Light emitting element, method for manufacturing the same, and display device including the light emitting element
By using a graphene layer as a separation layer in the manufacturing process of inorganic light-emitting diodes, the element rod is peeled off from the substrate to form a flat separation surface. This solves the problem of short circuits or open circuits caused by uneven end surfaces during the separation process of inorganic light-emitting diodes, and improves the reliability of the light-emitting element.
Patent Information
- Application Number
- CN201980051758.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-03
- Filing Date
- 2019-01-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-01-14
AI Technical Summary
In the separation process of existing inorganic light-emitting diodes, the surface of the longitudinal end is not flat, which makes it easy for short circuits or open circuits to occur when in contact with the contact electrode.
By growing a graphene layer on the substrate as a separation layer, the component rod is peeled off from the substrate by utilizing the difference in interfacial attraction of the graphene layer, forming a flat separation surface, and an insulating layer is formed on the outer surface of the component rod to avoid additional etching processes.
Inorganic light-emitting diodes with flat separation surfaces are manufactured to prevent short circuits or open circuits in the contact electrode materials during connection, thereby improving the reliability of the light-emitting element.
Smart Images

Figure CN112534591B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a light emitting element, a method for manufacturing the same, and a display device including the same, and in particular, to a light emitting element having one end with a smooth separation surface, a method for manufacturing the same, and a display device including the same. Background Art
[0002] As multimedia technology develops, the importance of display devices has steadily increased. Therefore, various types of display devices such as organic light emitting displays and liquid crystal displays (LCDs) have been used.
[0003] The display device is a device for displaying an image, and includes a display panel such as an organic light emitting display panel or a liquid crystal display panel. Among them, the light emitting display panel may include a light emitting element. Examples of light emitting diodes (LEDs) include organic light emitting diodes (OLEDs) using organic materials as fluorescent materials and inorganic light emitting diodes using inorganic materials as fluorescent materials.
[0004] Organic light emitting diodes (OLEDs) using organic materials as fluorescent materials of light emitting elements have advantages of simple manufacturing processes and can have flexibility in display devices. However, it is known that organic materials are susceptible to high temperature operating environments and have relatively low blue light efficiency.
[0005] On the other hand, inorganic light-emitting diodes using inorganic semiconductors as fluorescent materials have the advantages of durability even in high temperature environments and high blue light efficiency compared to organic light-emitting diodes. In addition, in the manufacturing process pointed out as a limitation of conventional inorganic light-emitting diodes, a transfer method using a dielectrophoresis (DEP) method has been developed. Therefore, inorganic light-emitting diodes having excellent durability and efficiency compared to organic light-emitting diodes have been continuously studied. Summary of the invention
[0006] Technical issues
[0007] Inorganic light emitting diodes can be manufactured by growing an n-type or p-type doped semiconductor layer and an inorganic fluorescent material layer on a base substrate to form a rod with a specific shape, and then separating the rod. However, in the case where the light emitting element is separated by a physical method, the longitudinal end surface of the light emitting element may be uneven. The unevenness, jaggedness or roughness of the longitudinal end surface of the light emitting element may cause a short circuit problem in the case of contact between the light emitting element and the contact electrode.
[0008] In view of the above circumstances, aspects of the present disclosure provide a light emitting element having a flat end surface for contacting a contact electrode and a method of manufacturing the same.
[0009] Aspects of the present disclosure also provide a display device including a light emitting element capable of preventing an open circuit or a short circuit problem of an electrode material from occurring in a case of connection with a contact electrode.
[0010] It should be noted that aspects of the present disclosure are not limited to the above-mentioned aspects, and those skilled in the art will clearly understand other not-mentioned aspects of the present disclosure from the following description.
[0011] Technical Solution
[0012] According to an exemplary example of the present disclosure, a method for manufacturing a display element includes: preparing a lower substrate, the lower substrate including a base substrate and a buffer material layer formed on the base substrate; forming a separation layer, the separation layer being arranged on the lower substrate and including at least one graphene layer; forming an element deposition structure by depositing a first conductive semiconductor layer, an active material layer, and a second conductive semiconductor layer on the separation layer; forming an element rod by etching the element deposition structure and the separation layer in a vertical direction; and separating the element rod from the lower substrate to form a light-emitting element.
[0013] In the formation of the element rods, the separation layer may be at least partially etched and patterned.
[0014] An interfacial attraction force between the separation layer and the lower substrate at a first interface between the separation layer and the lower substrate may be greater than an interfacial attraction force between the separation layer and the element rod at a second interface between the separation layer and the element rod.
[0015] In the formation of the light emitting element, the second interface may be peeled off, but the first interface may not be peeled off, and the patterned separation layer may remain on the lower substrate.
[0016] In the light emitting element, the separation surface may be substantially flat and parallel to the top surface of the second conductive type semiconductor layer, the separation surface being a surface where the element rod is peeled off from the second interface.
[0017] In the light emitting element, the separation surface may have a surface roughness within a range of 8 nm Ra to 12 nm Ra.
[0018] The formation of the element rod may also include forming an insulating layer, which is arranged to surround the side surface of the element rod, and the light-emitting element may also include an insulating layer arranged to surround the side surface of the first conductive semiconductor layer, the side surface of the active material layer and the side surface of the second conductive semiconductor layer.
[0019] The separation layer may include: a first graphene layer; and a second graphene layer, disposed on the first graphene layer, the first graphene layer may form a third interface with the buffer material layer, the second graphene layer may form a fifth interface with the element rod, and the first graphene layer and the second graphene layer may form a fourth interface.
[0020] In the formation of the light-emitting element, the third interface may not be peeled off, at least a portion of the fourth interface and the fifth interface may be peeled off, the first graphene layer may remain on the lower substrate, and the second graphene layer may form a fourth interface with the first graphene layer, or the second graphene layer may form a fifth interface with the element rod.
[0021] The separation layer may include: a first sub-separation layer disposed on the lower substrate; and a second sub-separation layer interposed between the base substrate and the buffer material layer.
[0022] The device deposition structure may further include an electrode material layer on the second conductive type semiconductor layer.
[0023] The formation of the element rod may include: forming an etching mask layer on the element deposition structure, and forming an etching pattern layer on the etching mask layer, the etching pattern layer including one or more nano-patterns separated from each other; forming a hole by vertically etching an area formed by the nano-patterns separated from each other; and removing the etching mask layer and the etching pattern layer.
[0024] The element deposition structure and the separation layer may include materials with different etching selectivities, and the formation of the hole may include vertically etching the element deposition structure to expose at least a portion of an overlapping area between the separation layer and an area formed by nanopatterns separated from each other; and etching the exposed area of the separation layer and patterning the exposed area of the separation layer.
[0025] In the vertical etching of the device deposition structure, the etchant may include chlorine (Cl 2 ) and oxygen (O 2 ), and the separation layer and the element deposition structure can be etched simultaneously.
[0026] According to another exemplary example of the present disclosure, a light-emitting element includes: a first conductive semiconductor doped with a dopant of a first polarity; an active layer disposed on the first conductive semiconductor; a second conductive semiconductor disposed on the active layer and doped with a dopant of a second polarity opposite to the first polarity; an electrode material layer disposed on the second conductive semiconductor; and an insulating material layer disposed to surround a side surface of the first conductive semiconductor, a side surface of the second conductive semiconductor, a side surface of the active layer, and a side surface of the electrode material layer, wherein a bottom surface of the first conductive semiconductor is substantially flat and parallel to a top surface of the second conductive semiconductor.
[0027] The bottom surface of the first conductive type semiconductor and the top surface of the second conductive type semiconductor may have a surface roughness within a range of 8 nm Ra to 12 nm Ra.
[0028] The length of the light emitting element measured in the long axis direction may be in the range of 3.0 μm to 6.0 μm, and the length of the light emitting element specified in another direction intersecting the long axis direction is in the range of 400 nm to 700 nm.
[0029] According to other exemplary examples of the present disclosure, a display device includes: a substrate; at least one first electrode and at least one second electrode, the at least one first electrode and the at least one second electrode extending in a first direction on the substrate and spaced apart from each other in a second direction different from the first direction; at least one light-emitting element arranged in a separation space between the first electrode and the second electrode; a first contact electrode partially covering the first electrode and contacting a first end of the light-emitting element; and a second contact electrode spaced apart from the first contact electrode and partially covering the second electrode to contact a second end of the light-emitting element opposite to the first end, wherein the light-emitting element has a flat shape so that each side surface of the first end and the second end is parallel to a plane perpendicular to the substrate.
[0030] The light-emitting element may include: a first conductive semiconductor; an active layer disposed on the first conductive semiconductor; a second conductive semiconductor disposed on the active layer and having a polarity opposite to that of the first conductive semiconductor; an electrode material layer disposed on the second conductive semiconductor; and an insulating material layer disposed to surround the side surface of the first conductive semiconductor, the side surface of the active layer, the side surface of the second conductive semiconductor, and the side surface of the electrode material layer.
[0031] Each of the side surfaces of the first and second ends of the light emitting element may have a surface roughness within a range of 8 nm Ra to 12 nm Ra.
[0032] The above and other features and advantages thereof will become more apparent by describing in detail exemplary embodiments of the present invention with reference to the accompanying drawings.
[0033] Beneficial Effects
[0034] According to the embodiment, the method for manufacturing a light-emitting element can manufacture a light-emitting element having a flat separation surface by separating an element rod grown on a base substrate from the base substrate by peeling off a graphene layer. The method for manufacturing a light-emitting element can also manufacture a light-emitting element in such a manner that an insulating layer is formed on the outer surface of the element rod and the element rod is separated from the base substrate. Therefore, the method for manufacturing a light-emitting element can manufacture a light-emitting element whose both ends are flat without any additional etching process.
[0035] The light emitting element disposed between two electrodes of the display device has two flat and substantially parallel end surfaces, which can prevent the open circuit or short circuit problem of the contact electrode material from occurring when connected to the contact electrode.
[0036] Advantageous effects according to the present disclosure are not limited to those mentioned above, and various other advantageous effects are included herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a plan view of a display device according to an embodiment.
[0038] Figure 2 It is along Figure 1 Cross-sectional views taken along line II', line II-II' and line III-III'.
[0039] Figure 3a is a schematic diagram of a light emitting element according to an embodiment.
[0040] Figure 3b It is along Figure 3a A cross-sectional view taken along line 3b-3b'.
[0041] Figure 4 yes Figure 3b A magnified view of a portion of .
[0042] Figure 5 yes Figure 2 An enlarged view of part A of FIG.
[0043] Figures 6 to 18 is a schematic cross-sectional view schematically illustrating a method for manufacturing a light emitting element according to an embodiment.
[0044] Figures 19 to 24 is a cross-sectional view schematically showing a part of a method for manufacturing a light emitting element according to another embodiment. DETAILED DESCRIPTION
[0045] The present invention will now be described more fully hereinafter with reference to the accompanying drawings in which preferred embodiments of the invention are shown. However, the present invention may be implemented in different forms and should not be construed as being limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete and will fully convey the scope of the invention to those skilled in the art.
[0046] It will also be understood that when a layer is referred to as being “on” another layer or substrate, it can be directly on the other layer or substrate, or intervening layers may also be present. The same reference numerals refer to the same components throughout the specification.
[0047] It will be understood that although the terms "first", "second", etc. may be used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. For example, the first element discussed below may be referred to as the second element without departing from the teachings of the present invention. Similarly, the second element may also be referred to as the first element.
[0048] Hereinafter, exemplary embodiments will be described with reference to the accompanying drawings.
[0049] Figure 1 is a plan view of a display device according to an embodiment.
[0050] The display device 10 may include at least one area defined as a pixel PX. The display device 10 may include a display area composed of a plurality of pixels PX, each pixel PX emitting light in a specific wavelength band to the outside of the display device 10. Figure 1 , three pixels PX1, PX2, and PX3 are exemplarily shown in FIG. 1 , but it is obvious that the display device 10 may also include a greater number of pixels. Although the drawings show that the plurality of pixels PX are arranged in one direction (e.g., the first direction D1) in the cross-sectional view, the plurality of pixels PX may also be arranged in a second direction D2 intersecting the first direction D1. In addition, Figure 1 Each of the pixels PX may be divided into a plurality of parts, and each part may constitute a pixel PX. Figure 1 The arrangement is shown in FIG. 1 only in parallel in the first direction D1 , and may have various structures such as being arranged in a vertical direction (or the second direction D2 ) or being arranged in a zigzag manner.
[0051] Although not shown in the drawings, the display device 10 may include an emission region in which a light emitting element 300 for emitting light of certain colors is arranged and a non-emission region defined as a region remaining after excluding the emission region. The non-emission region may be covered by certain components that are not visually perceived from the outside of the display device 10. Various components for driving the light emitting element 300 provided in the emission region may be provided in the non-emission region. For example, the non-emission region may include wiring, a circuit unit, and a driving unit for applying an electrical signal to the emission region, but the present disclosure is not limited thereto.
[0052] A plurality of pixels PX may display colors by including one or more light emitting elements 300 that emit light of a specific wavelength band. The light emitted from the light emitting element 300 may be projected to the outside through the emission area of the display device 10. In an embodiment, each of the pixels PX that express different colors may include different light emitting elements 300 that emit light of different colors. For example, the first pixel PX1 that expresses red may include a light emitting element 300 that emits red light, the second pixel PX2 that expresses green may include a light emitting element 300 that emits green light, and the third pixel PX3 that expresses blue may include a light emitting element 300 that emits blue light. However, the present disclosure is not limited thereto, and in some cases, pixels that express different colors may include light emitting elements 300 that emit light of the same color (e.g., blue light), or they may all include a wavelength conversion layer or a color filter on the light emission path to produce a pixel-specific color. However, the present disclosure is not limited thereto, and in some cases, adjacent pixels PX may emit light of the same color.
[0053] Reference Figure 1 , the display device 10 may include a plurality of electrodes 210 and 220 and a plurality of light emitting elements 300. At least a portion of each of the electrodes 210 and 220 may be disposed in each pixel PX and electrically connected to the light emitting element 300 to apply an electrical signal so that the light emitting element 300 emits light of a specific color.
[0054] At least a portion of each of the electrodes 210 and 220 may also contribute to generating an electric field in the pixel PX to align the light emitting element 300. In more detail, during the alignment of the light emitting elements 300 emitting light of different colors in a plurality of pixels PX, it is necessary to accurately align the pixel-specific (PX-specific) light emitting elements 300. In the case of using an electrophoresis method for aligning the light emitting elements 300, the light emitting elements 300 may be aligned in a manner that a solution including the light emitting elements 300 is deposited on the display device 10 and an AC power is applied thereto to generate a capacitor having an electric field that generates an electrophoretic force for the light emitting elements 300.
[0055] The plurality of electrodes 210 and 220 may include a first electrode 210 and a second electrode 220. In an exemplary embodiment, the first electrode 210 may be a pixel electrode branched for each pixel PX, and the second electrode 220 may be a common electrode commonly connected to the plurality of pixels PX. One of the first electrode 210 and the second electrode 220 may be an anode electrode of the light emitting element 300, and the other may be a cathode electrode of the light emitting element 300. However, the present disclosure is not limited thereto, and the situation may also be the opposite.
[0056] The first and second electrodes 210 and 220 may include respective electrode stems 210S and 220S arranged to extend in a first direction D1 and at least one respective electrode branch 210B and 220B extending from the respective electrode stems 210S and 220S in a second direction D2 crossing the first direction D1 .
[0057] In detail, the first electrode 210 may include a first electrode trunk 210S arranged to extend in the first direction D1 and at least one first electrode branch 210B branching from the first electrode trunk 210S and extending in the second direction D2. Although not shown in the drawings, the first electrode trunk 210S may be connected to a signal input pad (pad, or "pad") at one end thereof and extend in the first direction D1 at the other end thereof to maintain electrical disconnection between the pixels PX. The signal input pad may be connected to a power source or an outside of the display device 10 to apply an electrical signal to the first electrode trunk 210S, or apply AC power while aligning the light emitting element 300.
[0058] The first electrode trunk 210S of one pixel can be arranged substantially in the same row as the first electrode trunk 210S of the adjacent pixels (e.g., adjacent in the first direction D1) belonging to the same row. That is, the first electrode trunk 210S of one pixel can be arranged so that its two ends terminate between the corresponding pixels while being spaced apart from each other, and the first electrode trunk 210S of the adjacent pixels can be aligned with the extension line of the first electrode trunk 210S of one pixel. In this way, the first electrode trunk 210S can be arranged in such a way that it is formed as a continuous trunk electrode in the manufacturing process, and is disconnected by cutting with a laser or the like after performing the alignment process of the light emitting element 300. Therefore, the first electrode trunk 210S of the corresponding pixel PX can apply different electrical signals to the corresponding first electrode branch 210B, and the first electrode trunks 210S can operate independently of each other.
[0059] The first electrode branch 210B may branch from at least a portion of the first electrode trunk 210S and extend and terminate in the second direction D2 to maintain a certain distance from the second electrode trunk 220S arranged to face the first electrode trunk 210S. That is, the first electrode branch 210B may be arranged to be connected to the first electrode trunk 210S at one end thereof, and to be placed inside the pixel PX at the other end thereof and to maintain a certain distance from the second electrode trunk 220S. The first electrode branch 210B may be connected to the first electrode trunk 210S electrically separated for each pixel PX so that each pixel PX receives a different electrical signal.
[0060] It is also possible to arrange one or more first electrode branches 210B per pixel PX. Figure 1, two first electrode branches 210B are arranged and the second electrode branch 220B is arranged between them, but the present disclosure is not limited thereto, and more first electrode branches 210B may be arranged. In this case, the first electrode branches 210B may be alternately arranged to be separated from the plurality of second electrode branches 220B, so that the plurality of light-emitting elements 300 are arranged between the first electrode branches 210B and the plurality of second electrode branches 220B. In some embodiments, the second electrode branches 220B may be arranged between the first electrode branches 210B so that each pixel PX is symmetrical about the second electrode branches 220B. However, the present disclosure is not limited thereto.
[0061] The second electrode 220 may include a second electrode trunk 220S and at least one second electrode branch 220B, wherein the second electrode trunk 220S is arranged to extend in a first direction D1, and faces the first electrode trunk 210S and keeps a certain distance from the first electrode trunk 210S, and the at least one second electrode branch 220B branches from the second electrode trunk 220S to extend in a second direction D2, and faces the first electrode branch 210B and keeps a certain distance from the first electrode branch 210B. Like the first electrode trunk 210S, the second electrode trunk 220S may also be connected to the signal input pad at one end thereof. However, the second electrode trunk 220S may extend toward a plurality of adjacent pixels PX at the other end thereof in the first direction D1. That is, the second electrode trunk 220S may be electrically continuous between each pixel PX. Therefore, the second electrode trunk 220S of a certain pixel is connected to one end of the second electrode trunk 220S of the adjacent pixel between the pixels PX at its opposite ends to apply the same electrical signal to each pixel PX.
[0062] The second electrode branch 220B may branch from at least a portion of the second electrode trunk 220S and extend and terminate in the second direction D2 to maintain a certain distance from the first electrode trunk 210S. That is, the second electrode branch 220B may be arranged to be connected to the second electrode trunk 220S at one end thereof, and to be placed inside the pixel PX at the other end thereof and to maintain a certain distance from the first electrode trunk 210S. The second electrode branch 220B may be connected to the second electrode trunk 220S electrically continuous with respect to each pixel PX to receive the same electrical signal for each pixel PX.
[0063] The second electrode branch 220B may be arranged to face the first electrode branch 210B and to keep a certain distance from the first electrode branch 210B. Here, the first electrode trunk 210S and the second electrode trunk 220S face each other and keep a certain distance with respect to the center of each pixel PX, so that the first electrode branch 210B and the second electrode branch 220B extend in opposite directions. That is, the first electrode branch 210B may extend to one direction of the second direction D2, and the second electrode branch 220B may extend to another direction of the second direction D2, so that one end of the first electrode branch 210B and one end of the second electrode branch 220B are arranged to face the opposite direction with respect to the center of the pixel PX. However, the present disclosure is not limited thereto, and the first electrode trunk 210S and the second electrode trunk 220S may be arranged to face the same direction with respect to the center of the pixel PX and keep a certain distance from each other. In this case, the first electrode branch 210B and the second electrode branch 220B branched from the corresponding electrode trunks 210S and 220S may extend in the same direction.
[0064] Despite Figure 1 It is shown in FIG. 2 that one second electrode branch 220B is arranged in each pixel PX, but the present disclosure is not limited thereto, and more second electrode branches 220B may be arranged.
[0065] A plurality of light emitting elements 300 may be aligned between the first electrode branch 210B and the second electrode branch 220B. In detail, at least a portion of the plurality of light emitting elements 300 are electrically connected to the first electrode branch 210B at one end thereof and to the second electrode branch 220B at the other end thereof.
[0066] A plurality of light emitting elements 300 may be aligned substantially parallel to each other and maintain a certain distance in the second direction D2. There is no specific limitation on the intervals between the light emitting elements 300. Some light emitting elements 300 may be arranged adjacent to form a group, while other light emitting elements 300 may be arranged to maintain a predetermined distance from each other to form a group, and they may also be aligned facing one direction with uneven density.
[0067] The first electrode branch 210B and the second electrode branch 220B may have corresponding contact electrodes 260 disposed thereon.
[0068] A plurality of contact electrodes 260 may be arranged to extend in the second direction D2 and to be spaced apart from each other in the first direction D1. The contact electrode 260 may contact at least one end of the light emitting element 300, and may contact the first electrode 210 and the second electrode 220 to receive an electrical signal. Therefore, the contact electrode 260 may transmit the electrical signal received through the first electrode 220 and the second electrode 220 to the light emitting element 300.
[0069] In detail, the contact electrode 260 may include a first contact electrode 261 and a second contact electrode 262 disposed on the respective electrode branches 210B and 220B to partially cover the electrode branches 210B and 220B and contact one end or the other end of the light emitting element 300 .
[0070] The first contact electrode 261 may be disposed on the first electrode branch 210B to contact one end of the light emitting element 300 electrically connected to the first electrode 210. The second contact electrode 262 may be disposed on the second electrode branch 220B to contact the other end of the light emitting element 300 electrically connected to the second electrode 220.
[0071] In some embodiments, the opposite end of each of the light emitting elements 300 electrically connected to the first electrode branch 210B or the second electrode branch 220B may be an n-type doped or p-type doped conductive semiconductor layer. In the case where one end of the light emitting element 300 electrically connected to the first electrode branch 210B is a p-type doped conductive semiconductor layer, the other end of the light emitting element 300 electrically connected to the second electrode branch 220B may be an n-type doped conductive semiconductor layer. However, the present disclosure is not limited thereto, and the opposite situation is also possible.
[0072] The first contact electrode 261 and the second contact electrode 262 may be arranged to partially cover the corresponding first electrode branch 210B and the second electrode branch 220B. Figure 1 As shown in , the first contact electrode 261 and the second contact electrode 262 may be arranged to extend in the second direction D2 and face each other and maintain a certain distance. However, the first contact electrode 261 and the second contact electrode 262 may terminate at one end thereof to expose one end of the corresponding electrode branches 210B and 220B. The first contact electrode 261 and the second contact electrode 262 may also terminate at the other end thereof so as not to overlap with the corresponding electrode trunks 210S and 220S in a state spaced apart from the corresponding electrode trunks 210S and 220S. However, the present disclosure is not limited thereto, and the first contact electrode 261 and the second contact electrode 262 may cover the corresponding electrode branches 210B and 220B.
[0073] At the same time, if Figure 1 As shown in , the first electrode stem 210S and the second electrode stem 220S may be electrically connected to the thin film transistor 120 or the power wiring 161 (to be described later) via corresponding contact holes (eg, the first electrode contact hole CNTD and the second electrode contact hole CNTS). Figure 1, in each pixel PX, the first electrode trunk 210S and the second electrode trunk 220S have contact holes arranged thereon, but the present disclosure is not limited thereto. Because the second electrode trunk 220S can be extended to establish an electrical connection with an adjacent pixel PX as described above, in some embodiments, the second electrode trunk 220S can be electrically connected to the thin film transistor via a contact hole.
[0074] In the following, reference is made to Figure 2 The configurations of the plurality of components arranged on the display device 10 are described in more detail.
[0075] Figure 2 It is along Figure 1 The cross-sectional views taken along the lines II-I', II-II' and III-III'. Figure 2 A single pixel PX is shown, but the configuration may be equally applicable to other pixels. Figure 2 A cross section across one end and the other end of a light emitting element 300 is shown.
[0076] Reference Figure 1 and Figure 2 , the display device 10 may include a substrate 110, thin film transistors 120 and 140 disposed on the substrate 110, electrodes 210 and 220 disposed on the thin film transistors 120 and 140, and a light emitting element 300. The thin film transistors may include a first thin film transistor 120 and a second thin film transistor 140, and they may be a driving transistor and a switching transistor, respectively. Each of the thin film transistors 120 and 140 may include an active layer, a gate electrode, a source electrode, and a drain electrode. The first electrode 210 may be electrically connected to the drain electrode of the first thin film transistor 120.
[0077] Specifically, substrate 110 may be an insulating substrate. Substrate 110 may be made of an insulating material such as glass, quartz or a polymer resin. Examples of polymer resins may include polyethersulfone (PES), polyacrylate (PA), polyarylate (PAR), polyetherimide (PEI), polyethylene naphthalate (PEN), polyethylene terephthalate (PET), polyphenylene sulfide (PPS), polyallylate, polyimide (PI), polycarbonate (PC), cellulose triacetate (CAT), cellulose acetate propionate (CAP) or a combination thereof. In addition, substrate 110 may be a rigid substrate, but may also be a flexible substrate that may be bent, folded or curled.
[0078] The buffer layer 115 may be disposed on the substrate 110. The buffer layer 115 may prevent diffusion of impurity ions, prevent penetration of moisture or external air, and perform a surface planarization function. The buffer layer 115 may include silicon nitride, silicon oxide, silicon oxynitride, or the like.
[0079] The semiconductor layer is disposed on the buffer layer 115. The semiconductor layer may include an auxiliary layer 163, a first active layer 126 of the first thin film transistor 120, and a second active layer 146 of the second thin film transistor 140. The semiconductor layer may include polycrystalline silicon, single crystal silicon, oxide semiconductor, and the like.
[0080] The first gate insulating layer 170 is disposed on the semiconductor layer. The first gate insulating layer 170 covers the semiconductor layer. The first gate insulating layer 170 may be used as a gate insulating film of a thin film transistor. The first gate insulating layer 170 may include silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide, tantalum oxide, hafnium oxide, zirconium oxide, or titanium oxide, etc. These may be used alone or in combination with each other.
[0081] The first conductive layer is disposed on the first gate insulating layer 170. The first conductive layer may include a first gate electrode 121 disposed on the first active layer 126 of the first thin film transistor 120, a second gate electrode 141 disposed on the second active layer 146 of the second thin film transistor 140, and a power wiring 161 disposed on the auxiliary layer 163, respectively, with the first gate insulating layer 170 interposed therebetween. The first conductive layer may include at least one metal selected from the group consisting of molybdenum (Mo), aluminum (Al), platinum (Pt), palladium (Pd), silver (Ag), magnesium (Mg), gold (Au), nickel (Ni), neodymium (Nd), iridium (Ir), chromium (Cr), calcium (Ca), titanium (Ti), tantalum (Ta), tungsten (W), and copper (Cu). The first conductive layer may be a single layer or a multilayer.
[0082] The second gate insulating layer 180 is disposed on the first conductive layer. The second gate insulating layer 180 may be an interlayer insulating layer. The second gate insulating layer 180 may be formed of an inorganic insulating material such as silicon oxide, silicon nitride, silicon oxynitride, hafnium oxide, aluminum oxide, titanium oxide, tantalum oxide, and zinc oxide.
[0083] The second conductive layer is disposed on the second gate insulating layer 180. The second conductive layer includes a capacitor electrode 128 disposed on the first gate electrode 121 with the second gate insulating layer 180 interposed therebetween. The capacitor electrode 128 may cooperate with the first gate electrode 121 to form a storage capacitor.
[0084] In the same manner as the first conductive layer described above, the second conductive layer may include at least one metal selected from the group consisting of molybdenum (Mo), aluminum (Al), platinum (Pt), palladium (Pd), silver (Ag), magnesium (Mg), gold (Au), nickel (Ni), neodymium (Nd), iridium (Ir), chromium (Cr), calcium (Ca), titanium (Ti), tantalum (Ta), tungsten (W) and copper (Cu).
[0085] The interlayer insulating layer 190 is disposed on the second conductive layer. The interlayer insulating layer 190 may be an interlayer insulating film. In addition, the interlayer insulating layer 190 may perform a surface planarization function. The interlayer insulating layer 190 may include an organic insulating material selected from the group consisting of acrylic resin, epoxy resin, phenolic resin, polyamide resin, polyimide resin, unsaturated polyester resin, polyphenylene resin, polyphenylene sulfide resin, and benzocyclobutene (BCB).
[0086] The third conductive layer is disposed on the interlayer insulating layer 190 , and includes the first drain electrode 123 and the first source electrode 124 of the first thin film transistor 120 , the second drain electrode 143 and the second source electrode 144 of the second thin film transistor 140 , and the power electrode 162 disposed on the power wiring 161 .
[0087] The first source electrode 124 and the first drain electrode 123 may be electrically connected to the first active layer 126 through a first contact hole 129 passing through the interlayer insulating layer 190, the second gate insulating layer 180, and the first gate insulating layer 170. The second source electrode 144 and the second drain electrode 143 may be electrically connected to the second active layer 146 through a second contact hole 149 passing through the interlayer insulating layer 190, the second gate insulating layer 180, and the first gate insulating layer 170. The power electrode 162 may be electrically connected to the power wiring 161 through a third contact hole 169 passing through the interlayer insulating layer 190 and the second gate insulating layer 180.
[0088] The third conductive layer may include at least one metal selected from the group consisting of aluminum (Al), molybdenum (Mo), platinum (Pt), palladium (Pd), silver (Ag), magnesium (Mg), gold (Au), nickel (Ni), neodymium (Nd), iridium (Ir), chromium (Cr), calcium (Ca), titanium (Ti), tantalum (Ta), tungsten (W) and copper (Cu). The third conductive layer may be a single layer or a multilayer. For example, the third conductive layer may have a stacked structure of Ti / Al / Ti, Mo / Al / Mo, Mo / AlGe / Mo or Ti / Cu.
[0089] The insulating base layer 200 is disposed on the third conductive layer. The insulating base layer 200 may be formed of an organic insulating material selected from the group consisting of acrylic resin, epoxy resin, phenolic resin, polyamide resin, polyimide resin, unsaturated polyester resin, polyphenylene resin, polyphenylene sulfide resin, and benzocyclobutene (BCB). The surface of the insulating base layer 200 may be flat.
[0090] The insulating base layer 200 may include a plurality of banks 410 and 420. Inside each pixel PX, the plurality of banks 410 and 420 may be arranged to face each other and maintain a distance therebetween, and the spaced-apart banks 410 and 420 (e.g., first banks 410 and second banks 420) may have first electrodes 210 and second electrodes 220 arranged thereon, respectively. Figure 1 As shown in FIG. 4 , three banks 410 and 420 (ie, two first banks 410 and one second bank 420) are arranged to be covered by the corresponding first electrode 210 and second electrode 220 within one pixel PX. Figure 2 Only the cross-section of one first bank 410 and one second bank 420 is shown, but the arrangement structure thereof can also be applied to Figure 2 Another first bank 410 not shown in FIG.
[0091] However, the present disclosure is not limited thereto, and more banks 410 and 420 may be arranged within one pixel PX. For example, it may be possible to arrange more banks 410 and 420 together with more first electrodes 210 and second electrodes 220. The banks 410 and 420 may include at least one first bank 410 on which the first electrode 210 is arranged and at least one second bank 420 on which the second electrode 220 is arranged. In this case, the first bank 410 and the second bank 420 may be arranged to face each other and maintain a certain distance between them, so that a plurality of banks are alternately arranged in one direction. In some embodiments, it may be possible to arrange two first banks 410 and maintain a certain distance between them, and to arrange one second bank 420 between the spaced first banks 410.
[0092] In addition, despite the Figure 2 Although not shown in the figure, the first electrode 210 and the second electrode 220 may include the corresponding electrode trunks 210S and 220S and the corresponding electrode branches 210B and 220B as described above. Figure 2 It can be understood that the first electrode branch 210B and the second electrode branch 220B are arranged on the first bank 410 and the second bank 420, respectively.
[0093] The plurality of banks 410 and 420 may be formed of substantially the same material in a single process. In this case, the banks 410 and 420 may form a grid pattern. The banks 410 and 420 may include polyimide.
[0094] Meanwhile, although not shown in the drawings, at least a portion of the plurality of banks 410 and 420 may be arranged on the boundaries of the pixels PX to distinguish them. Such banks may be arranged in a basic grid pattern together with the aforementioned first bank 410 and second bank 420. At least a portion of the banks 410 and 420 arranged on the boundaries of the pixels PX may be formed to cover the electrode lines of the display device 10.
[0095] Each of the plurality of embankments 410 and 420 may have a structure that at least partially protrudes from the insulating base layer 200. The embankments 410 and 420 may protrude upward from a flat plane on which the light-emitting element 300 is arranged, so that the protruding portion may at least partially have an inclined surface. The embankments 410 and 420 having a protruding structure with an inclined surface may have reflective layers 211 and 221 (described later) arranged thereon to reflect incident light. Light guided from the light-emitting element 300 to the reflective layers 211 and 221 may be reflected to the outside of the display device 10 (i.e., reflected upward from the embankments 410 and 420 to the outside of the display device 10). The embankments 410 and 420 having a protruding structure may not be limited in shape. Although in Figure 2 3 shows that the bank has a shape with a flat top surface and angular corners, but the present disclosure is not limited thereto, and the bank may protrude to have arc-shaped corners.
[0096] Reflective layers 211 and 221 may be disposed on the plurality of banks 410 and 420 .
[0097] The first reflective layer 211 covers the first bank 410 and is partially electrically connected to the first drain electrode 123 of the first thin film transistor 120 via the fourth contact hole 319_1 penetrating the insulating base layer 200. The second reflective layer 221 covers the second bank 420 and is partially electrically connected to the power electrode 162 via the fifth contact hole 319_2 penetrating the insulating base layer 200.
[0098] The first reflective layer 211 may be electrically connected to the first drain electrode 123 of the first thin film transistor 120 via the fourth contact hole 319_1 in the pixel PX. Therefore, the first thin film transistor 120 may be disposed in a region overlapping the pixel PX. Figure 1 An electrical connection to the first thin film transistor 120 via the first electrode contact hole CNTD disposed on the first electrode stem 210S is shown. That is, the first electrode contact hole CNTD may be the fourth contact hole 319_1.
[0099] The second reflective layer 221 may also be electrically connected to the power electrode 162 via a fifth contact hole 319_2 within the pixel PX. Figure 2 It is shown that the second reflective layer 221 is connected through the fifth contact hole 319_2 within one pixel PX. Figure 1It is shown that the second electrode 220 of each pixel PX is electrically connected to the power wiring 161 via a plurality of second electrode contact holes CNTS on the second electrode stem 220S. That is, the second electrode contact hole CNTS may be a fifth contact hole 319_2.
[0100] As reference Figure 1 As described above, the first electrode contact hole CNTD and the second electrode contact hole CNTS may be arranged on the first electrode stem 210S and the second electrode stem 220S, respectively. Figure 2 It is shown that in the cross-sectional view of the display device 10, the first electrode 210 and the second electrode 220 are electrically connected to the first thin film transistor 120 or the power wiring 161 via the corresponding fourth contact hole 319_1 and the fifth contact hole 319_2 in the area separated from the embankments 410 and 420 on which the first electrode branches 210B and the second electrode branches 220B are arranged.
[0101] However, the present disclosure is not limited thereto. Figure 1 In the embodiment, the second electrode contact hole CNTS may be arranged at different positions on the second electrode trunk 220S, and in some cases, may be arranged on the second electrode branch 220B. In some embodiments, the second reflective layer 221 may also be connected to a second electrode contact hole CNTS or a fifth contact hole 319_2 in an area outside a pixel PX.
[0102] In a region outside the emission region of the pixel PX of the display device 10 (e.g., an outer region of the emission region), there may be a non-emission region in which the light emitting element 300 is not arranged. As described above, the second electrode 220 of each pixel PX may be electrically connected via the second electrode stem 220S to receive the same electrical signal.
[0103] In some embodiments, in the case of the second electrode 220, the second electrode stem 220S may be electrically connected to the power electrode 162 via one second electrode contact hole CNTS in the non-emission region as the outer region of the pixel PX. Figure 1 Unlike the display device 10 of the present invention, even if the second electrode trunk 220S is connected to the power electrode 162 via one contact hole, since the second electrode trunk 220S is arranged to extend to adjacent pixels and be electrically connected to each other, it may be possible to apply the same electrical signal to the second electrode branches 220B of each pixel PX. In the case of the second electrode 220 of the display device 10, the position of the contact hole for receiving the electrical signal from the power electrode 162 may vary according to the structure of the display device 10. However, the present disclosure is not limited thereto.
[0104] At the same time, return to the reference Figure 1 and Figure 2In order to reflect the light emitted from the light emitting element 300, the reflective layers 211 and 221 may include a material having a high reflectivity. For example, the reflective layers 211 and 221 may include, but are not limited to, materials such as silver (Ag) and copper (Cu).
[0105] The first electrode layer 212 and the second electrode layer 222 may be disposed on the first reflective layer 211 and the second reflective layer 221 , respectively.
[0106] The first electrode layer 212 may be directly disposed on the first reflective layer 211. The first electrode layer 212 may have a pattern substantially the same as that of the first reflective layer 211. The second electrode layer 222 may be directly disposed on the second reflective layer 221 to be spaced apart from the first electrode layer 212. The second electrode layer 222 may have a pattern substantially the same as that of the second reflective layer 221.
[0107] In an embodiment, the electrode layers 212 and 222 may cover the reflective layers 211 and 221 thereunder, respectively. That is, the electrode layers 212 and 222 may be formed to be larger in size than the reflective layers 211 and 221 to cover the side end surfaces of the reflective layers 211 and 221. However, the present disclosure is not limited thereto.
[0108] The first electrode layer 212 and the second electrode layer 222 may transmit an electrical signal directed to the first reflective layer 211 and the second reflective layer 221 connected to the first thin film transistor 120 or the power electrode 162 to the contact electrodes 261 and 262 (described later). The electrode layers 212 and 222 may include a transparent conductive material. For example, the electrode layers 212 and 222 may include materials such as indium tin oxide (ITO), indium zinc oxide (IZO), and indium tin zinc oxide (ITZO), but are not limited thereto. In some embodiments, the reflective layers 211 and 221 and the electrode layers 212 and 222 may have a structure in which at least one transparent conductive layer (such as ITO, IZO, or ITZO) and at least one metal layer (such as silver (Ag) or copper (Cu)) are stacked. For example, the reflective layers 211 and 221 and the electrode layers 212 and 222 may have a stacked structure of ITO / Ag / ITO.
[0109] The first reflective layer 211 and the first electrode layer 212 disposed on the first bank 410 form the first electrode 210. The first electrode 210 may protrude to a region extending from both ends of the first bank 410, and thus the first electrode 210 may contact the insulating base layer 200 in the protruding region. The second reflective layer 221 and the second electrode layer 222 disposed on the second bank 420 form the second electrode 220. The second electrode 220 may protrude to a region extending from both ends of the second bank 420, and thus the second electrode 220 may contact the insulating base layer 200 in the protruding region.
[0110] The first electrode 210 and the second electrode 220 may be arranged to cover the entire area of the first bank 410 and the second bank 420, respectively. However, as described above, the first electrode 210 and the second electrode 220 are arranged to face each other and maintain a certain distance therebetween. Between the electrodes, a first insulating layer 510 to be described later may be arranged, and the light emitting element 300 may be arranged on the first insulating layer 510.
[0111] In addition, the first reflective layer 211 may receive a driving voltage from the first thin film transistor 120, and the second reflective layer 221 may receive a power supply voltage from the power wiring 161. Therefore, the first electrode 210 and the second electrode 220 receive a driving voltage and a power supply voltage, respectively. The first electrode 210 may be electrically connected to the first thin film transistor 120, and the second electrode 220 may be electrically connected to the power wiring 161. Therefore, the first contact electrode 261 and the second contact electrode 262, which are respectively arranged on the first electrode 210 and the second electrode 220, may receive a driving voltage and a power supply voltage. The driving voltage and the power supply voltage may be transmitted to the light emitting element 300, so that the light emitting element 300 emits light with a predetermined current flowing therethrough.
[0112] The first insulating layer 510 is arranged to partially cover the first electrode 210 and the second electrode 220. The first insulating layer 510 may be arranged to mainly cover the top surfaces of the first electrode 210 and the second electrode 220 and partially expose the first electrode 210 and the second electrode 220. The first insulating layer 510 may also be arranged in the space between the first electrode 210 and the second electrode 220. The first insulating layer 510 may have an island shape or a line shape formed along the space between the first electrode branch 210B and the second electrode branch 220B in a plan view.
[0113] Figure 2 It is shown that the first insulating layer 510 is arranged in the space between one first electrode 210 (e.g., first electrode branch 210B) and one second electrode 220 (e.g., second electrode branch 220B). However, as described above, there may be a plurality of first electrodes 210 and second electrodes 220, so that the first insulating layer 510 may also be arranged between one first electrode 210 and another second electrode 220 or between one second electrode 220 and another first electrode 210. The first insulating layer 510 may be arranged to partially cover the side surfaces of the first electrode 210 and the second electrode 220 opposite to the side surfaces facing each other. That is, the first insulating layer 510 may be arranged to expose the central portion of the first electrode 210 and the second electrode 220.
[0114] On the first insulating layer 510, the light emitting element 300 is arranged. The first insulating layer 510 may be arranged between the light emitting element 300 and the insulating base layer 200. The first insulating layer 510 may have a bottom surface contacting the insulating base layer 200, and the light emitting element 300 may be arranged on the top surface of the first insulating layer 510. The first insulating layer 510 may contact the electrodes 210 and 220 at both side surfaces thereof to electrically insulate the first electrode 210 and the second electrode 220 from each other.
[0115] The first insulating layer 510 may overlap a partial region on the electrodes 210 and 220 (e.g., a portion of a region protruding in a direction in which the first electrode 210 and the second electrode 220 face each other). The first insulating layer 510 may also be disposed on a region where the inclined surfaces and the flat top surfaces of the banks 410 and 420 overlap the electrodes 210 and 220.
[0116] For example, the first insulating layer 510 may cover the ends of the first electrode 210 and the second electrode 220 that protrude in the direction in which the first electrode 210 and the second electrode 220 face each other. The first insulating layer 510 may partially contact the insulating base layer 200 on its bottom surface, and may partially contact the electrodes 210 and 220 on its bottom surface and its side surface. Therefore, the first insulating layer 510 may protect and electrically insulate the regions overlapping the corresponding electrodes 210 and 220. In addition, the first insulating layer 510 may prevent the first conductive type semiconductor 310 and the second conductive type semiconductor 320 of the light emitting element 300 from directly contacting other components, thereby preventing damage to the light emitting element 300.
[0117] However, the present disclosure is not limited thereto, and in some embodiments, the first insulating layer 510 may be disposed only on a region overlapping the inclined side surfaces of the banks 410 and 420 among the regions on the first electrode 210 and the second electrode 220. In this case, the bottom surface of the first insulating layer 510 may terminate on the inclined side surfaces of the banks 410 and 420, and the electrodes 210 and 220 disposed on a portion of the inclined side surfaces of the banks 410 and 420 may be exposed to contact the contact electrode 260.
[0118] The first insulating layer 510 may also be arranged to expose both ends of the light emitting element 300. Therefore, the contact electrode 260 may contact the exposed top surfaces of the electrodes 210 and 220 and both ends of the light emitting element 300, and the contact electrode 260 may transmit an electrical signal applied to the first electrode 210 and the second electrode 220 to the light emitting element 300.
[0119] At least one light emitting element 300 may be disposed between the first electrode 210 and the second electrode 220. Figure 2FIG. 1 shows that one light emitting element 300 is arranged between the first electrode 210 and the second electrode 220, but it is obvious that a plurality of light emitting elements 300 may be arranged between the first electrode 210 and the second electrode 220. Figure 1 In the plan view shown in , the two electrodes are arranged in different directions (eg, the second direction D2 ).
[0120] In detail, the light emitting element 300 may be electrically connected to the first electrode 210 at one end thereof and to the second electrode 220 at the other end thereof. Both ends of the light emitting element 300 may contact the first contact electrode 261 and the second contact electrode 262, respectively.
[0121] at the same time, Figure 1 The case where only the light emitting elements 300 emitting the same color light are arranged in each pixel PX is illustrated. However, the present disclosure is not limited thereto, and as described above, the light emitting elements 300 emitting different colors of light may be disposed together in one pixel PX.
[0122] The light emitting element 300 may be a light emitting diode. The light emitting element 300 may be a nanostructure having mainly nanometer size. The light emitting element 300 may be an inorganic light emitting diode made of an inorganic material. When the light emitting element 300 is an inorganic light emitting diode, a light emitting material having an inorganic crystal structure is disposed between two electrodes facing each other, and an electric field is formed in a specific direction between the two electrodes. Then, the inorganic light emitting diode may be aligned between two electrodes having a specific polarity.
[0123] In some embodiments, the light emitting element 300 may have a structure including: Figure 5 3. The stacked structure of the first conductive semiconductor 310, the element active layer 330, the second conductive semiconductor 320 and the electrode material layer 370 shown in FIG. The light emitting element 300 can be manufactured by horizontally depositing the first conductive semiconductor 310, the element active layer 330, the second conductive semiconductor 320 and the electrode material layer 370 on the insulating base layer 200 in sequence. That is, the light emitting element 300 formed by depositing a plurality of layers can be arranged in a width direction parallel to the insulating base layer 200. However, the present disclosure is not limited thereto, and the light emitting element 300 can be manufactured so that the layers are deposited between the first electrode 210 and the second electrode 220 in reverse order.
[0124] The second insulating layer 520 may be disposed to overlap at least a portion of the light emitting element 300. The second insulating layer 520 may protect the light emitting element 300 and fix the light emitting element 300 between the first electrode 210 and the second electrode 220 at the same time.
[0125] Despite Figure 22 shows that the second insulating layer 520 is arranged only on the top surface of the light emitting element 300 in the cross-sectional view, but the second insulating layer 520 may be arranged to surround the outer surface of the light emitting element 300. That is, like the first insulating layer 510, the second insulating layer 520 may be arranged to have an island shape or a line shape extending in the second direction D2 along the space between the first electrode branch 210B and the second electrode branch 220B in a plan view.
[0126] A portion of the material of the second insulating layer 520 may also be arranged at a region where the bottom surface of the light emitting element 300 and the first insulating layer 510 overlap each other. The portion may be formed during the manufacture of the display device 10 when the light emitting element 300 is aligned on the first insulating layer 510 and then the second insulating layer 520 is disposed on the light emitting element 300. The portion may also be formed by partially penetrating the second insulating layer 520 into a hole formed in a portion of the first insulating layer 510 that contacts the bottom surface of the light emitting element 300 during the formation of the second insulating layer 520.
[0127] The second insulating layer 520 may be arranged to expose the two end surfaces of the light emitting element 300. That is, in the cross-sectional view, the second insulating layer 520 arranged on the top surface of the light emitting element 300 is shorter than the light emitting element 300 in the axial direction, so that the second insulating layer 520 can be retracted inwardly compared with the two ends of the light emitting element 300. Therefore, the first insulating layer 510, the light emitting element 300 and the second insulating layer 520 may be deposited so that the side surfaces thereof are arranged in a stepped manner. This may facilitate the contact between the contact electrodes 261 and 262 and the two end surfaces of the light emitting element 300. However, the present disclosure is not limited thereto. The second insulating layer 520 and the light emitting element 300 may have the same length, and their two sides may be aligned.
[0128] At the same time, the second insulating layer 520 can be formed in such a manner that the corresponding material is deposited on the first insulating layer 510 and the corresponding material in the region (for example, the region exposed in order to make the light emitting element 300 contact the contact electrode 260) is patterned. Patterning the second insulating layer 520 can be performed using a conventional dry etching or wet etching process. Here, the first insulating layer 510 and the second insulating layer 520 may include materials with different etching selectivities to prevent the first insulating layer 510 from being patterned. That is, the first insulating layer 510 can be used as an etching stop layer when patterning the second insulating layer 520.
[0129] Therefore, even when the second insulating layer 520 covering the outer surface of the light emitting element 300 is patterned to expose both ends of the light emitting element 300, the first insulating layer 510 may not be subjected to material damage. Specifically, the first insulating layer 510 and the light emitting element 300 may have smooth contact surfaces at both ends of the light emitting element 300, wherein the light emitting element 300 and the contact electrode 260 contact each other at both ends of the light emitting element 300.
[0130] On the second insulating layer 520 , a first contact electrode 261 disposed on the first electrode 210 and overlapping at least a portion of the second insulating layer 520 and a second contact electrode 262 disposed on the second electrode 220 and overlapping at least a portion of the second insulating layer 520 may be disposed.
[0131] The first contact electrode 261 and the second contact electrode 262 may be arranged on the top surfaces of the first electrode 210 and the second electrode 220, respectively. In detail, the first contact electrode 261 and the second contact electrode 262 may contact the first electrode layer 212 and the second electrode layer 222, respectively, in the region where the first insulating layer 510 is patterned to expose the first electrode 210 and the second electrode 220. The first contact electrode 261 and the second contact electrode 262 may contact one end side of the light emitting element 300 (for example, the first conductive type semiconductor 310, the second conductive type semiconductor 320, or the electrode material layer 370). Therefore, the first contact electrode 261 and the second contact electrode 262 may transmit the electrical signal applied to the first electrode layer 212 and the second electrode layer 222 to the light emitting element 300.
[0132] The first contact electrode 261 may be disposed on the first electrode 210 to partially cover the first electrode 210, and partially contact the light emitting element 300 and the first insulating layer 510 and the second insulating layer 520 on the bottom surface of the first contact electrode 261. One end of the first contact electrode 261 facing the second contact electrode 262 is disposed on the second insulating layer 520. The second contact electrode 262 may be disposed on the second electrode 220 to partially cover the second electrode 220, and partially contact the light emitting element 300 and the first insulating layer 510, the second insulating layer 520, and the third insulating layer 530 on the bottom surface of the second contact electrode 262. One end of the second contact electrode 262 facing the first contact electrode 261 is disposed on the third insulating layer 530.
[0133] The first and second insulating layers 510 and 520 may be patterned to expose regions of the first and second electrodes 210 and 220 on top surfaces of the first and second banks 410 and 420. Thus, the first and second electrode layers 212 and 222 of the respective first and second electrodes 210 and 220 may be exposed to be electrically connected to the respective contact electrodes 261 and 262.
[0134] The first contact electrode 261 and the second contact electrode 262 may be spaced apart from each other on the second insulating layer 520 or the third insulating layer 530. That is, the first contact electrode 261 and the second contact electrode 262 may be arranged to contact the light emitting element 300 and the second insulating layer 520 and the light emitting element 300 and the third insulating layer 530, respectively, so as to be spaced apart in the deposition direction on the second insulating layer 520 for electrical insulation. Therefore, the first contact electrode 261 and the second contact electrode 262 may receive different powers from the first thin film transistor 120 and the power wiring 161, respectively. For example, the first contact electrode 261 may receive a driving voltage applied from the first thin film transistor 120 to the first electrode 210, and the second contact electrode 262 may receive a common power supply voltage applied from the power wiring 161 to the second electrode 220. However, the present disclosure is not limited thereto.
[0135] At the same time, if Figure 1 As shown in FIG. 1 , the first contact electrode 261 and the second contact electrode 262 are not arranged on the first electrode contact hole CNTD and the second electrode contact hole CNTS formed on the first electrode trunk 210S and the second electrode trunk 220S. That is, even if Figure 5 In the embodiment, the first contact electrode 261 and the second contact electrode 262 may not overlap with the region where the first electrode contact hole CNTD and the second electrode contact hole CNTS are arranged, respectively. However, the present disclosure is not limited thereto, and in some cases, the first contact electrode 261 and the second contact electrode 262 may partially overlap with the region where the first electrode contact hole CNTD or the second electrode contact hole CNTS is arranged on the corresponding first electrode 210 and the second electrode 220.
[0136] The contact electrodes 261 and 262 may include a conductive material. For example, they may include ITO, IZO, ITZO, or aluminum (Al), etc. However, the present disclosure is not limited thereto.
[0137] In addition, the contact electrodes 261 and 262 may include the same material as the electrode layers 212 and 222. The contact electrodes 261 and 262 may be arranged to have substantially the same pattern on the electrode layers 212 and 222 to contact the electrode layers 212 and 222. For example, the first contact electrode 261 contacting the first electrode 210 and the second contact electrode 262 contacting the second electrode 220 may transmit an electrical signal applied to the first electrode layer 212 and the second electrode layer 222 to the light emitting element 300.
[0138] The third insulating layer 530 may be disposed on the first contact electrode 261 to electrically insulate the first contact electrode 261 and the second contact electrode 262 from each other. The third insulating layer 530 may be disposed to cover the first contact electrode 261 without overlapping the region of the light emitting element 300 in contact with the second contact electrode 262, so that the light emitting element 300 contacts the second contact electrode 262. The third insulating layer 530 may partially contact the first contact electrode 261, the second contact electrode 262, and the second insulating layer 520 on the top surface of the second insulating layer 520. The third insulating layer 530 may be disposed to cover one end of the first contact electrode 261 on the top surface of the second insulating layer 520. Therefore, the third insulating layer 530 may protect the first contact electrode 261 and electrically insulate the first contact electrode 261 from the second contact electrode 262.
[0139] One end of the third insulating layer 530 facing the second electrode 220 may be aligned with one side surface of the second insulating layer 520 .
[0140] Meanwhile, in some embodiments, the third insulating layer 530 may be omitted in the display device 10. Therefore, the first contact electrode 261 and the second contact electrode 262 may be disposed substantially on the same plane and may be electrically insulated from each other by a passivation layer 550 to be described later.
[0141] The passivation layer 550 may be formed on the third insulating layer 530 and the second contact electrode 262 to protect the components disposed on the insulating base layer 200 from the external environment. When the first contact electrode 261 and the second contact electrode 262 are exposed, the problem of disconnection of the contact electrode material may occur due to electrode damage, so it is necessary to cover them with the passivation layer 550. That is, the passivation layer 550 may be provided to cover the first electrode 210, the second electrode 220, the light emitting element 300, etc. In addition, as described above, when the third insulating layer 530 is omitted, the passivation layer 550 may be formed on the first contact electrode 261 and the second contact electrode 262. In this case, the passivation layer 550 may electrically insulate the first contact electrode 261 and the second contact electrode 262 from each other.
[0142] Each of the first insulating layer 510, the second insulating layer 520, the third insulating layer 530, and the passivation layer 550 described above may include an inorganic insulating material. For example, the first insulating layer 510, the second insulating layer 520, the third insulating layer 530, and the passivation layer 550 may include an inorganic insulating material such as silicon oxide (SiO x ), Silicon Nitride (SiN x ), silicon oxynitride (SiO x N y ), aluminum oxide (Al 2 O 3) and aluminum nitride (AlN) and the like. The first insulating layer 510, the second insulating layer 520, the third insulating layer 530 and the passivation layer 550 may be made of the same material, but may also be made of different materials. In addition, various materials that impart insulating properties to the first insulating layer 510, the second insulating layer 520, the third insulating layer 530 and the passivation layer 550 are applicable.
[0143] Meanwhile, as described above, the etching selectivity of the first insulating layer 510 and the second insulating layer 520 may be different. As an example, when the first insulating layer 510 includes silicon oxide (SiO x ), the second insulating layer 520 may include silicon nitride (SiN x As another example, when the first insulating layer 510 includes silicon nitride (SiN x ), the second insulating layer 520 may include silicon oxide (SiO x ). However, the present disclosure is not limited thereto.
[0144] Meanwhile, the light emitting element 300 may be manufactured on the base substrate by epitaxial growth. A seed layer for forming a semiconductor layer may be formed on the base substrate, and a desired semiconductor material may be deposited to grow. Figure 3a and Figure 3b The structure of the light emitting element 300 according to various embodiments is described in detail.
[0145] Figure 3a is a schematic diagram of a light emitting element according to an embodiment. Figure 3b It is along Figure 3a A cross-sectional view taken along line 3b-3b'.
[0146] Reference Figure 3a and Figure 3b , the light emitting element 300 may include a plurality of conductive semiconductors 310 and 320, an electrode material layer 370, an insulating material layer 380, and an element active layer 330 disposed between the plurality of conductive semiconductors 310 and 320. The electrical signal received through the first electrode 210 and the second electrode 220 may be transmitted to the element active layer 330 via the plurality of conductive semiconductors 310 and 320 to emit light.
[0147] In detail, the light emitting element 300 may include a first conductive semiconductor 310, a second conductive semiconductor 320, an insulating material layer 380, an element active layer 330 disposed between the first conductive semiconductor 310 and the second conductive semiconductor 320, and an electrode material layer 370 disposed on the second conductive semiconductor 320. Figure 3a3 shows that the light emitting element 300 has a layered structure in which a first conductive semiconductor 310, an element active layer 330, a second conductive semiconductor 320, and an electrode material layer 370 are sequentially deposited in the length direction thereof, but the present disclosure is not limited thereto. The electrode material layer 370 may be omitted, and in some embodiments, the electrode material layer 370 may be arranged on at least one of the two side surfaces of each of the first conductive semiconductor 310 and the second conductive semiconductor 320. Figure 3a An exemplary light emitting element 300 is described, and it is apparent that the following description of the light emitting element 300 is also applicable to light emitting elements 300 including different structures.
[0148] The first conductive semiconductor 310 may be an n-type semiconductor layer. As an example, when the light emitting element 300 emits light in the blue wavelength band, the first conductive semiconductor 310 may include a semiconductor layer having a chemical formula of In x Al y Ga 1-x-y The first conductive semiconductor 310 may be a semiconductor material of N (0≤x≤1, 0≤y≤1, 0≤x+y≤1). For example, it may be any one or more of n-type doped InAlGaN, GaN, AlGaN, InGaN, AlN, and InN. The first conductive semiconductor 310 may be doped with a first conductive dopant. For example, the first conductive dopant may be Si, Ge, Se, or Sn, etc. The length of the first conductive semiconductor 310 may be in the range of 1.5 μm to 5 μm, but is not limited thereto.
[0149] The second conductive semiconductor 320 may be a p-type semiconductor layer. As an example, when the light emitting element 300 emits light in the blue wavelength band, the second conductive semiconductor 320 may include a semiconductor layer having a chemical formula In x Al y Ga 1-x-y The second conductive semiconductor 320 may be a semiconductor material of N (0≤x≤1, 0≤y≤1, 0≤x+y≤1). For example, it may be any one or more of p-doped InAlGaN, GaN, AlGaN, InGaN, AlN, and InN. The second conductive semiconductor 320 may be doped with a second conductive dopant. For example, the second conductive dopant may be Mg, Zn, Ca, or Ba, etc. The length of the second conductive semiconductor 320 may be in the range of 0.08 μm to 0.25 μm, but is not limited thereto.
[0150] The element active layer 330 is disposed between the first conductive semiconductor 310 and the second conductive semiconductor 320, and may include a material having a single quantum well structure or a multi-quantum well structure. When the element active layer 330 includes a material having a multi-quantum well structure, a plurality of quantum layers and well layers may be alternately stacked. The element active layer 330 may emit light by the combination of electron-hole pairs according to an electrical signal applied by the first conductive semiconductor 310 and the second conductive semiconductor 320. For example, when the element active layer 330 emits light in the blue band, it may include a material such as AlGaN or AlInGaN. Specifically, when the element active layer 330 has a multi-quantum well structure in which quantum layers and well layers may be alternately stacked, the quantum layers may include materials such as AlGaN or AlInGaN, and the well layers may include materials such as GaN or AlGaN. However, the present disclosure is not limited thereto, and the element active layer 330 may have a structure in which a semiconductor material having a large band gap energy and a semiconductor material having a small band gap energy are alternately stacked, and may include other III-group to V-group semiconductor materials according to the wavelength band of the emitted light. The light emitted by the element active layer 330 is not limited to the light of the blue wavelength band, but may also emit light of the red or green wavelength band in some cases. The length of the element active layer 330 may be in the range of 0.05 μm to 0.25 μm, but is not limited thereto.
[0151] Light emitted from the element active layer 330 may be projected in the longitudinal direction through both side surfaces and the outer surface of the light emitting element 300. Directivity of light emitted from the element active layer 330 is not limited to one direction.
[0152] The electrode material layer 370 may be an ohmic contact electrode. However, the present disclosure is not limited thereto, and the electrode material layer 370 may be a Schottky contact electrode. The electrode material layer 370 may include a conductive metal. For example, the electrode material layer 370 may include at least one of aluminum (Al), titanium (Ti), indium (In), gold (Au), and silver (Ag). The electrode material layer 370 may include the same material or different materials. However, the present disclosure is not limited thereto.
[0153] The insulating material layer 380 may be formed outside the light emitting element 300 to protect the light emitting element 300. For example, the insulating material layer 380 may be formed to surround the side surface of the light emitting element 300, and may not be formed at both ends of the light emitting element 300 in the longitudinal direction (for example, not formed at both ends where the first conductive semiconductor 310 and the second conductive semiconductor 320 are provided). However, the present disclosure is not limited thereto. The insulating material layer 380 may include a material having insulating properties, for example, silicon oxide (SiO x ), Silicon Nitride (SiN x ), silicon oxynitride (SiOx N y ), aluminum nitride (AlN) and aluminum oxide (Al 2 O 3 ) etc. Therefore, it is possible to prevent an electrical short circuit that may occur when the element active layer 330 directly contacts the first electrode 210 or the second electrode 220. In addition, the insulating material layer 380 protects the outer surface of the light emitting element 300 including the element active layer 330, which can prevent the deterioration of the light emitting efficiency.
[0154] The insulating material layer 380 may be formed to extend in the length direction to cover the outer surfaces of the first conductive type semiconductor 310 to the electrode material layer 370. However, the present disclosure is not limited thereto, and the insulating material layer 380 may only cover the outer surfaces of the first conductive type semiconductor 310, the element active layer 330, and the second conductive type semiconductor 320, or only cover a portion of the outer surface of the electrode material layer 370 and expose a portion of the outer surface of the electrode material layer 370.
[0155] In some embodiments, the insulating material layer 380 may be surface-treated to be dispersed in the solution rather than adhered to other insulating material layers 380. In this case, as will be described later, the light emitting elements 300 may be maintained in a dispersed state in the solution to be independently aligned between the first electrode 210 and the second electrode 220 during alignment of the light emitting elements 300. For example, the insulating material layer 380 may be surface-treated in a hydrophobic or hydrophilic manner so that the light emitting elements 300 are maintained in a mutually dispersed state in the solution.
[0156] The thickness of the insulating material layer 380 may be in the range of 0.5 μm to 1.5 μm, but is not limited thereto.
[0157] The light emitting element 300 may have a cylindrical shape. Figure 3b As shown in , the cross section taken by bisecting the light emitting element 300 in the length direction intersecting the two ends of the light emitting element 300 may have a rectangular shape. However, the shape of the light emitting element 300 is not limited thereto, and may have various shapes such as a regular cube, a cuboid, and a hexagonal prism. The light emitting element 300 may have a length l of 1 μm to 10 μm or 2 μm to 5 μm, and preferably a length l of about 4 μm. In addition, the diameter of the light emitting element 300 may be in the range of 400 nm to 700 nm, and preferably may be about 500 nm.
[0158] Although for ease of explanation Figure 3a The following description is made with respect to the exemplary light emitting element 300 shown in FIG. 3 , but the present disclosure may be equally applicable to light emitting elements including more electrode material layers 370 or other structures.
[0159] at the same time, Figure 4 yes Figure 3b An enlarged view of a portion of Figure 5 yes Figure 2 An enlarged view of part A of FIG.
[0160] Reference Figure 4 , the light emitting element 300 according to the embodiment may have a flat and relatively less rough separation surface 390. As described later, the light emitting element 300 may include a first conductive type semiconductor 310 whose end surface becomes the separation surface 390 in the manufacture of the light emitting element 300. The first conductive type semiconductor 310 of the light emitting element 300 may be formed to have a flat surface, which prevents an open circuit problem from occurring when contacting the first contact electrode 261.
[0161] Reference Figure 5 The shape of the separation surface 390 at one end of the light emitting element 300 may determine a plane where the separation surface 390 at one end of the light emitting element 300 and the surface of the first contact electrode 261 contact each other ( Figure 5 For example, if the separation surface 390 of the light emitting element 300 is rough or protrudes or is recessed to form an inclined surface, this may reduce the film step coverage of the contact electrode material when contacting the first contact electrode 261, which leads to a partial interruption of the electrode material. That is, in the contact area ( Figure 5 A faulty contact between the light emitting element 300 and the first contact electrode 261 at 5a-5a') may prevent an electrical signal from reaching the light emitting element 300, thereby causing a light emitting error.
[0162] Meanwhile, if the separation surface 390 of the light emitting element 300 is Figure 5 is flat, this makes it possible to prevent the light emitting element 300 and the contact electrode 260 from contacting each other in the region ( Figure 5 5a-5a') of the contact electrode material. This can improve the reliability of the light-emitting element 300 of the display device 10. According to an embodiment, the separation surface 390 of the light-emitting element 300 can have a roughness value of 8nm Ra to 12nm Ra. However, the present disclosure is not limited to this. At the same time, although not shown in the drawings, the above method can also be applied to the second conductive semiconductor 320 contacting the second contact electrode 262, or can also be applied to the side surface formed by the electrode material layer 370.
[0163] The flatness of the separation surface 390 of the light emitting element 300 can be improved by peeling off the separation layer 1300 ( Figure 7The light emitting element 300 can be separated from the lower substrate layer on which the light emitting element 300 is grown in such a manner as shown in FIG. That is, the light emitting element 300 can be separated from the lower substrate layer by peeling off the separation layer 1300 on which the light emitting element 300 is grown without any external physical force that interrupts the material grown on the separation surface 390 at one end of the light emitting element 300.
[0164] In this way, the light emitting element 300 according to the embodiment can be manufactured to have both ends having flat separation surfaces 390 contacting the first contact electrode 261 and the second contact electrode 262, which makes it possible to prevent a short circuit problem from occurring due to the materials of the contact electrodes 261 and 262. Figures 6 to 18 A method for manufacturing the light emitting element 300 is described in detail.
[0165] Figures 6 to 18 is a schematic cross-sectional view schematically illustrating a method for manufacturing a light emitting element according to an embodiment.
[0166] First, refer to Figure 6 , a lower substrate layer (or referred to as a lower substrate) 1000 including a base substrate 1100 and a buffer material layer 1200 formed on the base substrate 1100 is prepared. Figure 6 As shown in , the lower substrate layer 1000 may have a layered structure formed by sequentially depositing a base substrate 1100 and a buffer material layer 1200 .
[0167] The base substrate 1100 may include a sapphire (Al 2 O 3 ) substrate and a transparent substrate of a glass substrate. However, the present disclosure is not limited thereto, and it may be formed of a conductive substrate such as GaN, SiC, ZnO, Si, GaP, and GaAs. The following description is directed to a case where the base substrate 1100 is a sapphire (Al 2 O 3 Although not limited thereto, the base substrate 1100 may have a thickness in the range of, for example, 400 μm to 1500 μm.
[0168] On the base substrate 1100, a plurality of conductive semiconductor layers are formed. The plurality of conductive semiconductor layers grown by the epitaxial growth method can be grown by forming a seed crystal and depositing a crystalline material thereon. Here, one of electron beam deposition, physical vapor deposition (PVD), chemical vapor deposition (CVD), plasma laser deposition (PLD), dual-type thermal evaporation, sputtering, and metal organic chemical vapor deposition (MOCVD) (preferably using metal organic chemical vapor deposition (MOCVD)) can be used to form the conductive semiconductor layer. However, the present disclosure is not limited thereto.
[0169] Generally, a precursor material for forming a plurality of conductive semiconductor layers can be selected within a generally selectable range to form a target material without any limitation. For example, the precursor material can be a metal precursor including an alkyl group (e.g., a methyl group or an ethyl group). Examples of the precursor material can include, but are not limited to, trimethylgallium Ga (CH 3 ) 3 、Trimethylaluminum Al(CH 3 ) 3 and triethyl phosphate (C 2 H 5 ) 3 PO4. Hereinafter, description of the method and process conditions for forming a plurality of conductive type semiconductor layers is omitted, and the process sequence of the method for manufacturing the light emitting element 300 and the layered structure of the light emitting element 300 are described in detail.
[0170] The buffer material layer 1200 is formed on the base substrate 1100. Although it is shown in the drawings that one buffer material layer 1200 is deposited, the present disclosure is not limited thereto, and a plurality of layers may be formed.
[0171] In a step to be described later, a separation layer 1300 may be provided on the buffer material layer 1200, and then crystals for the first conductive type semiconductor layer 3100 may be grown on the separation layer 1300. The buffer material layer 1200 may be interposed between the base substrate 1100 and the separation layer 1300 to reduce a lattice constant difference of the first conductive type semiconductor layer 3100. Although the first conductive type semiconductor layer 3100 may be directly formed on the separation layer 1300 provided on the base substrate 1100, the buffer material layer 1200 may provide a seed crystal to promote crystal growth of the first conductive type semiconductor layer 3100.
[0172] For example, the buffer material layer 1200 may include an undoped semiconductor and may include a material that is substantially the same as the material of the first conductive type semiconductor layer 3100 and is neither n-type doped nor p-type doped. In an exemplary embodiment, the buffer material layer 1200 may be at least one of undoped InAlGaN, GaN, AlGaN, InGaN, AlN, and InN, but is not limited thereto.
[0173] Meanwhile, in some embodiments, a plurality of layers may be formed on the buffer material layer 1200, and the separation layer 1300 may be deposited on the buffer material layer 1200. The buffer material layer 1200 may also be omitted according to the base substrate 1100. A detailed description thereof will be given with reference to other embodiments. Hereinafter, an exemplary case in which the buffer material layer 1200 including an undoped semiconductor material is formed on the base substrate 1100 is described.
[0174] Next, refer to Figure 7 , a separation layer 1300 is formed on the lower substrate layer 1000 .
[0175] The separation layer 1300 may have the first conductive type semiconductor layer 3100 formed thereon. That is, the separation layer 1300 may be disposed between the first conductive type semiconductor layer 3100 and the buffer material layer 1200, and the separation layer 1300 may include a material that promotes crystal growth of the first conductive type semiconductor layer 3100. In a step to be described later, the separation layer 1300 may be peeled off from the lower substrate layer 1000 to separate the light emitting element 300 manufactured thereon.
[0176] In an exemplary embodiment, the separation layer 1300 may include a graphene layer. Due to the nature of the surface characteristics of graphene, graphene can promote the crystal growth of the conductive semiconductor layer. Specifically, in the case of pure graphene that hardly includes graphene oxide (GO) as an impurity, the conductive semiconductor can be grown in the epitaxial process for manufacturing the light emitting element 300.
[0177] The graphene layer may have a two-dimensional planar monolayer structure of carbon atoms, which forms a relatively weak mutual attraction between the layers. That is, the graphene layer may be provided at the interface between two different material layers to facilitate peeling of one material layer from another material layer. That is, a separation layer 1300 including a graphene layer may be provided at the interface between the buffer material layer 1200 and the first conductive type semiconductor layer 3100 to facilitate separation of the manufactured light emitting element 300.
[0178] For example, the separation layer 1300 may have a structure formed of a single pure graphene layer or two stacked graphene layers. Figure 7 1300 includes a single graphene layer, but in some cases the separation layer 1300 may have a structure of two stacked graphene layers. Therefore, in the separation process of the light-emitting element 300 to be described later, the separation layer 1300 and the first conductive semiconductor layer 3100 may be separated between them or at the interface between the multiple graphene layers constituting the separation layer 1300. In an exemplary embodiment, the separation layer 1300 may have a thickness in the range of 0.3nm to 1.0nm. A single graphene layer may have a thickness of about 0.35nm. Therefore, the separation layer 1300 composed of one or two graphene layers may have a thickness in the aforementioned range. It will be described in more detail later, and an exemplary case in which the separation layer 1300 includes a single graphene layer is described below.
[0179] During the process of etching the element deposition structure 3000, the separation layer 1300 may also be used as an etching stop layer between the element deposition structure 3000 and the buffer material layer 1200. That is, when etching the element deposition structure 3000, the separation layer 1300 may be patterned simultaneously in one process, or patterned separately in different processes. There is no limitation on the method of manufacturing the light emitting element 300.
[0180] However, the present disclosure is not limited thereto, and more separation layers 1300 may be arranged in the element deposition structure 3000 or the lower substrate layer 1000 in addition to the interface between the buffer material layer 1200 and the first conductive type semiconductor layer 3100, and more separation layers 1300 may be arranged in other regions. A detailed description thereof will be given with reference to other embodiments.
[0181] Next, refer to Figure 8 , the element deposition structure 3000 is formed by sequentially depositing a first conductive type semiconductor layer 3100 , an active material layer 3300 , a second conductive type semiconductor layer 3200 , and a conductive electrode material layer 3700 on the separation layer 1300 .
[0182] In a step to be described later, the element deposition structure 3000 may be partially etched to form the light emitting element 300. The plurality of material layers included in the element deposition structure 3000 may be formed by conventional processes as described above. On the separation layer 1300, a first conductive type semiconductor layer 3100, an active material layer 3300, a second conductive type semiconductor layer 3200, and a conductive electrode material layer 3700 may be sequentially deposited, and they may include the same materials as the first conductive type semiconductor 310, the element active layer 330, the second conductive type semiconductor 320, and the electrode material layer 370 of the light emitting element 300, respectively.
[0183] Meanwhile, the light emitting element 300 may be manufactured in the case where the electrode material layer 370 is omitted or in the case where a different electrode material layer 370 formed on the bottom surface of the first conductive type semiconductor 310 is further included. Fig.11 As shown in FIG. 3 , the conductive electrode material layer 3700 formed on the second conductive type semiconductor layer 3200 may be omitted. The following describes an exemplary case in which the element deposition structure 3000 includes the conductive electrode material layer 3700 .
[0184] Next, refer to Figures 9 to 12 The light emitting element 300 may be manufactured in such a manner that the element deposition structure 3000 is etched in a vertical direction to form an element rod ROD, and then an insulating layer 3800 is formed to partially cover the outer surface of the element rod ROD.
[0185] First, refer to Fig. 9 and Fig.10 , forming the element rod ROD by vertically etching the element deposition structure 3000 may include a patterning process that may be conventionally performed. For example, forming the element rod ROD by etching the element deposition structure 3000 may include: forming an etching mask layer 1600 and an etching pattern layer 1700 on the element deposition structure 3000; and etching the element deposition structure 3000 according to the pattern of the etching pattern layer 1700, and then removing the etching mask layer 1600 and the etching pattern layer 1700.
[0186] The etching mask layer 1600 may be used as a mask for sequentially etching the first conductive type semiconductor layer 3100, the active material layer 3300, the second conductive type semiconductor layer 3200, and the conductive electrode material layer 3700 of the element deposition structure 3000. The etching mask layer 1600 may include a first etching mask layer 1610 including an insulating material and a second etching mask layer 1620 including a metal.
[0187] The insulating material included in the first etching mask layer 1610 of the etching mask layer 1600 may be an oxide or a nitride. Examples of the insulating material may include silicon oxide (SiO x ), Silicon Nitride (SiN x ) and silicon oxynitride (SiO x N y ). The first etch mask layer 1610 may have a thickness in the range of 0.5 μm to 1.5 μm, but is not limited thereto.
[0188] The material of the second etching mask layer 1620 may not be limited as long as it can be used as a mask for continuously etching the element deposition structure 3000. For example, the second etching mask layer 1620 may include chromium (Cr). The second etching mask layer 1620 may have a thickness in the range of 30nm to 150nm, but is not limited thereto.
[0189] The etching pattern layer 1700 formed on the etching mask layer 1600 may include at least one nano-pattern separated from each other on the etching mask layer 1600. The etching pattern layer 1700 may be used as a mask for continuously etching the element deposition structure 3000. There is no limitation on the etching method as long as it can form a pattern including a polymer, polyethylene balls, or silicon dioxide balls on the etching pattern layer 1700.
[0190] For example, when the etching pattern layer 1700 includes a polymer, a conventional method may be used to form a pattern using the polymer. For example, the etching pattern layer 1700 including the polymer may be formed using a method such as photolithography, electron beam lithography, or nanoimprint lithography.
[0191] Specifically, the structure, shape, and separation interval of the etching pattern layer 1700 may be associated with the shape of the light emitting element 300 to be finally manufactured. However, since the light emitting element 300 may have different shapes as described above, the etching pattern layer 1700 is not specifically limited in structure. For example, if the etching pattern layer 1700 has circular patterns separated from each other, the element deposition structure 3000 may be vertically etched to manufacture a light emitting element 300 having a cylindrical shape. However, the present disclosure is not limited thereto.
[0192] Next, the element deposition structure 3000 may be etched to form an element rod ROD according to the pattern of the etching pattern layer 1700. Spaces between the plurality of nanopatterns in the etching pattern layer 1700 may be vertically etched to form holes selectively formed to have a depth h from the etching mask layer 1600 to the separation layer 1300.
[0193] The holes can be formed using conventional methods. For example, the etching process can be performed using dry etching, wet etching, reactive ion etching (RIE), or inductively coupled plasma reactive ion etching (ICP-RIE). Dry etching can perform anisotropic etching, which can be suitable for forming holes by vertical etching. In the case of using the aforementioned etching techniques, it can be possible to use Cl 2 or 2 As an etchant. However, the present disclosure is not limited thereto.
[0194] In some embodiments, a combination of dry etching and wet etching may be used to etch the element deposition structure 3000. For example, dry etching may be used to perform etching in the depth direction, and then wet etching may be used to perform anisotropic etching so that the etched sidewalls are located on a plane perpendicular to the surface.
[0195] Meanwhile, forming the element rod ROD by etching the element deposition structure 3000 may include patterning the separation layer 1300 together during one etching process, or patterning a portion of the separation layer 1300 after forming the element rod ROD by another etching process.
[0196] That is, the separation layer 1300 may be patterned together in an etching process for forming a hole by etching the element deposition structure 3000 , or may be patterned in a separate process after the separation layer 1300 serves as an etching stop layer in the process of etching the element deposition structure 3000 .
[0197] For example, in the case where an etchant used to pattern the element deposition structure 3000 includes a substance for removing the separation layer 1300, the element deposition structure 3000 and the separation layer 1300 may be patterned simultaneously in one process. Fig.11, if the etchant is prepared to etch only the element deposition structure 3000, the separation layer 1300 may be used as an etching stop layer so that the etchant etches only the element deposition structure without etching the separation layer 1300. Therefore, the element rod ROD may be formed in a state where the separation layer 1300 is not etched, and the separation layer 1300 may be patterned by different etching processes.
[0198] In some embodiments, if the separation layer 1300 includes a graphene layer and the etchant includes oxygen (O 2 ), the device deposition structure 3000 and the separation layer 1300 may be patterned simultaneously. In another embodiment, if the etchant does not include oxygen (O 2 ), the element rods ROD can be formed by patterning the element deposition structure 3000, and the separation layer 1300 can be selectively etched in another etching process.
[0199] As reference Fig.12 As described, the element rods ROD may be formed by removing the etching mask layer 1600 and the etching pattern layer 1700 remaining on the vertically etched element deposition structure 3000 through a conventional method (eg, dry etching and wet etching).
[0200] Next, refer to Fig.13 and Fig.14 , an insulating layer 3800 may be formed to partially cover the outer surface of the element rod ROD to manufacture the light emitting element 300 .
[0201] The insulating layer 3800 is an insulating material formed on the outer surface of the element rod ROD, and the insulating layer 3800 may be formed by depositing the insulating material on the outer surface of the vertically etched element rod ROD or immersing the element rod ROD in the insulating material, and is not limited thereto. For example, the insulating layer 3800 may be formed using atomic layer deposition (ALD). The insulating layer 3800 may form the insulating material layer 380 of the light emitting element 300. As described above, the insulating layer 3800 may include a silicon oxide (SiO x ), Silicon Nitride (SiN x ), silicon oxynitride (SiO x N y ), aluminum oxide (Al 2 O 3 ) and aluminum nitride (AlN) materials.
[0202] Reference Fig.13, an insulating layer 3800 may be formed on the side surface and the top surface of the element rod ROD and between the separation layer 1300 exposed to the outside during the etching process to form the separated element rod ROD. In order to expose the two end side surfaces of the element rod ROD, the insulating layer 3800 formed on the top surface of the element rod ROD may be removed. Therefore, it may be necessary to partially remove the insulating layer 3800 formed in the direction perpendicular to the length direction of the element rod ROD (i.e., in the direction parallel to the base substrate 1100). That is, as Fig.14 As shown in , the top surface of the element rod ROD can be exposed by removing at least the insulating layer 3800 on the top surface of the element rod ROD and between the separation layers 1300. To achieve this, a process such as dry etching or etching back as anisotropic etching can be performed. Through the above process, the light emitting element 300 including the insulating layer 3800 covering the outer surface of the element rod ROD can be manufactured.
[0203] Finally, if Fig.15 As shown in FIG. 1 , the light emitting element 300 may be separated from the separation layer 1300 formed on the lower substrate layer 1000 .
[0204] As described above, the separation layer 1300 including the graphene layer can form a relatively weak attraction at the interface between the different material layers. However, the separation layer 1300 can form a relatively strong attraction with one of the different material layers and a relatively weak attraction with the other material layer. In this case, when the separation layer 1300 is peeled off so that the two material layers are separated, the separation layer 1300 can remain on one of the two material layers.
[0205] In the method for manufacturing the light emitting element 300 according to the embodiment, the interface attraction force between the separation layer 1300 and the buffer material layer 1200 may be greater than another interface attraction force between the separation layer 1300 and the first conductive type semiconductor layer 3100. That is, when the manufactured light emitting element 300 is separated, the separation layer 1300 may remain on the buffer material layer 1200 with a relatively strong attraction force, and the first conductive type semiconductor layer 3100 may be peeled off so that the light emitting element 300 is separated. Here, when the first conductive type semiconductor layer 3100 is peeled off from the separation layer 1300, because the inter-crystal attraction force of the first conductive type semiconductor layer 3100 is stronger than the interface attraction force associated with the first conductive type semiconductor layer 3100 and the separation layer 1300, the first conductive type semiconductor layer 3100 may be separated from the lower substrate layer 1000 without any damage.
[0206] In this regard, separation layer 1300 on separation surface 390 of manufactured light emitting element 300 is peeled off, which makes it possible to keep separation surface 390 flat and simultaneously ensure uniformity of separation surfaces 390 of a plurality of light emitting elements 300 .
[0207] Meanwhile, there is no limitation on the method of separating the light emitting element 300 by peeling off the separation layer 1300. In some embodiments, the light emitting element 300 may be separated from the lower substrate layer 1000 by physical separation (mechanical peeling) or chemical separation (chemical peeling).
[0208] Figures 16 to 18 is a schematic diagram illustrating a method for separating the light emitting element 300 according to an embodiment.
[0209] First, refer to Fig.16 and Fig.17 , an adhesive layer LOA is formed on the top surface of the light emitting element 300 manufactured on the lower substrate layer 1000. The adhesive layer LOA may be a material layer having an adhesive component and is not limited as long as it does not damage the material of the light emitting element 300. Examples of the adhesive layer LOA may include, but are not limited to, polymethyl methacrylate (PMMA), polydimethylsiloxane (PMDS), a viscosity-changing film, and a thermal release tape (TRT).
[0210] like Fig.17 As shown in the figure, the plurality of light emitting elements 300 manufactured on the lower substrate layer 1000 can be simultaneously adhered to the adhesive layer LOA (simultaneously adhered to the adhesive layer LOA on the top surfaces of the plurality of light emitting elements 300) and the plurality of light emitting elements 300 are physically lifted so as to peel the plurality of light emitting elements 300 from the lower substrate layer 1000. Although not shown in the drawings, the adhesive layer LOA can be removed by conventional methods.
[0211] In another embodiment, the light emitting element 300 can be separated from the lower substrate layer 1000 by vibration in the solution. Fig.18 , the light emitting element 300 manufactured on the separation layer 1300 can be separated in such a manner that vibration is applied while the light emitting element 300 is immersed in a separation solution S together with the lower substrate layer 1000. As described above, because the interface attraction of the separation layer 1300 including the graphene layer is relatively weak, the separation layer 1300 can be peeled off by relatively weak vibration. Therefore, the light emitting element 300 can be separated from the lower substrate layer 1000 by immersing the light emitting element 300 and the lower substrate layer 1000 in the separation solution S and applying vibration thereto. The type of separation solution S is not limited as long as it does not cause damage to the light emitting element 300. Examples of the separation solution S may include organic solvents. The method for separating the light emitting element 300 is not limited to reference. Figures 16 to 18Although not shown in the drawings, the light emitting element 300 may also be manufactured by chemically dissolving the separation layer 1300 .
[0212] The method for manufacturing the light emitting element 300 according to the embodiment may include forming a separation layer 1300 on the lower substrate layer 1000, and separating the light emitting element 300 grown on the separation layer 1300 from the lower substrate layer 1000. The separation layer 1300 may include at least one graphene layer, which may facilitate the separation of the light emitting element 300 manufactured thereon from the separation layer 1300 with a relatively weak interface attraction. Since the attraction between the separation layer 1300 and the first conductive type semiconductor layer 3100 of the light emitting element 300 is weaker than the inter-crystal attraction of the first conductive type semiconductor layer 3100, the light emitting element 300 may be separated while the separation surface 390 remains flat, and there is no damage on the separation surface 390 thereof. This makes it possible to prevent an open circuit of the contact electrode material from occurring at the interface (e.g., the separation surface 390) where the light emitting element 300 and the contact electrode 260 contact each other, which leads to an improvement in the light emission reliability of the display device 10.
[0213] Meanwhile, the arrangement of the separation layer 1300 is not limited to Figure 7 As described above, in the process of manufacturing the light emitting element 300, one or more separation layers 1300 may be arranged on the element deposition structure 3000 or the lower substrate layer 1000, or one separation layer 1300 may include a plurality of sub-separation layers. The separation layer 1300 arranged on the lower substrate layer 1000 or the element deposition structure 3000 according to another embodiment is described below.
[0214] Fig.19 is a cross-sectional view schematically showing the structure of a separation layer according to another embodiment. Fig. 20 is shown for Fig.19 Schematic diagram of the process of separating the light-emitting elements using a separation layer.
[0215] Reference Fig.19 , the separation layer 1300_1 may include a plurality of graphene layers GL. The plurality of graphene layers GL may include a first graphene layer GL1 formed on and contacting the buffer material layer 1200_1 and a second graphene layer GL2 disposed on the first graphene layer GL1 and contacting the separation surface 390 of the light emitting element 300. The method for manufacturing the light emitting element is the same as that of the reference except that the separation layer 1300_1 includes the plurality of graphene layers GL. Figures 6 to 18 Hereinafter, a method for separating the separation layer 1300_1 and the light emitting element 300 from each other is described in detail.
[0216] Reference Fig.19 and Fig. 20 When the light emitting element 300 grown on the separation layer 1300_1 is separated, separation may occur at a first interface INF1 between the buffer material layer 1200_1 and the first graphene layer GL1, a second interface INF2 between the first graphene layer GL1 and the second graphene layer GL2, and a third interface INF3 between the second graphene layer GL2 and the separation surface 390 of the light emitting element 300.
[0217] By adjusting the interface attraction at the first interface INF1 between the buffer material layer 1200_1 and the first graphene layer GL1 as described above, the first graphene layer GL1 can remain on the buffer material layer 1200_1 after the light emitting element 300 is separated. That is, the light emitting element 300 can be separated from the lower substrate layer 1000_1 through the crack at the second interface INF2 or the third interface INF3 where the attraction is weak.
[0218] Here, in the case where the attraction at the second interface INF2 is greater than the attraction at the third interface INF3, the separated light emitting element 300 may expose the first conductive type semiconductor 310 (ie, the separation surface 390), as shown in FIG. Fig. 20 In contrast, if the attraction at the third interface INF3 is greater than the attraction at the second interface INF2, the separated light emitting element 300 may not expose the first conductive type semiconductor 310 because the second graphene layer GL2 partially remains on the separation surface 390. In this case, the second graphene layer GL2 including the graphene having conductivity may form the electrode material layer 370 at one end of the light emitting element 300.
[0219] Meanwhile, in some embodiments, it may further include removing impurities from the separation surface 390 of the separated light emitting element 300. As described above, in the case where the separation layer 1300_1 includes a plurality of graphene layers GL, the layered structure on the separation surface 390 of the light emitting element 300 may vary according to the attractive forces at the plurality of interfaces INF. However, in the case where the attractive forces of the interfaces INF are not precisely controlled, the uniformity of the separation surface 390 of the light emitting element 300 may be reduced, and in order to overcome this, a post-processing process may be performed on the separated light emitting element 300.
[0220] like Fig. 20 As shown in FIG. 1 , in order to remove the separation layer 1300_1 (for example, the second graphene layer GL2) remaining on the separation surface 390 of the separated light emitting element 300, the above separation process may be repeatedly performed. Because the attraction at the interface between the second graphene layer GL2 of the separation layer 1300_1 and the separation surface 390 of the light emitting element 300 is relatively weak, the separation process may be repeated by referring to FIG. Figures 18 to 20 The process described is used to remove the second graphene layer GL2.
[0221] Figure 21 to Figure 24 is a cross-sectional view schematically showing the arrangement of separation layers in an element deposition structure according to still another embodiment.
[0222] The separation layer 1300 may be disposed in the first conductive type semiconductor layer 3100 of the element deposition structure 3000 , and in some cases directly disposed on the base substrate 1100 while omitting the buffer material layer 1200 .
[0223] Reference Fig.21 , the separation layer 1300_2 may be disposed on the first sub-conductivity type semiconductor layer 3100'_2 deposited on the buffer material layer 1200, and the first conductivity type semiconductor layer 3100_2 may be deposited on the separation layer 1300_2. The first sub-conductivity type semiconductor layer 3100'_2 may include a material substantially the same as that of the first conductivity type semiconductor layer 3100_2. That is, the separation layer 1300_2 may be disposed in the first conductivity type semiconductor layer 3100_2.
[0224] As described above, the buffer material layer 1200 may provide a seed crystal of the first conductive type semiconductor layer 3100 grown on the separation layer 1300 and may reduce a lattice constant difference of an interface. Fig.21 The element deposition structure 3000_2 may promote crystal growth of the first conductive type semiconductor layer 3100_2 by substantially including the separation layer 1300_2 in the first conductive type semiconductor layer 3100_2.
[0225] Reference Fig. 22 In the case where the base substrate 1100_3 includes a material substantially the same as that of the first conductive type semiconductor layer 3100_3, the buffer material layer 1200 may be omitted and the separation layer 1300_3 may be directly disposed on the base substrate 1100_3.
[0226] For example, in the case where the first conductive semiconductor layer 3100_3 includes n-type doped gallium nitride (GaN) and the base substrate 1100_3 is a GaN substrate, the lattice constant difference between the base substrate 1100_3 and the first conductive semiconductor layer 3100_3 may be small. In this case, even if the buffer material layer 1200 is omitted, the lattice constant difference between the base substrate 1100_3 and the first conductive semiconductor layer 3100_3 may be small, and the GaN substrate may provide a seed crystal. According to an embodiment, in the process of manufacturing the light emitting element 300, the separation layer 1300_3 may be directly arranged on the base substrate 1100_3, and the first conductive semiconductor layer 3100_3 may be grown on the separation layer 1300_3.
[0227] Meanwhile, it may be possible to include one or more separation layers disposed on different layers in the element deposition structure 3000 and the lower base layer 1000 .
[0228] Reference Fig.23 , the separation layer 1300_4 may include a first sub-separation layer 1310_4 disposed between the buffer material layer 1200 and the first sub-conductivity type semiconductor layer 3100'_4 and a second sub-separation layer 1320_4 disposed between the first sub-conductivity type semiconductor layer 3100'_4 and the first conductivity type semiconductor layer 3100_4. That is, in Fig.23 In, with Figure 7 Compared with the element deposition structure 3000, the second sub-separation layer 1320_4 may be further arranged in the first conductive type semiconductor layer 3100_4.
[0229] In this case, if the manufactured light emitting element 300 is separated, the second sub-separation layer 1320_4 remains on the first sub-conductivity type semiconductor layer 3100'_4. The element deposition structure can be manufactured by removing the second sub-separation layer 1320_4 remaining on the first sub-conductivity type semiconductor layer 3100_4 and then forming the second sub-separation layer 1320_4 again. That is, the first sub-conductivity type semiconductor layer 3100'_4 providing the seed crystal of the first conductivity type semiconductor layer 3100_4 can be repeatedly used several times.
[0230] In addition, refer to Fig.24 , the first sub-separation layer 1310_5 may be disposed between the buffer material layer 1200_5 and the first conductive type semiconductor layer 3100_5, and the second sub-separation layer 1320_5 may be disposed between the base substrate 1100_5 and the buffer material layer 1200_5. Fig.24 In, with Figure 7 Compared with the lower substrate layer 1000 of FIG. 1 , it may be the case that the second sub-separation layer 1320_5 is further arranged between the base substrate 1100_5 and the buffer material layer 1200_5.
[0231] As described above, the separation layer 1300_5 including graphene has a weak interface attraction with a specific surface, which facilitates separation or peeling. Fig.24In the embodiment of the present invention, the first sub-separation layer 1310_5 can be used to separate the light emitting element 300 from the lower substrate layer 1000_5, and the second sub-separation layer 1320_5 can be used to separate the base substrate 1100_5 and the buffer material layer 1200_5 from each other. In the case where the interface attraction between the second sub-separation layer 1320_5 and the base substrate 1100_5 is stronger than the interface attraction between the second sub-separation layer 1320_5 and the buffer material layer 1200_5, the base substrate 1100_5 and the buffer material layer 1200_5 can be easily separated from each other. In this case, after manufacturing the light emitting element 300, the base substrate 1100_5 of the lower substrate layer 1000_5 can be reused by separating it from the buffer material layer 1200_5 of the lower substrate layer 1000_5. For example, if the base substrate 1100_5 is a high-priced substrate such as a SiC substrate, reusing the base substrate 1100_5 can reduce the manufacturing cost of the light emitting element 300.
[0232] In summarizing the detailed description, those skilled in the art will appreciate that many changes and modifications may be made to the preferred embodiments without departing substantially from the principles of the invention. Therefore, the preferred embodiments of the disclosed invention are used in a general and descriptive sense only and not for purposes of limitation.
Claims
1. A method for manufacturing a light-emitting element, the manufacturing method include: preparing a lower substrate, the lower substrate comprising a base substrate and a buffer material layer formed on the base substrate; forming a separation layer disposed on the lower substrate and comprising at least one graphene layer; forming an element deposition structure by depositing a first conductivity type semiconductor layer, an active material layer, and a second conductivity type semiconductor layer on the separation layer; forming an element rod by etching the element deposition structure and the separation layer in a vertical direction; as well as The element rod is separated from the lower substrate to form a light-emitting element, wherein, in forming the element rod, the separation layer is etched and patterned, and The step of separating the element rods from the lower substrate includes: immersing the element rods formed on the separation layer together with the lower substrate into a separation solution; and separating the element rods from the lower substrate by applying vibration to the separation solution.
2. The manufacturing method according to claim 1, in, In the formation of the element rod, the separation layer is at least partially etched and patterned.
3. The manufacturing method according to claim 2, in, An interfacial attraction force between the separation layer and the lower substrate at a first interface between the separation layer and the lower substrate is greater than an interfacial attraction force between the separation layer and the element rod at a second interface between the separation layer and the element rod.
4. The manufacturing method according to claim 3, in, In the formation of the light emitting element, the second interface is peeled off, but the first interface is not peeled off, and the patterned separation layer remains on the lower substrate.
5. The manufacturing method according to claim 4, in, In the light emitting element, a separation surface is flat and parallel to a top surface of the second conductive type semiconductor layer, and the separation surface is a surface on which the element rod is peeled from the second interface.
6. The manufacturing method according to claim 5, in, In the light emitting element, the separation surface has a surface roughness within a range of 8 nm Ra to 12 nm Ra.
7. The manufacturing method according to claim 6, in, The forming of the element bar further includes forming an insulating layer, the insulating layer being disposed to surround a side surface of the element bar, and The light emitting element further includes the insulating layer disposed to surround a side surface of the first conductive type semiconductor layer, a side surface of the active material layer, and a side surface of the second conductive type semiconductor layer.
8. The manufacturing method according to claim 2, in, The separation layer includes: a first graphene layer; and a second graphene layer, disposed on the first graphene layer, The first graphene layer and the buffer material layer form a third interface, The second graphene layer forms a fifth interface with the element rod, and The first graphene layer and the second graphene layer form a fourth interface.
9. The manufacturing method according to claim 8, in, In forming the light emitting element, The third interface does not peel off, At least a portion of the fourth interface and the fifth interface peels off, The first graphene layer remains on the lower substrate, and The second graphene layer and the first graphene layer form the fourth interface, or the second graphene layer and the element rod form the fifth interface.
10. The manufacturing method according to claim 9, in, The separation layer includes: a first sub-separation layer disposed on the lower substrate; and The second sub-separation layer is disposed between the base substrate and the buffer material layer.
11. The manufacturing method according to claim 1, in, The device deposition structure further includes an electrode material layer on the second conductive type semiconductor layer.
12. The manufacturing method according to claim 11, in, The forming of the element rod includes: forming an etching mask layer on the element deposition structure, and forming an etching pattern layer on the etching mask layer, wherein the etching pattern layer includes one or more nano patterns separated from each other; forming a hole by vertically etching a region formed by the nano patterns separated from each other; and The etching mask layer and the etching pattern layer are removed.
13. The manufacturing method according to claim 12, in, The element deposition structure and the separation layer include materials with different etching selectivities, and The formation of the hole includes vertically etching the element deposition structure to expose at least a portion of an overlapping area between the separation layer and the area formed by the nanopatterns separated from each other; and etching and patterning the exposed area of the separation layer.
14. The manufacturing method according to claim 13, in, In the vertical etching of the element deposition structure, an etchant includes chlorine gas and oxygen gas, and the separation layer and the element deposition structure are etched simultaneously.