Electrode material, preparation method and application thereof, and assembled water electrolysis device
By forming a nitrogen-doped cobalt oxyfluoride nanoarray structure on a carbon cloth electrode, the problem of high cost and poor stability of precious metal catalysts is solved, efficient water splitting under non-acidic or alkaline conditions is achieved, and electrocatalytic decomposition is promoted. Practical implementation of water technology.
Patent Information
- Application Number
- CN202110213236.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-25
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-02-25
AI Technical Summary
In existing water electrolysis technology, the high cost and scarcity of precious metal catalysts limit the wide application of water splitting. Especially under non-acidic or alkaline conditions, the stability and efficiency of non-noble metal catalysts cannot meet the demand.
Nitrogen-doped cobalt oxyfluoride is used as the electrocatalyst, and a nanoarray structure is formed on the carbon cloth electrode substrate through electrochemical deposition and gas-phase chemical conversion reaction. Combined with nitrogen plasma treatment, an electrode with efficient hydrogen evolution and oxygen evolution activity is prepared. Material.
In alkaline and neutral electrolytes, nitrogen-doped cobalt oxyfluoride electrode materials show good stability and efficient water splitting capabilities, achieving electrocatalytic water splitting with greater current density and lower applied potential, which is better than Traditional precious metal catalysts.
Smart Images

Figure CN113026031B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrocatalytic water decomposition, and in particular to an electrode material, a preparation method and application thereof, and an assembled water electrolysis device. Background Art
[0002] The global energy crisis and its related environmental issues have prompted scientists to search for renewable energy sources that can replace fossil fuels. Driven by nature, available resources such as solar or wind power generation and water splitting technology provide an attractive way - water electrolysis, which produces hydrogen (H2) and oxygen (O2) from water through hydrogen evolution reaction (HER) and oxygen evolution reaction (OER). This energy conversion technology has attracted widespread attention due to its high energy conversion efficiency, zero environmental pollution emissions, and potential wide applications.
[0003] In fact, water electrolyzers require effective catalysts to promote both reactions. Currently, Pt group metals are the most effective catalysts for HER, while the benchmark catalysts for OER are Ir / Ru-based compounds. However, the high cost and scarcity of these metals limit their widespread use. Therefore, it has become very important to develop non-precious and efficient electrocatalysts for water decomposition. Scientists have currently developed relevant non-precious metal electrocatalysts, including transition metal sulfides, carbides and phosphides for HER; transition metal phosphates, oxides and hydroxides for OER. However, catalysts for HER and OER must operate under the same conditions and can be used together for water decomposition. In addition, in order to minimize the overpotential of the electrolysis system, water decomposition is mostly carried out in strong acid or alkaline solutions. However, such conditions pose a challenge to most non-precious metal water decomposition catalysts.
[0004] Therefore, the study of electrode materials with new non-precious metal water-splitting catalysts is of great significance for improving the performance of water electrolysis systems.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The object of the present invention is to provide an electrode material and a preparation method and application thereof, as well as an assembled water electrolysis device, so as to improve the above-mentioned technical problems.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides an electrode material, which includes an electrode substrate and an electrocatalyst located on the surface of the electrode substrate, wherein the electrocatalyst is nitrogen-doped cobalt fluoride oxide.
[0009] Optionally, the cobalt oxyfluoride is a nanoarray.
[0010] Optionally, the electrode substrate is carbon cloth.
[0011] In a second aspect, the present invention further provides a method for preparing the above-mentioned electrode material, which comprises: forming nitrogen-doped cobalt fluoride oxide on the surface of an electrode substrate.
[0012] Optionally, the preparation method comprises: fluorinating an electrode material precursor and then nitrogen doping the electrode material precursor, wherein the electrode material precursor comprises an electrode substrate and a cobalt nanoarray precursor on the surface of the electrode substrate. Optionally, the cobalt nanoarray precursor is a Co(OH)2 nanosheet array.
[0013] Optionally, the electrode material precursor and NH4F powder are subjected to a gas phase chemical conversion reaction at a temperature of 200 to 500° C., preferably 400° C.; preferably, the reaction time is 1 to 4 hours.
[0014] Optionally, the electrode material precursor and NH4F powder react under an inert atmosphere. Preferably, the temperature is increased to a reaction temperature at 8-12°C / min in the inert atmosphere. Preferably, the inert atmosphere is a N2 atmosphere.
[0015] Optionally, nitrogen doping is to treat the fluorinated electrode material in a N2 plasma reactor. Preferably, the power of the N2 plasma reactor is 60-200 W, preferably 200 W, the treatment time is 0.5-5 min, preferably 50-70 s, more preferably 60 s, and N2 is pumped into the N2 plasma reactor at a flow rate of 1.5-2.5 mL / min, preferably 2 mL / min, until the pressure drops to 0.2-0.3 Pa.
[0016] Optionally, the electrode material precursor is mainly prepared by the following steps: using the electrode substrate as the working electrode, performing an electrochemical deposition reaction in an electrolyte of a cobalt salt solution, and growing a cobalt nanoarray precursor on the surface of the electrode substrate.
[0017] Optionally, the electrochemical deposition adopts a three-electrode system, with carbon cloth as the working electrode, a saturated calomel electrode as the reference electrode, and a cobalt nitrate solution as the electrode solution, wherein the concentration of the cobalt nitrate solution is 0.1 to 3 mol / L.
[0018] Optionally, the voltage of the electrochemical deposition is -0.8 to -1.2 V, preferably -1 V, and the time is 5 to 20 min.
[0019] Optionally, the preparation method of the electrode material further comprises washing and drying the electrode material precursor obtained after electrochemical deposition in sequence; preferably, washing is ultrasonic washing with deionized water and ethanol in sequence; the drying temperature is 50-80°C and the drying time is 2-10 hours.
[0020] Optionally, the method for preparing the electrode material further comprises sequentially cooling, washing and drying the electrode material after gas phase chemical conversion. Preferably, the washing is sequentially ultrasonically washing with deionized water and ethanol; the drying temperature is 50 to 80° C., and the drying time is 2 to 10 hours.
[0021] In a third aspect, the present invention further provides an anode or a cathode, wherein the anode or the cathode is prepared from the above-mentioned electrode material.
[0022] In a fourth aspect, the present invention further provides an assembled water electrolysis device, wherein the positive electrode material and the negative electrode material of the assembled water electrolysis device are both the above-mentioned electrode materials.
[0023] In a fifth aspect, the present invention also provides the use of the above-mentioned electrode material in electrolysis of water.
[0024] The technical solution of the present invention has the following beneficial effects: the electrode material with nitrogen-doped cobalt fluoride oxide as the electrocatalyst has good hydrogen evolution and oxygen evolution activity in both alkaline and neutral electrolytes when used as the positive electrode and the negative electrode, and has good stability, and can efficiently achieve complete water splitting, thereby promoting the development of electrocatalytic water splitting towards the practical direction of higher current density and lower applied potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 This is a SEM image of the electrode material NCoFO / CC prepared in Example 1;
[0027] Figure 2 TEM image of the electrode material NCoFO / CC prepared in Example 1;
[0028] Figure 3 This is the EDS image of the electrode material NCoFO / CC prepared in Example 1;
[0029] Figure 4 Comparative images of hydrogen evolution of different electrode materials in Example 1 and Comparative Examples 1-4;
[0030] Figure 5 Comparative images of oxygen evolution of different electrode materials in Example 1 and Comparative Examples 1-4;
[0031] Figure 6 The AC impedance spectroscopy images of different electrode materials prepared in Comparative Example 2 and Example 1;
[0032] Figure 7 This is a stability image of the electrode material prepared in Example 1;
[0033] Figure 8 The overall water splitting performance image of the assembled water electrolysis device assembled with the electrode materials prepared in Example 1;
[0034] Fig. 9 This is an image of the overall water splitting stability of the assembled water electrolysis device assembled with the electrode materials prepared in Example 1. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0036] The following is a detailed description of an electrode material provided by the present invention, a preparation method and application thereof, and an assembled water electrolysis device.
[0037] Some embodiments of the present invention provide an electrode material, which includes an electrode substrate and an electrocatalyst located on the surface of the electrode substrate, wherein the electrocatalyst is nitrogen-doped cobalt fluoride oxide.
[0038] Through extensive practice and research, the inventors have found that the electrode material with nitrogen-doped cobalt fluoride oxide as the electrocatalyst has good hydrogen and oxygen evolution activity in both alkaline and neutral electrolytes when used as the positive electrode and the negative electrode, and has good stability.
[0039] Specifically, in some embodiments, in order to achieve a better catalytic effect of the electrode material, the cobalt fluoride oxide is a nanoarray, that is, the electrocatalyst is attached to the surface of the electrode substrate in a nanoarray. In addition, the electrocatalyst is preferably formed by growth on the surface of the electrode substrate.
[0040] In some embodiments, the electrode substrate is carbon cloth (CC).
[0041] Some embodiments of the present invention also provide a method for preparing the above-mentioned electrode material, which comprises: forming nitrogen-doped cobalt fluoride oxide on the surface of an electrode substrate.
[0042] Specifically, the preparation method comprises:
[0043] S1. An electrochemical deposition reaction is carried out in an electrolyte of a cobalt salt solution using an electrode substrate as a working electrode to grow a cobalt nanoarray precursor on the surface of the electrode substrate to obtain an electrode material precursor.
[0044] Specifically, in some embodiments, the electrochemical deposition adopts a three-electrode system, with carbon cloth as the working electrode, saturated calomel electrode as the reference electrode, and cobalt nitrate solution as the electrode liquid, and the concentration of the cobalt nitrate solution is 0.1-3 mol / L, for example, the concentration of cobalt nitrate is 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L, etc. That is, the cobalt nanoarray precursor is a Co(OH)2 nanosheet array. It should be noted that in its embodiment, the electrode and the electrolyte can also be selected from other substances, as long as the growth of the cobalt nanodisplay precursor can be achieved, for example, the electrolyte can also be selected from cobalt chloride solution, etc.
[0045] In some embodiments, the voltage of electrochemical deposition is -0.8 to -1.2 V, such as -0.9 V, -1 V or -1.1 V, etc., preferably -1 V, and the time is 5 to 20 min, such as 5 min, 6 min, 7 min, 9 min, 11 min, 13 min, etc., preferably 5 min.
[0046] In some embodiments, in order to remove impurities and unreacted substances on the surface of the electrode material precursor, the method for preparing the electrode material also includes washing and drying the electrode material precursor obtained after electrochemical deposition in sequence; preferably, washing is ultrasonic washing using deionized water and ethanol in sequence; the drying temperature is 50 to 80°C, and the time is 2 to 10 hours.
[0047] S2. subjecting the electrode material precursor to a gas phase chemical conversion reaction to obtain a fluorinated electrode material.
[0048] Specifically, in some embodiments, the electrode material precursor and NH4F powder are subjected to a gas phase chemical conversion reaction at a temperature of 200 to 500° C., preferably 400° C., to obtain a secondary precursor. The reaction time may be 1 to 4 hours, for example, 1 hour, 2 hours, 3 hours or 4 hours, preferably 1 hour.
[0049] In some embodiments, during the above reaction, the mass of ammonium fluoride added may be 1 to 4 g, for example, 1.5 g.
[0050] In order to ensure that the electrode material precursor can generate fluorine-containing oxide at the above temperature, in some embodiments, the electrode material precursor and NH4F powder are reacted under an inert atmosphere to avoid the influence of air on the reaction process.
[0051] Furthermore, in order to enable the cobalt nanoarray precursor to stably generate a cobalt oxide coating and to combine well with the electrode substrate, in some embodiments, the reaction process is to heat up to the reaction temperature at 8 to 12°C / min under an inert atmosphere, and then react for 1 to 4 hours. In some embodiments, the inert atmosphere may be a N2 atmosphere. In some other embodiments, an argon atmosphere may also be selected as needed.
[0052] S3. Perform nitrogen doping treatment on the fluorinated electrode material in an N2 plasma reactor.
[0053] Specifically, in order to achieve better doping effect and doping ratio, in some embodiments, the power of the N2 plasma reactor is 60-200 W, for example, 80 W, 90 W, 100 W, 110 W, 120 W, 150 W, 160 W, 170 W, 180 W, 190 W or 200 W, etc., preferably 150-200 W, more preferably 200 W, the processing time is 0.5-5 min, preferably 50-70 s, more preferably 60 s, and N2 is pumped into the N2 plasma reactor at a flow rate of 1.5-2.5 mL / min, preferably 2 mL / min, until the pressure drops to 0.2-0.3 Pa.
[0054] In some embodiments, in order to further control the quality of the electrode material, the preparation method of the electrode material further includes sequentially cooling, washing and drying the electrode material after the gas phase chemical conversion. Specifically, the washing can be sequentially ultrasonically washed with deionized water and ethanol; the drying temperature is 50 to 80° C. and the drying time is 2 to 10 hours.
[0055] Some embodiments of the present invention further provide an anode or a cathode, wherein the anode or the cathode is prepared from the above-mentioned electrode material.
[0056] Some embodiments of the present invention further provide an assembled water electrolysis device, wherein the positive electrode material and the negative electrode material of the assembled water electrolysis device are both the above-mentioned electrode materials.
[0057] Some embodiments of the present invention also provide use of the above electrode material in electrolysis of water.
[0058] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0059] Example 1
[0060] This embodiment provides a method for preparing an electrode material, which specifically includes:
[0061] First, uniformly grown Co(OH)2 nanosheets on a carbon cloth (CC) substrate were obtained by electrochemical deposition. Specifically, a piece of carbon cloth (about 1cm*2cm) was cleaned with acetone, ethanol and deionized water in sequence. Then, electrochemical deposition was performed in 30mL of 0.1M Co(NO3)2 aqueous solution in a three-electrode system with platinum as the counter electrode, saturated calomel (SCE) as the reference electrode and blank CC as the working electrode. After timing the ampere time at -1.0V (relative to SCE) for 5 minutes, the sample was washed with deionized water and dried overnight.
[0062] Secondly, the prepared Co(OH)2 / CC nanosheet array precursor and 1.5g NH4F powder were placed in a porcelain furnace with two separate positions in the furnace. The furnace was then heated to 400℃ at a rate of 10℃ / min under N2 atmosphere and maintained for 1h, and then naturally cooled to room temperature to obtain CoFO / CC material.
[0063] Then, the CoFO / CC material was treated in a N2 plasma reactor at a power of 200 W for 60 s. N2 was pumped into the reactor at a flow rate of 2 mL / min until the pressure dropped to 0.2 Pa to obtain the electrode material, namely NCoFO / CC material.
[0064] The electrode material prepared in Example 1 was observed by scanning electron microscope. Figure 1 , which shows a SEM image of the electrode material in Example 1. Figure 1 It can be seen that the electrode material is a porous nanosheet structure.
[0065] The electrode material prepared in Example 1 was observed by TEM, and the following Figure 2 TEM images shown. Figure 2 It can also be seen that the electrode material is a porous nanosheet structure.
[0066] The electrode material prepared in Example 1 was observed by EDS. Figure 3 As shown, from Figure 3 It can be seen that Co, F, O and N elements are evenly distributed in the material.
[0067] Example 2
[0068] This embodiment provides a method for preparing an electrode material, which specifically includes:
[0069] First, uniformly grown Co(OH)2 nanosheets on a carbon cloth (CC) substrate were obtained by electrochemical deposition. Specifically, a piece of carbon cloth (about 1cm*2cm) was cleaned with acetone, ethanol and deionized water in sequence. Then, electrochemical deposition was performed in 30mL of 0.1M Co(NO3)2 aqueous solution in a three-electrode system with platinum as the counter electrode, saturated calomel (SCE) as the reference electrode and blank CC as the working electrode. After timing the ampere time at -1.0V (relative to SCE) for 5 minutes, the sample was washed with deionized water and dried overnight.
[0070] Secondly, the prepared Co(OH)2 / CC nanosheet array precursor and 1.5g NH4F powder were placed in a porcelain furnace with two separate positions in the furnace. The furnace was then heated to 400℃ at a rate of 10℃ / min under N2 atmosphere and maintained for 1h, and then naturally cooled to room temperature to obtain CoFO / CC material.
[0071] Then, the CoFO / CC material was treated in a N2 plasma reactor at a power of 200 W for 30 s. N2 was pumped into the reactor at a flow rate of 2 mL / min until the pressure dropped to 0.2 Pa to obtain the electrode material, namely NCoFO / CC material.
[0072] Example 3
[0073] This embodiment provides a method for preparing an electrode material, which specifically includes:
[0074] First, uniformly grown Co(OH)2 nanosheets on a carbon cloth (CC) substrate were obtained by electrochemical deposition. Specifically, a piece of carbon cloth (about 1cm*2cm) was cleaned with acetone, ethanol and deionized water in sequence. Then, electrochemical deposition was performed in 30mL of 0.1M Co(NO3)2 aqueous solution in a three-electrode system with platinum as the counter electrode, saturated calomel (SCE) as the reference electrode and blank CC as the working electrode. After timing the ampere time at -1.0V (relative to SCE) for 5 minutes, the sample was washed with deionized water and dried overnight.
[0075] Secondly, the prepared Co(OH)2 / CC nanosheet array precursor and 1.5g NH4F powder were placed in a porcelain furnace with two separated positions in the furnace chamber. The furnace was then heated to 400℃ at a rate of 10℃ / min under N2 atmosphere and maintained for 1h, and then naturally cooled to room temperature to obtain CoFO / CC material.
[0076] Then, the CoFO / CC material was treated in a N2 plasma reactor at a power of 200 W for 90 s. N2 was pumped into the reactor at a flow rate of 2 mL / min until the pressure dropped to 0.2 Pa to obtain the electrode material, namely NCoFO / CC material.
[0077] Comparative Example 1
[0078] This comparative example provides a method for preparing an electrode material, which specifically includes:
[0079] Co(OH)2 nanosheets uniformly grown on a carbon cloth (CC) substrate were obtained by electrochemical deposition. Specifically: a piece of carbon cloth (about 1cm*2cm) was cleaned with acetone, ethanol and deionized water in turn. Then, electrochemical deposition was carried out in 30mL 0.1M Co(NO3)2 aqueous solution in a three-electrode system with platinum as the counter electrode, saturated calomel (SCE) as the reference electrode and blank CC as the working electrode. After timing the ampere time at -1.0V (relative to SCE) for 5 minutes, the material was washed with deionized water and dried overnight to obtain the electrode material, namely Co(OH)2 / CC material. Co(OH)2 / CC was calcined at 450℃ in a muffle furnace for 2h to obtain Co3O4 / CC electrode material.
[0080] Comparative Example 2
[0081] This embodiment provides a method for preparing an electrode material, which specifically includes:
[0082] First, uniformly grown Co(OH)2 nanosheets on a carbon cloth (CC) substrate were obtained by electrochemical deposition. Specifically, a piece of carbon cloth (about 1cm*2cm) was cleaned with acetone, ethanol and deionized water in sequence. Then, electrochemical deposition was performed in 30mL of 0.1M Co(NO3)2 aqueous solution in a three-electrode system with platinum as the counter electrode, saturated calomel (SCE) as the reference electrode and blank CC as the working electrode. After timing the ampere time at -1.0V (relative to SCE) for 5 minutes, the sample was washed with deionized water and dried overnight.
[0083] Secondly, the prepared Co(OH)2 / CC nanosheet array precursor and 1.5g NH4F powder were placed in a porcelain furnace with two separate positions in the furnace. The furnace was then heated to 400℃ at a rate of 10℃ / min under N2 atmosphere and maintained for 1h, and then naturally cooled to room temperature to obtain the electrode material, namely CoFO / CC material.
[0084] Comparative Example 3
[0085] This comparative example provides a blank electrode material which specifically includes: a blank electrode CC as a comparative electrode.
[0086] Comparative Example 4
[0087] This comparative example provides a blank electrode material, which specifically includes: Pt / C / as a comparative electrode. 5 mg of Pt / C catalyst is dispersed in 980 μl of ethanol and 20 μl of Nafion solution, ultrasonicated for 30 min, and 40 μl of the dispersion is coated on carbon cloth to obtain a Pt / C electrode.
[0088] Comparative Example 5
[0089] This comparative example provides a blank electrode material, which specifically includes: RuO2 as a comparative electrode. 5 mg of RuO2 catalyst is dispersed in 980 μl of ethanol and 20 μl of Nafion solution, ultrasonicated for 30 min, and 40 μl of the dispersion is coated on carbon cloth to obtain a RuO2 electrode.
[0090] Test Example 1
[0091] In this test example, the electrode materials of Example 1 and Comparative Examples 1-4 were used as cathode materials and anode materials to assemble a water electrolysis device, the cathode material and the anode material were both NCoFO / CC, and the electrolyte was 1M KOH solution, and its water electrolysis performance was tested.
[0092] The electrodes in Examples 1 to 4 and Comparative Examples 1 to 4 were tested for hydrogen evolution performance, and the results are listed in Figure 4 In. By Figure 4 It can be seen that the NCoFO / CC material in Example 1 has good hydrogen evolution performance, while the electrode materials in other examples and comparative examples have poor hydrogen evolution performance.
[0093] The electrodes in Example 1 and Comparative Examples 1-4 were tested for oxygen evolution, and the results are listed in Figure 5 In. By Figure 5 It can be seen that the NCoFO / CC material in Example 1 has good oxygen evolution performance, while the electrode materials in other examples and comparative examples have poor oxygen evolution performance.
[0094] The electrodes prepared from the electrode materials of Example 1 and Comparative Example 2 were subjected to EIS tests, and the results are listed in Figure 6 In. By Figure 6 It can be seen that the NCoFO / CC material in Example 1 has good electron transport capability, while the CoFO / CC material in Comparative Example 2 has poor electron transport capability.
[0095] The cycling performance image of the electrode material in Example 1 is shown in Figure 7 In. By Figure 7It can be seen that the voltage curve of the NCoFO / CC material in Example 1 has almost no change after the 10,000 s test, so its stability is excellent.
[0096] The LSV curve of the assembled water electrolysis device prepared by the electrode material of Example 1 is as follows: Figure 8 As shown, from Figure 8 It can be seen that at 10 mA cm -2 NCoFO / CC material has a smaller overpotential at a discharge density of .
[0097] The stability test diagram of the assembled water electrolysis device prepared by the electrode material of Example 1 is as follows: Fig. 9 As shown, from Fig. 9 It can be seen that the full water electrolysis device using NCoFO / CC material has good stability performance.
[0098] In summary, compared with the prior art, the electrocatalyst of the electrode material provided in the embodiment of the present invention has good hydrogen evolution and oxygen evolution activity in both alkaline and neutral electrolytes when used as the cathode and anode of the electrocatalytic water splitting, and has good stability, that is, the electrocatalyst prepared in the embodiment of the present invention can efficiently realize the complete water splitting, and promote the development of the electrocatalytic water splitting towards the practical direction of higher current density and lower applied potential. The results of the embodiment show that the efficient bifunctional water splitting electrocatalyst on the surface of the electrode material has high hydrogen evolution activity and high oxygen evolution activity, and when used as the cathode and anode of the electrocatalytic water splitting, its large current catalytic activity and stability are significantly better than the precious metal platinum carbon / / ruthenium oxide composed of dual electrode complete water splitting system.
[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An electrode material, It is characterized in that It includes an electrode substrate and an electrocatalyst located on the surface of the electrode substrate, wherein the electrocatalyst is nitrogen-doped cobalt fluoride oxide; The preparation method of the electrode comprises: forming nitrogen-doped cobalt fluoride oxide on the surface of the electrode substrate; forming nitrogen-doped cobalt fluoride oxide on the surface of the electrode substrate comprises: fluorinating an electrode material precursor and then nitrogen-doping, wherein the electrode material precursor comprises the electrode substrate and a cobalt nanoarray precursor on the surface of the electrode substrate; The electrode material precursor is mainly prepared by the following steps: An electrochemical deposition reaction is carried out in an electrolyte of a cobalt salt solution with the electrode substrate as a working electrode, and the cobalt nano-array precursor is grown on the surface of the electrode substrate.
2. The electrode material according to claim 1, It is characterized in that The cobalt fluoride oxide is a nano array.
3. The electrode material according to claim 1 or 2, It is characterized in that The electrode substrate is carbon cloth.
4. The electrode material according to claim 1, It is characterized in that The electrode material precursor and NH 4 The F powder undergoes a gas phase chemical conversion reaction at a temperature of 200 to 500° C., and the reaction time is 1 to 4 hours.
5. The electrode material according to claim 4, It is characterized in that It includes: The electrode material precursor and NH 4 The F powder undergoes a gas phase chemical conversion reaction at a temperature of 400°C.
6. The electrode material according to claim 1, It is characterized in that The electrode material precursor and NH 4 The F powder was heated to the reaction temperature at 8-12°C / min in an inert atmosphere. The inert atmosphere was N 2 atmosphere.
7. The electrode material according to claim 1, It is characterized in that Nitrogen doping is to add N 2 Processing in a plasma reactor.
8. The electrode material according to claim 7, It is characterized in that The N 2 The power of the plasma reactor is 60-200W, the processing time is 0.5-5min, N 2 The N was pumped into the reactor at a flow rate of 1.5 to 2.5 mL / min. 2 Plasma reactor until the pressure drops to 0.2-0.3Pa.
9. The electrode material according to claim 7, It is characterized in that The N 2 The power of the plasma reactor is 200W, the processing time is 50-70s, N 2 The N was pumped in at a flow rate of 2 mL / min. 2 Plasma reactor until the pressure drops to 0.2-0.3Pa.
10. The electrode material according to claim 1, It is characterized in that The electrochemical deposition adopts a three-electrode system, with carbon cloth as a working electrode, a saturated calomel electrode as a reference electrode, and a cobalt nitrate solution as an electrode solution, wherein the concentration of the cobalt nitrate solution is 0.1-3 mol / L.
11. The electrode material according to claim 10, It is characterized in that The voltage of electrochemical deposition is -0.8 to -1.2 V, and the time is 5 to 20 minutes.
12. The electrode material according to claim 10, It is characterized in that The voltage for electrochemical deposition was -1.0V.
13. The electrode material according to claim 1, It is characterized in that The method also includes washing and drying the electrode material precursor obtained after electrochemical deposition in sequence; the washing is ultrasonic washing with deionized water and ethanol in sequence; the drying temperature is 50-80° C. and the drying time is 2-10 hours.
14. The electrode material according to claim 1, It is characterized in that The method also includes sequentially cooling, washing and drying the electrode material after gas phase chemical conversion, wherein the washing is sequentially ultrasonically washing with deionized water and ethanol; the drying temperature is 50 to 80° C. and the drying time is 2 to 10 hours.
15. An anode or cathode, It is characterized in that The anode or the negative electrode is prepared from the electrode material according to any one of claims 1 to 14.
16. An assembled water electrolysis device, It is characterized in that The positive electrode material and the negative electrode material of the assembled water electrolysis device are both electrode materials according to any one of claims 1 to 14.
17. Use of the electrode material according to any one of claims 1 to 14 in electrolysis of water.