Method for producing laminated optical film
By using adhesive layers of different components in the image display device to design the refractive index difference, the problem of uneven light reflected by the polarizing film in the prior art is solved, the visual recognition is improved, and it is suitable for organic EL display devices.
Patent Information
- Application Number
- CN202010919855.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-04
- Filing Date
- 2020-09-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-09-04
AI Technical Summary
The image display device using a polarizing film in the prior art has problems such as unevenness in reflected light generation and insufficient visual recognition.
By adopting a manufacturing method in which the first optical film and the second optical film are laminated with adhesive layers having different components, different refractive indices are designed on the surface side and the back side of the adhesive layer, the optical film and the adhesive are suppressed. Interface reflection of the layer.
It significantly reduces the reflectivity of external light and improves visual recognition, which is especially suitable for organic EL display devices.
Smart Images

Figure CN112440536B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a laminated optical film in which a first optical film and a second optical film different from the first optical film are laminated with an adhesive layer interposed therebetween. The laminated optical film is suitable for use in image display devices, particularly organic EL display devices. Background Art
[0002] In order to improve the poor visual recognition caused by external light reflection and background reflection in the display screen of the image display device, a display device is known to be provided with a circular polarizer on the visible side of the display panel. Patent documents 1 and 2 propose a polarizing film and a display device having the polarizing film, wherein the polarizing film reduces the reflection of incident light from an oblique direction in a black display, thereby achieving an excellent reflection hue in an oblique direction.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-111236
[0006] Patent Document 2: Japanese Patent Application Publication No. 2015-210459 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, the display devices using the polarizing film described in Patent Documents 1 and 2 have problems such as uneven reflection of light and insufficient visibility.
[0009] In view of the above-mentioned actual situation, an object of the present invention is to provide a method for producing a laminated optical film having reduced reflectance from external light and excellent visibility.
[0010] Solutions to the problem
[0011] The above problems can be solved by the following configuration. That is, the present invention relates to a method for manufacturing a laminated optical film, wherein the laminated optical film is formed by laminating a first optical film and a second optical film different from the first optical film via an adhesive layer, wherein the adhesive layer comprises a first cured layer of a first adhesive composition and a second cured layer of a second adhesive composition, wherein the first adhesive composition and the second adhesive composition contain at least a part of different components, and the method comprises: a first step of applying the first adhesive composition to the bonding surface of the first optical film; a second step of applying the second adhesive composition to the bonding surface of the second optical film; a third step of laminating the first adhesive composition-coated surface of the first optical film and the second adhesive composition-coated surface of the second optical film; and a fourth step of irradiating active energy rays from the first optical film surface side or the second optical film surface side to bond the first optical film to the second optical film, wherein in the first step, the first cured layer is cured before the second cured layer.
[0012] Preferably, in the manufacturing method of the above-mentioned laminated optical film, in the above-mentioned first step, the above-mentioned first adhesive composition after coating is irradiated with active energy rays from the above-mentioned first optical film surface side or the above-mentioned first adhesive composition coating surface side of the above-mentioned first optical film, so that the above-mentioned first adhesive composition is cured, and the above-mentioned first cured material layer is formed before the above-mentioned second cured material layer.
[0013] In the method for producing the laminated optical film, it is preferred that the in-plane refractive index R of the first optical film-side surface F1 of the adhesive layer is F1 The in-plane refractive index R of the second optical film side surface F2 is F2 different.
[0014] In the method for producing a laminated optical film, preferably, the first optical film has a thickness of 30 μm or less, and the second optical film has a thickness of 20 μm or less.
[0015] In the method for producing a laminated optical film, it is preferred that the adhesive layer has a thickness of 5 μm or less.
[0016] In the method for producing a laminated optical film, it is preferred that the first optical film is a transparent protective film, and the second optical film is a polarizer.
[0017] Effects of the Invention
[0018] The image display device has a laminated optical film having two or more optical films laminated thereon, and the optical films constituting the laminated optical film are usually laminated together with an adhesive layer in between. When two optical films of the same kind are laminated with an adhesive layer in between, the refractive index of the two optical films is the same, so by designing the adhesive layer in such a way that its refractive index is close to the refractive index of the optical film, the reflection of the interface between each optical film and the adhesive layer can be prevented. On the other hand, when two different optical films are laminated with an adhesive layer in between, the refractive index of the two optical films is usually different. Here, the adhesive layer of the existing laminated optical film has the same refractive index on one optical film side (which is expressed as the "surface side") and the other optical film side (which is expressed as the "back side"), and there is no concept of making the refractive index of the adhesive layer different on the surface side and the back side in order to suppress the reflection of the interface between the surface side optical film and the adhesive layer, and the interface between the back side optical film and the adhesive layer.
[0019] However, in the manufacture method of the optical film of the present invention, when two different optical films are laminated across an adhesive layer, an adhesive layer is formed by a material comprising a first cured product layer of a first adhesive composition and a second cured product layer of a second adhesive composition, so that at least a portion of the first adhesive composition and the second adhesive composition contain different components, and in the first step of applying the first adhesive composition to the bonding surface of the first optical film, the first cured product layer is cured earlier than the second cured product layer. Thus, an adhesive layer having a refractive index different from that on the surface side and the back side can be formed. By optimizing the coordination design of the first adhesive composition constituting the first cured product layer on the surface side, and similarly optimizing the coordination design of the second adhesive composition constituting the second cured product layer on the back side, the reflection at the interface of the first optical film and the adhesive layer and at the interface of the second optical film and the adhesive layer can be significantly suppressed.
[0020] Generally speaking, the thinner the laminated optical film is, the more uneven the reflected light is likely to be. As a result of paying attention to the above problem, especially for the laminated optical film of the present invention, even if the thickness of the first optical film and the second optical film and the adhesive layer is thin, the reflectivity of external light, especially natural light, can be reduced, and the visual recognition is also improved. Therefore, the laminated optical film of the present invention is particularly useful as an image display device, especially an organic EL display device. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a diagram showing an example of reflection of external light in an image display device including a conventional laminated optical film.
[0022] Figure 2 (a) to (b) are views showing an example of an image display device including the laminated optical film of the present invention. DETAILED DESCRIPTION
[0023] In the present invention, a laminated optical film is manufactured in which a first optical film and a second optical film different from the first optical film are laminated via an adhesive layer. Furthermore, the laminated optical film is characterized in that, in order to suppress reflection at the interface between each optical film and the adhesive layer, the adhesive layer is designed to have a different refractive index on the front side and the back side. The above-mentioned characteristics are compared with an image display device having a conventional laminated optical film and described below.
[0024] Figure 1 The figure shows the reflected light L from the external light (natural light) L in the image display device having the existing laminated optical film. R An example of a diagram. Figure 1 The image display device M shown is an organic EL image display device having an organic light emitting diode 7, and the image display device M has a laminated optical film 10 in which a first optical film (transparent protective film) 1 and a second optical film (polarizer) 3 are laminated via a first adhesive layer 2. Figure 1 In the case of the existing structure shown, since the refractive index of the first adhesive layer 2 is the same on the surface side and the back side, the refractive index of the transparent protective film 1 is different from that of the first adhesive layer 2, and the refractive index of the first adhesive layer 2 is different from that of the polarizer 3, external light (natural light) L is reflected at the interface between the transparent protective film 1 and the first adhesive layer 2, and at the interface between the first adhesive layer 2 and the polarizer 3. Therefore, the reflected light becomes uneven and visual recognition becomes insufficient.
[0025] Figure 2 This is a diagram showing an example of an image display device including a laminated optical film produced by the production method of the present invention. Figure 2 The image display device M shown is an organic EL image display device having an organic light emitting diode 7, and the image display device M has a laminated optical film 10 in which a first optical film (transparent protective film) 1 and a second optical film (polarizer) 3 are laminated via an adhesive layer 2. It should be noted that in the present invention, the laminated optical film may be composed of three or more optical films as long as it has a first optical film → an adhesive layer → a second optical film from at least the outer side (visible side) to the inner side. Figure 2 In the embodiment shown in (a), the image display device M includes a transparent protective film (first optical film) 1→a first adhesive layer 2→a polarizer (second optical film) 3→a second adhesive layer 4→a phase difference film (third optical film) 5→an adhesive layer 6 in order from the outermost surface to the organic light emitting diode 7. The first adhesive layer 2 of the laminated optical film 10 manufactured by the manufacturing method of the present invention is designed as follows: the in-plane refractive index R of the side surface F1 of the transparent protective film (first optical film) 1 is F1 The in-plane refractive index R of the side surface F2 of the polarizer (second optical film) 3 isF2 Different, and R F1 The difference in the average refractive index of the transparent protective film is within 0.02, R F2 The difference in the in-plane average refractive index with the polarizer is within 0.02. Thus, in the laminated optical film 10 manufactured by the manufacturing method of the present invention, the reflectivity of the external light (natural light) L at the interface between the transparent protective film and the adhesive layer and at the interface between the adhesive layer and the polarizer is reduced, and the visual recognition is excellent.
[0026] <First Adhesive Layer>
[0027] The adhesive layer of the laminated optical film produced by the production method of the present invention is described below. In the present invention, the adhesive layer is preferably thin, and specifically, the thickness of the adhesive layer is preferably 5 μm or less, more preferably 0.5 to 3 μm.
[0028] The adhesive layer of the laminated optical film produced by the production method of the present invention is characterized in that the refractive index is different between the front side and the back side. Specifically, the in-plane refractive index R of the first optical film side surface F1 is F1 The in-plane refractive index R of the second optical film side surface F2 is F2 Different, R F1 The difference between the in-plane average refractive index of the first optical film and the first optical film is within 0.02, R F2 The difference between the in-plane average refractive index of the first optical film and the second optical film is within 0.02. In order to further suppress the reflection at the interface between the first optical film and the adhesive layer and at the interface between the second optical film and the adhesive layer, it is more preferable to set R F1 The difference between the in-plane average refractive index of the first optical film and the first optical film is set to be within 0.01, and it is more preferable to set R F2 The difference in the in-plane average refractive index with the second optical film is set within 0.01.
[0029] It should be noted that, in the present invention, for the "in-plane refractive index" of the first optical film side surface F1 (or the second optical film side surface F2) of the adhesive layer, the in-plane refractive index of each surface side of the adhesive layer was measured using a prism coupler SPA-4000 (manufactured by Cylon Technology Co., Ltd.). The measurement temperature was set to 23°C and the measurement wavelength was set to 532nm.
[0030] In the present invention, the adhesive layer can be designed with any material as long as it meets the above characteristics, and is particularly preferably formed by a cured layer obtained by irradiating an active energy ray-curable adhesive composition with active energy rays. Active energy ray-curable adhesive compositions can be roughly divided into electron beam curing, ultraviolet curing, visible light curing, etc. Furthermore, ultraviolet curing and visible light curing adhesives can be roughly divided into free radical polymerization curing adhesives and cationic polymerization adhesives. In the present invention, active energy rays in the wavelength range of 10nm to 380nm can be recorded as ultraviolet rays, and active energy rays in the wavelength range of 380nm to 800nm can be recorded as visible light.
[0031] As compounds constituting the free radical polymerization curing adhesive, free radical polymerizable compounds can be cited. Free radical polymerizable compounds can be cited as compounds having free radical polymerizable functional groups of carbon-carbon double bonds such as (meth) acryloyl and vinyl. These curable components can use any of monofunctional free radical polymerizable compounds or difunctional or more multifunctional free radical polymerizable compounds. In addition, these free radical polymerizable compounds can be used alone or in combination of two or more. As these free radical polymerizable compounds, compounds with (meth) acryloyl are preferred. The active energy ray curing adhesive composition used in the present invention preferably contains a compound with a (meth) acryloyl group as the main component. Specifically, when the total amount of the active energy ray curing adhesive composition is set to 100% by weight, it is preferred to contain more than 50% by weight of the compound with a (meth) acryloyl group, and more preferably more than 80% by weight. It should be noted that in the present invention, (meth) acryloyl refers to acryloyl and / or methacryloyl, and "(meth)" has the same meaning below.
[0032] Examples of the monofunctional radical polymerizable compound include (meth)acrylamide derivatives having a (meth)acrylamide group. (Meth)acrylamide derivatives are preferred in terms of ensuring adhesion to polarizers and various transparent protective films, and in terms of high polymerization speed and excellent productivity. Specific examples of (meth)acrylamide derivatives include N-alkyl (meth)acrylamide derivatives such as N-methyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, and N-hexyl (meth)acrylamide; N-hydroxymethyl (meth)acrylamide derivatives such as N-hydroxyalkyl (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, and N-hydroxymethyl-N-propyl (meth)acrylamide; N-aminoalkyl (meth)acrylamide derivatives such as aminomethyl (meth)acrylamide and aminoethyl (meth)acrylamide; N-alkoxy (meth)acrylamide derivatives such as N-methoxymethylacrylamide and N-ethoxymethylacrylamide; N-mercaptoalkyl (meth)acrylamide derivatives such as mercaptomethyl (meth)acrylamide and mercaptoethyl (meth)acrylamide; and the like. Examples of heterocyclic-ring-containing (meth)acrylamide derivatives in which the nitrogen atom of the (meth)acrylamide group forms a heterocyclic ring include N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, and N-acryloylpyrrolidine.
[0033] Among the above-mentioned (meth)acrylamide derivatives, N-hydroxyalkyl (meth)acrylamide derivatives are preferred from the viewpoint of adhesion to polarizers and various transparent protective films. Examples of monofunctional radical polymerizable compounds include various (meth)acrylic acid derivatives having a (meth)acryloyloxy group. Specific examples include alkyl (meth)acrylates (having 1 to 20 carbon atoms) such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, tert-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, hexadecyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate.
[0034] Examples of the (meth)acrylic acid derivatives include cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-isobornyl (meth)acrylate, 2-norbornyl methyl (meth)acrylate, 2-norbornyl methyl (meth)acrylate, 5-norbornene-2-yl methyl (meth)acrylate, 3-methyl-2-norbornyl methyl (meth)acrylate, Polycyclic (meth)acrylates such as dicyclopentenyl acrylate, dicyclopentenyloxyethyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; (meth)acrylates containing alkoxy groups or phenoxy groups such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, and alkylphenoxypolyethylene glycol (meth)acrylate; and the like.
[0035] Examples of the (meth)acrylic acid derivatives include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; hydroxyl-containing (meth)acrylates such as [4-(hydroxymethyl)cyclohexyl]methyl acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate; epoxy-containing (meth)acrylates such as glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether; and 2,2,2-trifluoroethyl (meth)acrylate, 2,2 Halogen-containing (meth)acrylates such as 2-trifluoroethyl ethyl ester, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; alkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate; oxetanyl (meth)acrylate-containing (meth)acrylates such as 3-oxetanyl methyl (meth)acrylate, 3-methyloxetanyl methyl (meth)acrylate, 3-ethyloxetanyl methyl (meth)acrylate, 3-butyloxetanyl methyl (meth)acrylate, and 3-hexyloxetanyl methyl (meth)acrylate; (meth)acrylates having heterocyclic rings such as tetrahydrofurfuryl (meth)acrylate and butyrolactone (meth)acrylate, hydroxypivalic acid neopentyl glycol (meth)acrylate adduct, and p-phenylphenol (meth)acrylate.
[0036] Examples of the monofunctional radical polymerizable compound include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.
[0037] Examples of monofunctional free radical polymerizable compounds include lactam vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, and vinyl Vinyl monomers having a nitrogen-containing heterocyclic ring such as oxazole and vinyl morpholine, etc.
[0038] In addition, as a monofunctional free radical polymerizable compound, a free radical polymerizable compound having an active methylene group can be used. The free radical polymerizable compound having an active methylene group is a compound having an active double bond group such as a (meth) acrylic group at the end or in the molecule and having an active methylene group. Examples of the active methylene group include acetoacetyl, alkoxymalonyl, or cyanoacetyl. The above-mentioned active methylene group is preferably acetoacetyl. Specific examples of the radical polymerizable compound having an active methylene group include acetoacetoxyethyl alkyl (meth)acrylates such as 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxyethyl propyl (meth)acrylate, and 2-acetoacetoxyethyl-1-methylethyl (meth)acrylate; 2-ethoxymalonyloxyethyl (meth)acrylate, 2-cyanoacetoxyethyl (meth)acrylate, N-(2-cyanoacetoxyethyl)acrylamide, N-(2-propionylacetoxybutyl)acrylamide, N-(4-acetoacetoxyethylmethylbenzyl)acrylamide, and N-(2-acetoacetylaminoethyl)acrylamide. The radical polymerizable compound having an active methylene group is preferably acetoacetoxyethyl alkyl (meth)acrylate.
[0039] Examples of the difunctional or higher polyfunctional radical polymerizable compound include tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropylene glycol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal(meth)acrylate, dimethacrylate, and bisphenol A diglycidyl ether di(meth)acrylate. Esterification products of (meth)acrylic acid and polyols such as alkanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerol tetra(meth)acrylate, and 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene. Specific examples include ARONIX M-220 (manufactured by Toagosei Co., Ltd.), LIGHT ACRYLATE 1,9ND-A (manufactured by Kyoeisha Chemical Co., Ltd.), LIGHT ACRYLATE DGE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), LIGHT ACRYLATE TED CP-A (manufactured by Kyoeisha Chemical Co., Ltd.), SR-531 (manufactured by Sartomer Co., Ltd.), and CD-536 (manufactured by Sartomer Co., Ltd.). Moreover, various epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, various (meth)acrylate-based monomers, etc. can be mentioned as needed.
[0040] The active energy ray-curable adhesive composition does not need to contain a photopolymerization initiator when electron beams or the like are used as the active energy ray. However, when ultraviolet rays or visible light are used as the active energy ray, it preferably contains a photopolymerization initiator.
[0041] The photopolymerization initiator in the case of using a free radical polymerizable compound can be appropriately selected according to the active energy ray. In the case of curing by ultraviolet or visible light, a photopolymerization initiator that is cleaved by ultraviolet or visible light is used. The above-mentioned photopolymerization initiator can be used alone, but when a plurality of photopolymerization initiators are mixed and used, the curing speed and curability can be adjusted, so it is preferred. Examples of the photopolymerization initiator include benzophenone compounds such as benzil, benzophenone, benzoylbenzoic acid, and 3,3′-dimethyl-4-methoxybenzophenone; aromatic ketone compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α′-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, 1-hydroxycyclohexylphenylketone, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propane-1-one, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropane-1-one; and methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, 2-methyl -1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one and other acetophenone compounds; benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, anisole methyl ether and other benzoin ether compounds; aromatic ketal compounds such as benzyl dimethyl ketal; aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, dodecylthioxanthone; camphorquinone; halogenated ketone; acylphosphine oxide; acylphosphonate, etc.
[0042] The amount of the photopolymerization initiator is 20% by weight or less when the total amount of the active energy ray-curable adhesive composition is 100% by weight. The amount of the photopolymerization initiator is preferably 0.01 to 20% by weight, more preferably 0.05 to 10% by weight, and even more preferably 0.1 to 5% by weight.
[0043] In addition, when the curable adhesive for laminated optical films of the present invention is used as a visible light curable adhesive containing a free radical polymerizable compound as a curable component, it is particularly preferred to use a photopolymerization initiator that is highly sensitive to light of 380 nm or more. The photopolymerization initiator that is highly sensitive to light of 380 nm or more will be described later.
[0044] As the photopolymerization initiator, it is preferred to use a compound represented by the following general formula (1) alone, or to use a compound represented by the general formula (1) in combination with a photopolymerization initiator having high sensitivity to light of 380 nm or longer described later.
[0045] [Chemical formula 1]
[0046]
[0047] (Where R 1 and R 2 Represents -H, -CH2CH3, -iPr or Cl, R 1 and R 2 When the compound represented by the general formula (1) is used, the adhesiveness is excellent compared with the case where a photopolymerization initiator having high sensitivity to light of 380 nm or more is used alone. Among the compounds represented by the general formula (1), R 1 and R 2 When the total amount of the active energy ray-curable adhesive composition is 100 wt %, the composition ratio of the compound represented by the general formula (1) in the adhesive is preferably 0.1 to 5 wt %, more preferably 0.5 to 4 wt %, and further preferably 0.9 to 3 wt %.
[0048] In addition, it is preferred to add a polymerization initiation aid as needed. Examples of the polymerization initiation aid include triethylamine, diethylamine, N-methyldiethanolamine, ethanolamine, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isopentyl 4-dimethylaminobenzoate, and the like, with ethyl 4-dimethylaminobenzoate being particularly preferred. When a polymerization initiation aid is used, the amount thereof added is generally 0 to 5 parts by weight, preferably 0 to 4 parts by weight, and most preferably 0 to 3 parts by weight relative to 100 parts by weight of the total amount of the curable component.
[0049] In addition, as needed, known photopolymerization initiators can be used in combination. Since the transparent protective film with UV absorption ability does not transmit light below 380nm, it is preferred to use a photopolymerization initiator that is highly sensitive to light above 380nm as a photopolymerization initiator. Specifically, it can be listed as: 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(η5-2,4-cyclopentadiene-1-yl)bis(2,6-difluoro-3-(1H-pyrrole-1-yl)phenyl)titanium, etc.
[0050] In particular, as the photopolymerization initiator, it is preferred to further use a compound represented by the following general formula (2) in addition to the photopolymerization initiator represented by the general formula (1):
[0051] [Chemical formula 2]
[0052]
[0053] (Where R 3 , R 4 and R 5 represents -H, -CH3, -CH2CH3, -iPr or Cl, R 3 , R 4 and R 5 The compounds represented by the general formula (2) may be the same or different. As the compound represented by the general formula (2), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one (trade name: Omnirad907, manufacturer: IGMresins), which is a commercially available product, may be suitably used. In addition, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone (trade name: Omnirad369, manufacturer: IGMresins) and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholino)phenyl]-1-butanone (trade name: Omnirad379, manufacturer: IGMresins) are preferred because of their high sensitivity.
[0054] In the present invention, among the above-mentioned photopolymerization initiators, a hydroxyl-containing photopolymerization initiator is preferably used. When the active energy ray-curable adhesive composition contains a hydroxyl-containing photopolymerization initiator as a polymerization initiator, the solubility of the adhesive layer having a high concentration of component A on the polarizer side is improved, and the curability of the adhesive layer is improved. Examples of the photopolymerization initiator having a hydroxyl group include 2-methyl-2-hydroxypropiophenone (trade name "DAROCUR 1173", manufactured by IGM Resins), 1-hydroxycyclohexyl phenyl ketone (trade name "Omnirad 184", manufactured by IGM Resins), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one (trade name "Omnirad 2959", manufactured by IGM Resins), and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propane-1-one (trade name "Omnirad 127", manufactured by IGM Resins). In particular, 1-hydroxycyclohexyl phenyl ketone is more preferred because it has particularly excellent solubility in the adhesive layer having a high concentration of component A.
[0055] The active energy ray-curable adhesive composition used in the present invention may contain, in addition to the curable component of the above-mentioned free radical polymerizable compound, an acrylic oligomer formed by polymerizing a (meth) acrylic acid monomer. By containing an acrylic oligomer component in the active energy ray-curable adhesive composition, the curing shrinkage when the composition is irradiated with active energy rays and cured can be reduced, and the interfacial stress between the adhesive and the adherends such as polarizers and transparent protective films can be reduced. As a result, the adhesion between the adhesive layer and the adherend can be suppressed. In order to fully suppress the curing shrinkage of the cured product layer (adhesive layer), when the total amount of the active energy ray-curable adhesive composition is set to 100% by weight, it is preferred that the content of the acrylic oligomer is set to 5 to 30% by weight, and more preferably to 10 to 20% by weight.
[0056] In consideration of workability and uniformity during coating, the active energy ray-curable adhesive composition is preferably low in viscosity, and therefore, the acrylic oligomer obtained by polymerizing the (meth) acrylic acid monomer is also preferably low in viscosity. As a low-viscosity acrylic oligomer, its weight average molecular weight (Mw) is preferably 15,000 or less, more preferably 10,000 or less, and particularly preferably 5,000 or less. On the other hand, in order to make the components of the adhesive composition sandwiched between the polarizer and the transparent protective film more concentrated, the weight average molecular weight (Mw) of the acrylic oligomer (A) is preferably 500 or more, more preferably 1,000 or more, and particularly preferably 1,500 or more.Specific examples of the (meth)acrylic monomer constituting the acrylic oligomer (A) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, tert-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, and n-hexyl (meth)acrylate. , cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, n-octadecyl (meth)acrylate and the like (meth)acrylate (carbon number 1-20) alkyl esters, and for example: cycloalkyl (meth)acrylates (e.g. cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, etc.), aralkyl (meth)acrylates (e.g. benzyl (meth)acrylate, etc.), polycyclic (meth)acrylates (e.g. 2-isobornyl (meth)acrylate, 2- methyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropyl methyl butyl (meth)acrylate, etc.), alkoxy- or phenoxy-containing (meth)acrylates (2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, (meth)acrylate ethyl carbitol ester, (meth)acrylate phenoxyethyl ester, etc.), epoxy-containing (meth)acrylates (such as (meth)acrylate glycidyl ester, etc.), halogen-containing (meth)acrylates (such as (meth)acrylate 2,2,2-trifluoroethyl ester, (meth)acrylate 2,2,2-trifluoroethyl ester, (meth)acrylate tetrafluoropropyl ester, (meth)acrylate hexafluoropropyl ester, (meth)acrylate octafluoropentyl ester, (meth)acrylate heptadecafluorodecyl ester, etc.), (meth)acrylate alkylaminoalkyl esters (such as (meth)acrylate dimethylaminoethyl ester, etc.). These (meth)acrylates can be used alone or in combination of two or more. Specific examples of acrylic oligomers (A) include "ARUFON" manufactured by Toagosei Co., Ltd., "ACTFLOW" manufactured by Soken Chemical Co., Ltd., and "JONCRYL" manufactured by IGMresins Ltd.
[0057] When the acrylic oligomer is a liquid, there is no need to consider the solubility in the adhesive composition, so it can be used appropriately. Acrylic oligomers are usually liquid when the glass transition temperature (Tg) is less than 25°C. In addition, in order to take into account the compatibility with the adhesive composition and the concentrated presence of the components in the adhesive layer, it is preferred that the acrylic oligomer contains a polar functional group. As polar functional groups, hydroxyl groups, epoxy groups, carboxyl groups, alkoxysilyl groups, etc. can be listed. Specifically, for example: "ARUFONUH series", "ARUFON UC series", "ARUFON UF series", "ARUFON UG series", "ARUFON US series" (all manufactured by Toagosei Co., Ltd.) and the like can be listed. Among them, it is preferred to contain an epoxy group because it can achieve an improvement in adhesion brought about by the interaction with the polarizer. Specifically, for example: "ARUFON UG-4000", "ARUFON UG-4010" (all manufactured by Toagosei Co., Ltd.) can be listed.
[0058] <First optical film>
[0059] In the present invention, as the first optical film, a transparent protective film can be suitably used. Preferably, the thickness of the transparent protective film is thin, specifically, preferably less than 30 μm, more preferably 1 to 20 μm. As the transparent protective film, it is preferred that the transparency, mechanical strength, thermal stability, moisture barrier, isotropy, etc. are excellent. For example, polyester polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose polymers such as cellulose diacetate and cellulose triacetate, acrylic polymers such as polymethyl methacrylate, polystyrene, styrene polymers such as acrylonitrile-styrene copolymer (AS resin), polycarbonate polymers, etc. can be cited. In addition, polyethylene, polypropylene, polyolefins having a ring or norbornene structure, polyolefin polymers such as ethylene-propylene copolymers, vinyl chloride polymers, nylon, amide polymers such as aromatic polyamides, imide polymers, sulfone polymers, polyethersulfone polymers, polyetheretherketone polymers, polyphenylene sulfide polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl butyral polymers, polyarylate polymers, polyoxymethylene polymers, epoxy polymers, or mixtures of the above polymers can also be listed as examples of polymers forming the above transparent protective film. The transparent protective film may contain one or more of any appropriate additives. As additives, for example, ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, anti-coloring agents, flame retardants, nucleating agents, antistatic agents, pigments, colorants, etc. The content of the above thermoplastic resin in the transparent protective film is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, further preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. When the content of the thermoplastic resin in the transparent protective film is 50% by weight or less, there is a concern that high transparency inherent in the thermoplastic resin may not be fully exhibited.
[0060] In addition, as a transparent protective film, a polymer film described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can be cited, such as (A) a resin composition containing a thermoplastic resin having a substituted and / or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted and / or unsubstituted phenyl and nitrile group in the side chain. As a specific example, a film of a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be cited. The film can be formed by a mixed extrusion product of the resin composition. These films have a small phase difference and a small photoelastic coefficient, so they can eliminate the unevenness caused by the strain of the polarizing film. In addition, the moisture permeability is small, so the humidification durability is excellent.
[0061] It should be noted that in the present invention, the "in-plane average refractive index" of the transparent protective film is measured using a prism coupler SPA-4000 (manufactured by Cylon Technology Co., Ltd.) to measure the refractive index in the slow axis direction and the fast axis direction in the measurement plane to obtain their average value. The measurement temperature is set to 23° C. and the measurement wavelength is set to 532 nm.
[0062] <Second optical film>
[0063] In the present invention, a polarizer can be used as the second optical film. There is no particular limitation on the polarizer, and various polarizers can be used. As the polarizer, for example, there can be listed: a film formed by adsorbing dichroic materials such as iodine and dichroic dyes on hydrophilic polymer films such as polyvinyl alcohol films, partially methylated polyvinyl alcohol films, and partially saponified films of ethylene-vinyl acetate copolymers and uniaxially stretched, a polyene oriented film such as a dehydrated product of polyvinyl alcohol and a dehydrochlorinated product of polyvinyl chloride, etc. Among these, a polarizer formed by a polyvinyl alcohol film and a dichroic material such as iodine is suitable.
[0064] It should be noted that, in the present invention, for the "in-plane average refractive index" of the polarizer, the refractive index in the transmission axis direction and the refractive index in the absorption axis direction of the in-plane refractive index of the polarizer are measured using a prism coupler SPA-4000 (manufactured by Cylon technology), and their average value is taken as the in-plane average refractive index of the polarizer. The measurement temperature is set to 23° C. and the measurement wavelength is set to 532 nm.
[0065] The thickness of the polarizer is generally 1 to 30 μm, but as mentioned above, the thinner the laminated optical film is, the more uneven the reflected light is. In the present invention, the polarizer is preferably a thin polarizer, specifically, the thickness is preferably 20 μm or less, more preferably 1 to 12 μm.
[0066] As a thin polarizer, representative examples include: thin polarizing films described in Japanese Patent Application No. 51-069644, Japanese Patent Application No. 2000-338329, WO2010 / 100917, PCT / JP2010 / 001460, Japanese Patent Application No. 2010-269002, and Japanese Patent Application No. 2010-263692. These thin polarizing films can be obtained by a method including a step of stretching a polyvinyl alcohol resin (hereinafter, also referred to as a PVA resin) layer and a stretching resin substrate in a laminated state and a step of dyeing. According to this method, even if the PVA resin layer is thin, it can be stretched by being supported by the stretching resin substrate without causing undesirable conditions such as breakage caused by stretching.
[0067] As the above-mentioned thin polarizing film, in the method including the steps of stretching in the state of a laminate and the step of dyeing, from the aspect of being able to stretch at a high ratio and improving the polarization performance, it is preferably obtained by a method including a step of stretching in an aqueous boric acid solution as described in WO2010 / 100917 pamphlet, PCT / JP2010 / 001460, or Japanese Patent Application No. 2010-269002 and Japanese Patent Application No. 2010-263692. It is particularly preferred to obtain it by a method including a step of auxiliary stretching in a gas atmosphere before stretching in an aqueous boric acid solution as described in Japanese Patent Application No. 2010-269002 and Japanese Patent Application No. 2010-263692.
[0068] The laminated optical film produced by the production method of the present invention is characterized in that the in-plane refractive index is different between the front side and the back side of the adhesive layer. The laminated optical film including the adhesive layer can be produced by the following production method. A method for manufacturing a laminated optical film, wherein the laminated optical film is laminated with a first optical film and a second optical film different from the first optical film via an adhesive layer, the adhesive layer comprising a first cured layer of a first adhesive composition and a second cured layer of a second adhesive composition, the first adhesive composition and the second adhesive composition containing at least a portion of different components, the method comprising: a first step of applying the first adhesive composition to the bonding surface of the first optical film; a second step of applying the second adhesive composition to the bonding surface of the second optical film; a third step of bonding the first adhesive composition-coated surface of the first optical film and the second adhesive composition-coated surface of the second optical film; and a fourth step of irradiating active energy rays from the first optical film surface side or the second optical film surface side to bond the first optical film to the second optical film, wherein in the first step, the first cured layer is cured before the second cured layer.
[0069] In the above manufacturing method, the adhesive layer includes a first cured product layer of a first adhesive composition and a second cured product layer of a second adhesive composition, and the first adhesive composition and the second adhesive composition contain at least a part of different components, so that the in-plane refractive index R of the first optical film side surface F1 is formed. F1 The in-plane refractive index R of the second optical film side surface F2 is F2 Here, the in-plane average refractive index of the first optical film and the in-plane average refractive index of the second optical film can be measured in advance, and the in-plane refractive index R of the first optical film side surface F1 of the first cured layer of the first adhesive composition can be F1 and the in-plane refractive index R of the second optical film side surface F2 F2It is also possible to design it to any value by performing the best matching design. Therefore, in the above manufacturing method, it is possible to manufacture a F1 The difference between the in-plane average refractive index of the first optical film and the first optical film is within 0.02, R F2 A laminated optical film having an adhesive layer whose difference in in-plane average refractive index with the second optical film is within 0.02.
[0070] It should be noted that in the above-mentioned first step, the above-mentioned first adhesive composition after coating can be irradiated with active energy rays from the above-mentioned first optical film surface side or the above-mentioned first adhesive composition coating surface side of the above-mentioned first optical film to cure the above-mentioned first adhesive composition and form the above-mentioned first cured material layer in advance. The above-mentioned first adhesive composition after coating can also be air-dried, and then the solvent is removed when the above-mentioned first adhesive composition after coating contains a solvent, thereby curing the first adhesive composition in an uncured state.
[0071] In the laminated optical film of the present invention, when the first optical film is a transparent protective film and the second optical film is a polarizer, a surface modification treatment may be performed before the first step and / or the second coating step (coating step). Specific treatments include corona treatment, plasma treatment, saponification treatment, and the like.
[0072] In addition, in the above-mentioned first step and / or the second coating step (coating step), the coating method of the active energy ray-curable adhesive composition can be appropriately selected according to the viscosity and target thickness of the composition. As examples of coating methods, for example, reverse coaters, gravure coaters (direct, reverse, or offset), rod-type reverse coaters, roll coaters, die coaters, wire rod coaters, rod coaters, etc. can be cited. In addition, dipping methods and the like can be appropriately used during coating.
[0073] In the third step (bonding step), two different optical films are bonded together via the applied active energy ray-curable adhesive composition. The bonding of the optical films can be performed by, for example, a roll laminator or the like.
[0074] In the fourth step (bonding step), the active energy ray-curable adhesive composition can be used in the form of electron beam curing, ultraviolet curing, or visible light curing. As the active energy ray-curable adhesive composition, a visible light curing adhesive composition is preferred from the viewpoint of productivity.
[0075] For the active energy ray-curable adhesive composition, for example, after laminating the polarizer and the transparent protective film, the active energy ray (electron beam, ultraviolet light, visible light, etc.) is irradiated to cure the active energy ray-curable adhesive composition, thereby forming an adhesive layer. In the fourth step (bonding step), the irradiation direction of the active energy ray (electron beam, ultraviolet light, visible light, etc.) can be irradiated from any appropriate direction. It is preferably irradiated from the transparent protective film side. If irradiated from the polarizer side, there is a concern that the polarizer will deteriorate due to the active energy ray (electron beam, ultraviolet light, visible light, etc.).
[0076] In the electron beam curing type, the electron beam irradiation conditions can be any appropriate conditions as long as they can cure the above-mentioned active energy ray curing adhesive composition. For example, the acceleration voltage of electron beam irradiation is preferably 5kV to 300kV, and more preferably 10kV to 250kV. When the acceleration voltage is less than 5kV, there is a concern that the electron beam cannot reach the adhesive and the curing becomes insufficient. If the acceleration voltage is greater than 300kV, there is a concern that the penetration force through the sample is too strong and the transparent protective film and polarizer are damaged. As for the irradiation dose, it is 5 to 100kGy, and more preferably 10 to 75kGy. When the irradiation dose is less than 5kGy, the adhesive is not sufficiently cured. If it is greater than 100kGy, the transparent protective film and polarizer are damaged, the mechanical strength is reduced, yellowing occurs, and the given optical properties cannot be obtained.
[0077] Electron beam irradiation is usually performed in an inert gas, but can be performed in the atmosphere with a small amount of oxygen introduced as needed. Depending on the material of the transparent protective film, oxygen is appropriately introduced so that the surface of the transparent protective film that is first contacted by the electron beam is contacted, oxygen barrier occurs, and damage to the transparent protective film can be prevented, so that only the adhesive can be efficiently irradiated with the electron beam.
[0078] When manufacturing the laminated optical film of the present invention, as the active energy ray, it is preferred to use an active energy ray containing visible light in the wavelength range of 380nm to 450nm, especially an active energy ray with the largest irradiation amount of visible light in the wavelength range of 380nm to 450nm. In the case of ultraviolet curing type and visible light curing type, when a transparent protective film (ultraviolet non-transmissive transparent protective film) endowed with ultraviolet absorption ability is used, light with a wavelength shorter than about 380nm is absorbed. Therefore, light with a wavelength shorter than 380nm will not reach the active energy ray curing adhesive and will not contribute to its polymerization reaction. In addition, the light with a wavelength shorter than 380nm absorbed by the transparent protective film is converted into heat, and the transparent protective film itself generates heat, which becomes the cause of defects such as curling / wrinkling of the laminated optical film. Therefore, in the present invention, when using an ultraviolet curing type or a visible light curing type, it is preferred to use a device that does not emit light with a wavelength shorter than 380nm as an active energy ray generating device. More specifically, the ratio of the cumulative illuminance in the wavelength range of 380 to 440nm to the cumulative illuminance in the wavelength range of 250 to 370nm is preferably 100:0 to 100:50, and more preferably 100:0 to 100:40. As the active energy ray of the present invention, a metal halide lamp enclosed with gallium or an LED light source emitting light in the wavelength range of 380 to 440nm is preferred. Alternatively, a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, an incandescent lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a metal halide lamp, a fluorescent lamp, a tungsten lamp, a gallium lamp, an excimer laser or sunlight, etc., containing ultraviolet light and visible light, can be used, and ultraviolet light with a wavelength shorter than 380nm can be blocked by a bandpass filter. In order to improve the bonding performance of the adhesive layer between the polarizer and the transparent protective film and prevent curling of the laminated optical film, it is preferred to use a metal halide lamp encapsulated with gallium, and use active energy rays obtained by a bandpass filter that can block light with a wavelength shorter than 380nm, or active energy rays with a wavelength of 405nm obtained using an LED light source.
[0079] In the case of ultraviolet curing type or visible light curing type, it is also preferred to heat the active energy ray-curing adhesive after irradiation with ultraviolet light or visible light (heating after irradiation). In this case, it is preferably heated to 40° C. or higher, more preferably 50° C. or higher.
[0080] The active energy ray-curable adhesive used in the present invention can be used particularly preferably when forming an adhesive layer that bonds a polarizer to a transparent protective film having a transmittance of less than 5% at a wavelength of 365 nm. Here, the active energy ray-curable adhesive of the present invention can be cured to form an adhesive layer by irradiating ultraviolet rays through a transparent protective film having UV absorption ability by containing the photopolymerization initiator of the above-mentioned general formula (1). Therefore, even for a laminated optical film having a transparent protective film having UV absorption ability laminated on both sides of the polarizer, the adhesive layer can be cured. However, of course, for a laminated optical film having a transparent protective film without UV absorption ability laminated, the adhesive layer can also be cured. It should be noted that the transparent protective film having UV absorption ability refers to a transparent protective film having a transmittance of less than 10% for light at 380 nm.
[0081] Examples of a method for imparting UV absorption capability to a transparent protective film include a method of incorporating an ultraviolet absorber into the transparent protective film and a method of laminating a surface treatment layer containing an ultraviolet absorber on the surface of the transparent protective film.
[0082] Specific examples of the ultraviolet absorber include conventionally known oxybenzophenone compounds, benzotriazole compounds, salicylate compounds, benzophenone compounds, cyanoacrylate compounds, nickel complex compounds, triazine compounds, and the like.
[0083] <Second Adhesive Layer>
[0084] exist Figure 2 In the embodiment shown, the second adhesive layer 4 can be designed in the same manner as the first adhesive layer described above. Figure 2 In the embodiment shown, the light L incident on the second adhesive layer 4 is incident through the polarizer (second optical film) 3, and thus becomes polarized light in the transmission axis direction of the polarizer 3. Therefore, in order to suppress reflection at the interface between the polarizer 3 and the second adhesive layer 4, and at the interface between the phase difference film 5 and the second adhesive layer 4, it is preferred that the refractive index R in the transmission axis direction of the polarizer 3 of the polarizer 3 side surface F3 of the second adhesive layer 4 is F3 The refractive index R of the polarizer 3 in the transmission axis direction on the side surface F4 of the phase difference film 5 is F4 Different, R F3 The difference in refractive index in the transmission axis direction with the polarizer 3 is within 0.05, R F4 The difference in refractive index in the transmission axis direction of the polarizer 3 with the phase difference film 5 is within 0.05. In this case, the reflectivity of the entire image display device M is reduced, and the visibility is significantly improved.
[0085] <Third optical film>
[0086] The third optical film is not particularly limited, and may be, for example, a reflective film, a semi-transmissive film, a phase difference film (including 1 / 2, 1 / 4 wave plates), a visual compensation film, or other optical layers used in the formation of an image display device, etc. In the present invention, it is preferred that the thickness of the third optical film is thin, specifically, preferably 20 μm or less, more preferably 1 to 10 μm.
[0087] <Adhesive layer>
[0088] exist Figure 2 In the embodiment shown, the laminated optical film having the transparent protective film (first optical film) 1, the first adhesive layer 2, the polarizer (second optical film) 3, the second adhesive layer 4 and the phase difference film (third optical film) 5 is laminated on the organic light emitting diode 7 via the adhesive layer 6. The adhesive forming the adhesive layer is not particularly limited, and an adhesive having a base polymer such as acrylic polymer, silicone polymer, polyester, polyurethane, polyamide, polyether, fluorine, rubber, etc. can be appropriately selected and used. It is particularly preferable to use an adhesive having excellent optical transparency, adhesive properties such as moderate wettability, aggregation and adhesion, and excellent weather resistance, heat resistance, etc., such as acrylic adhesives.
[0089] The adhesive layer may be provided on one or both sides of the polarizing film or optical film in the form of a superimposed layer of layers of different compositions or types. In addition, when provided on both sides, adhesive layers of different compositions, types, thicknesses, etc. may be formed on the surface and back of the polarizing film or optical film. The thickness of the adhesive layer may be appropriately determined according to the purpose of use, adhesive strength, etc., and is usually 1 to 500 μm, preferably 1 to 200 μm, and particularly preferably 1 to 100 μm.
[0090] The exposed surface of the adhesive layer is temporarily covered by a diaphragm for the purpose of preventing contamination during the period until it is actually used. Thus, it is possible to prevent contact with the adhesive layer under normal handling conditions. As a diaphragm, in addition to the above-mentioned thickness conditions, a diaphragm such as a diaphragm coated with a suitable thin layer such as a plastic film, a rubber sheet, paper, a cloth, a non-woven fabric, a net, a foam sheet, a metal foil, or a laminate thereof with a suitable release agent such as silicone, a long-chain alkyl, a fluorine, or molybdenum sulfide as required can be used.
[0091] <Image display device>
[0092] The laminated optical film of the present invention can be preferably used for forming various image display devices such as organic EL image devices and liquid crystal display devices. The image display device can be formed in a conventional manner. That is, the image display device is usually formed by appropriately assembling components such as an organic light emitting diode, a liquid crystal unit and a laminated optical film, and a lighting system used as required, and then installing a drive circuit. In the present invention, there is no particular limitation except that the laminated optical film of the present invention is used, and the formation can be carried out in a conventional manner.
[0093] When the laminated optical film of the present invention is used in a liquid crystal display device, a suitable liquid crystal display device such as a liquid crystal display device with a laminated optical film disposed on one side or both sides of a liquid crystal cell, a liquid crystal display device using a backlight or a reflector in the lighting system can be formed. In this case, the laminated optical film of the present invention can be disposed on one side or both sides of the liquid crystal cell. When laminated optical films are disposed on both sides, they can be the same or different. Furthermore, when forming a liquid crystal display device, suitable components such as a diffusion plate, an anti-glare layer, an anti-reflection film, a protective plate, a prism array, a lens array sheet, a light diffusion plate, a backlight, etc. can be disposed at a suitable position.
[0094] Example
[0095] (First optical film (transparent protective film))
[0096] As the first optical film, a cycloolefin-based protective film (trade name: ZF14-013, manufactured by Nippon Zeon) having an in-plane average refractive index of 1.537 at 550 nm was used.
[0097] (Second optical film (polarizer))
[0098] As the second optical film, a polarizer (thickness 5 μm) having an in-plane average refractive index of 1.555 at 550 nm was used.
[0099] <Active energy rays>
[0100] Visible light (gallium-encapsulated metal halide lamp) was used as active energy ray. Irradiation device: Light HAMMER 10 manufactured by FusionUV Systems, Inc. Valve: V valve Peak illuminance: 1600 mW / cm 2 , cumulative exposure 1000 / mJ / cm 2 (Wavelength: 380 to 440 nm) The illuminance of visible light was measured using the Sola-Check system manufactured by Solatell.
[0101] (First Adhesive Composition and Second Adhesive Composition)
[0102] The following components were mixed according to the formulation table described in Table 1, and stirred at 50° C. for 1 hour to prepare a first adhesive composition and a second adhesive composition. The raw materials used are shown below.
[0103] "ACMO" (acryloylmorpholine), trade name "ACMO", manufactured by KJ Chemical Co., Ltd.
[0104] "1,9NDA" (1,9-nonanediol diacrylate), manufactured by Kyoeisha Chemical Co., Ltd.
[0105] "UP1190", trade name "ARUFONUP1190", manufactured by Toagosei Co., Ltd.
[0106] "POB-A", trade name "LIGHT ACRYLATE POB-A", manufactured by Kyoeisha Chemical Co., Ltd.
[0107] "OGSOL F5710", trade name "OGSOLEA-F5710", manufactured by Osaka Gas Chemical Co., Ltd.
[0108] “KAYACUREDETX-S (diethylthioxanthone, a compound described in the general formula (1)), trade name “KAYACUREDETX-S”, manufactured by Nippon Kayaku Co., Ltd. “Omnirad907 (2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, a compound described in the general formula (2)), trade name “Omnirad907”, manufactured by IGMresins
[0109] Example 1
[0110] Using an MCD coater (manufactured by Fuji Machine Co., Ltd.) (unit shape: honeycomb, gravure roller line count: 1000 lines / inch, rotation speed 140% / pair of line speed), apply the first adhesive composition adjusted to the amount recorded in Table 1 to the bonding surface of the transparent protective film so that the thickness becomes 1 μm, and irradiate the first adhesive composition coating surface with the above-mentioned visible light through an active energy ray irradiation device to first form a first cured layer (first step). Next, using an MCD coater, apply the second adhesive composition adjusted to the amount recorded in Table 1 to the bonding surface of the polarizer so that the thickness becomes 1 μm (second step). Then, the first cured layer on the transparent protective film and the second adhesive composition coating surface of the polarizer are bonded (third step). Then, the above-mentioned visible light is irradiated from the side of the bonded transparent protective film through an active energy ray irradiation device to cure the active energy ray-curable adhesive, and then hot air drying is performed at 70°C for 3 minutes to obtain a polarizing film (laminated optical film) having a transparent protective film on one side and a thin polarizer 1 (the fourth step).
[0111] Comparative Example 1
[0112] The first adhesive composition and the second adhesive composition of the same composition are respectively applied to the bonding surface of the transparent protective film and the bonding surface of the polarizer in a manner of 1 μm in thickness. The first adhesive composition is not cured first, but the first cured layer on the transparent protective film and the second adhesive composition coating surface of the polarizer are bonded, and then the above-mentioned visible light is irradiated from the bonded transparent protective film side by an active energy ray irradiation device to cure the active energy ray-curable adhesive. Except for this, a polarizing film (laminated optical film) having a transparent protective film on one side and a thin polarizer 1 is obtained by the same method as Example 1.
[0113] (Measurement of reflectivity of laminated optical film)
[0114] After the polarizer surface of the obtained polarizing film and the black acrylic plate were bonded together using a 20 μm thick adhesive (refractive index 1.492), the reflectivity at a polar angle of 10° was measured from the transparent protective film side at an interval of 1 nm in the range of 400 nm to 700 nm based on the azimuth angle of the same axis as the absorption axis direction of the polarizer using CARY7000UMS (manufactured by Agilent Technologies). The average value was taken as the reflectivity, and the results are shown in Table 1.
[0115] [Table 1]
[0116]
[0117] From the results in Table 1, it can be seen that in Comparative Example 1, the adhesive layer obtained is a uniform layer, so the reflectivity is the same on the front side and the back side. As a result, the refractive index difference between the polarizer and the adhesive layer becomes larger, so the reflectivity becomes larger. On the other hand, it can be seen that in Example 1, the in-plane refractive index R of the transparent protective film surface F1 of the adhesive layer obtained is F1 The in-plane refractive index R of the polarizer side surface F2 is F2 Different, and R F1 With R (a) , R F2 With R (b) The difference is designed to be within 0.004. As a result, it is found that the reflectance of the obtained polarizing film becomes small.
Claims
1. A method for producing a laminated optical film, wherein the laminated optical film is formed by laminating a first optical film and a second optical film different from the first optical film via an adhesive layer. The adhesive layer includes a first cured product layer of a first adhesive composition and a second cured product layer of a second adhesive composition, wherein the first adhesive composition and the second adhesive composition contain at least a portion of different components. The in-plane refractive index R of the first optical film-side surface F1 of the adhesive layer is F1 The in-plane refractive index R of the second optical film side surface F2 is F2 Different, R F1 The difference between the in-plane average refractive index of the first optical film and the first optical film is within 0.02, R F2 The difference in the in-plane average refractive index with the second optical film is within 0.02, The thickness of the adhesive layer is 0.5 to 3 μm. The thickness of the first optical film is 1 to 20 μm. The thickness of the second optical film is 1 to 12 μm. The method includes: a first step of applying the first adhesive composition on the bonding surface of the first optical film; a second step of applying the second adhesive composition on the bonding surface of the second optical film; a third step of laminating the surface of the first optical film coated with the first adhesive composition and the surface of the second optical film coated with the second adhesive composition; and a fourth step of irradiating the first optical film surface side or the second optical film surface side with active energy rays to bond the first optical film and the second optical film together; In the first step, the first cured material layer is cured earlier than the second cured material layer.
2. The method for producing a laminated optical film according to claim 1, wherein: In the first step, the applied first adhesive composition is irradiated with active energy rays from the first optical film surface side or the first adhesive composition-coated surface side of the first optical film to cure the first adhesive composition, so that the first cured layer is cured before the second cured layer.
3. The method for producing a laminated optical film according to claim 1, wherein: The first optical film is a transparent protective film, and the second optical film is a polarizer.