Build chamber for use in powder bed based laser additive manufacturing processes
By designing an improved airflow system during selective laser melting, entraining and ejecting splash particles, the quality problems of parts caused by splash contamination are solved, efficient splash removal is achieved, and the construction quality is improved.
Patent Information
- Application Number
- CN202011059770.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-03
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-09-30
AI Technical Summary
During the selective laser melting (SLM), splash contamination leads to damage to the quality of the parts, and the prior art is difficult to effectively remove splashes, affecting the construction quality.
A powder bed-based additive manufacturing equipment is designed, using an improved airflow system, through the reasonable layout and design of the airflow inlet and outlet channels, entraining and ejecting at least 85% of the splash particles, using computational fluid dynamics (CFD) ) and discrete phase model (DPM) simulations optimize the airflow system to reduce the amount of splash.
It significantly improves the removal rate of splashes, reduces the risk of part quality degradation, and achieves higher quality construction results, with a clearance rate of 85% to 99.99%.
Smart Images

Figure CN112605383B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure is generally directed to powder bed based laser additive manufacturing chamber configurations, such as those used in selective laser melting applications. More specifically, the present disclosure relates to powder bed based laser additive manufacturing build chambers that employ novel gas flow system designs that are configured to reduce generated spatter contamination and improve part quality. Background Art
[0002] Among metal additive manufacturing processes, selective laser melting (SLM) has attracted great interest because of its potential to produce high-resolution and high-density parts from a variety of different metals and metal alloys. In the SLM process, a high-energy laser beam is used to melt and fuse metal powder materials. Often, the high local temperatures associated with the SLM process environment can exceed the material vaporization point and cause evaporation. This vaporization process can cause a "steam jet" effect, which results in the generation of emissions from the molten pool. Due to the strong surface tension effects, this emission can include vaporized gases, powder particles within the steam jet, and droplets ejected from the molten pool.
[0003] The ejected particles within the exhaust (i.e., powder particles of the vapor jet and droplets from the melt pool) are often referred to as "spatter". This spatter can be redeposited on the powder bed, thereby contaminating the build area of the SLM build chamber and thereby creating the risk of adversely affecting the build quality of the resulting part. Therefore, in order to reduce the build quality risks associated with ejected particles and droplets, it is necessary to effectively design and implement spatter control and removal processes. Summary of the invention
[0004] In at least one embodiment, a powder bed-based additive manufacturing device is disclosed. The device may include: a build plate configured to support a powder bed including powder particles; and a laser assembly configured to direct a laser beam to the powder bed to form a part from the powder particles. The powder bed-based additive manufacturing device may further include a gas inlet channel configured to form a gas flow above the powder bed to entrain spatter particles formed by the powder particles through the laser beam. The device may also include an outlet channel configured to discharge (outlet) the entrained spatter particle gas flow, the outlet channel having a lower outlet surface positioned between 0 and 10 mm above the build plate, wherein the gas inlet channel and the outlet channel are configured to entrain and discharge at least 85% of the spatter particles.
[0005] In at least another embodiment, a powder bed-based additive manufacturing device is disclosed. The device may include: a build plate configured to support a powder bed including powder particles; and a laser assembly configured to direct a laser beam to the powder bed to form a part from the powder particles, the laser beam causing spatter particles to be formed from the powder particles. The powder bed-based additive manufacturing device may further include: a first gas inlet channel configured to form a first gas flow above the powder bed to entrain spatter particles to generate an entrained spatter particle gas flow; and a second gas inlet channel, which is positioned between 5 and 55 mm below the first gas inlet channel and is configured to form a second gas flow above the powder bed. The device may also include an outlet channel configured to discharge the entrained spatter particle gas flow, wherein the first gas inlet channel, the second gas inlet channel, and the outlet channel are configured to entrain and discharge at least 85% of the spatter particles.
[0006] In yet another embodiment, a selective laser melting apparatus is disclosed. The apparatus may include: a build plate configured to support a powder bed including powder particles; and a laser assembly adapted to form a part from the powder particles within the selective laser melting apparatus, the laser assembly causing spatter emissions to be formed from the powder particles. The selective laser melting apparatus may further include a primary gas inlet channel having an array of inlet nozzles positioned along its length, wherein the primary gas inlet channel is configured to form a gas flow above the powder bed to entrain spatter emissions to produce an entrained exhaust gas flow, and the length of each inlet nozzle is between approximately 20 and 150 mm. The apparatus may also include an outlet channel configured to discharge the entrained exhaust gas flow, wherein the primary gas inlet channel and the outlet channel are configured to entrain and discharge more than 85% of the spatter particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 Depicted are non-limiting examples of SLM build chambers and associated airflow systems;
[0008] Figure 2A and Figure 2B A perspective view showing a general SLM build chamber configuration;
[0009] Figure 3 Another example of a perspective view depicting a general SLM build chamber configuration;
[0010] FIG. 4A to FIG. 4D depicts simulation and experimental results related to the flow field inside the SLM chamber;
[0011] Figure 5A and Figure 5BA perspective view showing gas velocity contours within an SLM chamber;
[0012] Fig. 6A and Figure 6B A diagram showing simulated spatter redeposition and gas velocity contours directly above the powder bed of an SLM chamber;
[0013] Fig. 7A and Figure 7B is a graph showing airflow and splash emission trajectories generated by the Coanda effect within an SLM chamber;
[0014] Fig. 8A and Figure 8B The conditions that produce the Coanda effect in the SLM chamber are graphically depicted;
[0015] Fig. 9A and Fig. 9B Examples of perspective views of a general SLM build chamber configuration and spatter discharge trajectories associated therewith are depicted, respectively;
[0016] Fig. 10A and Fig. 10B depicts example SLM chamber and gas flow system configurations according to various disclosed embodiments;
[0017] Fig.11A and Fig. 11B Examples of splash redeposition maps and gas velocity contours are shown, respectively, for SLM chamber and gas flow system configurations according to various disclosed embodiments;
[0018] Fig. 12A and Fig. 12B depicts example SLM chamber and gas flow system configurations according to various disclosed embodiments;
[0019] Fig.13A and Fig. 13B Examples of airflow trajectories for SLM chambers and airflow system configurations according to various disclosed embodiments are shown, respectively; and
[0020] Fig.14A and Fig. 14B Depicted are graphs showing removal rate and maximum gas flow velocity of generated spatter contamination at 1 mm above an SLM build plate as a function of flow rate, in accordance with various disclosed embodiments.
[0021] FIG. 15A to FIG. 15C Examples of inlet channel configurations having different nozzle lengths are depicted in accordance with various disclosed embodiments.
[0022] Fig.16A and Fig. 16BDepicted are graphs showing removal rate and maximum gas flow velocity of generated spatter contamination at 1 mm above an SLM build plate as a function of flow rate, in accordance with various disclosed embodiments. DETAILED DESCRIPTION
[0023] Embodiments of the present disclosure are described herein. However, it will be understood that the disclosed embodiments are merely examples, and other embodiments may take various and alternative forms. The drawings are not necessarily drawn to scale; some features may be exaggerated or minimized to show the details of a particular component. Therefore, the specific structural and functional details disclosed herein will not be interpreted as restrictive, but merely as a representative basis for teaching those skilled in the art to adopt the present invention in various ways. As will be understood by those of ordinary skill in the art, the various features illustrated and described with reference to any one of the accompanying drawings may be combined with the features illustrated in one or more other figures to produce embodiments that are not explicitly illustrated or described. The combination of the illustrated features provides representative embodiments for typical applications. However, various combinations and modifications of the features that conform to the teachings of the present disclosure may be expected for specific applications or implementations.
[0024] In conjunction with one or more embodiments, describing a group or class of materials as suitable for a given purpose implies that mixtures of any two or more members of the group or class are suitable. Descriptions of ingredients in chemical terms refer to the ingredients when added to any combination specified in the description, and once mixed, do not necessarily preclude chemical interactions among the ingredients of the mixture.
[0025] Except where expressly indicated, all numerical quantities in this description indicating dimensions or material properties are modified by the word "about" in describing the broadest scope of the present disclosure.
[0026] The first definition of an acronym or other abbreviation applies to all subsequent uses of the same abbreviation herein and mutatis mutandis to normal grammatical variations of the initially defined abbreviation. Unless expressly stated to the contrary, measurements of properties are determined by the same technique as that previously or subsequently referenced for the same property.
[0027] Reference is made in detail to compositions, embodiments, and methods of embodiments known to the inventors. However, it should be understood that the disclosed embodiments are merely exemplary embodiments of the present invention, which may be embodied in various and alternative forms. Therefore, the specific details disclosed herein are not to be construed as limiting, but merely as a representative basis for teaching those skilled in the art to adopt the present invention in various ways.
[0028] The terms "substantially" or "approximately" may be used herein to describe embodiments disclosed or claimed. The terms "substantially" or "approximately" may modify a value or relative property disclosed or claimed in the present disclosure. In this case, "substantially" or "approximately" may mean that the value or relative property it modifies is within ±0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, or 10% of the value or relative property.
[0029] Given the significant potential of selective laser melting (SLM) technology for a variety of different industries and the inherent complexities in its process environment, material vaporization and associated particulate emissions need to be understood, modeled, and addressed to reduce their negative effects. The present disclosure describes designs and processes for efficiently removing emissions from and around the moving molten pool of an SLM build chamber, thereby reducing potential damage to build quality caused by contamination from generated spatter. Although many of the examples described herein describe SLM chamber designs and configurations, those of ordinary skill in the art will appreciate that such designs and configurations can also be effectively applied to various types of powder bed-based additive manufacturing devices.
[0030] Although the protective gas flow can actively help remove the ejected particles in the SLM build chamber, the efficiency of this technique depends on the design and optimization of the gas flow system utilized. The SLM build chamber design, combined with the applied gas flow system configuration and optimization, has not been extensively studied in the literature. Useful research on this interaction requires accurate models and understanding of many variables and effects, including but not limited to spatter parameters such as spatter count, diameter and speed. It is also important to identify how these parameters change based on different scanning speeds and laser powers for the design, development and implementation of efficient SLM chamber gas flow systems. Many other dynamics that appear in the SLM environment further complicate the SLM gas chamber design. These include increased spatter concentrations near the outlet of the SLM chamber and uneven gas flow, resulting in another area with increased spatter concentrations in the center of the build plate. Further complications are caused by the phenomenon of downward gas flow trends (known as the Coanda effect).
[0031] According to the present disclosure, improved airflow systems are described that improve the removability of SLM process emissions. These improved airflow systems are able to significantly reduce the amount of spatter without increasing the risk of blowing up powder bed particles. To achieve this result, the disclosed configurations and methods have been designed taking into account the numerous factors and complications inherent in the environment of the SLM chamber. Computational fluid dynamics (CFD) models and finite volume method (FVM) simulations have been used to develop the described SLM airflow systems. Such models and simulations have been used to better capture the complex dynamics of airflow behavior within the build chamber. In order to accurately simulate spatter generation within the chamber, discrete phase model (DPM) simulations have also been used. Finally, the disclosed designs and configurations have also been developed based on a fully coupled fluid-particle interaction approach, which is used to accurately capture the effects of airflow on solid particles within the chamber.
[0032] exist Figure 1 A non-limiting example of an SLM build chamber and associated gas flow system is depicted in . The SLM chamber 100 includes a laser assembly 110 above a build platform 112. A powder bed 114 includes a molten pool 116 in which a resulting part is manufactured by an SLM process. The SLM chamber 100 also includes a gas flow inlet channel 118 opposite a gas flow outlet 120. As will be appreciated, the gas flow inlet channel 118 may include one or more gas flow inlet nozzles. Additionally, the gas flow outlet 120 may be generally referred to as an outlet channel or simply an outlet. A flow of an inert gas, such as, for example, argon, is used to remove spatter from a build area 122 of the SLM chamber 100. The inert gas flow is typically provided by Figure 1 1. As indicated by these arrows, the gas flow is generally directed away from the gas flow inlet channel 118 and directed toward the gas flow outlet 120. This inert gas flow provides drag on the spatter particles discharged above the powder bed 114 and the melt pool 116. The general trajectory of the SLM exhaust (including the discharged spatter particles) is Figure 1 116 by the arrows above the molten pool 116. The removability of such SLM emissions depends on the characteristics of the inert gas flow achieved by the gas flow system of the SLM chamber 100.
[0033] According to various embodiments disclosed herein, the gas flow system of the SLM chamber can be designed to significantly improve the removability of SLM emissions. The percentage of spatter removed from the build area compared to the total amount of spatter generated is referred to as the removal rate. For example, the removal rate of generated spatter contamination is improved by such a gas flow system configuration, that is, in the gas system configuration, the gas flow outlet is lowered toward the substrate, the gas flow inlet channel length is increased, a multi-channel pump is used to achieve uniform gas flow, and / or one or more supplemental gas inlet flows are introduced into the chamber design.
[0034] Figure 2A and Figure 2B shows a general SLM build chamber configuration (such as, for example, Figure 1 ) of the SLM build chamber configuration described in the specification. Figure 1 Like, in Figure 2A and Figure 2B The measurement dimensions presented below are examples only. As will be appreciated by those skilled in the art, the chamber configuration designs described throughout this specification may be employed at a variety of different dimensions. Figure 2A Specifically depicted is a non-limiting example of an SLM chamber 200 that includes the location of a laser assembly 210 over a build region 222 that is positioned between an airflow inlet channel 218 and an airflow outlet 220 . Figure 2B The general configuration of SLM chamber 200 is depicted as seen from an angle directly above build area 222. As described in detail below, a model of spatter generation and exhaust within an SLM chamber, such as SLM chamber 200, can include a spatter generation line 224 oriented perpendicular to the airflow, from which spatter is randomly ejected from the surface of the build plate.
[0035] Similarly, Figure 3 Depicts a general SLM build chamber configuration (such as, for example, Figure 1 , Figure 2A and Figure 2B Another example of a perspective view of the SLM build chamber configuration described in FIG. Figure 3 The configuration of an SLM chamber 300 is shown, which includes a laser assembly 310 and airflow inlet channels 318 and airflow outlets 320 .
[0036] Accurate modeling techniques are needed to properly evaluate the gas flow and spatter conditions within the SLM chamber in order to design and develop novel chamber and gas flow system configurations - configurations that improve the removability of SLM emissions and thereby improve the build quality of the manufactured parts. In conjunction with such modeling techniques, computational fluid dynamics (CFD) methods can be used to calculate the amount of gas flow, and discrete phase models (DPMs) can be used to capture the relevant spatter generation characteristics. Additionally, coupled calculations of the discrete and continuous phases can be used to model the interaction of the metal particles and the inert gas continuous phase.
[0037] Example - Modeling an SLM environment
[0038] The SLM environment can be modeled by applying CFD methods combined with gas flow characteristics and discrete phase models to the generation and exhaust of spatter. Since there are no time-dependent features, the flow can be inferred to be steady state and incompressible. Additionally, the model assumes that spatter is ejected from the build plate along a straight line that spans the build plate width of approximately 280 mm and is oriented perpendicular to the inert gas flow. Figure 2B As shown in , the model contemplates that spatter is randomly ejected from the build plate along five straight spatter ejection lines 224 that span the width of the build plate and are oriented perpendicular to the gas flow. The spatter generation lines represent emissions from the entire build plate. The spatter particles can have varying particle diameters, including, for example, diameters between about 10 and 100 μm. The spatter particles can also exhibit a variety of ejection velocities, including, for example, velocities ranging from about 1.5 to 35 m / s. The model can further apply argon as an inert gas. According to this model, argon includes 1.6228 kg / m 3 The model further assumes that the powder metal material is 7950 kg / m 3 316L stainless steel.
[0039] exist FIG. 4A to FIG. 4D The simulation results based on this model are shown in combination with the experimental observations. FIG. 4A to FIG. 4D The flow fields shown in demonstrate reasonable agreement between simulation and experimental results. Figure 4A and Figure 4C The experimental results shown in come from Philo, AM et al., "A study into the effects of gas flow inlet design of the Renishaw AM250 laser powder bed fusion machine using computational modelling" (Solid Free. Fabr. (2017)). As explained in the paper, Figure 4A and Figure 4C The experimental data presented in is based on the configuration and environmental dynamics of a Renishaw AM250 SLM machine, and a series of hot wire anemometer (HWA) probes were used to measure velocity contours. For both the simulation model and the experiments, the centre plane was defined as 40 mm above the build plate, and the reference plane was defined as 3 mm above the build plate. Figure 4B The center plane velocity simulation data closely tracks the Figure 4A The experimental data of the center plane velocity are shown in . Similarly, Figure 4D The reference plane velocity simulation data shown in the Figure 4B The experimental data of the reference plane velocity are shown in .
[0040] If the velocity of the inert gas flow inside the SLM chamber is too high, additional powder bed particles can be blown up. Locally high gas velocities should be strictly limited in order to prevent this additional process complexity. In the simulation, the local gas velocity is collected at a position 1 mm above the powder bed. If the maximum local gas velocity exceeds a threshold velocity, the associated inlet flow velocity, which is initially applied at the inlet of the build chamber, needs to be reduced. The threshold velocity at 1 mm above the powder bed can be calculated analytically. For positions at the powder bed surface only, the threshold velocity is defined to describe the point at which the powder bed particles start to move when exposed to the gas flow above the powder bed. Calculations show that the threshold velocity at the powder bed surface is approximately 0.27 m / s. In order to calculate the threshold velocity at different positions above the powder bed, it is then related to the physical profile velocity by means of a logarithmic wind speed profile. For example, the threshold velocity at 1 mm above the powder bed can be calculated to be approximately 3.383 m / s. Therefore, if the gas velocity at 1 mm above the powder bed is less than 3.383 m / s, the powder bed particles will remain stationary.
[0041] Because the drag force applied to the spatter particles by the inert gas flow is closely related to the gas properties and velocity, the gas flow field is particularly important. In addition, a uniform velocity field just above the powder bed is preferred for spatter removal. Figure 5A and Figure 5B Gas velocity contours associated with the initial SLM chamber design described above are depicted. Figure 5A The velocity contour data shown in prove that the airflow is mainly concentrated in the rectangular region above the SLM chamber substrate and below the upper edge of the airflow inlet / outlet. Figure 5B The velocity contour data shown in show that the width of the airflow generally matches the width of the inlet / outlet. Figure 5A It is further shown that there is a recirculation flow over the cuboid area. Although this initial airflow system design could provide an acceptable flow field, certain unresolved design issues hampered the ability of the airflow to further remove splash from the build area.
[0042] According to one or more embodiments, the spatter contamination removal rate can be improved by an airflow system configuration in which the airflow outlet is lowered toward the SLM chamber substrate. In other embodiments, the spatter contamination removal rate can be improved by an airflow system configuration in which the length of the airflow inlet channel is increased. In still other embodiments, the spatter contamination removal rate can be improved by such an airflow system configuration, that is, in the airflow system configuration, the uniformity of the airflow is increased by utilizing a multi-channel pump. In yet other embodiments, the spatter contamination removal rate can be improved by an airflow system configuration in which one or more supplementary gas inlet flows are introduced into the chamber design. These airflow system design adjustments can be applied individually or combined in the same SLM chamber configuration to improve the airflow field and the resulting spatter removal. This adjustment can reduce the risk of emission-related part quality degradation.
[0043] Unremoved spatter can fall to the build bed and redeposit. Simply increasing the velocity of the airflow increases the risk of blowing up new stationary powder. To avoid this risk, the airflow at 1 mm above the powder bed should not exceed a critical threshold velocity value. Fig. 6A and Figure 6B Plots of simulated spatter redeposition and gas velocity contours directly above the powder bed are shown, respectively. Fig. 6A As shown in Figure 2, there are two areas with increased spatter concentration inside the chamber. The first area is located on the substrate near the chamber outlet. This is due to the configuration of the SLM chamber. Since the bottom of the gas outlet is higher than the build plate, the outlet at least partially blocks the outgoing flow of spatter, resulting in an increased concentration near the outlet. The second area with increased spatter concentration is within the build area itself near the center of the build plate. This area with increased spatter concentration is caused by uneven gas flow inside the SLM chamber. Figure 6B Velocity contours and non-uniform airflow within the chamber at 1 mm above the powder bed are shown. As evidenced by the velocity contours within the figure, there are two high velocity regions. If the typical flow rate (usually about 250 L / min) is increased without modifying the configuration of the SLM chamber and airflow components, the particles are blown up within these regions.
[0044] In addition to localized areas of increased spatter concentration and increased gas velocity, typical SLM chamber and gas flow system designs also exhibit a downward gas flow tendency (known as the Coanda effect). Under normal conditions, the combination of these factors results in observed removal rates of less than 50%. Removal rates of 50% or less are generally insufficient to manufacture high-quality engineering parts. Increasing the flow rate can only improve the removal rate to a certain extent, of course, at the risk of blowing particles. Fig. 7AAs shown in , this limitation is a result of the downward tendency of the flow (i.e., the Coanda effect). With higher flow velocities, the air velocity and the drag force imposed on the splash particles increase proportionally. Based on the force balance of the splash, as the flow velocity increases, the splash becomes more likely to follow the direction of the airflow. As shown in Figure 7B As shown in , a flow rate of 1500 L / min, for example, results in splash trajectories that are almost identical to the downward flow trend.
[0045] Fig. 8A and Figure 8B The conditions that produce the Coanda effect in an SLM chamber are graphically depicted. The incoming airflow from the inlet jet entrains air close to the inlet jet. This entrainment causes a pressure reduction near the inlet jet. The low-pressure region above the inlet jet is exposed to the entire SLM chamber. Therefore, this region can be quickly filled and reaches approximately ambient pressure. The region below the inlet jet is constrained by the substrate and a low-pressure region is created. The pressure difference across the airflow in the vertical direction causes the flow to turn downward.
[0046] An effective model of the SLM environment can also envision different spatter source locations and spray trajectories. Fig. 9A For example, the model may assume that the splash is approximately 45 degrees above the plane of the build surface. o Up to 70 o Instead of assuming that the spatter is ejected from the build plate in a straight line across the width of the build plate, the spatter is ejected away from the inlet channel at an angle between Fig. 9B The simulated spatter trajectories in the chamber are depicted in FIG.
[0047] Positioning the airflow outlet above the build plate (i.e., substrate) - as is common in existing SLM chamber designs - introduces an obstruction to spatter that might otherwise escape the build area. The higher spatter concentration near the outlet can be addressed by lowering the bottom of the outlet to the height of the build plate. According to certain embodiments, the airflow outlet can be lowered to the same level as the substrate surface so that there is no vertical displacement between the two. Fig. 10A A representative example of this configuration is shown in Fig. 10A A side view of an SLM chamber 400 is shown, which includes an airflow inlet channel 418 and an airflow outlet 420. As shown in the figure, a bottom portion 426 of the airflow outlet 420 is positioned at a vertical position approximately the same as a substrate surface 428. In at least another embodiment, the airflow outlet can be lowered so that its lower surface is positioned at a vertical position approximately the same as the substrate. In other embodiments, the airflow outlet can be lowered so that its lower surface is positioned between approximately 0 and 10 mm above the substrate surface. In yet other embodiments, the airflow outlet can be lowered so that its lower surface is positioned between approximately 10 and 30 mm above the substrate surface.
[0048] The following steps can be used to solve the problem of uneven airflow (which is Figure 6B Complications associated with (shown in ): having the nozzle associated with the gas inlet channel extend and provide uniform flow across all channels and associated jets. According to certain embodiments, the length of the gas inlet channel nozzle may be between about 20 mm and 150 mm. In other embodiments, the length of the gas inlet channel nozzle may be between about 50 mm and 120 mm. In still other embodiments, the length of the gas inlet channel nozzle may be between about 80 mm and 110 mm. Substantially uniform flow may be further achieved by using a multi-channel pump. In Fig. 10B A representative example of the SLM chamber and gas flow system configuration in such an embodiment is shown in . Fig. 10B A perspective view of an SLM chamber 500 is depicted, comprising a laser assembly 510 and a gas flow inlet channel 518 having a plurality of extended gas inlet channel nozzles 528 .
[0049] Fig.11A Depicted is a non-limiting example of a spatter redeposition graph for a chamber design incorporating a reduced outlet height and a gas flow rate of approximately 250 L / min. As shown, the increased spatter concentration near the outlet has been removed. Fig. 11B - which shows the gas velocity contours at 1 mm above the powder bed - demonstrates that by making the inlet gas flow more uniform, the localized region with increased spatter concentration in the middle of the build area can also be removed. Modifying the inlet design to provide a more uniform gas flow results in a more uniform flow field near the powder bed. This modification reduces the risk of blowing up powder bed particles. Additionally, this design increases the flow rate limitation so that the gas flow rate can be increased to between approximately 750 and 1500 L / min without exceeding the critical threshold velocity at 1 mm above the powder bed.
[0050] In one or more embodiments, the gas flow system of the SLM chamber may be configured such that at least one supplemental gas inlet channel is disposed below the primary gas inlet channel. Fig. 12A A representative example of this configuration is shown in Fig. 12A A side view of an SLM chamber 600 is depicted, including a primary airflow inlet channel 618 and an outlet 620. Fig. 12A As shown in , the SLM chamber 600 further includes a supplementary gas inlet channel 630 below the main gas inlet channel 618. This configuration may be referred to as a dual inlet design. According to other embodiments, at least one supplementary gas inlet channel is disposed below the main gas inlet channel, and at least one supplementary gas inlet channel is disposed above the main gas inlet channel. Fig. 12BA representative example of this configuration is shown in Fig. 12B A side view of an SLM chamber 700 is depicted, which includes a primary airflow inlet channel 718 and an outlet 720. As shown in the figure, the SLM chamber 700 further includes a first supplemental airflow inlet channel 730 below the primary airflow inlet channel 718 and a second supplemental airflow inlet channel 732 above the primary airflow inlet channel 718. This configuration, including supplemental airflow inlet channels both above and below the primary airflow inlet, may be referred to as a triple inlet design.
[0051] A system configuration including such a main gas flow inlet and a supplementary gas flow inlet, each of which may include one or more inlet nozzles, can be used to reduce the Coanda effect, which causes a vertical pressure difference, resulting in a downward flow within the SLM chamber. The downward flow tendency can be eliminated by reducing the pressure on the upper side of the flow or increasing the pressure on the lower side of the flow. When a continuous gas flow is supplied by one or more supplementary inlets positioned below the (one or more) main gas inlet channels, the low pressure area can be increased to ambient levels. Similarly, at least one supplementary gas flow disposed both above and below the (one or more) main gas inlet channels allows similar adjustments to the local pressure area, resulting in the cancellation of the Coanda effect.
[0052] In at least one embodiment, the supplemental gas inlet channel is disposed between approximately 5 and 55 mm below the primary gas inlet channel. In another embodiment, the supplemental gas inlet channel is disposed between approximately 15 and 40 mm below the primary gas inlet channel. In yet another embodiment, the supplemental gas inlet channel is disposed between approximately 20 and 30 mm below the primary gas inlet channel.
[0053] In at least one embodiment, the first supplemental gas inlet channel is disposed between approximately 5 and 55 mm below the primary gas inlet channel, and the second supplemental gas inlet channel is disposed between approximately 5 and 55 mm above the primary gas inlet channel. In other embodiments, the first supplemental gas inlet channel is disposed between approximately 15 and 40 mm below the primary gas inlet channel, and the second supplemental gas inlet channel is disposed between approximately 15 and 40 mm above the primary gas inlet channel. In still other embodiments, the first supplemental gas inlet channel is disposed between approximately 20 and 30 mm below the primary gas inlet channel, and the second supplemental gas inlet channel is disposed between approximately 20 and 30 mm above the primary gas inlet channel.
[0054] The flow rate from the supplemental inlet can be less than, equal to, or greater than the flow rate of the primary inlet. The flow rate values for these various flow designs are the sum of the flow rates of both the primary gas inlet and the supplemental gas inlet. Changing the flow rates can provide different efficiencies. In some embodiments, the flow rate from the lower supplemental inlet is between 25% and 200% of the primary inlet flow rate. In some embodiments, the flow rate from the lower supplemental inlet is between 25% and 100% of the primary inlet flow rate, and the flow rate from the higher supplemental inlet is between 25% and 100% of the primary inlet flow rate. Fig.13A and Fig. 13B Simulated velocity contours for gas flow system configurations employing supplemental gas inlets are shown in As these figures demonstrate, the downward flow tendency can be eliminated by applying these designs.
[0055] like Fig.14A and Fig. 14B As shown in, by adopting one or more of the SLM chamber and gas flow system configurations disclosed herein, the cleaning rate of the chamber can be significantly improved, resulting in the potential for higher part quality. According to some configurations, the cleaning rate obtained is between 60% and 100%. According to other configurations, the cleaning rate obtained is between 85% and 99.99%. According to still other configurations, the cleaning rate obtained is between 95% and 100%. For example, Fig.14A It was demonstrated that for a chamber featuring an initial design that did not employ the above configuration, adjustments achieved approximately 85% spatter removal at a flow rate of approximately 750 L / min, but did not exceed approximately 85% spatter removal even when the flow rate was increased to as high as 3,000 L / min. Additionally, as Fig. 14B As shown in , this initial design reaches a threshold velocity at 1 mm above the build plate at a flow rate of approximately 800 L / min. Therefore, in this initial design chamber, the flow rate cannot exceed approximately 800 L / min without risking particles being blown off the powder bed. Fig.14A As shown in , the maximum clearance of the initially designed chamber - at the maximum subcritical velocity (flow rate) - is about 84.4%. As further shown in Fig.14A and Fig. 14B As shown in , the chamber design using the efficient configuration described in this article can achieve significantly higher clearance rates (higher than the initial design) at high flow rates without exceeding the threshold velocity at 1 mm above the build plate. Therefore, this design can achieve high flow rates and clearance rates without risking particles being blown off the powder bed. Fig.14A and Fig. 14B It was demonstrated that each of the designs described herein can achieve greater than 85% clearance without exceeding a threshold velocity at 1 mm above the build plate. Specifically, Fig.14A and Fig. 14BThe reduced outlet design was shown to achieve a removal rate of approximately 93.3% at its maximum subcritical velocity (flow rate) of approximately 1,750 L / min. The dual inlet design achieved a removal rate of approximately 99.5% at its maximum subcritical velocity (flow rate) of approximately 3,000 L / min. Finally, Fig.14A and Fig. 14B The three-inlet design was shown to achieve approximately 99.9% clearance at a flow rate of approximately 3,000 L / min, which is still below its maximum subcritical velocity (flow rate).
[0056] As described above, the complications associated with uneven gas flow can be resolved by extending the length of the nozzle associated with the gas inlet channel. According to certain embodiments, the length of the gas inlet channel nozzle may be between about 20 mm and 150 mm. In other embodiments, the length of the gas inlet channel nozzle may be between about 50 mm and 120 mm. In still other embodiments, the length of the gas inlet channel nozzle may be between about 80 mm and 110 mm. FIG. 15A to FIG. 15C Depicted are examples of inlet channel configurations having different nozzle lengths according to embodiments of the present disclosure. Fig.15A An example of a single inlet channel configuration 818 is shown with a series of inlet nozzles 820 having an approximate length of 20 mm. Fig. 15B An example of a dual inlet channel configuration 918 is shown having a series of first inlet nozzles 920 and a series of second inlet nozzles 922. Fig. 15B As depicted in , the first inlet nozzle 920 and the second inlet nozzle 922 are both approximately 20 mm long. According to aspects of the present disclosure, extending the length of the gas inlet channel nozzle can be beneficially applied to a build chamber configuration that employs either a single or multiple inlet gas channels. For example, in a configuration with a supplemental gas inlet channel positioned below the primary gas inlet channel, lengthening the nozzles of both gas inlet channels can increase the uniformity of the gas flow, thereby resulting in better chamber clearance. For example, Fig. 15C A dual inlet channel configuration 938 is depicted in which the lengths of both the first inlet nozzle 940 and the second inlet nozzle 942 have been extended to approximately 100 mm. Further, in a configuration having supplemental gas inlet channels both above and below the primary gas inlet channel, lengthening the nozzles of all inlet channels may also increase the uniformity of gas flow, leading to better chamber clearance.
[0057] like Fig.16A As shown in , adding supplemental gas inlet channels and / or increasing the nozzle length of the gas inlet channel(s) may increase the purge rate of the associated chamber. Fig.16AIt was demonstrated that, depending on the specific inlet design configuration, the maximum clearance at certain flow rates could be increased from approximately 69% to greater than 95%. Fig. 16B The maximum velocity at 1 mm above the build plate is shown for the same inlet design configuration. As shown, when compared to a single inlet row configuration such as Fig.15A ) compared to the dual inlet row configuration (such as, Fig. 15B ) and a dual inlet row configuration with increased nozzle length (such as, Fig. 15C ) both beneficially reduce the maximum velocity at 1 mm above the build plate at all flow rates.
[0058] Although exemplary embodiments are described above, these embodiments are not intended to describe all possible forms of the present invention. On the contrary, the words used in the specification are descriptive words rather than restrictive words, and it should be understood that various changes can be made without departing from the spirit and scope of the present invention. Additionally, the features of the various embodiments implemented can be combined to form other embodiments of the present invention.
Claims
1. A powder bed-based additive manufacturing device, include: a build plate configured to support a powder bed including powder particles; a laser assembly configured to direct a laser beam at the powder bed to form a part from the powder particles, the laser beam causing spatter particles to be formed from the powder particles; a gas inlet passage configured to form a gas flow above the powder bed to entrain spatter particles to produce a gas flow entraining spatter particles; as well as An outlet channel is configured to be opposite to the gas inlet channel to discharge the gas flow with entrained spatter particles, the outlet channel having a lower outlet surface positioned between 0 and 10 mm above the building plate, wherein the gas inlet channel and the outlet channel are configured to entrain and discharge at least 85% of the spatter particles.
2. The powder bed-based additive manufacturing apparatus according to claim 1, in, The build plate includes a top surface, and the lower outlet surface of the outlet channel is positioned at the same vertical position as the top surface.
3. The powder bed-based additive manufacturing apparatus according to claim 1, in, The gas inlet passage and the outlet passage are configured to entrain and discharge greater than 90% of the splash particles.
4. The powder bed based additive manufacturing apparatus according to claim 1, in, The gas inlet passage and the outlet passage are configured to entrain and discharge greater than 95% of the splash particles.
5. The powder bed based additive manufacturing apparatus according to claim 1, in, The gas inlet channel is configured to form a gas flow of between 200 and 2000 L / min above the powder bed.
6. The powder bed based additive manufacturing apparatus according to claim 1, in, The gas inlet channel is configured to form a gas flow of between 500 and 1500 L / min above the powder bed.
7. A powder bed-based additive manufacturing device, include: a build plate configured to support a powder bed including powder particles; a laser assembly configured to direct a laser beam at the powder bed to form a part from the powder particles, the laser beam causing spatter particles to be formed from the powder particles; a first gas inlet channel configured to form a first gas flow above the powder bed to entrain spatter particles to generate a gas flow entraining spatter particles; a second gas inlet channel positioned between 5 and 55 mm below the first gas inlet channel and configured to form a second gas flow above the powder bed; as well as An outlet passage is configured to discharge the gas flow entrained with spatter particles, wherein the first gas inlet passage, the second gas inlet passage and the outlet passage are configured to entrain and discharge at least 85% of the spatter particles.
8. The powder bed based additive manufacturing apparatus according to claim 7, in, The first gas inlet passage, the second gas inlet passage, and the outlet passage are configured to entrain and discharge greater than 90% of the splash particles.
9. The powder bed based additive manufacturing apparatus according to claim 7, in, The second gas inlet channel is positioned between 15 and 40 mm below the first gas inlet channel.
10. The powder bed based additive manufacturing apparatus according to claim 7, further comprising a third gas inlet channel, the third gas inlet channel being positioned between 5 and 55 mm above the first gas inlet channel and being configured to form a third gas flow within the powder bed based additive manufacturing apparatus.
11. The powder bed based additive manufacturing apparatus according to claim 7, in, The outlet channel includes a lower outlet surface positioned between 10 and 30 mm above the build plate.
12. The powder bed based additive manufacturing apparatus according to claim 7, in, The build plate includes a top surface defining a horizontal build plane, and the lower outlet surface of the outlet channel is positioned at the same vertical position as the horizontal build plane.
13. The powder bed based additive manufacturing apparatus according to claim 12, further comprising a third gas inlet channel, the third gas inlet channel being positioned between 5 and 55 mm above the first gas inlet channel and being configured to form a third gas flow within the powder bed based additive manufacturing apparatus.
14. The powder bed based additive manufacturing apparatus according to claim 12, in, The first gas inlet channel has an array of inlet nozzles located along its length, and each inlet nozzle is between 50 and 120 mm in length.
15. A selective laser melting apparatus, wherein include: a build plate configured to support a powder bed including powder particles; a laser assembly adapted to form a part from said powder particles within said selective laser melting apparatus, said laser assembly causing spatter emissions to be formed from said powder particles; a primary gas inlet channel having an array of inlet nozzles positioned along its length, wherein the primary gas inlet channel is configured to form a gas flow over the powder bed to entrain spatter emissions to produce a gas flow entraining spatter emissions, and each inlet nozzle is between 20 and 150 mm in length; and An outlet passage configured to discharge the gas flow entrained with splash emissions, wherein the primary gas inlet passage and the outlet passage are configured to entrain and discharge more than 85% of the splash emissions.
16. The selective laser melting apparatus according to claim 15, in, The length of each inlet nozzle is between 50 and 120 mm.
17. The selective laser melting apparatus according to claim 15, in, The outlet channel includes a lower outlet surface positioned between 0 and 10 mm above the build plate.
18. The selective laser melting apparatus of claim 15, further comprising a supplemental gas inlet channel positioned below the primary gas inlet channel and having a supplemental array of inlet nozzles positioned along its length, in, The supplemental gas inlet passage is configured to form a supplemental gas flow within the selective laser melting apparatus.
19. The selective laser melting apparatus according to claim 18, in, Each inlet nozzle in said complementary array of inlet nozzles has a length of between 20 and 150 mm.
20. The selective laser melting apparatus of claim 18, further comprising a second supplemental gas inlet channel positioned above the primary gas inlet channel and having a second supplemental array of inlet nozzles positioned along its length, in, The second supplemental gas inlet passage is configured to form a second supplemental gas flow within the selective laser melting apparatus.