Curable adhesive, adhesive film and bonding method thereof
By using a combination of a polyepoxy compound, a product of the addition reaction of phenolphthalein and bisphenol A diglycidyl ether, a liquid polyepoxy compound and a curing agent, the bonding of epoxy resin-based adhesives at high temperatures in the prior art is solved. The problems of reduced strength and poor peel performance are achieved by achieving good adhesion and peel performance at high temperatures.
Patent Information
- Application Number
- CN201980072693.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-10-31
- Filing Date
- 2019-10-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-10-24
AI Technical Summary
The bonding strength of existing epoxy resin-based adhesives decreases at high temperatures, and the increased cross-linking density of multifunctional solid epoxy resin affects the peeling performance.
By replacing the bisphenol A-based epoxy compound with a phenolphthalein-based epoxy compound, a polyepoxy compound including the addition reaction product of phenolphthalein and bisphenol A diglycidyl ether is prepared, and is combined with a liquid polyepoxy compound and a curing agent to form Curable compositions having elevated glass transition temperatures.
It achieves maintaining good shear and peel performance at high temperatures, improves the adhesion and thermosetting properties of the adhesive, and improves peel performance.
Smart Images

Figure BDA0003049592620000021 
Figure BDA0003049592620000022 
Figure BDA0003049592620000023
Abstract
Description
Technical Field
[0001] The present disclosure relates broadly to epoxy-based adhesives and bonding films and methods of using the same. Background Art
[0002] Epoxy resin-based adhesives are often used as bonding adhesives in applications requiring high bond strength and durability. For ease of handling and / or ease of use, the adhesive is often formulated into a curable adhesive film, also referred to in the art as a "bonding film." Bonding films that have sufficiently high adhesion and durability after curing are typically referred to as structural bonding films.
[0003] Conventional adhesive films use bisphenol A extended solid epoxy compounds or multifunctional epoxy solids, which together with liquid epoxy resins and epoxy curing agents provide the adhesive film with desired handling characteristics. However, due to the presence of bisphenol A (BPA) moieties, the glass transition temperature (T g ) decreases with increasing BPA fraction content, resulting in reduced adhesive bond strength at elevated temperatures. Excessive amounts of multifunctional solid epoxy resin in the composition will increase the crosslink density of the thermosetting system, which will affect the adhesive peeling properties. Summary of the invention
[0004] It is desirable to have new epoxy-based adhesives that exhibit good adhesion with desirable shear and peel properties at elevated temperatures. Advantageously, the curable compositions of the present disclosure achieve such properties by replacing at least some of the bisphenol A-based epoxy compound with a phenolphthalein-based epoxy compound. The resulting curable compositions, when cured, generally have an increased T relative to their bisphenol A-based counterparts. g value.
[0005] In one aspect, the present disclosure provides a curable composition comprising, based on the total weight of the curable composition:
[0006] a) 1 to 65 weight percent of a polyepoxide comprising an addition reaction product of phenolphthalein and bisphenol A diglycidyl ether; and
[0007] b) 5 to 50 wt. % of a liquid polyepoxide, wherein the liquid polyepoxide does not contain component a); and
[0008] c) an effective amount of a curing agent for curing the curable composition.
[0009] In another aspect, the present disclosure provides a curable adhesive film including the curable composition according to the present disclosure.
[0010] In another aspect, the present disclosure provides a method of bonding a curable adhesive film to a substrate, the method comprising bringing the curable adhesive film according to the present disclosure into close contact with the substrate, and at least partially curing the curable adhesive film.
[0011] As used herein,
[0012] The terms "liquid" and "solid" refer to the physical state of matter at 20°C; and
[0013] The term "polyepoxide" refers to a compound having at least two monovalent epoxy groups as shown below;
[0014]
[0015] Bisphenol A has the structural formula shown below:
[0016]
[0017] Phenolphthalein has the structural formula shown below:
[0018]
[0019]
[0026] A further understanding of the features and advantages of the present disclosure will be achieved upon consideration of the detailed description and the appended claims. DETAILED DESCRIPTION
[0020] The curable composition comprises, based on the total weight of the curable composition:
[0021] 1 wt % to 65 wt %, preferably 5 wt % to 65 wt %, more preferably 20 wt % to 55 wt %, and more preferably 25 wt % to 45 wt % of a liquid polyepoxide;
[0022] 5 to 50 wt %, preferably 10 to 40 wt %, and more preferably 10 to 30 wt % of a polyepoxide comprising an addition reaction product of phenolphthalein and bisphenol A diglycidyl ether; and
[0023] An effective amount, typically 0.001 wt % to 50 wt %, preferably 0.1 wt % to 45 wt %, and more preferably 5 wt % to 40 wt % of a curing agent (which may include one or more curing agents) is used to cure the curable composition.
[0024] The components of the curable composition listed above may total less than 100% of the total weight of the curable composition, with the difference being made up of other optional components. Exemplary optional components include thixotropes, fillers, thermoplastic polymers, toughening agents (e.g., core-shell rubber particles), monofunctional epoxides, colorants, light stabilizers, antioxidants, surfactants, plasticizers / toughening agents, and antimicrobial agents.
[0025] The liquid polyepoxide may include one or more liquid polyepoxides. They may have two, three, four, five, six, seven, eight or more monovalent epoxy groups. Examples include: 1,4-butanediol diglycidyl ether; neopentyl glycol diglycidyl ether; bisphenol A diglycidyl ether; 1,4-cyclohexanedimethanol diglycidyl ether; polyoxypropylene glycol diglycidyl ether; 1,3-propylene glycol diglycidyl ether; ethylene glycol diglycidyl ether; trimethylolpropane triglycidyl ether; and pentaerythritol tetraglycidyl ether. Liquid polyepoxides are widely available from commercial sources. Exemplary liquid polyepoxides include: diglycidyl ethers of bisphenol A, such as, for example, Epon Resin 825, Epon Resin 826, Epon Resin 827, Epon Resin 828, Epon Resin 830, Epon Resin 834, Epon Resin 862, and Epon Resin 863 available from Momentive Specialty Chemicals, Columbus, Ohio, and DER 330, DER 330-EL, DER 331-EL, DER 331 LS, and DER 332 available from Olin Corporation, Clayton, Missouri; diglycidyl ethers of bisphenol F, such as DER 354 available from Olin Corp.; and combinations of the foregoing.
[0026] The polyepoxide comprising the addition reaction product of phenolphthalein and bisphenol A diglycidyl ether can be prepared according to the procedure contained in Preparation 1 described in the Examples section herein. In one embodiment, the addition reaction product comprises a compound having the following structural formula:
[0027]
[0028] Briefly, the reaction of phenolphthalein with bisphenol A diglycidyl ether can be accomplished by combining phenolphthalein with bisphenol A diglycidyl ether under conditions (e.g., at a temperature in the range of 165° C. to 180° C. in the presence of ethyltriphenylphosphonium acetate catalyst for 3 hours), wherein the phenolphthalein OH group on one phenolphthalein molecule condenses with one glycidyl group on each of two bisphenol A diglycidyl ether molecules.
[0029] Thus, the stoichiometric ratio of bisphenol A diglycidyl ether to phenolphthalein typically should be at least 2 moles of bisphenol A diglycidyl ether per mole of phenolphthalein, preferably at least 2.3 moles of bisphenol A diglycidyl ether per mole of phenolphthalein, or even at least 2.5 moles of bisphenol A diglycidyl ether per mole of phenolphthalein, but even using a ratio of less than 2 will produce some desired compounds.
[0030] For example, any curing agent capable of curing a glycidyl ether-based epoxy resin may be included as a curing agent. The term curing agent refers to one or more reactive components capable of reacting with and / or polymerizing epoxy functional groups. Preferably, the curing agent comprises a latent curing agent activated by heating (e.g., heating to at least 40° C., at least 50° C., or even at least 60° C.) and / or by exposure to actinic radiation (e.g., visible light and / or ultraviolet light).
[0031] Examples of suitable curing agents include guanidine, substituted guanidine, substituted urea, melamine resin, guanamine derivatives, blocked polyamines, aromatic polyamines, and / or mixtures thereof. The curing agent may participate stoichiometrically in the curing reaction; however, it may also be catalytically active. Examples of suitable substituted guanidines are methylguanidine, dimethylguanidine, trimethylguanidine, tetramethylguanidine, methylisobiguanide, dimethylisobiguanide, tetramethylisobiguanide, hexamethylisobiguanide, heptamethylisobiguanide and cyanoguanidine (dicyandiamide). Examples of suitable guanamine derivatives that may be mentioned are alkylated benzoguanamine resins, benzoguanamine resins or methoxymethylethoxymethylbenzoguanamine.
[0032] Exemplary curing agents also include substituted imidazoles (e.g., 1-N-substituted imidazoles and 2-C-substituted imidazoles, and imidazole metal salts as described in U.S. Pat. No. 4,948,449 (Tarbutton et al.)), substituted ureas, substituted hydrazides (e.g., aminodihydrazide, adipic acid dihydrazide, isophthalic acid hydrazide), substituted guanidines (e.g., tetramethylguanidine), primary and / or secondary polyamines, diaminodiaryl sulfones (diaminodiphenyl sulfone), and combinations thereof.
[0033] Additional examples of suitable curing agents include monomeric and oligomeric amine-functionalized polyarylenes, wherein between the arylenes are simple covalent bonds such as in diaminodiphenyl, or linking groups selected from alkylene groups of 1 to 8 carbon atoms, ethers, sulfones, ketones, carbonates, carbonyls, carboxylates, carboxamides, and combinations thereof. Examples include 3,3′-diaminodiphenyl sulfone and 4,4′-diaminodiphenyl sulfone.
[0034] Commercially available curing agents include, for example, ANCAMINE CG-1400 micronized dicyandiamide, available from Air Products and Chemicals Incorporated, Allentown, Pennsylvania; CUREZOL 2PHZ-S and CUREZOL 2MA-OK, also available from Air Products and Chemicals; ARADUR 3123, available from Huntsman Advanced Materials, The Woodlands, Texas; and OMICURE U-35 and OMICURE U-52, available from CVC Thermoset Specialties, Moorestown, New Jersey.
[0035] Optionally, based on the gross weight of curable composition, at least one thermoplastic polymer can be typically included in curable composition according to the present disclosure with an amount of 0.01 wt % to 10 wt %, preferably 0.5 wt % to 7 wt %, but other amounts can also be used. Suitable thermoplastic examples include polyoxazoline, polyamide, polysulfone, polycarbonate, polyester, polyurethane, polyetherketone (PEK), polyacrylate, polyarylether, polyphenylene oxide (PPO), polyphenylene sulfide (PPS) and combinations thereof. Thermoplastic polymer can contribute to reducing sagging, and its presence also contributes to reducing the shrinkage of the cured composition and improving the toughness of the cured composition.
[0036] The curable composition may include fillers (e.g., fibers and / or particles) in an amount typically of 0.01% to 60% by weight, preferably 1% to 50% by weight, and more preferably 5% to 40% by weight, but other amounts may also be used. Exemplary fillers include quartz glass, glass beads, glass bubbles, and glass fibers; silicates such as talc, clay, (montmorillonite) feldspar, mica, calcium silicate, calcium metasilicate, sodium aluminosilicate, sodium silicate; metal sulfates such as calcium sulfate, barium sulfate, sodium sulfate, sodium aluminum sulfate, aluminum sulfate; gypsum; vermiculite; wood flour; aluminum trihydrate; carbon black; alumina; titanium dioxide; cryolite; cone cryolite; and metal sulfites such as calcium sulfite. In some embodiments, the filler includes an inorganic filler having a density of at least 2 g / cm3. Exemplary such fillers include most metal particles (e.g., aluminum powder).
[0037] In some embodiments, based on the total weight of the curable composition, the curable composition includes 1 wt % to 35 wt % of a core-shell particle toughening agent. Each core-shell particle includes an elastomeric core and a polymer shell layer disposed on the elastomeric core. Examples include grades such as EXL-2691, EXL-3300, EXL-2300 / 3300, EXL-2330, EXL-2650J, and core-shell impact modifiers of combinations thereof obtained from Dow Chemical, Midland, Michigan, as PARALOID EXL. Core-shell particles pre-dispersed in liquid epoxy resins or solid epoxy resins may also be used, and exemplary types may be purchased from Kaneka Texas Corporation of Pasadena, Texas, as MX-type resins.
[0038] Any suitable technique such as calendering, pressing, molding, hot melt coating and solvent casting can be used to convert the curable composition into a curable adhesive film. The curable adhesive film can be in the form of, for example, an adhesive tape, a sheet or a gasket. Optionally, a scrim can be included in the curable adhesive film according to the present disclosure.
[0039] In some embodiments, the curable adhesive film is tacky, and in some cases, the curable adhesive film is a pressure sensitive adhesive, optionally paired with a suitable release liner.
[0040] The curable compositions and curable adhesive films according to the present disclosure can be used, for example, to bond to at least one substrate, preferably to bond two substrates together. Examples of suitable substrates include metals, plastics, glass, ceramics, bricks, composite materials (e.g., graphite fiber composite materials).
[0041] Selected Embodiments of the Disclosure
[0042] In a first embodiment, the present disclosure provides a curable composition comprising the following components, based on the total weight of the curable composition:
[0043] a) 1 to 65 weight percent of a polyepoxide comprising an addition reaction product of phenolphthalein and bisphenol A diglycidyl ether; and
[0044] b) 5 to 50 wt. % of a liquid polyepoxide, wherein the liquid polyepoxide does not contain component a); and
[0045] c) an effective amount of a curing agent for curing the curable composition.
[0046] In a second embodiment, the present disclosure provides a curable composition according to the first embodiment, wherein the components further comprise, based on the total weight of the curable composition:
[0047] d) 0.01 to 10% by weight of a thermoplastic polymer.
[0048] In a third embodiment, the present disclosure provides a curable composition according to the first embodiment or the second embodiment, wherein the components further comprise, based on the total weight of the curable composition:
[0049] e) 0.01 to 50% by weight of filler particles.
[0050] In a fourth embodiment, the present disclosure provides a curable composition according to any one of the first to third embodiments, wherein the addition reaction product of phenolphthalein and bisphenol A diglycidyl ether is present in an amount of 10 wt % to 40 wt %, based on the total weight of the curable composition.
[0051] In a fifth embodiment, the present disclosure provides a curable composition according to any one of the first to fourth embodiments, wherein the curing agent comprises dicyandiamide.
[0052] In a sixth embodiment, the present disclosure provides a curable composition according to any one of the first to fifth embodiments, wherein the curing agent is present in an amount of 0.01 wt % to 40 wt % based on the total weight of the curable composition.
[0053] In a seventh embodiment, the present disclosure provides a curable composition according to any one of the first to sixth embodiments, wherein the components further comprise:
[0054] f) Core-shell particles, wherein each core-shell particle comprises an elastomeric core and a polymeric shell layer disposed on the elastomeric core.
[0055] In an eighth embodiment, the present disclosure provides a curable composition according to the seventh embodiment, wherein the core-shell particles are present in an amount of 1 wt % to 35 wt %, based on the total weight of the curable composition.
[0056] In a ninth embodiment, the present disclosure provides a curable composition according to any one of the first to eighth embodiments, wherein the components further comprise:
[0057] g) an inorganic filler having a density of at least 2 g / cm3.
[0058] In a tenth embodiment, the present disclosure provides a curable composition according to the ninth embodiment, wherein the inorganic filler comprises aluminum powder.
[0059] In an eleventh embodiment, the present disclosure provides a curable composition according to the ninth embodiment or the tenth embodiment, wherein the inorganic filler is present in an amount of 5 to 40 weight percent based on the total weight of the curable composition.
[0060] In a twelfth embodiment, the present disclosure provides a curable adhesive film comprising the curable composition according to any one of the first to eleventh embodiments. Preferably, the curable adhesive film is self-supporting.
[0061] In a thirteenth embodiment, the present disclosure provides a curable adhesive film according to the twelfth embodiment, wherein the curable adhesive film is tacky.
[0062] In a fourteenth embodiment, the present disclosure provides a curable adhesive film according to the twelfth embodiment or the thirteenth embodiment, wherein the curable adhesive film is a pressure sensitive adhesive.
[0063] In a fifteenth embodiment, the present disclosure provides a method of bonding a curable adhesive film to a substrate, the method comprising:
[0064] bringing the curable adhesive film according to any one of the twelfth to fourteenth embodiments into close contact with a substrate; and
[0065] The curable adhesive film is at least partially cured.
[0066] Objects and advantages of this disclosure are further illustrated by the following non-limiting examples, but the particular materials and amounts thereof recited in these examples, as well as other conditions and details, should not be construed to unduly limit this disclosure.
[0067] Example
[0068] Unless otherwise indicated, all parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight.
[0069] Table 1 below lists the names and materials used in the Examples.
[0070] Table 1
[0071]
[0072]
[0073] Test Method :
[0074] 2024T3 grade bare aluminum panels were obtained from Erickson Metals of Minnesota, Inc., Coon Rapids, Minnesota. Prior to bonding with the structural adhesive, the panels were subjected to the following surface preparation process:
[0075] The bare aluminum panels were immersed in OAKITE 165 caustic cleaning solution at 85°C for 10 minutes. The panels were then immersed in tap water at 21°C for 10 minutes, followed by a continuous jet rinse with tap water for about 3 minutes. The panels were then immersed in Forest Products Laboratory (FPL) etching solution at 66°C for 10 minutes, after which the panels were jet rinsed with water at 21°C for about 3 minutes, allowed to drip dry for an additional 10 minutes, and then dried in an oven at 54°C for 30 minutes. The etched panels were then anodized in an 85% phosphoric acid bath at 22.2°C at 15 volts and 100 amps maximum current for about 25 minutes, rinsed with water at 21°C for about 3 minutes, allowed to drip dry for an additional 10 minutes, and then dried in an oven at 66°C for 10 minutes. Within 24 hours of anodizing, the aluminum panels were treated with a corrosion inhibiting primer obtained from 3M Company as SCOTCH-WELD STRUCTURAL ADHESIVE PRIMER, EC-3917, according to the manufacturer's instructions. The dry primer thickness was between 0.1-0.2 mils (2.5-5.1 microns).
[0076] Overlap Shear Test (OST) of Adhesive Films
[0077] Primed panels of 2024-T3 bare aluminum measuring 10.16 cm x 17.78 cm x 0.16 cm (4 inches long x 7.0 inches x 0.063 inches) were prepared for testing as described above. The primed panels were bonded to one another in overlapping relationship along their longitudinal dimension. After removing the liner from one side, an exemplary adhesive film was applied manually using a small rubber roller in such a manner as to exclude entrapped air and ensure intimate contact between the exposed adhesive and the test panel substrate. After removing the second liner, the resulting assembly was fastened together using tape and cured in an autoclave (referring to the Adhesive Curing Cycle Method defined below). The bonded panels were sawn across their width into 2.54 cm (1 inch) wide strips and evaluated for overlap shear strength using a tensile tester in accordance with ASTM D1002-05 "Standard Test Method for Apparent Shear Strength of Single-Lap-Joint Adhesively Bonded Metal Specimens by Tension Loading (Metal-to-Metal)" using a grip separation rate of 0.05 in / min (1.3 mm / min). Seven test panels were prepared and evaluated (one for each example).
[0078] Floating Roll Peel (FRP) Strength Testing of Adhesive Films
[0079] Primed panels of 2024-T3 bare aluminum measuring 20.3 cm x 7.6 cm x 0.16 cm (8.0 in x 3.0 in x 0.063 in) and 25.4 cm x 7.6 cm x 0.064 cm (10 in x 3 in x 0.025 in) were prepared for testing as described above. After removing the liner from one side, the exemplary adhesive film was applied manually using a small rubber roller in such a way as to exclude entrapped air and ensure close contact between the exposed adhesive and the test panel substrate. The primed panels were bonded together and cured in an autoclave (referring to the adhesive cure cycle method defined below), and then the floating roller peel strength was evaluated according to ASTM D3167-76 "Standard Test Method for Floating Roller Peel Resistance of Adhesives", with the following modifications. Test strips measuring 1.27 cm (0.5 in) wide were cut along the longitudinal direction of the bonded aluminum panels. A tensile tester operating at a rate of 30.5 cm / minute (6 inches / min) was used to peel the thinner substrate from the thicker substrate, and the results were normalized to a width of 2.54 cm (1 inch).Seven test panels were prepared and evaluated (one for each example).
[0080] Adhesive curing cycle
[0081] The bonded samples using the film adhesive prepared in the present invention were vacuum bagged to approximately 28 inches of mercury pressure (94.8 kPa) in an autoclave, model ECONOCLAVE 3x5, obtained from ASC Process Systems, Sylmar, California. The autoclave pressure was raised to 45 psi (310.3 kPa), during which the vacuum bag was vented to the atmosphere once the autoclave pressure exceeded 15 psi (103.4 kPa). The autoclave temperature was then raised to 350°F (177°C) at a rate of 4.5°F (2.5°C) / minute. After reaching the set point, the sample was held at this temperature for 60-90 minutes and then cooled to 72°F (22.2°C) at a rate of 5°F (2.8°C) / minute before releasing the pressure.
[0082] Preparation Example 1
[0083] Phenolphthalein (127.5 grams (g)) was added to a three-necked flask containing 300 g of EPON 828 at 100 ° C. Then 1.0 grams of ETPPAC catalyst was added. The mixture was heated to 130 ° C to 140 ° C under stirring, and the exothermic process was monitored and the temperature was controlled so that it did not reach above 180 ° C. After the exothermic process subsided, the reaction was continued at 165 ° C to 180 ° C for another 2 to 3 hours under stirring. The reaction mixture was cooled to 130 ° C to 150 ° C and then discharged. The product is designated as PI epoxy resin and is used in adhesives.
[0084] Examples 1-6 and Comparative Example A
[0085] These examples were prepared according to the following sequential steps.
[0086] Step 1-Pre-reaction of ATPES and epoxy resin :
[0087] EPON 828, MY-9655, PI epoxy resin, TACTIX 742, SU 8 and other values were combined in the amounts shown in Table 2 and melted together at 149°C (300°F). After the mixture was melted, ATPES was added and stirring was continued at 149°C (300°F) until the ATPES was dissolved. The mixture was kept for 1 to 3 hours to allow the amine groups to react with the epoxy groups.
[0088] Step 2 - Premixing of PKHP-200 and epoxy resin :
[0089] EPON 828, MY-9655, PI epoxy resin, TACTIX 742, SU 8 and other values were combined in the amounts shown in Table 2 and melted together at 149°C (300°F). After the mixture was melted, PKHP 200 was added and stirring was continued at 149°C (300°F) until PKHP200 was dissolved.
[0090] Step 3 :
[0091] After step 1 or step 2 reaches the desired level, add the other remaining epoxy resin component (e.g., MX-257) and mix thoroughly in the amount shown in Table 2. Add fumed silica (R816) in the amount shown in Table 2 and disperse using a high-speed mixer. After thorough mixing, add aluminum powder in the amount shown in Table 2 along with the curing agent (in the amount determined in Table 2) and mix using a high-speed mixer (mixing time is limited to no more than three minutes, and care is taken to ensure that the mixture is not overheated during mixing).
[0092] Step 4 :
[0093] The mixture from step 3 was immediately used to stretch a film on a silicone coated liner.For each of the examples listed in Table 2 below, a film adhesive was obtained.
[0094] Table 2
[0095]
[0096] The overlap shear and floating roll peel test results for Examples 1 to 6 and Comparative Example A are shown in Table 3 below.
[0097] Table 3
[0098]
[0099] All references, patents and patent applications cited in the above patent applications are incorporated herein by reference in their entirety in a consistent manner. In the event of inconsistency or conflict between the incorporated references and the present application, the information in the foregoing description shall prevail. The foregoing description, which is given to enable a person of ordinary skill in the art to practice the present disclosure protected by the claims, should not be construed as limiting the scope of the present disclosure, which is defined by the claims and all equivalents thereof.
Claims
1. A curable composition, comprising the following components based on the total weight of the curable composition: a) 10 to 30 wt % of a polyepoxide, wherein the polyepoxide is an addition reaction product of phenolphthalein and bisphenol A diglycidyl ether, wherein the addition reaction product of phenolphthalein and bisphenol A diglycidyl ether is a compound having the following structural formula: and b) 25% to 45% by weight of a liquid polyepoxide, wherein the liquid polyepoxide does not contain component a); and c) an effective amount of a curing agent for curing the curable composition.
2. The curable composition according to claim 1, wherein the component further comprises, based on the total weight of the curable composition: d) 0.01 to 10% by weight of a thermoplastic polymer.
3. The curable composition according to claim 1, wherein the component further comprises, based on the total weight of the curable composition: e) 0.01 to 50% by weight of filler particles.
4. The curable composition of claim 1, wherein the curing agent comprises dicyandiamide. 5 . The curable composition of claim 1 , wherein the curing agent is present in an amount of 0.01 wt % to 40 wt % based on the total weight of the curable composition.
6. The curable composition according to claim 1, wherein the components further comprise: f) Core-shell particles, wherein each core-shell particle comprises an elastomeric core and a polymeric shell layer disposed on the elastomeric core.
7. The curable composition of claim 6, wherein the core-shell particles are present in an amount of 1 wt% to 35 wt%, based on the total weight of the curable composition.
8. The curable composition according to claim 1, wherein the components further comprise: g) an inorganic filler having a density of at least 2 g / cm3.
9. The curable composition of claim 8, wherein the inorganic filler comprises aluminum powder.
10. The curable composition of claim 9, wherein the inorganic filler is present in an amount of 5 to 40 wt%, based on the total weight of the curable composition. 11 . A curable adhesive film comprising the curable composition according to claim 1 .
12. The curable adhesive film of claim 11, wherein the curable adhesive film is tacky.
13. The curable adhesive film of claim 11, wherein the curable adhesive film is a pressure sensitive adhesive.
14. A method of bonding a curable adhesive film to a substrate, the method comprising: bringing the curable adhesive film according to claim 11 into close contact with the substrate; as well as The curable adhesive film is at least partially cured.
Citation Information
Patent Citations
Diorthosubstituted benzene derivatives, especially for use in a method of therapy, processes for their preparation, and pharmaceutical compositions containing them
EP0000826A1
Floor drainage gully for wet areas
EP0000862A1
Epoxy resin composition
US4948449A
Copolymer of bisphenol diglycidyl ether and phenolphthalene and / or phenolphthalimidine, method for preparation thereof, article comprising copolymer, and compositions comprising copolymer
CN105940037A
Epoxy resin, epoxy resin composition, hardened product and laminate sheet for electric / electronic circuit
JP2015199931A