Coated sulphoaluminate phosphor particles

By using a nitride coating on the sulfur aluminate phosphor particles, the degradation problem caused by the reaction of sulfur aluminate phosphor materials with water and oxygen in the LED is solved, and a more efficient waterproof barrier is achieved and the LED is extended. Lifespan and reduce color shift.

CN112437801BActive Publication Date: 2024-12-06GE LIGHTING SOLUTIONS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980048101.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-05-30
Filing Date
2019-05-15
Publication Date
2024-12-06
Estimated Expiration
2039-05-15

AI Technical Summary

Technical Problem

Sulfur aluminate phosphor materials are prone to react with water and oxygen in LED lighting, resulting in degradation and color shift, affecting the lifetime and performance of LEDs. The existing oxide and nitride coating methods are not effective.

Method used

Using a nitride coating, such as aluminum nitride or gallium nitride, as a waterproof barrier, a coating is formed on the sulfur aluminate phosphor particles by chemical vapor deposition or atomic layer deposition techniques, replacing the traditional alumina coating.

Benefits of technology

It significantly improves the waterproof performance and stability of sulfur aluminate phosphor, extends the life of LEDs, reduces color shift and light output degradation, and improves the effectiveness of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112437801B_ABST
    Figure CN112437801B_ABST
Patent Text Reader

Abstract

Sulfoaluminate phosphor particles having a coating comprising or consisting essentially of a nitride, and methods of making such phosphor particles are disclosed. Phosphor-converted light-emitting diodes may include such coated phosphor particles. Nitride coatings on sulfoaluminate phosphor particles provide a significantly improved water barrier compared to alumina coatings and extend the operating life of such phosphor-converted light-emitting diodes.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority to U.S. Patent Application No. 15 / 993,116, filed May 30, 2018, entitled “Coated Thioaluminate Phosphor Particles.” U.S. Patent Application No. 15 / 993,116 claims the benefit of priority to U.S. Provisional Patent Application No. 62 / 672,729, filed May 17, 2018, entitled “Coated Thioaluminate Phosphor Particles,” and also claims the benefit of priority to U.S. Provisional Patent Application No. 62 / 673,044, filed May 17, 2018, entitled “Phosphors With Narrow Green Emission.” Each of the patent applications identified in this paragraph is incorporated herein by reference in its entirety.

[0003] This application is related to U.S. Patent Application No. 15 / 990,378, filed on May 25, 2018, entitled “Phosphors With Narrow Green Emission,” which is incorporated herein by reference in its entirety.

[0004] This application is also related to U.S. Patent Application No. 15 / 591,629, filed on May 10, 2017, entitled “Phosphors With Narrow Green Emission,” which is incorporated herein by reference in its entirety. Technical Field

[0005] The present invention generally relates to coated sulphoaluminate phosphor particles and methods for coating sulphoaluminate phosphor particles. Background Art

[0006] Over the past several years, LED lighting has made great progress in energy-efficient lighting while achieving high quality. Another feature of LED lighting is that the service life of lighting products is very long, typically with an L70 (the amount of time a light source will operate before its lumen output drops to 70% of its initial output) greater than 25,000 hours. In contrast, the L70 of existing light sources replaced by LEDs is typically 10,000 hours (fluorescent lamps) or catastrophic failure occurs at around 1000 hours (incandescent lamps). This long life depends on all the components in the LED light source, especially the blue or purple light-emitting diodes and the down-converting phosphor materials that absorb the light emitted by the diodes and convert it to other colors to form the visible spectrum. When the diode degrades, the LED becomes less bright but maintains its color balance. However, when the phosphor degrades, the LED typically becomes less bright and also loses its color balance. The LED may have a non-white hue. From the user's perspective, color shift is usually more problematic.

[0007] The most common architecture for LED packages is to disperse the phosphor material in a silicone matrix to form a slurry and deposit the slurry into a reflective cup area that also includes the light-emitting diode. The package has two types of reflective areas: a diffuse reflective surface, usually composed of plastic or ceramic, and a more specular reflective surface formed by electrical contacts. Typically, the specular reflective surface is plated with silver to significantly improve reflectivity and increase light extraction from the package.

[0008] LED phosphors are usually composed of activator ions (usually divalent europium or trivalent cerium) in a host. The activator ions directly absorb incident light and emit longer wavelength light in a process commonly known as down-conversion. That is, the incident photons are down-converted from higher energy blue photons to lower energy photons (such as cyan, green, yellow, orange or red). The host helps tune the absorption and emission wavelengths of the activator. In addition, the crystallinity of the host around the activator can play an important role in the efficiency of absorption and emission.

[0009] Phosphor degradation is often attributed to the action of water or oxygen in the presence of heat and light generated by the LED. It is common practice to coat many types of phosphors with layers to prevent water or oxygen from coming into contact with the phosphor and promoting degradation. Typically, these coatings are inorganic oxides and are deposited on the phosphor by either a liquid phase (e.g., sol-gel) reaction or a gas phase reaction.

[0010] Phosphors can typically degrade through three mechanisms. First, oxidation of the activator may eliminate its charge transfer absorption from the 4f orbital to the 5d orbital, rendering it unable to absorb incident light. Second, the host may chemically deform, thereby changing the energy absorbed and emitted by the activator. Third, the host may physically deform, thereby losing crystallinity around the activator and reducing the efficiency of the activator's absorption and emission. Typically, low-temperature chemical changes in the host will also result in a loss of crystallinity. The overall impact of these degradations depends on the extent to which the host (original or degraded state) allows water or oxygen to penetrate through the material. For example, cerium-doped yttrium aluminum garnet phosphor materials degrade very slowly relative to europium-doped alkaline earth orthosilicate phosphors.

[0011] Unlike oxide phosphors and nitride phosphors, which make up almost all of the commercially used phosphors, sulfide-based phosphors (e.g., sulfoaluminate phosphors) add additional LED failure mechanisms. Hydrolysis reactions with water can release sulfur from the phosphor, which can degrade performance by, for example, dulling reflective surfaces in the LED package. This darkening can greatly reduce the light output of the phosphor-converted LED. Therefore, failure to properly coat sulfide phosphors creates a greater problem than failure to properly coat oxide or nitride phosphors.

[0012] Differences in surface chemistry between these phosphors and their oxide or nitride analogs hinder the ability to effectively coat sulfide phosphors. Summary of the invention

[0013] In one aspect of the invention, the sulphoaluminate phosphor particles have a coating that includes, consists essentially of, or consists of a nitride. For example, the nitride coating may include, consist essentially of, or consist of aluminum nitride, gallium nitride, or a mixture thereof. The nitride coating on the sulphoaluminate phosphor particles provides a significantly improved barrier to water compared to an aluminum oxide coating. This improvement may be due to the fact that the nitride coating precursor does not react with gases volatilized from the unstable sulfide phosphor surface.

[0014] In another aspect of the present invention, a method of preparing such nitride-coated sulfoaluminate phosphor particles is disclosed.

[0015] In yet another aspect of the invention, a phosphor-converted LED includes such nitride-coated sulfoaluminate phosphor particles.

[0016] These and other embodiments, features and advantages of the present invention will become more readily apparent to those skilled in the art when reference is made to the following more detailed description of the invention and taken in conjunction with the accompanying drawings which are first briefly described. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A schematic diagram of an example fluidized bed reactor for chemical vapor deposition on phosphor particles is shown.

[0018] Figure 2 X-ray photoelectron spectra of two coated phosphor samples in the sulfur 2p region are shown.

[0019] Figure 3 Example thermogravimetric analysis-mass spectrometry data for an uncoated calcium sulfoaluminate phosphor sample is shown.

[0020] Figure 4A Microscope images of ZnS samples coated with Al2O3 after AgNO3 testing are shown.

[0021] Figure 4B Microscope images of the ZnS sample coated with AlN after AgNO3 test are shown.

[0022] Figure 4C Microscope images of calcium sulfoaluminate phosphor particles coated with Al2O3 after AgNO3 testing are shown.

[0023] Figure 4D Microscope images of calcium sulfoaluminate phosphor particles coated with AlN after AgNO3 testing are shown. DETAILED DESCRIPTION

[0024] The following detailed description should be read with reference to the accompanying drawings, which depict selective embodiments and are not intended to limit the scope of the invention. This detailed description illustrates the principles of the invention by way of example and not limitation. This specification will clearly enable those skilled in the art to make and use the invention, and describes several embodiments, adaptations, changes, substitutions and uses of the invention, including the methods currently considered to be the best modes for performing the invention. As used in this specification and the appended claims, the singular forms "a", "an" and "the" include multiple references unless the context clearly indicates otherwise.

[0025] Sulfide phosphors can have very attractive spectral properties. Specifically, the emission spectra of many sulfide phosphors can be very narrow, characterized by a full width at half maximum (FWHM) of less than 50 nm, and sometimes as little as 25 to 30 nm. This spectral narrowness can be very attractive in display backlighting and general lighting applications.

[0026] Divalent rare earth activated sulfide phosphors of interest include RE 1-w A w M x E y, where RE may be one or more rare earth elements (e.g., Eu or Gd), A may be one or more elements selected from the group Mg, Ca, Sr or Ba, M may be one or more elements selected from the group Al, Ga, B, In, Sc, Lu or Y, E includes sulfur and may be one or more elements selected from the group S, Se, O and Te, w is greater than or equal to zero and less than or equal to about 0.99 or less than or equal to 1.0, 2≤x≤4, and 4≤y≤7. Such phosphors may be referred to herein as sulfoaluminate or calcium sulfoaluminate phosphors. Typically, they are capable of absorbing blue light or ultraviolet light and are capable of responsively emitting light having a peak wavelength in the green region of the visible spectrum.

[0027] These sulfoaluminate phosphors can react with water to release H2S and convert part of the sulfide host into an oxide. This change affects the optical properties of the phosphor, typically shifting the absorption to higher energies due to reduced crystallinity around the activator center and reducing the absorption and emission intensities.

[0028] Free sulfide, such as that which can be released from a sulfide phosphor when it hydrolyzes to H2S or similar, can damage the package on several levels. At high concentrations, it can inhibit the cure of the silicone used for the encapsulation. This inhibition of cure means that the phosphor can move within the package, shifting the color point of the LED, and that the wire bonds from the contacts to the chip are unprotected, making the LED more susceptible to catastrophic failure due to broken electrical connections. At lower concentrations, sulfide reacts over time, corroding the silver of the electrical contact pads and the gold of the wire bonds from the contacts to the chip and turning them black. The latter degradation mechanism can also come into play if a cationic sulfur source, such as SO2, is present, and the electrochemical potential present when current flows through the package can accelerate the latter degradation mechanism.

[0029] All of these mechanisms shorten the lifetime of phosphor-converted LED light sources.

[0030] As mentioned above, it is known that coating phosphor particles can inhibit water from entering the phosphor and prevent its degradation. Common coating methods are to form a silicon dioxide layer by a sol-gel process or an aluminum oxide layer by chemical vapor deposition.

[0031] In the sol-gel process, phosphor particles are suspended in a solvent. The solvent contains a coating precursor, and a reaction is initiated to form the precursor into a continuous coating on the phosphor particles. Depending on the system, the precursor can be initiated in the presence of the phosphor, or it can be initiated before the phosphor is introduced. For example, the phosphor can be stirred in an aqueous or ethanolic solution of tetraethoxysilane (TEOS). The coating process can then be initiated by adding an ammonia solution to change the pH and accelerate the hydrolysis rate of the silane, thereby forming a silica coating on the phosphor. Other types of precursors are known, such as titanium ethanol isopropoxide and aqueous aluminum nitrate. Many other sol-gel chemistries are known and can be utilized.

[0032] The chemical vapor deposition process is typically performed on particles that have been fluidized in a fluidized bed. The creation of a fluidized bed typically requires placing the phosphor powder in a column that has a gas-permeable but powder-impermeable membrane or frit at the bottom. The powder is suspended by the upward force of the gas, which counteracts the downward force of gravity. This fluidization enables access to all surfaces of the phosphor particles that might not otherwise be exposed to the solid powder or even to the stirred solution. The second gas stream can carry the second precursor of the coating and can deliver it near the middle of the fluidized zone. Figure 1 An example fluidized particle coating system is depicted in .

[0033] One such fluidizing system arrangement uses argon as the fluidizing gas, and in two separate streams the argon is bubbled through water, then up through the frit and through trimethylaluminum (TMA), and then into the middle of the fluidizing zone. These reactants are mixed in the fluidizing zone, and the zone is heated to 100°C–300°C. Hydrolysis of the TMA then occurs to form an amorphous alumina coating on the phosphor particles. In addition to argon, other inert carrier gases, such as nitrogen, may also be used.

[0034] The aluminum oxide coating can also be deposited in a layer by layer process, sometimes referred to as atomic layer deposition (ALD), in which the phosphor particles are treated with a small concentration of water to form a water / hydroxide layer on the surface of the particles, the reaction chamber is evacuated to remove all of the water, and then filled with a small concentration of TMA, which reacts with the surface hydroxyl groups left by the water to form an aluminum oxide layer. The chamber is again evacuated and filled with a small concentration of water, and the steps are repeated until the desired number of layers have been deposited.

[0035] The exact thickness of the coating will be determined in part by the method used; ALD will form the thinnest coating layer, CVD will form thicker coatings, and sol-gel will generally form much thicker coatings.

[0036] Attempts to coat sulfoaluminate phosphor materials by various sol-gel methods have resulted in significant degradation of the absorption and emission properties of the phosphor materials due to the chemical reactivity of the phosphor.

[0037] Attempts to form a coating of aluminum oxide or aluminum oxide plus other metal oxides on the sulfoaluminate phosphor material by CVD / fluidized bed methods or ALD methods with trimethylaluminum and water have been more successful in that the material does not show complete degradation during the coating process. However, these coating methods do not form a barrier that enables the phosphor material to withstand normal LED reliability testing.

[0038] Typically, phosphors are tested as part of a packaged LED by observing the lumen maintenance and color shift of the phosphor over a period of time under different conditions. A typical test would be a high temperature operating life (HTOL) test, in which the LED is powered on in a test oven at elevated temperatures. Typical temperatures for HTOL testing are 85°C and 125°C, and typical durations are 1008 hours and 6000 hours. Another typical test is a wet high temperature operating life (WHTOL) test, in which the LED may be powered on all the time, or may be powered on periodically at regular intervals in a test oven at elevated temperatures and elevated controlled humidity. Typical conditions for WHTOL testing are 60°C / 90% relative humidity (60 / 90) and 85°C / 85% relative humidity (85 / 85), and a typical duration is 1008 hours. The success criteria may depend on who is administering the test, but typically lumen maintenance should be at least greater than 80% after 1008 hours of WHTOL testing. That is, the final brightness should be at least 80% of the initial brightness, and the color shift measured by Δu'v' (the change in color coordinates measured in the CIE 1976 color space from the beginning to the end of the test period) should be at least less than 0.007.

[0039] In addition, the coated sulfide phosphor can be tested by subjecting the phosphor powder to a silver nitrate solution to obtain the effectiveness of the coating to seal the sulfur. The silver ions in the solution will react with any sulfide that has not been protected by the coating and form black Ag2S. This black precipitate is easy to see once it forms, and the time of its appearance can be used as a gauge of the effectiveness of the coating.

[0040] For example, some samples of europium-doped strontium thiogallate (a well-studied phosphor) coated with aluminum oxide did not turn black for about 336 hours in a silver nitrate solution and retained 80% of their initial brightness after 1008 hours of 60 / 90 testing.

[0041] In contrast, some of the more robust alumina-coated europium-doped calcium sulfoaluminate samples turned black after about 20 minutes in the silver nitrate solution and failed to retain 80 percent of their initial brightness after only 168 hours of testing.

[0042] like Figure 2 As shown in, analysis of alumina-coated strontium thiogallate (STG) phosphors and alumina-coated calcium sulfoaluminate phosphors by XPS in the sulfur 2p region shows negligible signal (if any) for STG, but very significant intensity between 160 and 172 eV (about 3 atomic %) for the calcium sulfoaluminate phosphor. This sulfur is expected to react with moisture and promote failure of the phosphor as determined by various test methods (silver nitrate solution and packaged LED testing). It is speculated that the sulfoaluminate phosphor volatilizes sulfide during the coating process, which is then continuously redeposited with the outer layer of the coating.

[0043] To help test the speculation about the sulfur in the coating of the sulfoaluminate, several uncoated calcium sulfoaluminate phosphors were analyzed by thermogravimetric analysis coupled to mass spectrometry (TGA-MS). In this technique, the sample is heated under flowing gas, its mass is monitored, and the outgoing gas is analyzed by mass spectrometry. Specifically, the calcium sulfoaluminate phosphors subjected to several different work-up schemes were heated under inert gas (argon) and showed a mass number of 34 corresponding to H2S as the main mass loss at temperatures up to about 300°C. Figure 3 An example dataset is shown in . Also in Figure 3 It shows that mass number 44 corresponds to CO2 or CH2CHO, mass 48 corresponds to SO or CH3SH, mass 64 corresponds to SO2, and mass 66 corresponds to H2S2.

[0044] These analyses point to an incompatibility of the sulfoaluminate phosphor surface with the chemistry used to deposit the oxide-based coating. This incompatibility occurs when the coating chemistry volatilizes some of the sulfur from the surface and redeposits it as part of the coating, thereby creating a continuous reactive pathway for water to penetrate into the coating and react with / degrade the phosphor material.

[0045] As a result of the defects discovered when attempting to apply an oxide coating to a calcium sulphoaluminate phosphor, it became apparent to the inventors that significant changes had to be made to the coating process. The inventors then developed an improved coating process that involves coating the sulphoaluminate phosphor material with a nitride layer instead of an aluminum oxide layer. For example, aluminum nitride, gallium nitride, and mixtures of the two may be suitable for such coatings. In this process, pure ammonia or ammonia with an inert gas is used as a fluidizing gas, and trimethylaluminum may be used as an aluminum source to deposit the aluminum nitride layer. Alternatively, trimethylgallium may be used in place of trimethylaluminum to deposit a gallium nitride layer instead of an aluminum nitride layer. In this process, both trimethylaluminum and trimethylgallium may be used to deposit a mixed aluminum nitride and gallium nitride layer.

[0046] Another coating layer (such as, for example, aluminum oxide, silicon dioxide, or aluminum oxide and silicon dioxide) may optionally be added over the aluminum nitride layer, for example, by one of the coating methods described above. In some variations, there may be an oxide layer beneath the aluminum nitride coating, which is formed during cleaning of the phosphor particles prior to deposition of the nitride coating. Thus, in some variations, there may be an oxide layer or other layer above and below the nitride layer.

[0047] Table 1 below presents data from a series of coating runs, all of which were run with the same phosphor batch. For each coating experiment, these data are reference values, the amount of phosphor charged to the reactor, the amount of phosphor recovered, the temperature maintained at the reactor during the coating cycle, the duration of the coating cycle, the flow rate of argon gas (L / min) passing through the trimethylaluminum bubbler and into the reactor, the flow rate of anhydrous ammonia (L / min) into the reactor, the weight ratio of nitrogen to aluminum precursor used, and the theoretical amount of aluminum nitride formed relative to the amount of phosphor in the reactor.

[0048] Table 2 below presents the spectral data of the phosphor samples before coating and after each coating run. Additionally, another batch of phosphors was coated using ALD and the spectral data of the samples before and after coating are presented.

[0049] The sulphoaluminate samples coated with aluminum nitride or Al2O3 were tested by subjecting the phosphor powder to the silver nitrate solution test described above. In these tests, several milligrams of the coated phosphor were placed in a vial. Several milliliters of 0.01 MAgNO3 ( aq )(AgNO3( 水溶液)) was added to the vial, and the time to reach a predetermined degree of blackening due to the formation of silver sulfide was recorded by visual observation. The time recorded is the failure time (TTF) and gives a relative measure of the effectiveness of the coating. Table 3 below reports the AgNO3 failure times of a sample with the best Al2O3 coating, a sample with an AlN coating deposited by ALD, and two samples with CVD AlN coatings. After 19 minutes, blackening of the best Al2O3 coating was observed. By 40 minutes, the AlN sample by ALD was blackening. After 3 hours, blackening was observed in the earlier AlN sample by CVD (NBG20180326), and after 4.5 hours, blackening was observed in the later AlN sample by CVD (NBG20180327).

[0050] These test results (e.g., for NBG20180327) indicate that a reaction temperature of 300°C is sufficient to provide a barrier coating of aluminum nitride on sulphoaluminate phosphor particles that is more effective than the best alumina coating prepared for this study. Scanning electron microscopy (SEM) and transmission electron microscopy of cross-sectioned NBG20180327 phosphor particles showed that the aluminum nitride barrier coating was polycrystalline and 50-60 nm thick. Aluminum nitride was identified by EDS. Scanning electron microscopy (SEM) and transmission electron microscopy of cross-sectioned sulphoaluminate phosphor particles coated with the best alumina coating showed that the thickness of the alumina coating was greater than 200 nm.

[0051] In other tests, samples were attached to glass slides with double-sided tape, immersed in a silver nitrate solution, and observed over the course of several hours. Four samples were compared: Figure 4A As shown, zinc sulfide coated with Al2O3; Figure 4B As shown, zinc sulfide coated with AlN; Figure 4C As shown, the sulphoaluminate phosphor sample NBG20180301 coated with the best alumina coating previously identified; and Figure 4D As shown, a sample of the same phosphor batch coated with AlN (Example NBG20180327). After about 8 hours, the samples were compared. The zinc sulfide with aluminum oxide coating showed no blackening, while the zinc sulfide coated with aluminum nitride showed some degree of blackening. The phosphor sample with aluminum oxide coating had some green phosphor particles remaining, but it was almost completely blackened ( Figure 4C ), while the aluminum nitride coated sample appeared less than half blackened ( Figure 4D ).

[0052] The nitride-coated sulfoaluminate phosphors of the present invention can be optically coupled to an excitation source in any conventional manner. A more common method is to combine a green-emitting phosphor (such as the nitride-coated sulfoaluminate phosphors disclosed herein) with a red phosphor and optionally a blue and / or yellow phosphor. The phosphors can be combined together and then added to an encapsulant such as a silicone, epoxy, or some other polymer, or the phosphors can be combined during the addition of the phosphors to the encapsulant. The encapsulant loaded with the phosphors can then be placed in the light path of an excitation source, such as an LED or laser diode that emits ultraviolet, violet, or blue light. A common method is to deposit a slurry of one or more phosphors into an LED (light emitting diode) package containing an LED chip. The slurry is then cured to form a sealed LED package. Other methods include forming the encapsulant into a certain shape, or applying the encapsulant to a substrate that may already have a specific shape or may be subsequently formed into a specific shape. Additionally, an encapsulant comprising a phosphor may be disposed on or near (e.g., coated on) an in-coupling region of a lightguide, or on an out-coupling region of a lightguide such as a lightguide intended for use in a display. Alternatively, the phosphor composition may be deposited as a thin film on an LED chip or on another substrate and subsequently optically coupled to a light source. The combination of the excitation source and phosphor of the present invention may be used in general lighting, niche lighting applications, display backlighting, or other lighting applications.

[0053] Table 1 Coating operation data

[0054]

[0055] Table 2 Spectral data:

[0056]

[0057] Table 3 AgNO3 resistance test data:

[0058]

[0059] This disclosure is intended to be illustrative rather than restrictive. Further modifications will be apparent to those skilled in the art in view of this disclosure and are intended to fall within the scope of the appended claims.

Claims

1. A luminescent composition comprising: Particles of sulfide phosphor material, the sulfide phosphor material being of formula RE 1-w A w M x E y Characterization, where: RE is a rare earth element or a mixture of rare earth elements; A is selected from the group consisting of magnesium, calcium, strontium, barium and mixtures thereof; M is selected from the group consisting of aluminum, gallium, boron, indium, scandium, lutetium, yttrium, and mixtures thereof; E includes sulfur; 0≤w≤0.99; 2≤x≤4; and 4≤y≤7; and A nitride coating layer is formed on each particle, wherein the nitride coating layer includes aluminum nitride, gallium nitride, or a mixture of aluminum nitride and gallium nitride.

2. The luminescent composition according to claim 1, wherein The nitride coating layer includes aluminum nitride.

3. The luminescent composition according to claim 1, wherein The nitride coating layer consists of aluminum nitride.

4. The luminescent composition according to claim 1, wherein The nitride coating layer includes gallium nitride.

5. The luminescent composition according to claim 1, wherein The nitride coating layer consists of gallium nitride.

6. The luminescent composition according to claim 1, wherein The sulfide phosphor material is capable of absorbing blue, violet, or ultraviolet light and responsively emits light having a peak wavelength in the green region of the visible spectrum.

7. The luminescent composition of claim 1, wherein: The nitride coating layer is disposed directly on the sulfide phosphor material.

8. The luminescent composition of claim 1, wherein: Each particle includes an oxide layer disposed between the sulfide phosphor material and the aluminum nitride coating layer.

9. The luminescent composition of claim 1, wherein: Each particle includes at least a second coating layer disposed on the nitride coating layer.

10. The luminescent composition of claim 9, wherein: The second coating layer includes at least one oxide.

11. The luminescent composition of claim 1, wherein: E also includes at least one of selenium, oxygen, tellurium and mixtures thereof.

12. The luminescent composition of claim 11, wherein The nitride coating layer consists of aluminum nitride.

13. The luminescent composition of claim 12, wherein: The nitride coating layer is disposed directly on the sulfide phosphor material.

14. The luminescent composition of claim 12, wherein: Each particle includes an oxide layer disposed between the sulfide phosphor material and the aluminum nitride coating layer.

15. A light emitting device comprising: a light emitting diode that emits the main light; as well as Particles of sulfide phosphor material, the sulfide phosphor material being of formula RE 1-w A w M x E y Characterization, where: RE is a rare earth element or a mixture of rare earth elements; A is selected from the group consisting of magnesium, calcium, strontium, barium and mixtures thereof; M is selected from the group consisting of aluminum, gallium, boron, indium, scandium, lutetium, yttrium, and mixtures thereof; E includes sulfur; 0≤w≤0.99; 2≤x≤4; and 4≤y≤7; The sulfide phosphor material is capable of absorbing at least a portion of the primary light and responsively emitting secondary light having a wavelength longer than that of the primary light, and each particle of the sulfide phosphor material includes a nitride coating layer, the nitride coating layer including aluminum nitride, gallium nitride, or a mixture of aluminum nitride and gallium nitride.

16. The light emitting device according to claim 15, wherein: The nitride coating layer includes aluminum nitride.

17. The light emitting device according to claim 15, wherein: The nitride coating layer consists of aluminum nitride.

18. The light emitting device according to claim 15, wherein: The nitride coating layer includes gallium nitride.

19. The light emitting device according to claim 15, wherein: The nitride coating layer consists of gallium nitride.

20. The light emitting device according to claim 15, wherein: The secondary light has a peak wavelength in the green region of the visible spectrum.

21. The light emitting device according to claim 20, wherein: E also includes at least one of selenium, oxygen, tellurium and mixtures thereof.

22. The light emitting device according to claim 21, wherein: RE is europium.

23. The light emitting device according to claim 22, wherein: The main light is blue light.

24. The light emitting device according to claim 23, wherein: The secondary light has a peak wavelength in the green region of the visible spectrum.