but should be interpreted as meanings and concepts consistent with the technical concept of the present invention based on the principle that the inventor can appropriately define the concepts of the terms to describe his invention in the best possible manner.

[0044] Sulfur-carbon complex

[0045] One embodiment of the present invention is directed to a sulfur-carbon composite comprising a conductive polymer coating.

[0046] Figure 1 Schematic diagram of a sulfur-carbon composite comprising a conductive polymer coating according to the present invention.

[0047] Reference Figure 1 The sulfur-carbon composite 10 including a conductive polymer coating may be a sulfur-carbon composite in which a conductive polymer coating 12 is formed on the surface of the sulfur-carbon composite 11 .

[0048] The conductive polymer forming the conductive polymer coating 12 may be any one selected from the group consisting of polyaniline, polypyrrole, polythiophene, poly(3,4-ethylenedioxythiophene), polyacetylene, polydiacetylene, poly(thiophenevinylene), polyfluorene, and derivatives thereof, and preferably, the conductive polymer may be polyaniline.

[0049] In addition, the shape of the conductive polymer coating 12 may be a network type. In this case, the network type means that the coating formed on the surface of the sulfur-carbon complex is not formed on the entire surface of the sulfur-carbon complex, but is formed in a mesh shape so that a portion of the surface of the sulfur-carbon complex can be exposed. In the network type conductive polymer coating 12, a space is formed in the portion where a portion of the surface of the sulfur-carbon complex is exposed, and thus there is an advantage that lithium ions can freely move through the space.

[0050] In order to form a conductive polymer coating in a network-type form, the conductive polymer may have one or more nanostructures selected from the group consisting of nanowires, nanorods and nanotubes. Preferably, the conductive polymer may have a nanofiber shape, in which case it may be advantageous to form a network-type coating.

[0051] In addition, when the conductive polymer has a nanofiber shape, the diameter of the nanofiber may be 10 nm to 1 μm, preferably 20 nm to 500 nm, and more preferably 50 nm to 200 nm. If the diameter of the nanofiber is less than the above range, the effect of improving the conductivity of the sulfur-carbon composite may not be significant. If the diameter of the nanofiber is greater than the above range, the space formed in the coating formed into a network type may become narrow, making it difficult for lithium ions to move.

[0052] The content of the conductive polymer may be 0.1 wt % to 10 wt %, preferably 0.5 wt % to 7 wt %, and more preferably 1 wt % to 5 wt %, based on the total weight of the sulfur-carbon composite including the conductive polymer coating. If the content of the conductive polymer is less than the above range, the effect of improving the conductivity of the sulfur-carbon composite may not be significant. If the content of the conductive polymer exceeds the above range, when applied to a battery, the performance of the battery may be reduced.

[0053] The sulfur-carbon composite 11 may include sulfur particles including at least one carbon particle therein; and carbon particles located on a portion or the entire surface of the sulfur particles.

[0054] Furthermore, since the sulfur-carbon composite 11 has a structure in which carbon particles are contained inside and outside sulfur particles and thus sulfur and carbon can be mixed at a uniform ratio, there is an advantage that carbon as a conductive material effectively provides electron conductivity to sulfur.

[0055] In the sulfur-carbon composite 11, sulfur may be selected from sulfur (S8), Li2S n (n is a real number satisfying n ≥ 1), organic sulfur compounds and carbon-sulfur polymers [(C2S x ) n , wherein x is a real number from 2 to 50 and n is a real number satisfying n≥2].

[0056] In addition, the carbon may be selected from graphite, graphene, Super P, carbon black, DENKA carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, carbon nanofiber, carbon nanotube, carbon nanowire, carbon nanoring, carbon cloth and fullerene (C 60 ) in the group consisting of any one of the following.

[0057] In addition, the diameter of the sulfur-carbon composite 11 can be 5 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 15 μm to 60 μm. In this case, the diameter of the sulfur-carbon composite 11 refers to the length of the longest axis in the cross section of the particle of the sulfur-carbon composite. If the diameter is less than the above range, the surface area to be coated with the conductive polymer nanofibers will be too large to coat all of the surface area, and thus the coating effect may not be exhibited. If the diameter exceeds the above range, the non-uniformity during electrode formation may increase, which may have an adverse effect on performance.

[0058] The weight ratio of sulfur to carbon may be 60:40 to 90:10, preferably 65:35 to 85:15, and more preferably 70:30 to 80:20. If the weight ratio of carbon to sulfur is less than the range, the conductivity may be reduced. If the weight ratio of carbon to sulfur is greater than the range, the amount of active material may be reduced, thereby reducing the energy density.

[0059] Method for preparing sulfur-carbon composite

[0060] The present invention also relates to a method for preparing a sulfur-carbon composite containing a conductive polymer coating, the method comprising the following steps: (S1) preparing a concentrated dispersion containing a conductive polymer; (S2) preparing a sulfur-carbon composite by mixing sulfur powder and a carbon material; and (S3) mixing the concentrated dispersion and the sulfur-carbon composite and drying to form a conductive polymer coating on the sulfur-carbon composite.

[0061] Hereinafter, each step of the method for preparing the sulfur-carbon composite according to the present invention will be described in more detail.

[0062] Step (S1)

[0063] In step (S1), a concentrated dispersion containing a conductive polymer may be prepared.

[0064] The conductive polymer may have a shape capable of forming a network-type coating. The specific type and shape of the conductive polymer are as described above. Preferably, the conductive polymer may be polyaniline nanofibers.

[0065] A concentrated dispersion containing the conductive polymer can be prepared by repeating the process of dispersing and filtering the conductive polymer in water several times.

[0066] Step (S2)

[0067] In step (S2), the sulfur-carbon composite may be prepared by mixing sulfur and carbon.

[0068] In this case, sulfur and carbon are respectively in the form of particles, and the specific types and diameters of sulfur and carbon are as described above.

[0069] Specifically, sulfur and carbon may be dispersed in an organic solvent, heated and mixed while the sulfur is melted by a melt diffusion method to form a sulfur-carbon composite.

[0070] In this case, the organic solvent may be at least one selected from the group consisting of dimethyl sulfoxide, diethylene glycol methyl ethyl ether, ethylene glycol butyl ether, and 2-butoxyethyl acetate, but is not limited thereto. An organic solvent capable of dispersing sulfur and carbon may be widely used.

[0071] In addition, the heating temperature may be equal to or greater than the melting point of sulfur. That is, the heating temperature may be at least 115.21°C, preferably 130°C to 200°C, and more preferably 150°C to 200°C. If the heating temperature is lower than the above range, sulfur will not dissolve and sulfur-carbon composites cannot be formed. If the heating temperature exceeds the above range, the sulfur-carbon composite may be denatured, and therefore when used as a positive electrode material for a lithium secondary battery, the performance improvement effect of the battery may not be significant.

[0072] Step (S3)

[0073] In step (S3), the concentrated dispersion containing the conductive polymer obtained in step (S1), the sulfur-carbon composite obtained in step (S2), and a solvent may be mixed and dried to form a conductive polymer coating on the sulfur-carbon composite.

[0074] The solvent may be a solvent having good affinity with the sulfur-carbon complex, and may be at least one selected from the group consisting of water, ethanol, acetone, dichloromethane, and 1-methyl-2-pyrrolidone.

[0075] Lithium secondary battery

[0076] Another embodiment of the present invention also relates to a lithium secondary battery, which includes the sulfur-carbon composite as described above. In this case, the sulfur-carbon composite may be preferably included as a positive electrode active material.

[0077] The lithium secondary battery according to the present invention may include a positive electrode, a negative electrode, a separator interposed therebetween, and an electrolyte.

[0078] In the present invention, the positive electrode of the lithium secondary battery may include a positive electrode collector and a positive electrode mixture layer having a positive electrode active material formed on the positive electrode collector.

[0079] As the positive electrode active material, a lithium-containing transition metal oxide can be preferably used. For example, it can be selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(Ni a Co b Mn c )O2 (0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), LiNi 1-y Co y O2, LiCo 1-y Mn y O2, LiNi 1-y Mn y O2 (0 ≤ y < 1), Li(Ni a Co b Mn c )O4 (0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-z Ni z O4, LiMn 2-z Co z O4 (0 < z < 2), LiCoPO4, and LiFePO4, or a mixture of two or more thereof. In addition, in addition to these oxides, sulfides, selenides, halides, etc. can also be used.

[0080] In addition, the positive electrode current collector is not particularly limited as long as it has high conductivity and does not cause chemical changes in the relevant battery. For example, stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. can be used. In this case, the positive electrode current collector can be formed in various forms, such as a film, sheet, foil, mesh, net, porous body, foam, or non-woven fabric, with fine irregularities formed on its surface to enhance the adhesion to the positive electrode active material.

[0081] In the present invention, the negative electrode of the lithium secondary battery can include a negative electrode current collector and a negative electrode mixture layer having a negative electrode active material formed on the negative electrode current collector.

[0082] As the negative electrode active material, carbon materials, lithium metal, silicon, tin, etc., in which lithium ions can be embedded and deintercalated, can be used. Preferably, carbon materials can be used, and as carbon materials, both low-crystalline carbon and high-crystalline carbon can be used. The low-crystalline carbon is generally soft carbon and hard carbon. The high-crystalline carbon is generally natural graphite, primary graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, mesophase carbon microspheres, mesophase pitch and high-temperature calcined carbon, such as coke derived from petroleum or coal tar pitch. In this case, the negative electrode may include a binder. The binder may be various binder polymers, such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP copolymer), polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, etc.

[0083] In addition, the negative electrode current collector is not particularly limited as long as it has conductivity and does not cause chemical changes in the relevant battery, and for example, copper, stainless steel, aluminum, nickel, titanium, sintered carbon, or copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy can be used. In this case, like the positive electrode current collector, the negative electrode current collector can be formed in various forms such as a film, a sheet, a foil, a net, a porous body, a foam body, or a non-woven fabric, and the negative electrode current collector has fine concavoconvexity formed on its surface.

[0084] At this time, the positive electrode mixture layer or the negative electrode mixture layer may further contain a binder resin, a conductive material, a filler, and other additives.

[0085] The binder resin is used for bonding of electrode active materials and conductive materials and for bonding with current collectors. Examples of such binder resins may include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluorine-containing rubber and various copolymers thereof.

[0086] The conductive material is used to further improve the conductivity of the electrode active material. The conductive material is not particularly limited as long as it has conductivity and does not cause chemical changes in the relevant battery, and for example, graphite such as natural graphite or artificial graphite; carbon blacks such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; polyphenylene derivatives.

[0087] The filler is selectively used as a component for suppressing electrode expansion and is not particularly limited as long as it is a fiber material that does not cause chemical changes in the relevant battery, and for example, includes olefin polymers such as polyethylene and polypropylene; and fiber materials such as glass fiber and carbon fiber.

[0088] In the present invention, the separator may be formed of a porous substrate, and the porous substrate may be any porous substrate conventionally used in electrochemical devices. For example, a polyolefin-based porous film or nonwoven fabric may be used as the porous substrate, but is not particularly limited thereto.

[0089] Examples of the polyolefin-based porous film may include films formed of polyolefin-based polymers alone or in mixtures thereof, such as polyethylene, such as high-density polyethylene, linear low-density polyethylene, low-density polyethylene, and ultra-high molecular weight polyethylene; polypropylene; polybutene; and polypentene.

[0090] In addition to polyolefin nonwoven fabrics, the nonwoven fabrics may include, for example, polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, and polyphenylene sulfide, either alone or in combination. The structure of the nonwoven fabric may be a spunbond nonwoven fabric or a meltblown nonwoven fabric composed of long fibers.

[0091] The thickness of the porous substrate is not particularly limited, but may be 1 μm to 100 μm, preferably 5 μm to 50 μm.

[0092] The size and porosity of pores present in the porous substrate are also not particularly limited, but may be 0.001 μm to 50 μm and 10% to 95%, respectively.

[0093] In the present invention, the electrolyte may be a non-aqueous electrolyte, and the electrolyte salt contained in the non-aqueous electrolyte is a lithium salt. The lithium salt is not particularly limited as long as it can be conventionally used in an electrolyte for a lithium secondary battery. For example, the lithium salt may be selected from LiFSI, LiPF6, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiPF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, lithium chloroborane and lithium tetraphenylborate.

[0094] As the organic solvent contained in the nonaqueous electrolyte, those conventionally used for lithium secondary battery electrolytes can be used without restriction, and for example, ethers, esters, amides, linear carbonates, cyclic carbonates etc. can be used alone or in combination of two or more. Among them, representatively, carbonate compounds as cyclic carbonates, linear carbonates or their mixtures can be included.

[0095] Specific examples of cyclic carbonate compounds may include at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinyl ethylene carbonate and their halides, or a mixture of two or more thereof. Examples of such halides include, but are not limited to, fluoroethylene carbonate (FEC) and the like.

[0096] In addition, the specific examples of linear carbonate compounds can representatively include but are not limited to at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate and ethyl propyl carbonate, or a mixture of two or more thereof. Particularly, in carbonate organic solvents, ethylene carbonate and propylene carbonate as cyclic carbonates are high viscosity organic solvents and have high dielectric constants, thus lithium salts can be dissociated better in electrolytes. When these cyclic carbonates are mixed with the linear carbonates (such as dimethyl carbonate and diethyl carbonate) with low viscosity and low dielectric constant in a suitable ratio, an electrolyte with higher specific conductivity can be prepared.

[0097] In addition, the ether in the above organic solvent may be, but is not limited to, any one selected from the group consisting of dimethyl ether, ethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether and ethyl propyl ether, or a mixture of two or more thereof.

[0098] In addition, the ester in the above-mentioned organic solvent can be but is not limited to any one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone and ε-caprolactone, or a mixture of two or more thereof.

[0099] The injection of the non-aqueous electrolyte can be performed at an appropriate stage in the manufacturing process of the electrochemical device, depending on the manufacturing process and the desired physical properties of the final product. That is, such injection can be performed before assembling the electrochemical device or at the final stage of assembling the electrochemical device.

[0100] In the case of the lithium secondary battery according to the present invention, in addition to the winding process as a general process, a lamination or stacking and folding process of the separator and the electrode may be performed.

[0101] In addition, the shape of the battery case is not particularly limited, and may have various shapes such as a cylinder, a laminate, a prism, a pouch, or a coin. The structure and manufacturing method of these batteries are widely known in the art, and therefore a detailed description thereof will be omitted.

[0102] In addition, lithium secondary batteries may be classified into various batteries such as lithium-sulfur secondary batteries, lithium-air batteries, lithium oxide batteries, and lithium all-solid-state batteries according to the positive electrode materials / negative electrode materials used.

[0103] Furthermore, the present invention provides a battery module including the lithium secondary battery as a unit cell.

[0104] The battery module may be used as a power source for medium- or large-sized devices requiring high temperature stability, long cycle characteristics, and high capacity characteristics.

[0105] Examples of the medium or large-sized devices may include, but are not limited to, electric tools driven and moved by electric motors; electric vehicles, including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc.; electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems.

[0106] Lithium-sulfur secondary battery

[0107] The sulfur-carbon composite according to the present invention can be applied to a positive electrode of a lithium-sulfur secondary battery among lithium secondary batteries.

[0108] In this case, the lithium-sulfur secondary battery may be a battery including the above-mentioned sulfur-carbon composite as a positive electrode active material.

[0109] The sulfur-carbon composite can exhibit high ion conductivity by ensuring a migration path of lithium ions to the inside of pores, and serve as a carrier of sulfur, thereby increasing reactivity with sulfur as a positive electrode active material to simultaneously improve capacity and life characteristics of a lithium-sulfur secondary battery.

[0110] Modes for carrying out the invention

[0111] Hereinafter, preferred embodiments are provided to help understand the present invention, but the following embodiments are only used to illustrate the present invention, and it is obvious to those skilled in the art that various changes and modifications can be made within the scope and spirit of the present invention, and these changes and modifications fall within the scope of the appended claims.

[0112] Preparation Example 1: Synthesis of polyaniline nanofibers

[0113] The synthesis of polyaniline nanofibers as a conductive polymer was performed according to Jiaxing Huang et al. (Nanofiber Formation in the Chemical Polymerization of Aniline: A Mechanistic Study, Angew. Chem. Int. Ed., 2004, 43, 5817-5821).

[0114] Dissolve aniline in 1 M HCl to prepare 100 ml of 0.32 M aniline solution.

[0115] Dissolve ammonium persulfate in 1 M HCl to prepare 100 ml of 0.08 M ammonium persulfate solution.

[0116] The aniline solution and the ammonium persulfate solution are mixed to obtain a mixed solution.

[0117] When the mixed solution was formed, an initial reaction was performed while rapidly mixing at room temperature, and then the reaction was further performed for 10 hours in the state of the mixed solution to prepare a polyaniline nanofiber dispersion.

[0118] Example 1

[0119] (1) Preparation of sulfur-carbon composites

[0120] (1-1) Preparation of Concentrated Dispersion Containing Conductive Polymer

[0121] The polyaniline nanofiber dispersion obtained in Preparation Example 1 was filtered to filter out the polyaniline nanofibers except for the remaining reactants, and then these materials were redispersed in water and filtered several times to neutralize the pH value to above 6, thereby obtaining a polyaniline nanofiber concentrated dispersion having a concentration of 5%.

[0122] (1-2) Preparation of sulfur-carbon composite

[0123] Carbon nanotubes and sulfur were mixed in a weight ratio of 25:75, and sulfur was supported on carbon by melt diffusion at 155° C. to prepare a sulfur-carbon composite.

[0124] (1-3) Formation of network-type conductive polymer coating

[0125] The concentrated dispersion of polyaniline nanofibers obtained in (1-1), the sulfur-carbon composite obtained in (1-2), and ethanol were mixed at a weight ratio of 1:1:1.

[0126] After mixing, the obtained mixed solution was dried to remove the solvent, thereby preparing a sulfur-carbon composite having a polyaniline nanofiber coating. At this time, the sulfur-carbon composite having a polyaniline nanofiber coating contained 5 wt % of polyaniline.

[0127] (2) Preparation of positive electrode

[0128] The positive electrode was prepared by forming a positive electrode mixture layer including the sulfur-carbon composite on one surface of an aluminum current collector. At this time, the positive electrode mixture layer was prepared by mixing the above-mentioned sulfur-carbon composite, polyacrylic acid (PAA) as a binder, and carbon black in a weight ratio of 88:7:5, and then dispersing it in water to obtain a slurry, and coating the slurry on one surface of the aluminum current collector and drying it.

[0129] (3) Manufacturing of lithium-sulfur secondary batteries

[0130] A lithium-sulfur secondary battery in the form of a coin-type battery was prepared using a lithium foil having a thickness of 100 μm as a negative electrode, the positive electrode prepared in the above (2), an electrolyte (2-METHF: 2-methyltetrahydrofuran, DME: dimethoxyethane) using 2-METHF / DME (1:1 (volume ratio)) as an electrolyte solvent and containing LiTFSI (0.3 M) and LiNO3 (0.7 mass %), and a polyolefin separator.

[0131] Comparative Example 1

[0132] A sulfur-carbon composite was prepared in the same manner as in Example 1, except that the polyaniline nanofiber coating layer was not formed.

[0133] Comparative Example 2

[0134] After preparing the sulfur-carbon composite in which the polyaniline nanofiber coating layer was not formed as in Comparative Example 1, aniline was added to the electrolyte when manufacturing a coin-type battery, and a charging voltage was applied to form a polyaniline coating layer in the form of a film on the surface of the sulfur-carbon composite. At this time, the amount of aniline added was such that the content of polyaniline was 5% by weight based on the total weight of the sulfur-carbon composite on which the polyaniline coating layer was formed.

[0135] Figure 2 Graph showing the correlation between potential and current when a charging voltage is applied to an electrolyte solution containing aniline and an electrolyte solution not containing aniline according to Comparative Example 2.

[0136] Reference Figure 2, when aniline is added to the electrolyte and a charging voltage is applied, it can be seen that a polyaniline coating in the form of a film is formed on the surface of the sulfur-carbon composite. This is because of the following principle: when a charging voltage is applied, oxidation of aniline occurs electrochemically at the electrode to polymerize to produce polyaniline. That is, it can be confirmed from the increase in current observed at a voltage of 3.5 V that aniline is electrochemically polymerized into polyaniline, and a polyaniline coating is formed on the surface of the active material (J. Mater. Chem. A, 2014, 2, 18613-18623 | 18613).

[0137] Experimental Example 1: Scanning Electron Microscope (SEM) Analysis

[0138] Figure 3a and Figure 3b 1 and 2 are SEM images of the polyaniline nanofibers synthesized in Preparation Example 1 and the polyaniline nanofiber coating formed on the surfaces of the sulfur-carbon composite prepared in Example 1.

[0139] Reference Figure 3a and Figure 3b , it was confirmed that a coating was formed on the surface of the sulfur-carbon composite using polyaniline nanofibers to form a network-type coating.

[0140] Experimental Example 2: Analysis of the performance improvement effect of porous carbon structure on lithium-sulfur secondary batteries

[0141] The performance of lithium-sulfur secondary batteries in which the sulfur-carbon composites prepared in Example 1 and Comparative Example 1 were applied to the positive electrode was tested. A charge / discharge experiment was performed using the manufactured coin-type battery, and after 3 cycles at 0.1C / 0.1C and 3 cycles at 0.2C / 0.2C, the charge / discharge current density was evaluated at 0.3C / 0.5C.

[0142] Figure 4 is a graph showing first discharge curves as evaluation results of coin-type batteries of lithium-sulfur secondary batteries prepared in Example 1 and Comparative Examples 1 and 2, respectively, and Figure 5 Graphs showing cycle-discharge capacity curves of lithium-sulfur secondary batteries prepared in Example 1 and Comparative Examples 1 and 2, respectively.

[0143] Reference Figure 4 and Figure 5 , it was confirmed that the initial discharge capacity of the lithium-sulfur secondary battery of Example 1 was higher than that of Comparative Example 1, and furthermore, the overvoltage in the initial discharge end was improved and the life characteristics were improved.

[0144] In addition, it was confirmed that in Comparative Example 2, the overvoltage was partially improved compared to Comparative Example 1, but a polyaniline coating was formed in a film form, and thus the voltage decreased at the end of discharge, thereby not showing sufficient capacity, and showing poor performance compared to Example 1.

[0145] Although the present invention has been described above by limited embodiments and drawings, the present invention is not limited thereto, and it is obvious to those skilled in the art that various modifications and changes can be made within the technical concept of the present invention and the equivalent scope of the claims described below.

[0146] [Description of symbols]

[0147] 10: Sulfur-carbon composites containing conductive polymer coatings

[0148] 11: Sulfur-carbon complex

[0149] 12: Conductive polymer coating

Claims

1. A sulfur-carbon composite comprising a network-type conductive polymer coating, The network type means that the coating formed on the surface of the sulfur-carbon composite is not formed on the entire surface of the sulfur-carbon composite, but is formed in a network shape, with a portion of the surface of the sulfur-carbon composite exposed. In the network type conductive polymer coating, a space is formed in a portion where a portion of the surface of the sulfur-carbon composite is exposed, The sulfur-carbon composite comprises: a sulfur particle containing at least one carbon particle therein, and a carbon particle located on a part or all of the surface of the sulfur particle, The conductive polymer is contained in an amount of 0.1 wt % to 7 wt % based on the total weight of the sulfur-carbon composite including the network-type conductive polymer coating layer.

2. The sulfur-carbon composite according to claim 1, wherein the network-type conductive polymer is at least one selected from the group consisting of polyaniline, polypyrrole, polythiophene, poly(3,4-ethylenedioxythiophene), polyacetylene, polydiacetylene, poly(thiophene vinylene), polyfluorene and derivatives thereof. 3 . The sulfur-carbon composite according to claim 1 , wherein the network-type conductive polymer is in the form of at least one nanostructure selected from the group consisting of nanofibers, nanowires, nanorods, and nanotubes.

4. The sulfur-carbon composite according to claim 1, wherein the weight ratio of sulfur to carbon is 6:4 to 9:

1.

5. The sulfur-carbon composite according to claim 1, wherein the sulfur is selected from sulfur S8, Li2S n , organic sulfur compounds and (C2S x ) n At least one of the group consisting of carbon-sulfur polymers represented by The Li2S n where n is a real number satisfying n ≥ 1, and The (C2S x ) n Where x is a real number from 2 to 50 and n is a real number satisfying n≥2.

6. The sulfur-carbon composite according to claim 1, wherein the carbon is selected from the group consisting of graphite, graphene, carbon black, carbon fiber, carbon nanofiber, carbon nanotube, carbon nanowire, carbon nanoring, carbon cloth and fullerene (C 60 ) is at least one of the group consisting of. 7 . A positive electrode comprising the sulfur-carbon composite according to claim 1 . 8 . A lithium secondary battery comprising the sulfur-carbon composite according to claim 1 . 9 . The lithium secondary battery according to claim 8 , wherein the lithium secondary battery is a lithium-sulfur secondary battery.

Citation Information

Patent Citations

  • Exothermic body band and exothermic under-shirt with spandex fabric made in one piece ,and exothermic pad with spandex fabric and other fabrics made of split and a method fixing the same

    KR1020180112636A

  • Organic polymer-silicon composite particle, preparation method for same, and cathode and lithium secondary battery including same

    CN102792498A

  • Carbon-sulfur-shell matter composite material having network dual-core shell structure and preparation method thereof

    CN103474633A

  • Sulfur carbon composite material based on polyaniline nanotubes and preparation method thereof, and secondary battery

    CN104157829A

  • Nano carbon / sulfur composite for lithium-sulfur batteries

    CN106159221A