Positive active material

By placing the cover layer of lithium metal composite oxide and specific element oxide on the surface of the core particles of the electrode active substance, and adjusting the molar ratio of Li/M, the increase in the interface resistance of the electrode active substance and the sulfide solid electrolyte in the all-solid battery is solved. The problem of improving the conductivity of lithium ions and the circulation characteristics of the battery.

CN112368862BActive Publication Date: 2024-11-01MITSUI MINING & SMELTING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN201980044668.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-25
Filing Date
2019-07-23
Publication Date
2024-11-01
Estimated Expiration
2039-07-23

AI Technical Summary

Technical Problem

In all-solid batteries containing sulfide solid electrolytes, the interface resistance between the electrode active substance and the sulfide solid electrolyte is prone to rise, limiting the migration of lithium ions.

Method used

By placing a cover layer on the surface of the core particles of the electrode active material, the cover layer consists of oxides containing lithium metal composite oxides and specific elements, such as Li and M (such as B, Nb, Ti, Zr, Ta, Zn, W ) oxide, adjust the molar ratio of Li/M to 0.85 or more and 3.95 or less to suppress the rise of the interface resistance.

Benefits of technology

It effectively suppresses the rise of the interface resistance between the electrode active substance and the sulfide solid electrolyte, improves the conductivity of lithium ions, extends the cycling characteristics of the battery, and reduces the interface resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002878527230000131
    Figure BDA0002878527230000131
Patent Text Reader

Abstract

The present invention provides a positive electrode active material that can suppress the interface resistance between a positive electrode active material and a sulfide solid electrolyte from increasing over time and has a low interface resistance. The positive electrode active material of the present invention comprises particles having a core material particle containing a lithium metal composite oxide and a covering layer disposed on the surface of the core material particle, and is used for an all-solid battery comprising a sulfide solid electrolyte. The above-mentioned covering layer is composed of an oxide comprising Li and M (M is one or more elements selected from the group consisting of B, Nb, Ti, Zr, Ta, Zn, W and Al, and one is B.). The molar ratio of Li / M in the surface of the above-mentioned covering layer obtained by X-ray photoelectron spectroscopy is greater than 0.85 and less than 3.95.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material for an all-solid-state battery containing a sulfide solid electrolyte. Background Art

[0002] Lithium ion secondary batteries are widely used as power sources for portable electronic devices such as notebook personal computers and mobile phones due to their high energy density, small size and light weight. In addition, the development of high-output, high-capacity lithium ion secondary batteries for electric vehicles and hybrid electric vehicles has been promoted recently.

[0003] At present, most lithium-ion secondary batteries use electrolytes containing flammable organic solvents. Therefore, when the battery becomes hot due to a short circuit, there is a risk of the electrolyte catching fire. In contrast, all-solid batteries that use solid electrolytes instead of electrolytes and do not contain flammable organic solvents have a lower risk of catching fire, so they are expected to be practical as batteries that have both safety and high energy density.

[0004] As one of the solid electrolytes used in all-solid batteries, sulfide solid electrolytes have been studied. However, all-solid batteries containing sulfide solid electrolytes have the following problems: if they are charged and discharged, the interface resistance between the electrode active material and the sulfide solid electrolyte becomes high, and the migration of lithium ions is restricted. It is believed that the reason is that the electrode active material reacts with the sulfide solid electrolyte to form a resistance layer at their interface. In response to this problem, attempts have been made to suppress the increase in interface resistance by covering the surface of the positive electrode active material with a specific compound (Patent Documents 1 to 3).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2012-99323

[0008] Patent Document 2: US2014 / 072875A1

[0009] Patent Document 3: Japanese Patent Application Publication No. 2015-201388 Summary of the invention

[0010] If the surface of the positive electrode active material is covered with a specific compound or the like for the purpose of reducing the interface resistance between the electrode active material and the sulfide solid electrolyte, the increase in interface resistance over time can be suppressed. However, on the other hand, there is a problem that the interface resistance is likely to increase.

[0011] The present invention has been made in view of the above-mentioned problems, and a main object of the present invention is to provide a positive electrode active material which can suppress the interface resistance between the electrode active material and the sulfide solid electrolyte from increasing over time and has a low interface resistance.

[0012] The present inventors have conducted in-depth research and found that the above-mentioned problem can be solved by configuring a specific covering layer on the surface of the electrode active material particles. That is, the present invention provides a positive electrode active material, which comprises a core particle containing a lithium metal composite oxide and a covering layer configured on the surface of the core particle, and is used for a fully solid battery comprising a sulfide solid electrolyte, wherein the covering layer is composed of an oxide comprising Li and M (M is one or more elements selected from the group consisting of B, Nb, Ti, Zr, Ta, Zn, W and Al, and in the case of one element, B.), and the molar ratio of Li / M in the surface of the covering layer determined by X-ray photoelectron spectroscopy is greater than 0.85 and less than 3.95. DETAILED DESCRIPTION

[0013] The present invention relates to a positive electrode active material used in an all-solid-state battery. The positive electrode active material of the present invention comprises a particle having a core particle containing a lithium metal composite oxide and a covering layer disposed on the surface of the core particle. The covering layer may completely cover the surface of the core particle, or may partially cover the surface of the core particle in a manner that a portion of the surface of the core particle is exposed.

[0014] As the lithium metal composite oxide, a known lithium metal composite oxide can be used. As the metal, both transition elements and main group elements (typical elements) can be used, preferably transition elements. As the lithium metal composite oxide, for example, lithium transition metal oxides such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4) and lithium nickel cobalt manganese oxide (Li(Ni, Co, Mn)O2) can be listed.

[0015] In the present invention, as the lithium metal composite oxide, it is preferred to use the general formula (1): Li 1+x M 1 1-x O2(where M 1 The compound represented by Mn, Co and Ni, and a metal selected from the group consisting of transition elements between Group 3 elements and Group 11 elements in the periodic table and main group elements up to the third period of the periodic table. The structure of the above-mentioned compound is not particularly limited, for example, it can be a layered rock salt type compound, or it can also be a spinel type compound.

[0016] In the general formula (1), "1+x" is preferably 1.00 or more and 1.07 or less, more preferably 1.01 or more and 1.06 or less, and further preferably 1.02 or more and 1.05 or less. If the value of "1+x" is 1.00 or more, that is, the lithium ion is 1.00 or more, the instability of the structure caused by charge and discharge can be suppressed, and high cycle characteristics can be achieved, which is preferred.

[0017] In the above general formula (1), "M 1 "It can be any metal as long as it is Mn, Co and Ni, and a metal selected from the group consisting of transition elements existing between the 3rd group elements and the 11th group elements of the periodic table and main group elements up to the 3rd period of the periodic table. Examples of transition elements existing between the 3rd group elements and the 11th group elements of the periodic table and main group elements up to the 3rd period of the periodic table include Al, V, Fe, Ti, Mg, Cr, Ga, In, Cu, Zn, Nb, Zr, Mo, W, Ta, Re, etc. "Mn 1 " may be composed of only three elements of Mn, Co and Ni, or may contain other elements mentioned above in addition to these three elements.

[0018] In the above “M 1 "When containing three elements of Mn, Co and Ni, the molar ratio of Mn, Co and Ni is preferably Mn:Co:Ni=0.10~0.45:0.03~0.40:0.30~0.85, among which Mn:Co:Ni=0.10~0.40:0.03~0.40:0.30~0.80 is further preferred. It should be noted that in the above general formula (1), the ratio of oxygen atoms is recorded as "2" for convenience, but it can also have a certain non-stoichiometric amount.

[0019] The core particles used in the present invention preferably contain 80% by mass or more of lithium metal composite oxide, more preferably 90% by mass or more, and particularly preferably 95% by mass or more. In addition, the core particles may also be formed only of lithium metal composite oxide. Only one lithium metal composite oxide may be used, or two or more may be used in combination.

[0020] The covering layer disposed on the surface of the core material particle is composed of an oxide containing Li and M (M is one or more elements selected from the group consisting of B, Nb, Ti, Zr, Ta, Zn, W and Al, and in the case of one element, it is B.). In the case where the covering layer contains Li and B and contains elements other than these elements, the covering layer may also be composed of a single oxide containing Li, B and other elements. Alternatively, the covering layer may also be composed of a mixture of multiple oxides containing oxides containing Li and B, and oxides containing Li and other elements. Examples of oxides constituting the covering layer include LiBO2, Li3BO3, Li8Nb6O 19 , Li2B4O7, LiB5O8, LiNbO3, etc., but are not limited to these.

[0021] The molar ratio of Li / M in the surface of the above-mentioned covering layer obtained by X-ray photoelectron spectroscopy (XPS) is preferably 0.85 or more and 3.95 or less, more preferably 1.0 or more and 3.8 or less, further preferably 1.5 or more and 3.5 or less, and most preferably 1.9 or more and 3.3 or less. By setting the molar ratio of Li / M within these ranges, the interface resistance between the positive electrode active material and the sulfide solid electrolyte can be suppressed from rising over time, and the interface resistance can be reduced. Specifically, by setting the molar ratio of Li / M to more than 0.85, the Li ion conductivity of the covering layer is improved. On the other hand, by setting the molar ratio of Li / M to less than 3.95, the generation of lithium carbonate and Li3BO3 can be suppressed, and the rise of interface resistance can be suppressed. In addition, by setting the molar ratio of Li / M within the above range, not only the generation of lithium carbonate is suppressed, but also LiBO2 becomes easy to generate. Since it is believed that LiBO2 is not easy to increase the interface resistance compared with Li3BO3, it is advantageous to generate LiBO2 instead of Li2BO3. The molar ratio of Li / M can be set to a desired value by adjusting the molar ratio of Li / M in the raw material used for forming the covering layer.

[0022] The proportion of B in the positive electrode active material of the present invention is preferably 0.02% by mass or more and 3.5% by mass or less, more preferably 0.1% by mass or more and 3.3% by mass or less, and further preferably 0.5% by mass or more and 3.0% by mass or less. By setting the proportion of B within this range, the interface resistance can be effectively reduced. The proportion of B in the positive electrode active material can be set to a desired value by adjusting the amount ratio of the core material particles and the raw material of the covering layer when forming the covering layer.

[0023] In the present invention, the above-mentioned covering layer may be composed only of an oxide containing Li and B. In this case, the molar ratio of Li / B in the surface of the covering layer obtained by XPS is preferably 0.85 or more and 3.95 or less, more preferably 1.0 or more and 3.8 or less, further preferably 1.5 or more and 3.5 or less, and most preferably 1.9 or more and 3.3 or less. It should be noted that the value of Li in the above-mentioned Li / B also includes the value of Li caused by the core particles.

[0024] In the present invention, as described above, the above-mentioned covering layer can also be composed of oxides containing other elements in addition to Li and B. As the covering layer, an oxide containing one or more elements selected from the group consisting of, for example, Nb, Ti, Zr, Ta, Zn, W and Al can be used in addition to Li and B. Among them, an oxide containing Nb can be preferably used. The mass ratio of Nb / B in the positive electrode active material in this case is preferably greater than 1 and less than 30, more preferably greater than 3 and less than 25, and further preferably greater than 5 and less than 20. By setting the mass ratio of Nb / B within these ranges, a positive electrode active material with low interface resistance is obtained. The mass ratio of Nb / B in the positive electrode active material can be set to a desired value by adjusting the mass ratio of Nb / B of the covering layer when forming the covering layer. In addition, Nb is common to Ti, Zr, Ta, Zn, W and Al in being a valve metal. Since the oxide of the valve metal exhibits excellent corrosion resistance, it has a function of suppressing surface reaction, and it is considered that the same effect can be obtained even if the oxide contains the above-mentioned elements other than Nb.

[0025] The total amount of B and Nb in the positive electrode active material of the present invention preferably accounts for more than 0.5 mass % and less than 2.5 mass %, more preferably less than 2.0 mass %, and more preferably less than 1.5 mass %. If the ratio of the total amount of B and Nb exceeds this range, the interface resistance sometimes becomes larger. The total amount of B and Nb in the positive electrode active material can be adjusted when forming the covering layer. The ratio of the raw material of the core material particles and the covering layer can be set to the desired value.

[0026] When an oxide containing Li and Nb is used as a constituent component, the molar ratio of Li / (B+Nb) in the surface of the covering layer obtained by XPS is preferably 1.5 to 3.6, and more preferably 2.5 to 3.5. By setting the molar ratio of Li / (B+Nb) within these ranges, the generation of Nb2O5 or B2O3 that can become a resistance layer can be suppressed, and the increase in interface resistance over time can be suppressed.

[0027] The core particles containing lithium metal composite oxide used in the present invention are obtained by, for example, weighing and mixing raw materials such as lithium salt compounds, manganese salt compounds, nickel salt compounds and cobalt salt compounds, crushing them by a wet pulverizer, granulating, calcining, heat treating as needed, crushing under preferred conditions, and further classifying as needed. Instead of this method, the core particles can also be obtained by adding an alkaline substance such as sodium hydroxide to an aqueous solution containing a manganese salt compound, a nickel salt compound and a cobalt salt compound to precipitate a metal composite hydroxide, and then mixing the metal composite hydroxide with a lithium salt compound and calcining.

[0028] Examples of raw material lithium salt compounds include lithium hydroxide (LiOH), lithium carbonate (Li2CO3), lithium nitrate (LiNO3), LiOH·H2O, lithium oxide (Li2O), fatty acid lithium, and lithium halides, among which lithium hydroxide, carbonate, and nitrate are preferred.

[0029] Examples of the manganese salt compound include manganese carbonate, manganese nitrate, manganese chloride, and manganese dioxide, among which manganese carbonate and manganese dioxide are preferred, and electrolytic manganese dioxide obtained by electrolysis is particularly preferred.

[0030] Examples of the nickel salt compound include nickel carbonate, nickel nitrate, nickel chloride, nickel oxyhydroxide, nickel hydroxide, and nickel oxide. Among them, nickel carbonate, nickel hydroxide, and nickel oxide are preferred.

[0031] Examples of the cobalt salt compound include basic cobalt carbonate, cobalt nitrate, cobalt chloride, cobalt oxyhydroxide, cobalt hydroxide, and cobalt oxide. Among them, basic cobalt carbonate, cobalt hydroxide, cobalt oxide, and cobalt oxyhydroxide are preferred.

[0032] The raw materials are preferably mixed by adding a liquid medium such as water or a dispersant and wet mixing to form a slurry. When the spray drying method described below is used, the obtained slurry is preferably pulverized with a wet pulverizer, but dry pulverization may also be performed.

[0033] The granulation method can be either wet or dry as long as the various raw materials crushed in the previous step are dispersed in the granulated particles without separation. Examples thereof include extrusion granulation, tumbling granulation, fluidized bed granulation, mixing granulation, spray drying granulation, pressure molding granulation, and sheet granulation using a roller or the like.

[0034] In the case of wet granulation, it is necessary to fully dry before calcination. As a drying method, it is sufficient to dry it by a known drying method such as spray heat drying, hot air drying, vacuum drying, freeze drying, etc., wherein spray heat drying is preferred. Spray heat drying is preferably carried out using a thermal spray dryer (spray dryer).

[0035] The calcination is preferably carried out in a calcination furnace in an atmosphere, an oxygen atmosphere, an atmosphere with an adjusted oxygen partial pressure, a carbon dioxide gas atmosphere, or other atmospheres, at a temperature higher than 800° C. and lower than 1000° C., preferably 810 to 1000° C., and more preferably 810 to 950° C., for 0.5 to 30 hours. At this time, it is preferred to select a calcination condition in which the transition metal is solid-dissolved at the atomic level and becomes a single phase. The type of calcination furnace is not particularly limited, and for example, a rotary kiln, a static furnace, and other calcination furnaces can be used for calcination.

[0036] The heat treatment after sintering is preferably performed when it is necessary to adjust the crystal structure. For example, the heat treatment is performed under oxidizing atmosphere conditions such as air atmosphere, oxygen atmosphere, or atmosphere with adjusted oxygen partial pressure.

[0037] The crushing after sintering or heat treatment is not limited, but is preferably performed using a high-speed rotating pulverizer. By using a high-speed rotating pulverizer for crushing, particles can be agglomerated or portions weakened by sintering can be crushed, thereby suppressing the generation of strain in the particles.

[0038] As a method for forming a coating layer on the surface of the core material particles obtained by the above operation, it is sufficient to bring a treatment solution containing Li and B and other elements as needed into contact with the core material particles. For example, in the case of forming a coating layer composed of oxides containing Li and B, a method of mixing a treatment solution containing Li and B with the core material particles and drying them can be cited. Specifically, by mixing a treatment solution obtained by dissolving LiOH·H2O and H3BO3 in water with the core material particles and drying them, the core particles are crushed and heat-treated as needed, so that a coating layer composed of oxides containing Li and B can be formed on the surface of the core material particles. The raw materials used in the preparation of the treatment solution can be any compound as long as they contain the required elements, for example, oxides, halides, hydroxides, carbonates and nitrates can be used.

[0039] The amount of the treatment solution is preferably adjusted so that the proportion of B in the positive electrode active material is 0.02 mass % or more and 3.5 mass % or less, more preferably adjusted so that the proportion of B in the positive electrode active material is 0.1 mass % or more and 3.3 mass % or less, and further preferably adjusted so that the proportion of B in the positive electrode active material is 0.5 mass % or more and 3.0 mass % or less. The concentration of the treatment solution is not particularly limited, but is preferably 1 to 10 mass % because the operation becomes easy.

[0040] The volume cumulative particle size D of the positive electrode active material obtained in this manner at a cumulative volume of 50% by volume was obtained by laser diffraction scattering particle size distribution measurement. 50is 20 μm or less, where it is less than 15 μm, where it is more than 1 μm and less than 10 μm, and where it is further more than 2 μm and 8 μm or less. If D 50 being 20 μm or less is more preferable, good contact with the solid electrolyte in the binder can be ensured, and the utilization rate of lithium ions in the active material can be increased, so it is preferable. Also, if D 50 is greater than 1 μm, particle aggregation can be prevented and the viscosity of the slurry can be increased. In order to adjust the D 50 of the positive electrode active material to the above range, it is sufficient to adjust the D 50 of the starting material, adjust the firing temperature or firing time, or adjust the crushing conditions after firing, etc., but it is not limited to these adjustment methods.

[0041] The positive electrode active material of the present invention is a positive electrode active material for an all-solid battery having a solid electrolyte. In particular, it is advantageous that the positive electrode active material of the present invention is used in an all-solid battery containing a sulfide solid electrolyte as the solid electrolyte. In the all-solid battery, the effects of the present invention can be enjoyed by the presence of the contact portion between the positive electrode active material of the present invention and the sulfide solid electrolyte. The so-called "presence of the contact portion between the positive electrode active material and the sulfide solid electrolyte" means any of (a) containing a sulfide solid electrolyte in the positive electrode binder (in this case, the solid electrolyte layer may also be a non-sulfide), (b) not containing a sulfide solid electrolyte in the positive electrode binder and containing a sulfide solid electrolyte in the solid electrolyte layer, and (c) containing a sulfide solid electrolyte in the positive electrode binder and containing a sulfide solid electrolyte in the solid electrolyte layer.

[0042] The sulfide solid electrolyte used in the present invention only needs to contain Li and S and have lithium ion conductivity. The sulfide solid electrolyte can be any of a crystalline material, a glass-ceramic, and a glass. As the sulfide solid electrolyte, for example, Li2S-P2S5, Li2S-P2S5-LiHa ("Ha" represents one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 、Li 3.25 Ge 0.25 P 0.75 S4、Li7P3S 11 、Li 3.25 P 0.95 S4、Li 7-x PS 6-x Ha x (lithium germanium sulfide solid electrolyte, "Ha" represents one or more halogen elements, 0.2 < x < 1.8), etc.

[0043] The positive electrode active material of the present invention may also be used in combination with other positive electrode active materials. As other positive electrode active materials, particles formed from the above-mentioned known lithium metal composite oxides may be listed, and the particles may or may not have a covering layer. When used in combination, it is preferred that the positive electrode active material of the present invention is contained in an amount of 50 mol% or more, more preferably 70% or more, relative to the entire active material.

[0044] The positive electrode active material of the present invention can be made into a positive electrode mixture of a fully solid-state battery by mixing with the above-mentioned sulfide solid electrolyte as needed. The ratio of the mixed sulfide solid electrolyte to the whole positive electrode mixture is typically 10 to 50% by weight. In addition, the positive electrode mixture may also contain other materials such as a conductive additive or a binder as needed. In addition, the positive electrode can be made by mixing the above-mentioned positive electrode mixture with a solvent to make a paste, applying it to a collector such as aluminum foil and drying it.

[0045] As conductive auxiliary agent, for example, artificial graphite, carbon black (acetylene black) etc. can be preferably used. As adhesive, for example, PVdF copolymer resins such as the copolymer of polyvinylidene fluoride (PVdF), PVdF and hexafluoropropylene (HFP) or perfluoromethyl vinyl ether (PFMV) and tetrafluoroethylene, polytetrafluoroethylene, fluorine-based resins such as fluorine-based resins such as fluororubber, styrene-butadiene copolymer, styrene-acrylonitrile copolymer, hydrocarbon polymers such as carboxymethyl cellulose, polyimide resin etc. can be used, but are not limited to this. In addition, they can be used alone, and two or more can be mixed and used.

[0046] A fully solid battery can be produced by a known method using the positive electrode active material of the present invention. For example, a fully solid battery can be produced by stacking the three layers of the positive electrode, solid electrolyte layer and negative electrode produced as described above and performing pressure molding.

[0047] As the negative electrode active material used in the negative electrode, materials for intercalating and deintercalating lithium ions, such as carbon materials, silicon and Si-O silicon oxide compounds, lithium titanate and other known materials can be used. As the carbon material, for example, materials obtained by sintering organic polymer compounds such as polyacrylonitrile, phenolic resin, novolac resin, cellulose, artificial graphite or natural graphite can be listed. In addition to using such a negative electrode active material, the negative electrode can be manufactured in the same manner as the positive electrode.

[0048] Example

[0049] Hereinafter, the present invention will be described in more detail based on examples. However, the present invention is not limited to the examples shown below.

[0050] [Example 1]

[0051] (1) Production of core particles

[0052] Sodium hydroxide was supplied to an aqueous solution obtained by dissolving nickel sulfate, cobalt sulfate and manganese sulfate, and a metal composite hydroxide was prepared by a coprecipitation method. The molar ratio of nickel, cobalt and manganese in the metal composite hydroxide was Ni:Co:Mn=0.6:0.2:0.2. The metal composite hydroxide was mixed with lithium carbonate, pre-calcined at 720°C for 5 hours in an atmospheric furnace, and then formally calcined at 905°C for 22 hours in the atmospheric atmosphere to obtain a lithium metal composite oxide. The lithium metal composite oxide was crushed with a mortar, and then classified with a sieve with a mesh of 53μm, and the core particles composed of lithium metal composite oxide powder under the sieve were recovered. The core particles are layered rock salt type compounds, and the molar ratio of nickel, cobalt and manganese is the same as the above-mentioned metal composite hydroxide, Ni:Co:Mn=0.6:0.2:0.2.

[0053] (2) Manufacturing of positive electrode active material

[0054] 4.194 g of LiOH·H2O and 6.181 g of H3BO3 were dissolved in 200 mL of water to prepare a treatment solution. The treatment solution was referred to as treatment solution A. 4.8 mL of treatment solution A was added to 10 g of the core particles obtained in (1) above, stirred at 25°C for 1 hour, and dried at 130°C for 2 hours. The obtained solid was heat-treated at 350°C for 5 hours in an atmospheric atmosphere to obtain a positive electrode active material.

[0055] [Example 2]

[0056] A positive electrode active material was obtained by the same method as in Example 1 except that 12 mL of the treatment solution A was added.

[0057] [Example 3]

[0058] A positive electrode active material was obtained by the same method as in Example 1 except that 28 mL of the treatment solution A was added.

[0059] [Example 4]

[0060] A positive electrode active material was obtained by the same method as in Example 1 except that 55 mL of the treatment solution A was added.

[0061] [Example 5]

[0062] 0.76 g of LiOH·H2O and 3.75 g of (NH4)3Nb(O2)4 were dissolved in 75 mL of water to prepare a treatment solution. The treatment solution was referred to as treatment solution B. 3.3 mL of treatment solution A and 4.7 mL of treatment solution B were added to 10 g of the core particles used in Example 1, stirred at 25°C for 1 hour, and dried at 130°C for 2 hours. The obtained solid was heat-treated at 350°C for 5 hours in an atmospheric atmosphere to obtain a positive electrode active material.

[0063] [Example 6]

[0064] A positive electrode active material was obtained by the same method as in Example 5 except that 6.6 mL of the treatment solution A and 9.5 mL of the treatment solution B were added.

[0065] [Example 7]

[0066] A positive electrode active material was obtained by the same method as in Example 5 except that 6.6 mL of the treatment solution A and 9.5 mL of the treatment solution B were added.

[0067] [Example 8]

[0068] 12.582 g of LiOH·H2O and 6.181 g of H3BO3 were dissolved in 200 mL of water to prepare a treatment liquid. This treatment liquid is referred to as treatment liquid C. 10.4 mL of treatment liquid C was added to 10 g of the core particles used in Example 1. A positive electrode active material was obtained by the same method as in Example 1 except for the above.

[0069] [Example 9]

[0070] 0.04194 g of LiOH·H2O and 6.181 g of H3BO3 were dissolved in 200 mL of water to prepare a treatment liquid. This treatment liquid is referred to as treatment liquid D. 10.4 mL of treatment liquid D was added to 10 g of the core particles used in Example 1. A positive electrode active material was obtained by the same method as in Example 1 except for the above.

[0071] [Comparative Example 1]

[0072] The core particles obtained in Example 1 were used as positive electrode active material as they were.

[0073] [Comparative Example 2]

[0074] A positive electrode active material was obtained by the same method as in Example 8 except that 55 mL of the treatment solution C was added.

[0075] [Comparative Example 3]

[0076] A positive electrode active material was obtained by the same method as in Example 9 except that 28 mL of the treatment solution D was added.

[0077] 〔evaluate〕

[0078] The content of each element and D of the positive electrode active materials obtained in the examples and comparative examples were measured by the following steps. 50 In addition, the positive electrode active materials obtained in the examples and comparative examples were analyzed by XPS. Furthermore, batteries using the positive electrode active materials obtained in the examples and comparative examples were prepared by the following method, and the interface resistance was measured. The results are shown in Table 1 below.

[0079] 〔Content of each element〕

[0080] The positive electrode active material was dissolved in aqua regia, and the solution was diluted with water. The diluted solution was analyzed by an ICP emission spectrometer to determine the content of each element.

[0081] 〔D 50 Determination of

[0082] An automatic sample feeder for a laser diffraction particle size distribution measuring device ("Microtorac SDC" manufactured by Nikkiso Co., Ltd.) was used. The positive electrode active material was put into a water-soluble solvent (water: ethanol = 80:20 (volume ratio)), and the solution was put into the specified line of the device. Then, after irradiating with 40W ultrasonic waves for 360 seconds at a flow rate of 80%, the particle size distribution was measured using a laser diffraction particle size distribution measuring device "MT3000II" manufactured by Nikkiso Co., Ltd. The measuring liquid was passed through a 60μm filter, and D was calculated from the volume-based particle size distribution chart obtained by the measurement. 50 The setting conditions of the device are as follows.

[0083] Solvent refractive index: 1.33

[0084] Particle Transmittance Condition: Transmittance

[0085] Particle refractive index: 2.46

[0086] Shape: Non-spherical

[0087] Measuring range: 0.133~704.0μm

[0088] The measurement time is set to 30 seconds, and the average value of the two measurements is set as D 50 .

[0089] [Analysis using XPS]

[0090] As an XPS analysis apparatus, "XPS Quantam 2000" manufactured by ULVAC-PHI was used. The molar ratio of Li / M was calculated from the ratio of the elements present on the outermost surface of the positive electrode active material. The equipment specifications and conditions used in the measurement are as follows.

[0091] X-ray source: monochromated AlKα1 (1486.7eV)

[0092] X-ray output power: 100W

[0093] X-ray irradiation area: 100μmφ×1mm

[0094] Pass energy: 23.5eV

[0095] Measurement interval: 0.1eV

[0096] Determination of elements and orbitals:

[0097] Li: 1s

[0098] Nb: 3d

[0099] B: 1s

[0100] O: 1s

[0101] C: 1s

[0102] 〔Measurement of interface resistance〕

[0103] The positive electrode active materials of the examples and comparative examples were used to prepare a positive electrode according to a conventional method. Specifically, the obtained positive electrode active material and Li sulfide solid electrolyte (argyrodite-type solid electrolyte) were mixed. 5.8 PS 4.8 Cl 1.2 The positive electrode mixture was prepared by mixing VGCF (registered trademark) as a conductive additive at a mass ratio of 80:17:3, and this was used as the positive electrode. In addition, graphite was used as the negative electrode active material, and the negative electrode was prepared according to a conventional method. Next, the positive electrode and Li 2+ as a sulfide solid electrolyte (argyrodite-type solid electrolyte) were mixed. 5.8 PS 4.8 Cl 1.2 ) and the negative electrode are sequentially stacked and press-formed to produce an all-solid-state battery. For this all-solid-state battery, after the 3rd and 300th cycles of charge and discharge, the AC impedance was measured after charging to 40% of the discharge capacity respectively. The interface resistance value (Ω) is calculated from the intersection of the complex impedance plane diagram of the measurement results, i.e., the Cole-Cole diagram, with the horizontal axis. Furthermore, the difference between the interface resistance value R2 after 300 cycles and the interface resistance value R1 (the increase in reaction resistance, R2-R1) is expressed as a percentage relative to the interface resistance value R1, which is taken as the interface resistance increase rate. That is, the interface resistance increase rate is expressed as (R2-R1) / R1×100.

[0104] The equipment specifications and conditions used in the measurement are as follows.

[0105] ·Measurement device: SOLARTRON 1255B FREQUENCY RESPONSIVE ANALYZER from TOYO CORPORATION

[0106] AC amplitude: 10mV

[0107] Frequency range: 1.0×10 6 ~1.0×10 1 Hz

[0108]

[0109] As shown in the results shown in Table 1, it is judged that the interface resistance of the all-solid-state battery using the positive electrode active material obtained in each example and the rate of increase of the interface resistance after 300 cycles are both reduced. In contrast, the all-solid-state battery using the positive electrode active material obtained in Comparative Example 1 has a low interface resistance, but the rate of increase of the interface resistance becomes very high.

[0110] The all-solid-state battery using the positive electrode active material obtained in Comparative Example 2 has a high molar ratio of Li / M, so it is believed that lithium carbonate and BO3 are generated. 3- , the interface resistance and the rate of increase of interface resistance become higher.

[0111] In the all-solid-state battery using the positive electrode active material obtained in Comparative Example 3, the Li / M molar ratio was low, so it is considered that the Li ion conductivity of the covering layer could not be ensured, and the interface resistance and the rate of increase in interface resistance increased.

[0112] Industrial Applicability

[0113] As described above in detail, according to the present invention, it is possible to provide a cathode active material that can suppress the interface resistance between the cathode active material and the sulfide solid electrolyte from increasing over time and has a low interface resistance.

Claims

1. A positive electrode active material comprising particles having a core particle and a covering layer, wherein the core particle contains a lithium metal composite oxide, the covering layer is arranged on the surface of the core particle, and the positive electrode active material is used for an all-solid battery containing a sulfide solid electrolyte, The capping layer is composed of an oxide containing Li and M, wherein: M is B, or B and one or more elements selected from the group consisting of Nb, Ti, Zr, Ta, Zn, W and Al, The molar ratio of Li / M on the surface of the covering layer determined by X-ray photoelectron spectroscopy is 0.85 or more and 3.95 or less, The ratio of B in the positive electrode active material is 0.02 mass % or more and 3.5 mass % or less.

2. The positive electrode active material according to claim 1, wherein The M contains Nb in addition to B.

3. The positive electrode active material according to claim 2, wherein The total amount of Nb and B in the positive electrode active material is greater than or equal to 0.5 mass % and less than or equal to 2.5 mass %.

4. The positive electrode active material according to claim 2 or 3, wherein A molar ratio of Li / (B+Nb) on the surface of the cap layer determined by X-ray photoelectron spectroscopy is 1.5 to 3.

6.

5. The positive electrode active material according to claim 2 or 3, wherein The mass ratio of Nb / B in the positive electrode active material is 1 or more and 30 or less.

6. The positive electrode active material according to claim 1, wherein The lithium metal composite oxide is a layered rock salt type compound or a spinel type compound.

7. The positive electrode active material according to claim 1, wherein The sulfide solid electrolyte is a substance containing Li and S and having lithium ion conductivity.

8. The positive electrode active material according to claim 1, wherein The sulfide solid electrolyte is an argyrodite-type solid electrolyte. 9 . A positive electrode mixture comprising the positive electrode active material according to claim 1 .

10. The positive electrode mixture according to claim 9, wherein The invention further comprises a sulfide solid electrolyte.

11. An all-solid battery, comprising a positive electrode, a negative electrode and a solid electrolyte, wherein: The solid electrolyte comprises a sulfide, The positive electrode includes the positive electrode active material according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Cathode active substance material, cathode active substance layer, all-solid battery, and method for producing cathode active substance material

    JP2012099323A

  • Cathode active material for non-aqueous secondary battery and manufacturing method for the same

    JP2015201388A

  • Positive-electrode active material particle for all-solid battery and method for production thereof

    US20140072875A1

  • Positive electrode active material particles, and positive electrode and all-solid-state battery using same

    CN103548186A

  • All solid-state battery and manufacturing method therefor

    CN103650230A