Positive electrode active material for secondary battery, preparation method thereof, and lithium secondary battery containing the same

By coating fluorine and boron on the particle surface of lithium composite transition metal oxide, the problem of thermal stability and electrochemical performance degradation of NCM materials with high nickel content under high voltage is solved, and high capacity and excellent electrochemical performance are achieved. chemical properties.

CN112673494BActive Publication Date: 2024-10-08LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980059000.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-28
Filing Date
2019-09-30
Publication Date
2024-10-08
Estimated Expiration
2039-09-30

AI Technical Summary

Technical Problem

Existing high-nickel-content NCM lithium-like composite transition metal oxides have problems with thermal stability and electrochemical performance degradation at high voltages. Especially above 4.3V, capacity reduction and output reduction are serious.

Method used

By coating fluorine (F) and boron (B) on the particle surface of lithium composite transition metal oxide, using MgF2 and H3BO3 as coating sources, dry mixing and heat treatment are performed to form a coating part to improve the thermal stability of the material. and electrochemical performance.

Benefits of technology

It significantly improves the thermal stability and electrochemical performance of high-nickel-content NCM cathode active materials, suppresses the increase in resistance and decreases in output, ensures high capacity and extends the service life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005003403630000171
    Figure GDA0005003403630000171
  • Figure GDA0005003403630000181
    Figure GDA0005003403630000181
  • Figure GDA0005003403630000191
    Figure GDA0005003403630000191
Patent Text Reader

Abstract

The present invention provides a method for preparing a positive electrode active material for a secondary battery, the method comprising the following steps: preparing a lithium composite transition metal oxide containing nickel (Ni), cobalt (Co) and manganese (Mn), wherein the content of the nickel (Ni) is 60 mol% or more based on the total content of the transition metals; and dry mixing and heat treating the lithium composite transition metal oxide, MgF2 as a fluorine (F) coating source and a boron (B) coating source to form a coating portion on the particle surface of the lithium composite transition metal oxide. In addition, the positive electrode active material prepared as described above comprises: a lithium composite transition metal oxide, the lithium composite transition metal oxide comprising nickel (Ni), cobalt (Co) and manganese (Mn); and a coating portion, the coating portion being formed on the particle surface of the lithium composite transition metal oxide, wherein the lithium composite transition metal oxide has a nickel (Ni) content of 60 mol% or more based on the total content of the transition metals, and the coating portion comprises fluorine (F) and boron (B).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit of Korean Patent Application No. 10-2018-0115731 filed on September 28, 2018, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field

[0004] The present invention relates to a positive electrode active material for a secondary battery, a preparation method thereof and a lithium secondary battery comprising the same. Background Art

[0005] Recently, due to the rapid popularization of electronic devices such as mobile phones, notebook computers, electric vehicles, etc. using batteries, the demand for small and lightweight secondary batteries with relatively high capacity has increased rapidly. In particular, lithium secondary batteries are lightweight and have high energy density, so they are of interest as driving power sources for portable devices. Therefore, efforts to improve the performance of lithium secondary batteries have been actively studied and developed.

[0006] When an organic electrolyte or a polymer electrolyte is filled between a positive electrode and a negative electrode made of an active material capable of intercalating and deintercalating lithium ions, a lithium secondary battery generates electric energy through oxidation and reduction reactions when lithium ions are intercalated / deintercalated from the positive and negative electrodes.

[0007] As the positive electrode active material of lithium secondary battery, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2, LiMn2O4, etc.), lithium iron phosphate compound (LiFePO4), etc. are used. In addition, as a method of improving the thermal stability of LiNiO2 with low thermal stability while maintaining its excellent reversible capacity, a lithium composite transition metal oxide (hereinafter referred to as "NCM-type lithium oxide") in which a part of nickel (Ni) is replaced by cobalt (Co) and manganese (Mn) has been developed. However, the typical NCM-type lithium composite transition metal oxide that has been developed does not have sufficient capacity performance, so its application is limited.

[0008] In order to solve these problems, in recent years, research has been conducted to increase the Ni content in NCM-based lithium composite transition metal oxides. However, in the case of a nickel-rich positive electrode active material with a high nickel content, its capacity is improved, but depending on the charge depth, as Ni 2+ To You 3+ / 4+ The oxygen deintercalation occurs rapidly due to oxidation. The deintercalated oxygen reacts with the electrolyte, thereby changing the inherent properties of the material and causing instability in the lattice structure and further structural collapse.

[0009] Therefore, in order to ensure the stability of Ni-rich high-Ni NCM-type lithium composite transition metal oxides, a lot of research is being conducted on surface modification combined with coating technology. However, there is still a need to develop a high-Ni NCM-type positive electrode active material that can suppress the degradation of battery performance (such as capacity reduction and output reduction) while improving thermal stability. In particular, there is still a need to develop a high-Ni NCM-type positive electrode active material that has stability at a high voltage of more than 4.3V. Summary of the invention

[0010] Technical issues

[0011] One aspect of the present invention provides a high-Ni NCM-based positive electrode active material containing more than 60 mol% nickel (Ni) to ensure high capacity, which can significantly improve stability while suppressing resistance increase and output reduction depending on the coating material. In particular, the present invention provides a secondary battery positive electrode active material that achieves excellent thermal stability and excellent electrochemical performance even at a high voltage of more than 4.3V.

[0012] Technical Solution

[0013] According to one aspect of the present invention, there is provided a method for preparing a positive electrode active material for a secondary battery, the method comprising the following steps: preparing a lithium composite transition metal oxide comprising nickel (Ni), cobalt (Co) and manganese (Mn), wherein the content of the nickel (Ni) is 60 mol % or more based on the total content of the transition metals; and dry mixing and heat treating the lithium composite transition metal oxide, MgF2 as a fluorine (F) coating source, and a boron (B) coating source to form a coating portion on the particle surface of the lithium composite transition metal oxide.

[0014] According to another aspect of the present invention, a positive electrode active material for a secondary battery is provided, the material for the secondary battery comprising: a lithium composite transition metal oxide, the lithium composite transition metal oxide comprising nickel (Ni), cobalt (Co) and manganese (Mn); and a coating portion, the coating portion being formed on the surface of particles of the lithium composite transition metal oxide, wherein the lithium composite transition metal oxide has a nickel (Ni) content of more than 60 mol% based on the total content of the transition metals, and the coating portion comprises fluorine (F) and boron (B).

[0015] According to still another aspect of the present invention, a positive electrode including the positive electrode active material and a lithium secondary battery including the positive electrode are provided.

[0016] Beneficial Effects

[0017] The positive electrode active material for secondary batteries prepared according to the present invention is a high-Ni NCM-type positive electrode active material containing more than 60 mol% of nickel (Ni), which can ensure high capacity and solve the problem of structural / chemical stability degradation caused by the increase of nickel (Ni) in the high-Ni NCM system. Therefore, excellent thermal stability can be ensured, and the resistance increase and output reduction depending on the coating material can also be suppressed. In particular, excellent thermal stability and excellent electrochemical performance can be achieved even at high voltages above 4.3V. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a graph showing the results of evaluating the low temperature output performance of lithium secondary batteries manufactured using the positive electrode active materials prepared according to the examples and comparative examples; and

[0019] Figure 2 is a graph showing the results of evaluating the amount of gas generated during high-temperature storage of lithium secondary batteries manufactured using the positive electrode active materials prepared according to Examples and Comparative Examples. DETAILED DESCRIPTION

[0020] Hereinafter, the present invention will be described in more detail to help understand the present invention. In this case, it should be understood that the words or terms used in the specification and claims should not be interpreted as having the meaning defined in a common dictionary. It should be further understood that based on the principle that the inventor can appropriately define the meaning of the words or terms to best explain the present invention, the words or terms should be interpreted as having the meaning consistent with their meaning in the relevant art background and technical concept of the present invention.

[0021] <Method for preparing positive electrode active material>

[0022] A positive electrode active material for a secondary battery is prepared by: preparing a lithium composite transition metal oxide containing nickel (Ni), cobalt (Co) and manganese (Mn), wherein the content of nickel (Ni) is 60 mol % or more based on the total content of transition metals; and dry mixing and heat treating the lithium composite transition metal oxide, MgF2 as a fluorine (F) coating source and a boron (B) coating source to form a coating portion on the particle surface of the lithium composite transition metal oxide.

[0023] The method for preparing a positive electrode active material of the present invention will be described in detail step by step below.

[0024] First, a lithium composite transition metal oxide containing nickel (Ni), cobalt (Co), and manganese (Mn) is prepared, wherein the content of nickel (Ni) is 60 mol % or more based on the total content of transition metals.

[0025] The lithium composite transition metal oxide is a high-nickel (Ni) NCM system with a nickel (Ni) content of 60 mol% or more based on the total content of transition metals. More preferably, based on the total content of transition metals, the nickel (Ni) content can be 65 mol% or more, and even more preferably 80 mol% or more. When the nickel (Ni) content of the lithium composite transition metal oxide satisfies 60 mol% or more based on the total content of transition metals, high capacity can be ensured.

[0026] More specifically, the lithium composite transition metal oxide can be represented by the following formula 1.

[0027] [Formula 1]

[0028] Li p Ni 1-(x1+y1+z1) Co x1 Mn y1 M a z1 O 2+δ

[0029] In the above formula, M a is at least one selected from the following: Zr, W, Mg, Al, Ce, Hf, Ta, La, Ti, Sr, Ba, Nb, Mo, and Cr, and 0.9 ≤ p ≤ 1.5, 0 < x1 ≤ 0.2, 0 < y1 ≤ 0.2, 0 ≤ z1 ≤ 0.1, -0.1 ≤ δ ≤ 1, and 0 < x1 + y1 + z1 ≤ 0.4.

[0030] In the lithium composite transition metal oxide of the above formula 1, Li can be included in an amount corresponding to p (i.e., 0.9 ≤ p ≤ 1.5). If p is less than 0.9, the capacity may deteriorate. If p is greater than 1.5, the particles may sinter during the firing process, making it difficult to prepare the positive electrode active material. When considering the significant effect of improving the capacity performance of the positive electrode active material by controlling the Li content and the balance of sintering in the preparation of the active material, it is more preferable that Li can be included in an amount of 1.0 ≤ p ≤ 1.15.

[0031] In the lithium composite transition metal oxide of the above formula 1, Ni can be included in an amount corresponding to 1 - (x1 + y1 + z1) (for example, 0.60 ≤ 1 - (x1 + y1 + z1) < 1). When the Ni content in the lithium composite transition metal oxide of the above formula 1 is 0.06 or more, an amount of Ni sufficient to contribute to charge and discharge can be ensured, thereby enabling high capacity. More preferably, Ni can be included in an amount of 0.65 ≤ 1 - (x1 + y1 + z1) ≤ 0.99.

[0032] In the lithium composite transition metal oxide of Formula 1 above, Co may be included in an amount corresponding to x1 (i.e., 0 < x1 ≤ 0.2). When the Co content in the lithium composite transition metal oxide of Formula 1 above is greater than 0.2, the cost may increase. When considering the significant effect of improving the capacity performance according to the inclusion of Co, more specifically, Co may be included in an amount of 0.05 ≤ x1 ≤ 0.2.

[0033] In the lithium composite transition metal oxide of Formula 1 above, when considering the effect of improving the life performance, Mn may be included in an amount corresponding to y1 (i.e., 0 < y1 ≤ 0.2). When y1 in the lithium composite transition metal oxide of Formula 1 above is greater than 0.2, the output performance and capacity performance of the battery may instead deteriorate significantly. Therefore, more specifically, Mn may be included in an amount of 0.05 ≤ y1 ≤ 0.2.

[0034] In the lithium composite transition metal oxide of Formula 1 above, M a may be a doping element included in the crystal structure of the lithium composite transition metal oxide, and M may be included in an amount corresponding to z1 (i.e., 0 ≤ z1 ≤ 0.1) a .

[0035] Next, the lithium composite transition metal oxide, MgF2 as a fluorine (F) coating source, and a boron (B) coating source are dry-mixed and heat-treated to form a coating portion on the surface of the particles of the lithium composite transition metal oxide.

[0036] In the present invention, MgF2 is used as a fluorine (F) coating source to coat fluorine (F), and a boron (B) coating source is mixed therewith to coat boron (B). When MgF2 is used to coat fluorine (F), during the heat treatment, F of MgF2 replaces some oxygen on the surface of the positive electrode active material and lithium borate oxide (LiBO) to form electron holes, thereby improving the electron mobility. Since some oxygen is replaced by F, the distance between the transition metal and oxygen becomes closer, thereby minimizing the oxygen deintercalation that may occur when the oxidation number of the transition metal changes during the electrochemical reaction. Through the above, the generation of gas can be suppressed, the formation of the SEI film can be promoted, and the corrosion of the surface of the positive electrode active material caused by HF generated due to the decomposition of the electrolyte can be prevented. As in the present invention, by using MgF2 as a fluorine (F) coating source, there is a significant effect of suppressing the structural deterioration of the positive electrode active material. However, MgF2 has a high melting point of about 1263 °C, making it difficult to use it as a coating source in the prior art. Even considering wet coating, it is difficult to apply wet coating to MgF2 due to its low solubility. In addition, Mg has the disadvantage of reducing the charge / discharge capacity even in small amounts.

[0037] Therefore, the present invention uses MgF2 and a boron (B) coating source together when dry coating is performed to reduce the melting point of MgF2, thereby increasing the ease of coating and significantly improving the electrochemical performance. In addition, the lithium boron oxide (LiBO) produced by the boron (B) coating has the effect of increasing the charge / discharge capacity. The positive electrode active material prepared as described above can significantly improve the stability while suppressing the resistance increase and output reduction depending on the coating material, and in particular, even at a high voltage of more than 4.3V, excellent thermal stability and excellent electrochemical performance can be achieved.

[0038] The boron (B) coating source may include at least one selected from the group consisting of B4C, B2O3, and H3BO3, and may preferably be H3BO3. H3BO3 has a melting point of about 170°C, which is relatively lower than the melting points of other boron (B) coating sources, such as B4C (about 2,763°C) and B2O3 (about 450°C). In the case of coating with H3BO3, when heat treatment is performed, hydrogen is easily deintercalated and boron oxide (BO) anions are simply formed, thereby making coating easy and the effect of improving electrochemical properties can be more excellent.

[0039] The boron (B) coating source (particularly H3BO3) is easily anionized in a relatively low temperature range, which can cause a reaction with residual lithium and can lower the melting point of MgF2 by a driving force generated when lithium boron oxide (LiBO) is formed. That is, by using a boron (B) coating source, particularly by using a mixture of H3BO3 and MgF2, the ease of coating can be significantly improved and uniform coating can be achieved, and the structural stability can be effectively improved and the charge / discharge capacity can be increased.

[0040] Based on 100 parts by weight of the lithium composite transition metal oxide, MgF2 can be mixed in an amount of 0.002 to 0.08 parts by weight, more preferably 0.008 to 0.06 parts by weight, and even more preferably 0.01 to 0.04 parts by weight. By mixing and using MgF2 in the above-mentioned range of parts by weight, the generation of gas can be suppressed, the formation of SEI film can be promoted, and the corrosion of the surface of the positive electrode active material caused by HF generated by the decomposition of the electrolyte can be prevented, while the degradation of the charge / discharge capacity caused by Mg can be minimized.

[0041] Based on 100 parts by weight of the lithium composite transition metal oxide, the boron (B) coating source can be mixed in an amount of 0.09 to 0.75 parts by weight, more preferably 0.1 to 0.6 parts by weight, and even more preferably 0.2 to 0.4 parts by weight. By mixing the boron (B) coating source, especially H3BO3, in the above-mentioned range of parts by weight, the melting point of MgF2 can be effectively reduced, and the charge / discharge capacity can be increased.

[0042] MgF2 and a boron (B) coating source and a lithium composite transition metal oxide are dry mixed, and then the mixture is heat treated to form a coating portion. The heat treatment can be performed at 200°C to 600°C, more preferably 300°C to 500°C. The heat treatment can be performed in an atmospheric atmosphere and can be performed for 2 hours to 8 hours, more preferably 3 hours to 6 hours.

[0043] <Positive Electrode Active Material>

[0044] The positive electrode active material prepared as described above includes: a lithium composite transition metal oxide, which includes nickel (Ni), cobalt (Co) and manganese (Mn); and a coating portion formed on the particle surface of the lithium composite transition metal oxide, wherein the lithium composite transition metal oxide has a nickel (Ni) content of more than 60 mol% based on the total content of transition metals, and the coating portion includes fluorine (F) and boron (B).

[0045] The lithium composite transition metal oxide is applied in the same composition and chemical formula as those of the lithium composite transition metal oxide in the above-mentioned method of preparing a positive electrode active material.

[0046] The positive electrode active material prepared according to the preparation method of the present invention comprises a coating portion formed on the surface of the lithium composite transition metal oxide particle, wherein the coating portion comprises fluorine (F) and boron (B). By forming a coating portion comprising fluorine (F) and boron (B) in a high nickel (Ni) NCM system having more than 60 mol% nickel (Ni) as described above, the present invention can solve the problem of structural / chemical stability degradation caused by the increase of nickel (Ni) in the high Ni NCM system, and can ensure excellent thermal stability. In addition, the generation of gas can be suppressed, the formation of SEI film can be promoted, and the corrosion of the surface of the positive electrode active material caused by HF generated by the decomposition of the electrolyte can be prevented, while the resistance increase and output reduction depending on the coating material can be suppressed, and the degradation of the charge / discharge capacity can be suppressed. In particular, the positive electrode active material prepared as described above can achieve excellent thermal stability and excellent electrochemical performance even at a high voltage of more than 4.3V.

[0047] Fluorine (F) contained in the coating portion may be contained at 100 ppm to 300 ppm, more preferably 100 ppm to 250 ppm, still more preferably 120 ppm to 200 ppm, based on the total weight of the positive electrode active material.

[0048] The boron (B) contained in the coating portion may be contained at 300 ppm to 700 ppm, more preferably 300 ppm to 650 ppm, still more preferably 350 ppm to 600 ppm, based on the total weight of the positive electrode active material.

[0049] By coating fluorine (F) and boron (B) in a content satisfying the above range, excellent thermal stability can be ensured even in the case of a high nickel (Ni) NCM system having more than 60 mol % of nickel (Ni), and it has the effects of lowering room temperature resistance and reducing gas generation.

[0050] <Positive Electrode and Secondary Battery>

[0051] According to another embodiment of the present invention, a positive electrode for a lithium secondary battery including the positive electrode active material and a lithium secondary battery including the positive electrode are provided.

[0052] Specifically, the positive electrode includes a positive electrode collector and a positive electrode active material layer, the positive electrode active material layer being formed on the positive electrode collector and including the positive electrode active material.

[0053] In the positive electrode, the positive electrode collector is not particularly limited as long as it has conductivity and does not cause chemical changes in the battery. For example, stainless steel; aluminum; nickel; titanium; fired carbon; or aluminum or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode collector can typically have a thickness of 3 μm to 500 μm, and fine concavoconvexities can be formed on the surface of the positive electrode collector to improve the adhesion of the positive electrode active material. For example, the positive electrode collector can be used in various forms such as films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.

[0054] In addition, the positive electrode active material layer may include a conductive material and a binder as well as the above-mentioned positive electrode active material.

[0055] At this time, the conductive material is used to impart conductivity to the electrode, and any conductive material can be used without particular limitation as long as it has electronic conductivity and does not cause chemical changes in the battery to be constructed. Specific examples of conductive materials may include: graphite, such as natural graphite or artificial graphite; carbon materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers, such as zinc oxide whiskers and potassium titanate whiskers; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives, and any one of the above materials or a mixture of two or more thereof can be used. Based on the total weight of the positive electrode active material layer, the conductive material may be included in an amount of 1 wt % to 30 wt %.

[0056] In addition, the binder is used to improve the bonding between the positive active material particles and the adhesion between the positive active material and the positive current collector. Specific examples of binders may include: polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber or its various copolymers, and any one of the above materials or a mixture of two or more thereof can be used. Based on the gross weight of the positive active material layer, the binder may be included in an amount of 1 wt % to 30 wt %.

[0057] In addition to using the above-mentioned positive electrode active material, the positive electrode can be manufactured according to a typical method for manufacturing a positive electrode. Specifically, the positive electrode can be manufactured by coating a composition for forming a positive electrode active material layer containing the above-mentioned positive electrode active material and an optional binder and a conductive material on a positive electrode collector, followed by drying and rolling. At this time, the types and contents of the positive electrode active material, the binder and the conductive material are as described above.

[0058] The solvent may be a commonly used solvent in the art. Examples of solvents may include dimethyl sulfoxide (DMSO), isopropanol, N-methylpyrrolidone (NMP), acetone or water, and any one of the above materials or a mixture of two or more thereof may be used. If, in consideration of the coating thickness and preparation yield of the slurry, the solvent may dissolve and disperse the positive electrode active material, the binder and the conductive material, and thereafter have a viscosity that can show excellent thickness uniformity during the coating for the manufacture of the positive electrode, the amount of the solvent used is sufficient.

[0059] Alternatively, in another method, the positive electrode may be manufactured by casting a composition for forming a positive electrode active material layer on a separate support and then laminating a film obtained by peeling off from the support on a positive electrode current collector.

[0060] According to another embodiment of the present invention, an electrochemical device comprising the positive electrode is provided. The electrochemical device may be a battery, a capacitor, etc., and more specifically a lithium secondary battery.

[0061] The lithium secondary battery comprises a positive electrode, a negative electrode arranged facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode is the same as above. In addition, the lithium secondary battery may also optionally comprise: a battery case for accommodating an electrode assembly consisting of a positive electrode, a negative electrode and a separator; and a sealing member for sealing the battery case.

[0062] In a lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.

[0063] The negative electrode collector is not particularly limited as long as it has high conductivity and does not cause chemical changes in the battery. For example, copper; stainless steel; aluminum; nickel; titanium; fired carbon; copper or stainless steel surface-treated with one of carbon, nickel, titanium, silver, etc.; and aluminum-cadmium alloys, etc. can be used. In addition, the negative electrode collector typically may have a thickness of 3 μm to 500 μm, and as in the case of the positive electrode collector, fine concavoconvexities may be formed on the surface of the negative electrode collector to improve the adhesion of the negative electrode active material. For example, the negative electrode collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric body, and the like.

[0064] In addition to the negative electrode active material, the negative electrode active material layer also selectively contains a binder and a conductive material. As an example, the negative electrode active material layer can be prepared by coating a composition for forming a negative electrode containing a negative electrode active material and a selective binder and a conductive material on a negative electrode collector and then drying. Alternatively, the negative electrode active material layer can be prepared by casting the composition on a separate carrier and then laminating the film obtained by peeling off the carrier on the negative electrode collector.

[0065] As the negative electrode active material, a compound capable of reversibly inserting and extracting lithium can be used. Specific examples of the negative electrode active material may include: carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; (semi)metallic materials capable of forming an alloy with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; metal oxides that may or may not be doped with lithium, such as SiO α (0<α<2), SnO2, vanadium oxide, lithium titanium oxide and lithium vanadium oxide; or a composite material comprising a (semi)metallic material and a carbonaceous material, such as a Si-C composite material or a Sn-C composite material, and any one of the above materials or a mixture of two or more thereof can be used. In addition, a metallic lithium film can be used as a negative electrode active material. In addition, low-crystalline carbon and high-crystalline carbon can be used as carbonaceous materials. Typical examples of low-crystalline carbon may include soft carbon and hard carbon, and typical examples of high-crystalline carbon may include irregular, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite, condensed graphite, pyrolytic carbon, mesophase pitch-type carbon fibers, mesophase carbon microbeads, mesophase pitch, and high-temperature sintered carbon (such as coke derived from petroleum or coal tar pitch).

[0066] Furthermore, the binder and the conductive material may be the same as those described above in the description of the positive electrode.

[0067] On the other hand, in lithium secondary batteries, the separator is used to separate the negative electrode from the positive electrode and provide a mobile path for lithium ions. Any separator can be used without particular restriction, as long as it is commonly used as a separator in a lithium secondary battery. In particular, it is preferred to have a high moisture retention capacity for the electrolyte and a low resistance to the movement of electrolyte ions. Specifically, it can be used: a porous polymer film, for example, a porous polymer film prepared by a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a laminated structure having more than two layers in the above porous polymer film. In addition, a typical porous non-woven fabric can be used, such as a non-woven fabric formed by glass fibers or polyethylene terephthalate fibers with a high melting point. In addition, a coated separator containing a ceramic component or a polymer material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single-layer or multi-layer structure.

[0068] In addition, the electrolyte used in the present invention may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc. that can be used in the manufacture of a lithium secondary battery, but is not limited thereto.

[0069] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0070] Any organic solvent can be used without particular limitation, as long as it can be used as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, as an organic solvent, ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone and ε-caprolactone can be used; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; or carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) and propylene carbonate (PC); alcohol solvents such as ethanol and isopropanol; nitrile such as R-CN (wherein R is a linear, branched or cyclic hydrocarbon group having C2 to C20 and may contain a double bond, an aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolanes; or cyclopentane sulfone. Among these solvents, carbonate solvents are preferred, and more preferably a mixture of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) having high ion conductivity and high dielectric constant and linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) having low viscosity, which can improve the charge / discharge performance of the battery. In this case, when the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte can be excellent.

[0071] Any compound can be used as a lithium salt without particular limitation, as long as it can provide the lithium ions used in the lithium secondary battery. Specifically, as a lithium salt, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI or LiB(C2O4)2 can be used. The lithium salt can be used in a concentration range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has suitable conductivity and viscosity, thereby showing excellent performance, and the lithium ions can be effectively moved.

[0072] In the electrolyte, in addition to the electrolyte components, in order to improve the life characteristics of the battery, suppress the reduction of the battery capacity and increase the discharge capacity of the battery, at least one additive may be included, such as halogenated alkylene carbonate compounds (such as difluoroethylene carbonate), pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, (condensed) glycol dimethyl ethers, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N, N-substituted imidazolidinones, ethylene glycol dialkyl ethers, ammonium salts, pyrroles, 2-methoxyethanol or aluminum chloride. At this time, based on the total weight of the electrolyte, the additive may be included in an amount of 0.1% to 5% by weight.

[0073] The above-mentioned lithium secondary battery containing the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output performance and capacity retention rate, and can therefore be used in: portable devices such as mobile phones, notebook computers and digital cameras; and electric vehicle fields such as hybrid electric vehicles (HEV).

[0074] Therefore, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit battery and a battery pack including the battery module are provided.

[0075] The battery module or battery pack can be used as a power source for one or more medium and large devices, such as: power tools; electric vehicles such as electric vehicles (EV), hybrid electric vehicles (HEV) and plug-in hybrid electric vehicles (PHEV); or power storage systems.

[0076] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement the present invention. However, the present invention can be implemented in many different forms and is not limited to the embodiments set forth herein.

[0077] Example 1

[0078] Lithium carbonate (Li2CO3) was added to a precursor having a molar ratio of Ni:Co:Mn of 65:15:20 so that the molar ratio of Li / metal (Ni, Co, Mn) became 1.06, and the mixed powder was introduced into an alumina crucible for heat treatment. Thereafter, the mixed powder was heat treated at 750°C for 5 hours in an oxygen atmosphere and then at 870°C for 10 hours to prepare a lithium composite transition metal oxide.

[0079] After that, the heat-treated lithium composite transition metal oxide powder was crushed using a mortar, and then 0.025 parts by weight of MgF2 and 0.3 parts by weight of H3BO3 were added based on 100 parts by weight of the lithium composite transition metal oxide. The mixture was heat-treated at 380°C for 5 hours in an atmospheric atmosphere to prepare a positive electrode active material having a coating portion (F 150ppm, B 500ppm).

[0080] Example 2

[0081] A positive electrode active material having a coating portion (F 150 ppm, B 300 ppm) was prepared in the same manner as in Example 1, except that 0.025 parts by weight of MgF 2 and 0.18 parts by weight of H 3 BO 3 were mixed.

[0082] Example 3

[0083] A positive electrode active material having a coating portion (F 150 ppm, B 700 ppm) was prepared in the same manner as in Example 1, except that 0.025 parts by weight of MgF 2 and 0.42 parts by weight of H 3 BO 3 were mixed.

[0084] Example 4

[0085] A positive electrode active material having a coating portion (F 150 ppm, B 700 ppm) was prepared in the same manner as in Example 1, except that 0.025 parts by weight of MgF2 and 0.09 parts by weight of B4C were mixed and heat treatment was performed at 600°C for 5 hours in an air atmosphere.

[0086] Example 5

[0087] A positive electrode active material was prepared in the same manner as in Example 1, except that the heat treatment was performed at 420° C. for 5 hours.

[0088] Comparative Example 1

[0089] A positive electrode active material was prepared in the same manner as in Example 1, except that the heat treatment was performed without adding the coating source to the lithium composite transition metal oxide.

[0090] Comparative Example 2

[0091] A positive electrode active material was prepared in the same manner as in Example 1, except that 0.25 parts by weight of AlF 3 was used instead of MgF 2 .

[0092] Comparative Example 3

[0093] A positive electrode active material was prepared in the same manner as in Example 1, except that 0.63 parts by weight of WO 3 and 0.42 parts by weight of H 3 BO 3 were used instead of MgF 2 .

[0094] Comparative Example 4

[0095] A positive electrode active material was prepared in the same manner as in Comparative Example 3, except that 0.32 parts by weight of WO 3 and 0.42 parts by weight of H 3 BO 3 were used.

[0096] Comparative Example 5

[0097] A positive electrode active material was prepared in the same manner as in Example 1, except that 0.025 parts by weight of MgF 2 was mixed into the lithium composite transition metal oxide as a coating source.

[0098] [Preparation Example: Production of Lithium Secondary Battery]

[0099] Each positive electrode active material prepared in Examples 1 to 5 and Comparative Examples 1 to 5, a carbon black conductive material and a PVdF binder were mixed in an N-methylpyrrolidone solvent in a weight ratio of 96.5:1.5:2 to prepare a positive electrode mixture material (viscosity: 5000 mPa·s), and the mixture material was coated on one surface of an aluminum current collector, dried at 130° C., and roll-pressed to manufacture a positive electrode.

[0100] The natural graphite negative electrode active material, the carbon black conductive material and the PVDF binder were mixed in an N-methylpyrrolidone solvent at a weight ratio of 85:10:5 to prepare a composition for forming a negative electrode. The composition was then coated on one surface of a copper current collector to manufacture a negative electrode.

[0101] A porous polyethylene separator is inserted between the positive electrode and the negative electrode prepared as described above to prepare an electrode assembly, which is then placed in a housing. Afterwards, an electrolyte is injected into the housing to manufacture a lithium secondary battery. At this point, an electrolyte is prepared by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1.0 M in an organic solvent consisting of ethylene carbonate / dimethyl carbonate / ethyl methyl carbonate (mixed volume ratio of EC / DMC / EMC = 3 / 4 / 3).

[0102] [Experimental Example 1: Evaluation of Room Temperature Resistance]

[0103] Lithium secondary batteries manufactured in the same manner as in Preparation Example using each of the positive electrode active materials of Examples 1 to 5 and Comparative Examples 1 to 5 were measured for discharge 10-second resistance at room temperature (25° C.) in a state of SOC 50%, and the results are shown in Table 1.

[0104] [Table 1]

[0105]

[0106] Referring to Table 1, when compared with Comparative Examples 1 to 5, Examples 1 to 5 in which the coating part is formed according to the present invention have improved room temperature output.

[0107] [Experimental Example 2: Evaluation of Low-Temperature Output Performance]

[0108] The lithium secondary batteries manufactured in the same manner as in the preparation example using each of the positive electrode active materials in Examples 1 to 5 and Comparative Examples 1 to 5 were discharged at 0.6C until 3V at -25°C and SOC 20% to evaluate the low temperature output using the resulting voltage difference, and the results are shown in the following Tables 2 and Figure 1 middle.

[0109] [Table 2]

[0110]

[0111] Refer to Table 2 and Figure 1 , when compared with Comparative Examples 1 to 5, Examples 1 to 5 in which the coating portion is formed according to the present invention have improved low-temperature output.

[0112] [Experimental Example 3: Evaluation of Gas Generation]

[0113] Lithium secondary batteries manufactured in the same manner as in Preparation Example using each of the positive electrode active materials of Examples 1 to 5 and Comparative Examples 1 to 5 were stored at SOC 100% and 90° C. for 4 weeks to evaluate gas generation per week, and the results are shown in Table 2.

[0114] refer to Figure 2 , it can be seen that, when compared with Comparative Examples 1 to 5, Examples 1 to 5 in which the coating portion is formed according to the present invention have reduced gas generation amounts after the second week.

[0115] [Experimental Example 4: Evaluation of Life Performance]

[0116] The lithium secondary battery manufactured in the same manner as in the preparation example using each positive electrode active material in Examples 1 to 5 and Comparative Examples 1 to 5 was charged in CCCV mode at 45°C (termination current 1 / 20C) until the battery reached 1.0C and 4.25V, and then discharged at a constant current of 1.0C until the battery reached 3.0V, thereby performing 400 charge / discharge experiments, and measuring the capacity retention rate for life performance evaluation. The results are shown in Table 3.

[0117] [Table 3]

[0118]

[0119] Referring to Table 3, each of the positive active materials prepared in Examples 1 to 5 had a slightly higher initial capacity than that of Comparative Examples 1 to 5, but had significantly improved lifespan performance after 400 charge / discharge cycles.

Claims

1. A method for preparing a positive electrode active material for a secondary battery, the method comprising the following steps: preparing a lithium composite transition metal oxide containing nickel (Ni), cobalt (Co) and manganese (Mn), wherein the content of the nickel (Ni) is 60 mol % or more based on the total content of the transition metals; and dry-mixing and heat-treating the lithium composite transition metal oxide, MgF2 as a fluorine (F) coating source, and a boron (B) coating source to form a coating portion on the surface of the lithium composite transition metal oxide particles, wherein the boron (B) coating source is H3BO3 or B4C, Wherein, based on 100 parts by weight of the lithium composite transition metal oxide, 0.002 parts by weight to 0.08 parts by weight of MgF2 is mixed, The boron (B) coating source is mixed at 0.09 to 0.75 parts by weight based on 100 parts by weight of the lithium composite transition metal oxide so that the boron (B) is contained at 300 to 700 ppm based on the total weight of the positive electrode active material. 2 . The method according to claim 1 , wherein the heat treatment is performed at 200° C. to 600° C.

3. A positive electrode active material for a secondary battery, the positive electrode active material comprising: A lithium composite transition metal oxide comprising nickel (Ni), cobalt (Co), and manganese (Mn); and a coating portion formed on a surface of a particle of the lithium composite transition metal oxide, wherein the lithium composite transition metal oxide has a nickel (Ni) content of 60 mol % or more based on the total content of the transition metal, and The coating portion contains fluorine (F) and boron (B), wherein the fluorine (F) is contained in an amount of 100 ppm to 300 ppm based on the total weight of the positive electrode active material, The boron (B) is contained in an amount of 300 ppm to 700 ppm based on the total weight of the positive electrode active material. 4 . A positive electrode comprising the positive electrode active material according to claim 3 . 5 . A secondary battery comprising the positive electrode according to claim 4 .