Display substrate and manufacturing method thereof, and display device
By introducing a silicon nitride compound impurity absorption layer into the circuit layer of the OLED display substrate, the problem of bright spots in production is solved, the product yield and display effect are improved, and the stability and uniformity of electrical characteristics are ensured.
Patent Information
- Application Number
- CN202110309608.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-03-23
AI Technical Summary
Existing OLED display substrates have a large number of bright spot problems during the production process, resulting in substandard displays and affecting product yields.
An impurity absorption layer is introduced into the circuit layer of the display substrate. The atomic ratio of silicon to nitrogen is 1:5 to 1:35. A nitrogen-silicon compound layer is formed through plasma treatment to reduce the penetration of hydrogen and metal elements and protect the transistor. electrical properties.
It effectively prevents the transistor from being in a high current state, improves the yield rate and display effect, and ensures electrical stability and uniformity.
Smart Images

Figure CN113078192B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to but is not limited to the field of display technology, and in particular to a display substrate and a preparation method thereof, and a display device. Background Art
[0002] Organic Light Emitting Diode (OLED) is an active light-emitting display device with the advantages of self-luminescence, wide viewing angle, high contrast, low power consumption, extremely high response speed, lightness, flexibility and low cost. With the continuous development of display technology, display devices with OLED as the light-emitting device and thin film transistor (TFT) for signal control have become the mainstream products in the current display field.
[0003] Although OLED display devices have been widely used, there are still many technical problems, such as compensation technology. Compensation technology is mainly used to overcome defects such as uneven brightness and afterimages to improve the display quality of display devices. At present, compensation technologies include electrical compensation technology and optical compensation technology. Since the effect of electrical compensation technology is limited, some OLED display devices use optical compensation technology, which sets a photosensitive sensor in the sub-pixel, uses the photosensitive sensor to sense the intensity of the emitted light, and feeds the signal detected by the photosensitive sensor back to the pixel drive circuit to achieve corresponding compensation.
[0004] The inventors of the present application have found through research that in the production of display substrates using optical compensation technology, there is a problem of unqualified display due to the appearance of a large number of bright spots, which seriously affects the product yield. Summary of the invention
[0005] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0006] The technical problem to be solved by the present disclosure is to provide a display substrate and a preparation method thereof, and a display device, so as to solve the problem of unqualified display caused by the appearance of a large number of bright spots in the existing production.
[0007] The present disclosure provides a display substrate, comprising a circuit layer arranged on a substrate, and a light-emitting structure layer and a photoelectric structure layer arranged on a side of the circuit layer away from the substrate, the circuit layer comprising at least one impurity absorption layer and at least one transistor, the transistor comprising an active layer, at least one insulating layer being arranged between the impurity absorption layer and the active layer; the atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:5 to 1:35.
[0008] In an exemplary embodiment, an atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:10 to 1:25.
[0009] In an exemplary embodiment, an atomic ratio of silicon element to hydrogen element in the impurity absorption layer is 1:5 to 1:30.
[0010] In an exemplary embodiment, an atomic ratio of silicon element to hydrogen element in the impurity absorption layer is 1:5 to 1:15.
[0011] In an exemplary embodiment, a material of the impurity absorption layer includes any one or more of the following: silicon nitride, silicon oxynitride, and aluminum silicon nitride.
[0012] In an exemplary embodiment, the display substrate includes a light-emitting area and a sensing area; the circuit layer includes a driving circuit layer arranged in the light-emitting area and a sensing circuit layer arranged in the sensing area, the driving circuit layer includes a first transistor, and the sensing circuit layer includes a second transistor, the light-emitting structure layer is arranged on a side of the driving circuit layer away from the substrate, and the photoelectric structure layer is arranged on a side of the sensing circuit layer away from the substrate; the light-emitting structure layer includes an anode, an organic light-emitting layer and a cathode; the photoelectric structure layer includes a photodiode and an electrode lead; the anode and the electrode lead are arranged on the same layer.
[0013] In an exemplary embodiment, the thickness of the impurity absorbing layer is to The photodiode has a thickness of 0.8 μm to 1.2 μm.
[0014] In an exemplary embodiment, the driving circuit layer includes: a first blocking layer arranged on the substrate, an impurity absorption layer arranged on a side of the first blocking layer away from the substrate, a first insulating layer arranged on a side of the impurity absorption layer away from the substrate, and a first transistor arranged on a side of the first insulating layer away from the substrate; the sensing circuit layer includes: a second blocking layer arranged on the substrate, an impurity absorption layer arranged on a side of the second blocking layer away from the substrate, a first insulating layer arranged on a side of the impurity absorption layer away from the substrate, and a second transistor arranged on a side of the first insulating layer away from the substrate.
[0015] In an exemplary embodiment, the first transistor includes: a first active layer arranged on a side of the first insulating layer away from the substrate, a second insulating layer arranged on a side of the first active layer away from the substrate, a first gate electrode arranged on a side of the second insulating layer away from the substrate, a third insulating layer arranged on a side of the first gate electrode away from the substrate, a first source electrode and a first drain electrode arranged on a side of the third insulating layer away from the substrate, and the first source electrode is connected to the first blocking layer through a via; the second active layer of the second transistor is arranged on the same layer as the first active layer, the second gate electrode of the second transistor is arranged on the same layer as the first gate electrode, and the second source electrode and the second drain electrode of the second transistor are arranged on the same layer as the first source electrode and the first drain electrode.
[0016] In an exemplary embodiment, the sensing circuit layer further includes: a fourth insulating layer disposed on a side of the second transistor away from the substrate, a flat island disposed on a side of the fourth insulating layer away from the substrate, the flat island disposed in the sensing area, and the photodiode disposed on a side of the flat island away from the substrate.
[0017] In an exemplary embodiment, the photodiode includes a first electrode arranged on a side of the flat island away from the substrate, and a first doped layer, an intrinsic layer, a second doped layer and a second electrode arranged in sequence on the first electrode, the first electrode is connected to the second drain electrode of the second transistor through a via, and the second electrode is connected to the electrode lead through a via; the flat island, the first electrode and the second electrode are all rectangles whose long sides extend along the first direction; in the second direction, the orthographic projection of the edge of the first electrode on the substrate is within the range of the orthographic projection of the edge of the flat island on the substrate, and the first distance between the edge of the first electrode and the edge of the flat island is 2μm to 4μm; the orthographic projection of the edge of the second electrode on the substrate is within the range of the orthographic projection of the edge of the first electrode on the substrate, and the distance between the edge of the second electrode and the edge of the first electrode is 1.5μm to 5.5μm; the second direction intersects with the first direction.
[0018] The present disclosure also provides a display device, comprising the aforementioned display substrate.
[0019] The present disclosure also provides a method for preparing a display substrate, comprising:
[0020] A circuit layer is formed on a substrate; the circuit layer includes at least one impurity absorption layer and at least one transistor, the transistor includes an active layer, and at least one insulating layer is provided between the impurity absorption layer and the active layer; the atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:5 to 1:35;
[0021] A light-emitting structure layer and a photoelectric structure layer are formed on the circuit layer.
[0022] In an exemplary embodiment, forming a circuit layer on a substrate includes:
[0023] forming a first metal layer on a substrate;
[0024] depositing an impurity absorbing film on a side of the first metal layer away from the substrate, and performing plasma treatment on the impurity absorbing film to form an impurity absorbing layer covering the first metal layer;
[0025] forming a first insulating layer on a side of the impurity absorption layer away from the substrate;
[0026] A first transistor and a second transistor are formed on a side of the first insulating layer away from the substrate.
[0027] In an exemplary embodiment, depositing an impurity absorbing film includes: using chemical vapor deposition to deposit a thickness of 500W to 1200W at a deposition power of 330°C to 450°C and a deposition pressure of 1000mT to 1800mT. to The impurity absorption film is made of any one or more of the following materials: silicon nitride, silicon oxynitride and aluminum silicon nitride.
[0028] In an exemplary embodiment, the plasma treatment of the impurity absorption film includes: plasma treatment of the impurity absorption film using nitrous oxide at a plasma power of 600 W to 1500 W and a plasma pressure of 600 mT to 2000 mT.
[0029] The exemplary embodiments of the present disclosure disclose a display substrate and a preparation method thereof, and a display device. By setting an impurity absorption layer, when the display substrate is exposed to a hydrogen atmosphere, the impurity absorption layer can effectively reduce the penetration of hydrogen elements into the active layer of the transistor, effectively avoiding the appearance of a large number of bright spots on the display substrate, improving the yield rate, and improving the display effect.
[0030] Other aspects will be apparent upon reading and understanding the drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings are used to provide a further understanding of the technical solution of the present disclosure and constitute a part of the specification. Together with the embodiments of the present disclosure, they are used to explain the technical solution of the present disclosure and do not constitute a limitation on the technical solution of the present disclosure. The shapes and sizes of the components in the accompanying drawings do not reflect the actual proportions and are only intended to illustrate the contents of the present disclosure.
[0032] Figure 1is a structural schematic diagram of a display device;
[0033] Figure 2 It is a schematic diagram of a planar structure of a display substrate;
[0034] Figure 3 is a schematic diagram of an equivalent circuit of a pixel driving circuit;
[0035] Figure 4 A schematic cross-sectional structure diagram of a display substrate according to an exemplary embodiment of the present disclosure;
[0036] Figure 5 It is a schematic diagram after forming a first metal layer pattern according to an exemplary embodiment of the present disclosure;
[0037] Figure 6 It is a schematic diagram of an exemplary embodiment of the present disclosure after forming an impurity absorption layer pattern;
[0038] Figure 7 A schematic diagram of an exemplary embodiment of the present disclosure after forming a first insulating layer and a semiconductor pattern;
[0039] Figure 8 It is a schematic diagram of an exemplary embodiment of the present disclosure after forming a second metal layer pattern;
[0040] Fig. 9 It is a schematic diagram after forming a third insulating layer pattern according to an exemplary embodiment of the present disclosure;
[0041] Fig.10 It is a schematic diagram after forming a third metal layer pattern according to an exemplary embodiment of the present disclosure;
[0042] Fig.11 It is a schematic diagram after forming a first planar layer pattern according to an exemplary embodiment of the present disclosure;
[0043] Fig.12 It is a schematic diagram of an exemplary embodiment of the present disclosure after forming a fourth metal layer pattern;
[0044] Fig.13 It is a schematic diagram after forming a fifth insulating layer pattern according to an exemplary embodiment of the present disclosure;
[0045] Fig.14 A schematic diagram of an exemplary embodiment of the present disclosure after a photodiode pattern is formed;
[0046] Fig.15 It is a schematic diagram after forming a second planar layer pattern according to an exemplary embodiment of the present disclosure;
[0047] Fig.16 It is a schematic diagram after forming a second conductive layer pattern according to an exemplary embodiment of the present disclosure;
[0048] Fig.17A schematic diagram of an exemplary embodiment of the present disclosure after forming a pixel definition layer pattern;
[0049] Fig.18 It is a schematic diagram of an exemplary embodiment of the present disclosure after forming an organic light emitting layer and a cathode pattern;
[0050] Fig.19 A diagram showing the electrical characteristics of a transistor in a substrate;
[0051] Fig. 20 A diagram showing electrical characteristics of a transistor in a substrate for an exemplary embodiment of the present disclosure;
[0052] Fig.21 This is a test result diagram of the hydrogen content in the active layer;
[0053] Fig. 22 This is a test result diagram of the silicon content in the active layer;
[0054] Fig.23 is a schematic cross-sectional structure diagram of another display substrate according to an exemplary embodiment of the present disclosure;
[0055] Fig.24 is a schematic cross-sectional structure diagram of another display substrate according to an exemplary embodiment of the present disclosure;
[0056] Fig.25 is a schematic diagram of a planar structure of a flat island and a photodiode according to an exemplary embodiment of the present disclosure;
[0057] Fig.26 for Fig.25 Sectional view along AA direction;
[0058] Fig. 27 The figure is a schematic cross-sectional structure diagram of another display substrate according to an exemplary embodiment of the present disclosure.
[0059] Description of reference numerals:
[0060] 10—substrate; 11—first insulating layer; 12—second insulating layer;
[0061] 13—third insulating layer; 14—fourth insulating layer; 15—fifth insulating layer;
[0062] 16—sixth insulating layer; 18—first flat layer; 19—second flat layer;
[0063] 20—flat island; 31—first shielding layer; 32—first active layer;
[0064] 33—first gate electrode; 34—first source electrode; 35—first drain electrode;
[0065] 41—second shielding layer; 42—second active layer; 43—second gate electrode;
[0066] 44—second source electrode; 45—second drain electrode; 61—connecting electrode;
[0067] 71—first electrode; 72—first doping layer; 73—intrinsic layer;
[0068] 74—second doping layer; 75—second electrode; 81—anode;
[0069] 82—pixel definition layer; 83—organic light emitting layer; 84—cathode;
[0070] 85—color film layer; 91—electrode lead; 100—impurity absorption layer;
[0071] 101—driving circuit layer; 102—light emitting structure layer; 110—first transistor;
[0072] 201—sensing circuit layer; 202—photoelectric structure layer; 210—second transistor. DETAILED DESCRIPTION
[0073] In order to make the purpose, technical solutions and advantages of the present disclosure clearer, the embodiments of the present disclosure will be described in detail in conjunction with the accompanying drawings below. Note that the embodiments can be implemented in multiple different forms. A person of ordinary skill in the art can easily understand the fact that the methods and contents can be transformed into various forms without departing from the purpose and scope of the present disclosure. Therefore, the present disclosure should not be interpreted as being limited to the contents described in the following embodiments. In the absence of conflict, the embodiments in the present disclosure and the features in the embodiments can be arbitrarily combined with each other.
[0074] In the drawings, the size of each component, the thickness of a layer, or the area is sometimes exaggerated for the sake of clarity. Therefore, one embodiment of the present disclosure is not necessarily limited to this size, and the shape and size of each component in the drawings do not reflect the true proportion. In addition, the drawings schematically show ideal examples, and one embodiment of the present disclosure is not limited to the shapes or values shown in the drawings.
[0075] In the present specification, ordinal numbers such as “first”, “second” and “third” are provided to avoid confusion among constituent elements, and are not intended to limit the number.
[0076] In this specification, for the sake of convenience, the words and phrases indicating the orientation or positional relationship, such as "middle", "upper", "lower", "front", "back", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., are used to illustrate the positional relationship of the constituent elements with reference to the drawings. This is only for the convenience of describing this specification and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as a limitation of the present disclosure. The positional relationship of the constituent elements is appropriately changed according to the direction in which each constituent element is described. Therefore, it is not limited to the words and phrases described in the specification, and can be appropriately replaced according to the situation.
[0077] In this specification, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate, or the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this disclosure can be understood according to specific circumstances.
[0078] In this specification, a transistor refers to an element including at least three terminals: a gate electrode, a drain electrode, and a source electrode. The transistor has a channel region between a drain electrode (drain electrode terminal, drain region, or drain electrode) and a source electrode (source electrode terminal, source region, or source electrode), and current can flow through the drain electrode, the channel region, and the source electrode. Note that in this specification, the channel region refers to a region where current mainly flows.
[0079] In this specification, the first electrode may be a drain electrode and the second electrode may be a source electrode, or the first electrode may be a source electrode and the second electrode may be a drain electrode. In the case of using transistors with opposite polarities or when the direction of current changes during circuit operation, the functions of the "source electrode" and the "drain electrode" are sometimes interchanged. Therefore, in this specification, the "source electrode" and the "drain electrode" may be interchanged.
[0080] In this specification, "electrical connection" includes the case where components are connected together through an element having some electrical function. There is no particular limitation on the "element having some electrical function" as long as it can transmit and receive electrical signals between the connected components. Examples of "element having some electrical function" include not only electrodes and wiring, but also switching elements such as transistors, resistors, inductors, capacitors, and other elements having various functions.
[0081] In this specification, "parallel" means a state where the angle formed by two straight lines is greater than -10° and less than 10°, and therefore, also includes a state where the angle is greater than -5° and less than 5°. In addition, "perpendicular" means a state where the angle formed by two straight lines is greater than 80° and less than 100°, and therefore, also includes a state where the angle is greater than 85° and less than 95°.
[0082] In this specification, "film" and "layer" may be interchanged. For example, "conductive layer" may be replaced by "conductive film". Similarly, "insulating film" may be replaced by "insulating layer".
[0083] The term "about" in the present disclosure refers to a numerical value that is not strictly limited to allow for process and measurement errors.
[0084] Figure 1 FIG. 1 is a schematic diagram of the structure of a display device. Figure 1 As shown, the OLED display device may include a timing controller, a data signal driver, a scan signal driver and a pixel array, and the pixel array may include a plurality of scan signal lines (S1 to Sm), a plurality of data signal lines (D1 to Dn) and a plurality of sub-pixels Pxij. In an exemplary embodiment, the timing controller may provide a grayscale value and a control signal suitable for the specification of the data signal driver to the data signal driver, and may provide a clock signal, a scan start signal, etc. suitable for the specification of the scan signal driver to the scan signal driver. The data signal driver may generate a data voltage to be provided to the data signal lines D1, D2, D3, ... and Dn using the grayscale value and the control signal received from the timing controller. For example, the data signal driver may sample the grayscale value using the clock signal, and apply the data voltage corresponding to the grayscale value to the data signal lines D1 to Dn in units of sub-pixel rows, where n may be a natural number. The scan signal driver may generate a scan signal to be provided to the scan signal lines S1, S2, S3, ... and Sm by receiving a clock signal, a scan start signal, etc. from the timing controller. For example, the scan signal driver may sequentially provide a scan signal having an on-level pulse to the scan signal lines S1 to Sm. For example, the scan signal driver may be constructed in the form of a shift register, and may generate a scan signal in a manner that sequentially transmits a scan start signal provided in the form of an on-level pulse to a next level circuit under the control of a clock signal, and m may be a natural number. The sub-pixel array may include a plurality of pixel sub-PXij. Each pixel sub-PXij may be connected to a corresponding data signal line and a corresponding scan signal line, and i and j may be natural numbers. The sub-pixel PXij may refer to a sub-pixel in which a transistor is connected to the i-th scan signal line and to the j-th data signal line.
[0085] Figure 2FIG. 1 is a schematic diagram of a planar structure of a display substrate. Figure 2 As shown, the display substrate may include a plurality of pixel units P arranged in a matrix, at least one of the plurality of pixel units P includes a first sub-pixel P1 emitting a first color light, a second sub-pixel P2 emitting a second color light, and a third sub-pixel P3 emitting a third color light, and the first sub-pixel P1, the second sub-pixel P2, and the third sub-pixel P3 each include a pixel driving circuit and a light-emitting device. The pixel driving circuits in the first sub-pixel P1, the second sub-pixel P2, and the third sub-pixel P3 are respectively connected to the scanning signal line and the data signal line, and the pixel driving circuit is configured to receive the data voltage transmitted by the data signal line under the control of the scanning signal line, and output a corresponding current to the light-emitting device. The light-emitting devices in the first sub-pixel P1, the second sub-pixel P2, and the third sub-pixel P3 are respectively connected to the pixel driving circuits of the sub-pixels in which they are located, and the light-emitting devices are configured to emit light of corresponding brightness in response to the current output by the pixel driving circuit of the sub-pixel in which they are located.
[0086] In an exemplary embodiment, the pixel unit P may include a red (R) sub-pixel, a green (G) sub-pixel, and a blue (B) sub-pixel, or may include a red sub-pixel, a green sub-pixel, a blue sub-pixel, and a white sub-pixel, which is not limited in the present disclosure. In an exemplary embodiment, the shape of the sub-pixel in the pixel unit may be rectangular, rhombus, pentagonal, or hexagonal. When the pixel unit includes three sub-pixels, the three sub-pixels may be arranged in horizontal parallel, vertical parallel, or in a herringbone manner. When the pixel unit includes four sub-pixels, the four sub-pixels may be arranged in horizontal parallel, vertical parallel, or in a square manner, which is not limited in the present disclosure.
[0087] In exemplary embodiments, the pixel driving circuit may be a 3T1C, 4T1C, 5T1C, 5T2C, 6T1C, or 7T1C structure. Figure 3 FIG. 1 is a schematic diagram of an equivalent circuit of a pixel driving circuit. Figure 3 As shown, the pixel driving circuit is a 3T1C structure, which may include three transistors (a first transistor T1, a second transistor T2, and a third transistor T3), a storage capacitor C STand 6 signal lines (data signal line Dn, first scan signal line Gn, second scan signal line Sn, compensation signal line Se, first power line VDD and second power line VSS). In an exemplary embodiment, the first transistor T1 is a switch transistor, the second transistor T2 is a drive transistor, and the third transistor T3 is a compensation transistor. The gate electrode of the first transistor T1 is coupled to the first scan signal line Gn, the first electrode of the first transistor T1 is coupled to the data signal line Dn, the second electrode of the first transistor T1 is coupled to the gate electrode of the second transistor T2, and the first transistor T1 is used to receive the data signal transmitted by the data signal line Dn under the control of the first scan signal line Gn, so that the gate electrode of the second transistor T2 receives the data signal. The gate electrode of the second transistor T2 is coupled to the second electrode of the first transistor T1, the first electrode of the second transistor T2 is coupled to the first power line VDD, the second electrode of the second transistor T2 is coupled to the first electrode of the OLED, and the second transistor T2 is used to generate a corresponding current at the second electrode under the control of the data signal received by its gate electrode. The gate electrode of the third transistor T3 is coupled to the second scan signal line Sn, the first electrode of the third transistor T3 is coupled to the compensation signal line Se, the second electrode of the third transistor T3 is coupled to the second electrode of the second transistor T2, and the third transistor T3 is used to extract the threshold voltage Vth and mobility of the second transistor T2 in response to the compensation timing to compensate for the threshold voltage Vth. The first electrode of the OLED is coupled to the second electrode of the second transistor T2, the second electrode of the OLED is coupled to the second power line VSS, and the OLED is used to emit light of corresponding brightness in response to the current of the second electrode of the second transistor T2. The storage capacitor C ST The first electrode of the storage capacitor C is coupled to the gate electrode of the second transistor T2. ST The second electrode of the second transistor T2 is coupled to the second electrode of the storage capacitor C ST Used to store the potential of the gate electrode of the second transistor T2.
[0088] In an exemplary embodiment, the signal of the first power line VDD continuously provides a high level signal, and the signal of the second power line VSS is a low level signal. The first transistor T1 to the third transistor T3 can be a P-type transistor, or can be an N-type transistor. Using the same type of transistors in the pixel driving circuit can simplify the process flow, reduce the process difficulty of the display panel, and improve the yield of the product.
[0089] In an exemplary embodiment, the first transistor T1 to the third transistor T3 may be a low-temperature polysilicon thin film transistor, or an oxide thin film transistor, or a low-temperature polysilicon thin film transistor and an oxide thin film transistor. The active layer of the low-temperature polysilicon thin film transistor is low-temperature polysilicon (LTPS), and the active layer of the oxide thin film transistor is oxide. Low-temperature polysilicon thin film transistors have advantages such as high mobility and fast charging, and oxide thin film transistors have advantages such as low leakage current. In an exemplary embodiment, low-temperature polysilicon thin film transistors and oxide thin film transistors can be integrated on a display substrate to form a low-temperature polycrystalline oxide (LTPO) display substrate, which can take advantage of the advantages of both, can achieve high resolution (Pixel Per Inch, PPI), low-frequency driving, can reduce power consumption, and can improve display quality. In an exemplary embodiment, the light-emitting device can be an organic light-emitting diode (OLED), including a stacked first electrode (anode), an organic light-emitting layer, and a second electrode (cathode).
[0090] The inventor of the present application has found through research that the problem of a large number of bright spots on the display substrate using the optical compensation technology is caused to a certain extent by the process of preparing the photodiode. In the existing preparation process, the gas atmosphere for preparing each film layer of the photodiode is mainly silicon tetrahydride (SiH4) and hydrogen (H2), so the display substrate is exposed to the hydrogen atmosphere for a long time, and the hydrogen element easily penetrates into the oxide active layer of the thin film transistor, making the oxide active layer conductive, and the conductive oxide active layer will put the thin film transistor in a state of high current. In addition, after the photodiode is prepared, a protective layer needs to be formed. Since the protective layer is thick and in order to ensure the film quality, the deposition time usually takes 10 minutes to 30 minutes, which will also cause the display substrate to be exposed to the hydrogen atmosphere for a long time. Since the thin film transistor is in a state of high current and it is difficult to restore to a normal state in the subsequent process, a large number of bright spots appear in the dot screen, resulting in unqualified display.
[0091] In order to solve the problem of unqualified display due to the appearance of a large number of bright spots in existing production, the exemplary embodiment of the present disclosure provides a display substrate. In an exemplary embodiment, the display substrate may include a circuit layer arranged on a substrate and a light-emitting structure layer and a photoelectric structure layer arranged on a side of the circuit layer away from the substrate, the circuit layer includes at least one impurity absorption layer and at least one transistor, the transistor includes an active layer, and at least one insulating layer is arranged between the impurity absorption layer and the active layer; the atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:5 to 1:35, and the impurity absorption layer is configured to reduce the penetration of hydrogen element into the circuit layer to ensure the normal electrical characteristics of the transistor in the circuit layer, thereby avoiding the appearance of a large number of bright spots on the display substrate and improving the yield rate.
[0092] Figure 4 The cross-sectional structure diagram of a display substrate of an exemplary embodiment of the present disclosure is shown in FIG. The display substrate is a bottom emission type display substrate. On a plane parallel to the display substrate, the display substrate may include a plurality of sub-pixels arranged in a matrix manner. Figure 4 The structure of a sub-pixel on the display substrate is shown in FIG. Figure 4 As shown, on a plane parallel to the display substrate, the sub-pixel may include a light-emitting region A and a sensing region B. On a plane perpendicular to the display substrate, the display substrate may include a driving circuit layer 101 and a light-emitting structure layer 102 arranged in the light-emitting region A, and a sensing circuit layer 201 and an optoelectronic structure layer 202 arranged in the sensing region B, and the driving circuit layer 101 and the sensing circuit layer 201 constitute the circuit layer of the present disclosure. Among them, the driving circuit layer 101 of the light-emitting region A is arranged on the substrate 10, the light-emitting structure layer 102 is arranged on the side of the driving circuit layer 101 away from the substrate, the sensing circuit layer 201 of the sensing region B is arranged on the substrate 10, the optoelectronic structure layer 202 is arranged on the side of the sensing circuit layer 201 away from the substrate, the light-emitting structure layer 102 is configured to emit light of corresponding brightness, and the optoelectronic structure layer 202 is configured to sense the intensity of the emitted light. In an exemplary embodiment, the driving circuit layer 101 and the sensing circuit layer 201 include transistors and an impurity absorption layer 100, the impurity absorption layer 100 is located on a side of the active layer of the transistor adjacent to the substrate, and a first insulating layer is disposed between the impurity absorption layer 100 and the active layer of the transistor. The atomic ratio of silicon element to nitrogen element in the impurity absorption layer 100 may be about 1:5 to 1:35, and the impurity absorption layer is configured to reduce the penetration of hydrogen element, oxygen element and metal element into the transistors in the driving circuit layer 101 and the sensing circuit layer 201 to ensure the normal electrical characteristics of the transistors, thereby avoiding a large number of bright spots on the display substrate and improving the yield rate.
[0093] In an exemplary embodiment, the impurity absorption layer uses the nitrogen element in the impurity absorption layer to form H=N bonds, N=O bonds, and N=M bonds with hydrogen elements, oxygen elements, and metal elements, respectively, to effectively reduce the penetration of hydrogen elements, oxygen elements, and metal elements into the active layer of the transistor. In an exemplary embodiment, the atomic ratio of silicon elements to nitrogen elements is in the range of 1:5 to 1:35, and the binding energy of hydrogen elements and nitrogen elements to form bonds is relatively strong. When the atoms of silicon elements and nitrogen elements are relatively small, the bond energy is relatively small, and hydrogen elements are not easily fixed in the impurity absorption layer and will be freed to the active layer. When the atoms of silicon elements and nitrogen elements are relatively large, the bond energy is fully combined and the hydrogen elements can no longer be fixed, and the additional hydrogen elements will also be freed to the active layer.
[0094] In an exemplary embodiment, the atomic ratio of silicon element to nitrogen element in the impurity absorption layer may be about 1:10 to 1:25. For example, the atomic ratio of silicon element to nitrogen element in the impurity absorption layer may be about 1:17.
[0095] In an exemplary embodiment, the impurity absorption layer forms an H=N bond by utilizing the nitrogen element in the impurity absorption layer and the hydrogen element, so that the impurity absorption layer contains the hydrogen element, and the atomic ratio of the silicon element to the hydrogen element in the impurity absorption layer is 1:5 to 1:30. This ratio relationship is formed after the impurity absorption layer absorbs the hydrogen element.
[0096] In an exemplary embodiment, the atomic ratio of silicon element to hydrogen element in the impurity absorption layer is 1:5 to 1:15. For example, the atomic ratio of silicon element to hydrogen element in the impurity absorption layer may be about 1:13.
[0097] In an exemplary embodiment, the material of the impurity absorption layer 100 may be a silicon nitride compound, and may include any one or more of the following: silicon nitride, silicon oxynitride, and aluminum silicon nitride.
[0098] In an exemplary embodiment, the driving circuit layer 101 of the light emitting region A may include: a first blocking layer 31 disposed on the substrate, an impurity absorption layer 100 covering the first blocking layer 31, a first insulating layer 11 disposed on a side of the impurity absorption layer 100 away from the substrate, and a first transistor 110 disposed on a side of the first insulating layer 11 away from the substrate. In an exemplary embodiment, the first transistor 110 of the top gate structure may include a first gate electrode, a first active layer, a first source electrode, and a first drain electrode. The position of the first transistor 110 corresponds to the position of the first blocking layer 31. The orthographic projection of the first active layer of the first transistor 110 on the substrate is located within the range of the orthographic projection of the first blocking layer 31 on the substrate. The first source electrode of the first transistor 110 is connected to the first blocking layer 31 through a via hole, forming a first transistor 110 of a dual-gate structure. In an exemplary embodiment, the driving circuit layer 101 may include a plurality of transistors and storage capacitors constituting a pixel driving circuit. Figure 4 Only one first transistor in a sub-pixel is taken as an example for illustration.
[0099] In an exemplary embodiment, the light-emitting structure layer 102 may include an anode 81, an organic light-emitting layer 83 and a cathode 84 constituting a light-emitting device, the anode 81 is connected to the first drain electrode of the first transistor 110, the organic light-emitting layer 83 is arranged between the anode 81 and the cathode 84, and the organic light-emitting layer 83 emits light of corresponding color under the control of the anode 81 and the cathode 84.
[0100] In an exemplary embodiment, the sensing circuit layer 201 of the sensing region B may include: a second shielding layer 41 disposed on a substrate, an impurity absorption layer 100 covering the second shielding layer 41, a first insulating layer 11 disposed on a side of the impurity absorption layer 100 away from the substrate, and a second transistor 210 as a switching device disposed on a side of the first insulating layer 11 away from the substrate. In an exemplary embodiment, the second transistor 210 of a top-gate structure may include a second gate electrode, a second active layer, a second source electrode, and a second drain electrode, the position of the second transistor 210 corresponds to the position of the second shielding layer 41, and the orthographic projection of the second active layer of the second transistor 210 on the substrate is within the range of the orthographic projection of the second shielding layer 41 on the substrate.
[0101] In an exemplary embodiment, the photoelectric structure layer 202 may include an electrode lead 91 and a first electrode 71, a first doped layer, an intrinsic layer, a second doped layer and a second electrode 75 constituting a PIN photodiode, the first electrode 71 being connected to the second drain electrode of the second transistor 210 through a via, and the second electrode 75 being connected to the electrode lead 91 through a via.
[0102] In an exemplary embodiment, the first transistor 110 of the driving circuit layer 101 and the second transistor 210 of the sensing circuit layer 201 are arranged on the same layer and can be formed simultaneously by the same process, that is, the first gate electrode and the second gate electrode are arranged on the same layer and are formed simultaneously by the same patterning process, the first active layer and the second active layer are arranged on the same layer and are formed simultaneously by the same patterning process, and the first source electrode and the first drain electrode are arranged on the same layer as the second source electrode and the second drain electrode, and are formed simultaneously by the same patterning process.
[0103] In an exemplary embodiment, the first shielding layer 31 and the second shielding layer 41 are disposed in the same layer and are formed simultaneously through the same patterning process.
[0104] In example embodiments, the first transistor 110 and the second transistor 210 may include oxide transistors.
[0105] In an exemplary embodiment, the anode 81 of the light emitting structure layer 102 and the electrode lead 91 of the optoelectronic structure layer 202 may be disposed in the same layer and formed simultaneously through the same patterning process.
[0106] In an exemplary embodiment, the driving circuit layer 101 also includes a connecting electrode 61, which is connected to the first drain electrode of the first transistor 110 through a via, and the anode 81 of the light-emitting structure layer 102 is connected to the connecting electrode 61 through a via. The connecting electrode 61 of the driving circuit layer 101 and the first electrode 71 of the photoelectric structure layer 202 can be arranged in the same layer and formed simultaneously through the same patterning process.
[0107] In an exemplary embodiment, the display substrate may include other film layers, such as a color filter layer or an encapsulation layer, etc., which is not limited in the present disclosure.
[0108] The following is an exemplary explanation through the preparation process of the display substrate. The "patterning process" mentioned in the present disclosure includes processes such as coating photoresist, mask exposure, development, etching, and stripping photoresist for metal materials, inorganic materials or transparent conductive materials, and includes processes such as coating organic materials, mask exposure and development for organic materials. Deposition can be any one or more of sputtering, evaporation, and chemical vapor deposition, coating can be any one or more of spraying, spin coating and inkjet printing, and etching can be any one or more of dry etching and wet etching, which are not limited in the present disclosure. "Thin film" refers to a layer of thin film made by deposition, coating or other processes of a certain material on a substrate. If the "thin film" does not require a patterning process during the entire production process, the "thin film" can also be called a "layer". If the "thin film" requires a patterning process during the entire production process, it is called a "thin film" before the patterning process and a "layer" after the patterning process. The "layer" after the patterning process contains at least one "pattern". The "A and B are arranged in the same layer" mentioned in the present disclosure means that A and B are formed simultaneously through the same patterning process, and the "thickness" of the film layer is the size of the film layer in the direction perpendicular to the display substrate. In the exemplary embodiments of the present disclosure, "the orthographic projection of B is within the range of the orthographic projection of A" means that the boundary of the orthographic projection of B falls within the boundary of the orthographic projection of A, or the boundary of the orthographic projection of A overlaps with the boundary of the orthographic projection of B.
[0109] Figures 5 to 18 FIG. 1 is a schematic diagram of a display substrate preparation process. In an exemplary embodiment, the display substrate preparation process may include the following operations.
[0110] (1) Providing a substrate In an exemplary embodiment, the substrate 10 may be a rigid substrate, and the rigid substrate may be glass or quartz.
[0111] In a possible exemplary embodiment, the substrate may be a flexible substrate, and the flexible substrate may be a single-layer structure or a laminated structure. In an exemplary embodiment, the flexible substrate may include a first flexible material layer, a first inorganic material layer, a second flexible material layer, and a second inorganic material layer stacked on a glass carrier.
[0112] (2) Forming a first metal layer pattern. In an exemplary embodiment, forming the first metal layer pattern may include: depositing a first metal film on the substrate 10, patterning the first metal film through a patterning process, and forming a first metal layer pattern disposed on the substrate 10, wherein the first metal layer pattern includes at least a first shielding layer 31 located in the light emitting region A and a second shielding layer 41 located in the sensing region B, such as Figure 5 shown.
[0113] In an exemplary embodiment, the thickness of the first shielding layer 31 and the second shielding layer 41 may be approximately to
[0114] (3) Forming an impurity absorption layer pattern. In an exemplary embodiment, forming the impurity absorption layer pattern may include: depositing an impurity absorption film on the substrate having the aforementioned pattern, and performing plasma treatment on the impurity absorption film to form an impurity absorption layer 100 pattern, wherein the impurity absorption layer 100 covers the first metal layer, that is, covers the first shielding layer 31 and the second shielding layer 41, such as Figure 6 shown.
[0115] In an exemplary embodiment, the thickness of the impurity absorption layer 100 may be approximately to For example, the thickness of the impurity absorption layer 100 may be approximately
[0116] In an exemplary embodiment, by strictly controlling the process parameters for depositing the impurity absorption film, the deposited impurity absorption film has a stricter atomic ratio of silicon to nitrogen, so that the impurity absorption layer can effectively reduce the penetration of hydrogen, oxygen and metal elements into the active layer of the transistor.
[0117] In an exemplary embodiment, the strictly controlled process parameters may include deposition power, deposition temperature, and deposition pressure.
[0118] In an exemplary embodiment, depositing the impurity absorption film may include: using chemical vapor deposition (CVD) to deposit silicon nitride, silicon oxynitride, aluminum silicon nitride, or a mixture of silicon nitride and silicon oxynitride at a deposition power of 500 W to 1200 W, a deposition temperature of 330° C. to 450° C., and a deposition pressure of 1000 mT to 1800 mT (millitor). Controlling the atomic ratio of silicon element to nitrogen element in the impurity absorption layer to be approximately 1:5 to 1:35.
[0119] In an exemplary embodiment, by strictly controlling the process parameters of the plasma treatment, the formed impurity absorption layer can have strong adhesion with the subsequently formed buffer layer, so that the impurity absorption layer and the buffer layer form a buffer+cutoff structure.
[0120] In an exemplary embodiment, the tightly controlled process parameters may include plasma power, plasma pressure, and plasma gas.
[0121] In an exemplary embodiment, plasma-treating the impurity absorption film may include plasma-treating the impurity absorption film using nitrous oxide (N2O) at a plasma power of 600 W to 1500 W and a plasma pressure of 600 mT to 2000 mT.
[0122] In an exemplary embodiment, the atomic ratio of silicon element to nitrogen element in the impurity absorption layer may be about 1:10 to 1:25. For example, the atomic ratio of silicon element to nitrogen element in the impurity absorption layer 100 may be about 1:17.
[0123] (4) Forming a first insulating layer and a semiconductor layer pattern. In an exemplary embodiment, forming the first insulating layer and the semiconductor layer pattern may include: depositing a first insulating film and a semiconductor film in sequence on the substrate on which the aforementioned pattern is formed, patterning the semiconductor film by a patterning process, forming a first insulating layer 11 pattern covering the impurity absorption layer 100, and a semiconductor layer pattern disposed on the first insulating layer 11, wherein the semiconductor layer pattern includes at least a first active layer 32 located in the light emitting region A and a second active layer 42 located in the sensing region B, such as Figure 7 shown.
[0124] In an exemplary embodiment, the thickness of the first insulating layer 11 may be approximately to For example, the thickness of the first insulating layer 11 may be approximately
[0125] In an exemplary embodiment, the material of the first insulating layer 11 may be silicon oxide (SiOx), and the first insulating layer may be referred to as a buffer layer.
[0126] In an exemplary embodiment, the semiconductor film may be made of polysilicon or oxide, which is not limited in the present disclosure. The oxide may be any one or more of the following: indium gallium zinc oxide (InGaZnO), indium gallium zinc oxynitride (InGaZnON), zinc oxide (ZnO), zinc oxynitride (ZnON), zinc tin oxide (ZnSnO), cadmium tin oxide (CdSnO), gallium tin oxide (GaSnO), titanium tin oxide (TiSnO), copper aluminum oxide (CuAlO), strontium copper oxide (SrCuO), lanthanum copper oxysulfide (LaCuOS), gallium nitride (GaN), indium gallium nitride (InGaN), aluminum gallium nitride (AlGaN) and indium gallium aluminum nitride (InGaAlN). In some possible implementations, the semiconductor film may be made of indium gallium zinc oxide (IGZO), which has a higher electron mobility.
[0127] In an exemplary embodiment, the position of the first active layer 32 corresponds to the position of the first shielding layer 31, and the orthographic projection of the first active layer 32 on the substrate is located within the range of the orthographic projection of the first shielding layer 31 on the substrate. The position of the second active layer 42 corresponds to the position of the second shielding layer 41, and the orthographic projection of the second active layer 42 on the substrate is located within the range of the orthographic projection of the second shielding layer 41 on the substrate.
[0128] In an exemplary embodiment, the impurity absorption layer, the first insulating layer and the semiconductor layer may be formed by the same patterning process. For example, the impurity absorption film is first deposited and then plasma treated, and then the first insulating film and the semiconductor film are sequentially deposited, and then the semiconductor layer is patterned.
[0129] (5) Forming a second metal layer pattern. In an exemplary embodiment, forming the second metal layer pattern may include: depositing a second insulating film and a second metal film in sequence on the substrate on which the aforementioned pattern is formed, patterning the second insulating film and the second metal film through a patterning process to form a second insulating layer 12 pattern disposed on the semiconductor layer, and a second metal layer pattern disposed on the second insulating layer 12, wherein the second metal layer pattern includes at least a first gate electrode 33 located in the light emitting region A and a second gate electrode 43 located in the sensing region B, such as Figure 8 shown.
[0130] In an exemplary embodiment, the second metal layer pattern may include a first capacitor electrode constituting a storage capacitor, the first capacitor electrode may be located in the light emitting region A, and the first capacitor electrode may be disposed on the first insulating layer.
[0131] In an exemplary embodiment, during the etching process of patterning the second metal layer and the second insulating layer, the semiconductor layer not covered by the second metal layer and the second insulating layer is conductorized to form a conductorized source region and a conductorized drain region, and the source region and the drain region are configured to connect to a subsequently formed source electrode and a drain electrode.
[0132] In an exemplary embodiment, patterns of the second metal layer and the second insulating layer may be substantially the same, and an orthographic projection of the second metal layer on the substrate is located within a range of an orthographic projection of the second insulating layer on the substrate.
[0133] In example embodiments, the second insulating layer may be referred to as a gate insulating (GI) layer, and the second metal layer may be referred to as a gate metal (GATE) layer.
[0134] (6) Forming a third insulating layer pattern. In an exemplary embodiment, forming the third insulating layer pattern may include: depositing a third insulating film on the substrate on which the aforementioned pattern is formed, and patterning the third insulating film through a patterning process to form a third insulating layer 13 pattern covering the second metal layer pattern. A first via hole K1 and a second via hole K2 are provided in the third insulating layer 13 of the light emitting region A, and the third insulating layer 13, the first insulating layer 11 and the impurity absorption layer 100 in the first via hole K1 are etched away to expose the surface of the first blocking layer 31, and the third insulating layer 13 in the second via hole K2 is etched away to expose the surface of the first active layer 32. A third via hole K3 is provided in the third insulating layer 13 of the sensing region B, and the third insulating layer 13 in the third via hole K3 is etched away to expose the surface of the second active layer 42, as shown in FIG. Fig. 9 shown.
[0135] In an exemplary embodiment, in the process of patterning the third insulating layer, the second vias K2 respectively expose the conductive source region and the conductive drain region in the first active layer 32, and the third vias K3 respectively expose the conductive source region and the conductive drain region in the second active layer 42.
[0136] In example embodiments, the third insulating layer may be referred to as an interlayer insulating (ILD) layer.
[0137] (7) Forming a third metal layer pattern. In an exemplary embodiment, forming the third metal layer pattern may include: depositing a third metal film on the substrate on which the aforementioned pattern is formed, patterning the third metal film through a patterning process to form a third metal layer pattern, wherein the third metal layer pattern includes at least a first source electrode 34 and a first drain electrode 35 located in the light emitting region A, and a second source electrode 44 and a second drain electrode 45 located in the sensing region B, wherein the first source electrode 34 and the first drain electrode 35 are respectively connected to the first active layer 32 through the second via hole K2, the first source electrode 34 is simultaneously connected to the first shielding layer 31 through the first via hole K1, and the second source electrode 44 and the second drain electrode 45 are respectively connected to the second active layer 42 through the third via hole K3, as shown in FIG. Fig.10 shown.
[0138] In an exemplary embodiment, the third metal layer pattern may include a second capacitor electrode constituting a storage capacitor, and a position of the second capacitor electrode corresponds to a position of the first capacitor electrode.
[0139] In example embodiments, the third metal layer may be referred to as a first source-drain metal (SD1) layer.
[0140] (8) Forming a fourth insulating layer and a first planar layer pattern. In an exemplary embodiment, forming the fourth insulating layer and the first planar layer pattern may include: first depositing a fourth insulating film on the substrate on which the aforementioned pattern is formed, then coating a planar film on the fourth insulating film, patterning the aforementioned film through a patterning process to form a fourth insulating layer 14 pattern covering the third metal layer, and a first planar layer 18 pattern covering the fourth insulating layer 14, a fourth via hole K4 is formed in the light emitting region A, the first planar layer 18 and the fourth insulating layer 14 in the fourth via hole K4 are removed to expose the surface of the first drain electrode 35, a fifth via hole K5 is formed in the sensing region B, the first planar layer 18 and the fourth insulating layer 14 in the fifth via hole K5 are removed to expose the surface of the second drain electrode 45, as shown in FIG. Fig.11 shown.
[0141] In example embodiments, the fourth insulating layer may be referred to as a first passivation (PVX1) layer.
[0142] At this point, the driving circuit layer 101 and the sensing circuit layer 201 are formed on the substrate. The driving circuit layer 101 may include a first shielding layer 31, an impurity absorption layer 100 and a first transistor 110. The first transistor 110 of the top gate structure may include a first active layer 32, a first gate electrode 33, a first source electrode 34 and a first drain electrode 35. The first source electrode 34 is connected to the first shielding layer 31 through a first via hole to form a double-gate structure. The sensing circuit layer 201 may include a second shielding layer 41, an impurity absorption layer 100 and a second transistor 210. The second transistor 210 of the top gate structure may include a second active layer 42, a second gate electrode 43, a second source electrode 44 and a second drain electrode 45.
[0143] (9) Forming a fourth metal layer pattern. In an exemplary embodiment, forming the fourth metal layer pattern may include: depositing a fourth metal film on the substrate on which the aforementioned pattern is formed, patterning the fourth metal film through a patterning process to form a fourth metal layer pattern, wherein the fourth metal layer pattern at least includes a connecting electrode 61 located in the light emitting region A and a first electrode 71 located in the sensing region B, wherein the connecting electrode 61 is connected to the first drain electrode of the first transistor 110 through a fourth via hole K4, and the first electrode 71 is connected to the second drain electrode of the second transistor 210 through a fifth via hole K5, as shown in FIG. Fig.12 shown.
[0144] In example embodiments, the fourth metal layer may be referred to as a second source-drain metal (SD2) layer.
[0145] (10) Forming a fifth insulating layer pattern. In an exemplary embodiment, forming the fifth insulating layer pattern may include: depositing a fifth insulating film on the substrate on which the aforementioned pattern is formed, patterning the fifth insulating film through a patterning process to form a fifth insulating layer 15 pattern covering the fourth metal layer, forming a sixth via hole K6 on the fifth insulating layer 15 in the sensing area B, and etching the fifth insulating layer 15 in the sixth via hole K6 to expose the surface of the first electrode 71, such as Fig.13 shown.
[0146] In example embodiments, the fifth insulating layer may be referred to as a second passivation (PVX2) layer.
[0147] (11) Forming a photodiode pattern. In an exemplary embodiment, forming a photodiode pattern may include: depositing a first doped film, an intrinsic film, a second doped film, and a first conductive film in sequence on a substrate on which the aforementioned pattern is formed, patterning the first doped film, the intrinsic film, the second doped film, and the first conductive film by a patterning process, forming a stacked first doped layer 72, an intrinsic layer 73, a second doped layer 74, and a second electrode 75 on the first electrode 71 in the sixth via hole K6, the first doped layer 72 being disposed on a side of the first electrode 71 away from the substrate, the intrinsic layer 73 being disposed on a side of the first doped layer 72 away from the substrate, the second doped layer 74 being disposed on a side of the intrinsic layer 73 away from the substrate, and the second electrode 75 being disposed on a side of the second doped layer 74 away from the substrate, as shown in FIG. Fig.14 shown.
[0148] In an exemplary embodiment, the material of the first doped film and the second doped film may be a silicon-based semiconductor such as amorphous silicon, microcrystalline silicon or silicon-germanium alloy, and the doped film may be formed by doping after deposition. In an exemplary embodiment, the doping process may be N-type ion implantation or P-type ion implantation to form an N-type doped layer or a P-type doped layer. The material of the intrinsic film may be a silicon-based semiconductor such as amorphous silicon, microcrystalline silicon or silicon-germanium alloy, and the material of the conductive film may be a metal oxide transparent conductive material with a high work function, such as indium tin oxide (ITO) or indium zinc oxide (IZO).
[0149] In an exemplary embodiment, the first doping layer 72 may be a P-type doping layer and the second doping layer 74 may be an N-type doping layer, or the first doping layer 72 may be an N-type doping layer and the second doping layer 74 may be a P-type doping layer.
[0150] At this point, a PIN photodiode as a photosensitive device is formed, and the photodiode includes a first electrode 71, a first doped layer 72, an intrinsic layer 73, a second doped layer 74, and a second electrode 75 arranged in sequence along a direction perpendicular to the substrate, and the first electrode 71 is connected to the second drain electrode of the second transistor 210 through a via hole. In an exemplary embodiment, the thickness of the photodiode may be about 0.8 μm to 1.2 μm. For example, the thickness of the photodiode may be about 1 μm.
[0151] (12) Forming a sixth insulating layer and a second planar layer pattern. In an exemplary embodiment, forming the sixth insulating layer and the second planar layer pattern may include: first depositing a sixth insulating film on the substrate on which the aforementioned pattern is formed, then coating a planar film on the sixth insulating film, patterning the aforementioned film through a patterning process to form a sixth insulating layer 16 pattern covering the PIN photodiode, and a second planar layer 19 pattern covering the sixth insulating layer 16, a seventh via hole K7 is formed in the light emitting region A, an eighth via hole K8 is formed in the sensing region B, the second planar layer 19, the sixth insulating layer 16, and the fifth insulating layer 15 in the seventh via hole K7 are removed to expose the surface of the connecting electrode 61, and the second planar layer 19 and the sixth insulating layer 16 in the eighth via hole K8 are removed to expose the surface of the second electrode 75, as shown in FIG. Fig.15 shown.
[0152] In exemplary embodiments, the sixth insulating layer 16 may be referred to as a third passivation (PVX3) layer.
[0153] (13) Forming a second conductive layer pattern. In an exemplary embodiment, forming the second conductive layer pattern may include: depositing a second conductive film on the substrate on which the aforementioned pattern is formed, patterning the second conductive film through a patterning process to form a second conductive layer pattern, wherein the second conductive layer pattern includes at least an anode 81 and an electrode lead 91 that are isolated and arranged, wherein the anode 81 may be located in the light emitting region A and the sensing region B, and the electrode lead 91 may be located in the sensing region B, wherein the anode 81 is connected to the connection electrode 61 through the seventh via hole K7, and the electrode lead 91 is connected to the second electrode 75 through the eighth via hole K8, as shown in FIG. Fig.16 shown.
[0154] In an exemplary embodiment, the second conductive layer may be a single-layer transparent conductive film, such as indium tin oxide (ITO) or indium zinc oxide (IZO), or may be a multi-layer composite structure, such as ITO / Al / ITO.
[0155] At this point, the photoelectric structure layer 202 is prepared. The photoelectric structure layer 202 may include an electrode lead 91 and a PIN photodiode. The photodiode includes a first electrode 71, a first doped layer 72, an intrinsic layer 73, a second doped layer 74, and a second electrode 75 arranged in sequence along a direction perpendicular to the substrate. The first electrode 71 is connected to the second drain electrode of the second transistor 210 through a via, and the second electrode 75 is connected to the electrode lead 91 through a via.
[0156] (14) Forming a pixel definition layer pattern. In an exemplary embodiment, forming a pixel definition layer pattern may include: coating a pixel definition film on a substrate on which the aforementioned pattern is formed, patterning the pixel definition film through a patterning process to form a pixel definition (PDL) layer 82 pattern covering the second conductive layer pattern, the pixel definition layer 82 being provided with a first pixel opening V1 and a second pixel opening V2, the first pixel opening V1 being located in the light emitting region A, the second pixel opening V2 being located in the sensing region B, the pixel definition layers within the first pixel opening V1 and the second pixel opening V2 being removed, and both exposing the surface of the anode 81, as shown in FIG. Fig.17 shown.
[0157] In an exemplary embodiment, the pixel definition layer may be made of polyimide (PI), acrylic, or polyethylene terephthalate (PET), etc. In a plane parallel to the display substrate, the shape of the first pixel opening and the second pixel opening may be a triangle, a rectangle, a polygon, a circle, an ellipse, etc. In a plane perpendicular to the display substrate, the cross-sectional shape of the first pixel opening and the second pixel opening may be a rectangle or a trapezoid, etc.
[0158] In an exemplary embodiment, the spacer pillars (PS) may be formed simultaneously in forming the pixel definition layer pattern, and the pixel definition layer and the spacer pillars may be formed through a single patterning process using a gray tone mask.
[0159] (15) Forming an organic light-emitting layer and a cathode pattern. In an exemplary embodiment, forming an organic light-emitting layer and a cathode pattern may include: forming an organic light-emitting layer 83 pattern on a substrate formed with the aforementioned pattern by evaporation or inkjet printing, wherein the organic light-emitting layer 83 in each sub-pixel is connected to the anode 81 through a first pixel opening V1 in the light-emitting region A and a second pixel opening V2 in the sensing region B. Subsequently, forming a cathode 84 pattern by evaporation, wherein the cathode 84 may be an integral structure connected together and connected to the organic light-emitting layer 83 in each sub-pixel, such as Fig.18 shown.
[0160] In an exemplary embodiment, the organic light-emitting layer may include an emitting layer (Emitting Layer, referred to as EML), and any one or more of the following layers: a hole injection layer (Hole Injection Layer, referred to as HIL), a hole transport layer (Hole Transport Layer, referred to as HTL), an electron blocking layer (Electron Block Layer, referred to as EBL), a hole blocking layer (Hole Block Layer, referred to as HBL), an electron transport layer (Electron Transport Layer, referred to as ETL) and an electron injection layer (Electron Injection Layer, referred to as EIL).
[0161] In an exemplary embodiment, the organic light-emitting layers of different sub-pixels can emit light of different colors, such as red light, green light and blue light. The light-emitting layer in the sub-pixel emitting red light uses a red light-emitting material, the light-emitting layer in the sub-pixel emitting green light uses a green light-emitting material, and the light-emitting layer in the sub-pixel emitting blue light uses a blue light-emitting material. In an exemplary embodiment, the hole injection layer, hole transport layer, electron blocking layer, hole blocking layer, electron transport layer and electron injection layer of all sub-pixels can be a common layer connected together, and the light-emitting layers of adjacent sub-pixels can have a small amount of overlap, or can be isolated. In an exemplary embodiment, the organic light-emitting layer can be formed by evaporation using a fine metal mask (Fine Metal Mask, referred to as FMM) and an open mask (Open Mask), or by inkjet technology.
[0162] At this point, the light emitting structure layer 102 is prepared, and the light emitting structure layer 102 may include an anode 81, a pixel definition layer 82, an organic light emitting layer 83 and a cathode 84. The anode 81 is connected to the first drain electrode of the first transistor 110 through the connecting electrode 61, and the organic light emitting layer 83 in the first pixel opening and the second pixel opening region is arranged between the anode 81 and the cathode 84. In an exemplary embodiment, the light emitted by the organic light emitting layer in the first pixel opening region passes through the driving circuit layer and the substrate, and then is emitted from the side of the substrate away from the driving circuit layer (bottom emission) to achieve image display. The light emitted by the organic light emitting layer in the second pixel opening region is incident on the photodiode, which senses the intensity of the light, converts the light signal into an electrical signal, and then feeds it back to the pixel driving circuit to achieve corresponding compensation.
[0163] In an exemplary embodiment, after the light-emitting structure layer is prepared, an encapsulation structure layer can be formed. The encapsulation structure layer can include a stacked first encapsulation layer, a second encapsulation layer, and a third encapsulation layer. The first encapsulation layer and the third encapsulation layer can be made of inorganic materials, and the second encapsulation layer can be made of organic materials. The second encapsulation layer is arranged between the first encapsulation layer and the third encapsulation layer to form a stacked structure of inorganic material / organic material / inorganic material, which can ensure that external water vapor cannot enter the light-emitting structure layer.
[0164] In an exemplary embodiment, the first metal film, the second metal film, the third metal film and the fourth metal film may be made of metal materials, such as any one or more of silver (Ag), copper (Cu), aluminum (Al), titanium (Ti) and molybdenum (Mo), or alloy materials of the above metals, such as aluminum neodymium alloy (AlNd) or molybdenum niobium alloy (MoNb), and may be a single-layer structure, or a multi-layer composite structure, such as Ti / Al / Ti, etc. The second insulating layer, the third insulating layer, the fourth insulating layer, the fifth insulating layer and the sixth insulating layer may be made of any one or more of silicon oxide (SiOx), silicon nitride (SiNx) and silicon oxynitride (SiON), and may be a single layer, a multi-layer or a composite layer. The first planar layer and the second planar layer may be made of organic materials, such as resin, etc., which are not limited in the present disclosure.
[0165] In an OLED display substrate structure, a shielding layer of a metal material is arranged on a substrate, a buffer layer covers the shielding layer and the substrate, and an active layer of a transistor is arranged on the buffer layer. When the display substrate is exposed to a hydrogen environment for a long time, hydrogen elements will penetrate through the circuit layer to the buffer layer. Since the buffer layer using silicon oxide has a poor absorption capacity for hydrogen elements, more hydrogen elements will penetrate into the active layer of the transistor. For the active layer using oxide, the penetration of hydrogen elements will make the oxide conductive, thereby causing the transistor to be in a state of high current. Although the buffer layer uses silicon nitride or silicon hydroxide to improve the absorption capacity of the buffer layer for hydrogen elements, since the active layer of the transistor is arranged on the buffer layer, the use of a buffer layer of silicon nitride or silicon hydroxide will not only cause a negative bias problem in the first transistor and the second transistor, which has a greater impact on the electrical characteristics of the transistor, but also deteriorate the contact interface between the active layer and the buffer layer, which has a greater impact on the overall performance of the display substrate. In addition, in the high-temperature environment of preparing the circuit layer, the oxygen elements in the substrate and the metal elements in the shielding layer will also penetrate through the buffer layer to the active layer of the transistor, affecting the electrical characteristics of the transistor.
[0166] According to the structure and preparation process of the display substrate of the exemplary embodiment of the present disclosure, it can be seen that the exemplary embodiment of the present disclosure can effectively reduce the penetration of hydrogen, oxygen and metal elements into the active layer of the transistor by setting an impurity absorption layer, and the impurity absorption layer is set between the metal layer and the buffer layer. When the display substrate is exposed to a hydrogen atmosphere, the hydrogen element penetrates through the circuit layer and the buffer layer to the impurity absorption layer. Since the impurity absorption layer of the present disclosure adopts a nitrogen silicon compound, and the atomic ratio of silicon and nitrogen in the impurity absorption layer is strictly controlled by controlling the process parameters in the process of forming the impurity absorption layer, the hydrogen element that penetrates into the impurity absorption layer forms an H=N bond with the nitrogen element in the impurity absorption layer. The formed H=N bond can effectively reduce the penetration of hydrogen into the oxide active layer, weaken the influence of hydrogen on the oxide active layer, avoid the conductorization of the oxide active layer, and avoid the transistor being in a state of high current. In the high temperature environment of the preparation process, when the oxygen element in the substrate and the metal element in the shielding layer penetrate into the impurity absorption layer, the oxygen element and the metal element (M) form N=O bonds and N=M bonds with the nitrogen element in the impurity absorption layer, respectively. The formed N=O bonds and N=M bonds can effectively reduce the influence of the oxygen element and the metal element on the oxide active layer, avoid the shift of the transistor threshold voltage, and ensure the electrical performance of the transistor. The exemplary embodiment of the present disclosure shows that the substrate can effectively reduce the penetration of hydrogen elements, oxygen elements, metal elements, etc. into the active layer of the transistor, effectively ensure the electrical stability of the transistor, effectively ensure the uniformity of the electrical characteristics of the transistor, effectively avoid the appearance of a large number of bright spots on the display substrate, improve the yield rate, and improve the display effect.
[0167] The exemplary embodiment of the present disclosure forms a first transistor with a dual-gate structure by setting the first source electrode of the first transistor to be connected to the first shielding layer, that is, the first transistor may include a lower transistor and an upper transistor with the same channel. Even if hydrogen penetrates into the first active layer, since the signal voltage value of the gate electrode (first shielding layer) of the lower transistor is less than the signal voltage value of the gate electrode (first gate electrode) of the upper transistor, the negative bias degree of the threshold voltage of the lower transistor is less than the negative bias degree of the threshold voltage of the upper transistor, thereby reducing the overall negative bias degree of the first transistor, which can ensure the stability of the first transistor and the uniformity of the electrical characteristics of the transistor.
[0168] In the exemplary embodiment of the present disclosure, the thickness of the photodiode is set to be about 0.8 μm to 1.2 μm, and the thickness of the impurity absorption layer is about to The diffusion amount of hydrogen elements in the process of preparing photodiodes can be absorbed by the impurity absorption layer, which can effectively ensure the absorption efficiency of the impurity absorption layer, minimize the penetration of hydrogen elements into the active layer, and ensure the normal electrical characteristics of the transistor.
[0169] In the exemplary embodiment of the present disclosure, the thickness of the first shielding layer and the second shielding layer is set to be approximately to The thickness of the impurity absorption layer is to The diffusion amount of metal elements can be absorbed by the impurity absorption layer, which can effectively ensure the absorption efficiency of the impurity absorption layer, minimize the penetration of hydrogen elements into the active layer, and ensure the normal electrical characteristics of the transistor.
[0170] The manufacturing process of the display substrate of the exemplary embodiment of the present disclosure is simple and has good process compatibility, which is beneficial to ensuring display uniformity and reducing production costs.
[0171] Fig.19 A diagram showing the electrical characteristics of transistors in a substrate. Fig. 20 This is a diagram of electrical characteristics of transistors in a display substrate of an exemplary embodiment of the present disclosure, illustrating electrical characteristics of transistors at multiple locations on the display substrate. The width-to-length ratio (W / L) of the transistors at multiple locations is 15 / 6, and the data voltage Vd is 15.1V. Fig.19 This is the test result of the display substrate without the impurity absorption layer. Fig. 20 This is the test result of a display substrate with an impurity absorption layer. In the impurity absorption layer, the atomic ratio of silicon to nitrogen is 1:17. Fig.19 and Fig. 20 It can be seen that, compared with a display substrate without an impurity absorption layer, the display substrate of the exemplary embodiment of the present disclosure effectively ensures the stability of the transistor and the uniformity of the electrical characteristics of the transistor by providing the impurity absorption layer.
[0172] Fig.21 This is the test result diagram of the hydrogen content in the active layer. Fig. 22 The figure is a test result of the silicon content in the active layer. The dotted line in the figure is the test result without the impurity absorption layer, and the solid line is the test result of the display substrate with the impurity absorption layer. In the impurity absorption layer, the atomic ratio of silicon to nitrogen is 1:17. After the impurity absorption layer absorbs hydrogen, the atomic ratio of silicon to hydrogen in the impurity absorption layer is about 1:13. Fig.21 and Fig. 22 As shown, compared with the structure without an impurity absorption layer, the exemplary embodiment of the present disclosure provides an impurity absorption layer, which effectively reduces the penetration of hydrogen elements into the active layer, effectively reduces the hydrogen content in the active layer, and the silicon element content in the active layer does not change significantly, thereby avoiding the conductorization of the oxide active layer and ensuring the stability of the transistor.
[0173] Fig.23 FIG. 2 is a schematic cross-sectional structure diagram of another display substrate according to an exemplary embodiment of the present disclosure. Fig.23 As shown, the main structure of the display substrate of this exemplary embodiment is similar to that of the above-mentioned embodiment, and may include a driving circuit layer 101 and a light-emitting structure layer 102 arranged in the light-emitting region A, and a sensing circuit layer 201 and an optoelectronic structure layer 202 arranged in the sensing region B. The driving circuit layer 101 and the sensing circuit layer 201 include transistors and an impurity absorption layer 100. The atomic ratio of silicon element to nitrogen element in the impurity absorption layer 100 is 1:5 to 1:35. The impurity absorption layer is configured to reduce the penetration of hydrogen elements into the transistors in the driving circuit layer 101 and the sensing circuit layer 201 to ensure the normal electrical characteristics of the transistors, thereby avoiding a large number of bright spots on the display substrate and improving the yield rate. Different from the above-mentioned embodiment, the impurity absorption layer 100 of this exemplary embodiment is located on the side of the active layer of the transistor away from the substrate, and at least a third insulating layer is provided between the impurity absorption layer 100 and the active layer of the transistor.
[0174] In an exemplary embodiment, the driving circuit layer 101 of the light emitting region A may include: a first shielding layer disposed on the substrate, a first insulating layer 11 covering the first shielding layer, and a first active layer disposed on a side of the first insulating layer 11 away from the substrate, a second insulating layer 12 disposed on a side of the first active layer away from the substrate, a first gate electrode disposed on a side of the second insulating layer 12 away from the substrate, a third insulating layer 13 covering the first gate electrode, a first source electrode and a first drain electrode disposed on a side of the third insulating layer 13 away from the substrate, an impurity absorption layer 100 covering the first source electrode and the first drain electrode, and a first planar layer 18 disposed on a side of the impurity absorption layer 100 away from the substrate. The first gate electrode, the first active layer, the first source electrode, and the first drain electrode constitute a first transistor 110, and the first source electrode is connected to the first shielding layer 31 through a via.
[0175] In an exemplary embodiment, the sensing circuit layer 201 of the sensing region B may include: a second blocking layer disposed on the substrate, a first insulating layer 11 covering the second blocking layer, and a second active layer disposed on a side of the first insulating layer 11 away from the substrate, a second insulating layer 12 disposed on a side of the second active layer away from the substrate, a second gate electrode disposed on a side of the second insulating layer 12 away from the substrate, a third insulating layer 13 covering the second gate electrode, a second source electrode and a second drain electrode disposed on a side of the third insulating layer 13 away from the substrate, an impurity absorption layer 100 covering the second source electrode and the second drain electrode, and a first planar layer 18 disposed on a side of the impurity absorption layer 100 away from the substrate. The second gate electrode, the second active layer, the second source electrode, and the second drain electrode constitute a second transistor 210.
[0176] In an exemplary embodiment, the structures of the light emitting structure layer 102 and the optoelectronic structure layer 202 may be the same as those in the previous embodiment.
[0177] The manufacturing process of the display substrate of this exemplary embodiment is similar to that of the aforementioned embodiment, except that the first insulating layer and the semiconductor layer pattern are directly formed after the first metal layer pattern is formed, and after the third metal layer pattern is formed, an impurity absorption layer covering the third metal layer pattern is first formed, and then the first planarization layer pattern is formed. The process of forming the impurity absorption layer is the same as that of the aforementioned embodiment, and will not be repeated here.
[0178] The exemplary embodiment of the present disclosure sets an impurity absorption layer, and the impurity absorption layer is set on the side of the active layer away from the substrate, which can effectively reduce the penetration of hydrogen elements into the active layer of the transistor. When the display substrate is exposed to a hydrogen atmosphere, when the hydrogen element penetrates into the impurity absorption layer, since the impurity absorption layer of the present disclosure adopts a nitrogen silicon compound, and in the process of forming the impurity absorption layer, the atomic ratio of silicon elements and nitrogen elements in the impurity absorption layer is strictly controlled by controlling the process parameters, so that the hydrogen elements that penetrate into the impurity absorption layer form an H=N bond with the nitrogen elements in the impurity absorption layer. The formed H=N bond can effectively reduce the number of hydrogen elements that penetrate into the oxide active layer, weaken the influence of hydrogen elements on the oxide active layer, avoid the conductorization of the oxide active layer, and avoid the transistor from being in a state of high current. The display substrate of the exemplary embodiment of the present disclosure can effectively reduce the penetration of hydrogen elements into the active layer of the transistor, effectively ensure the electrical stability of the transistor, effectively ensure the uniformity of the electrical characteristics of the transistor, effectively avoid the appearance of a large number of bright spots on the display substrate, improve the yield rate, and improve the display effect.
[0179] The exemplary embodiment of the present disclosure forms a first transistor with a dual-gate structure by setting the first source electrode of the first transistor to be connected to the first shielding layer, that is, the first transistor may include a lower transistor and an upper transistor with the same channel. Even if hydrogen penetrates into the first active layer, since the signal voltage value of the gate electrode (first shielding layer) of the lower transistor is less than the signal voltage value of the gate electrode (first gate electrode) of the upper transistor, the negative bias degree of the threshold voltage of the lower transistor is less than the negative bias degree of the threshold voltage of the upper transistor, thereby reducing the overall negative bias degree of the first transistor, which can ensure the stability of the first transistor and the uniformity of the electrical characteristics of the transistor.
[0180] Fig.24 FIG. 2 is a schematic cross-sectional structure diagram of another display substrate according to an exemplary embodiment of the present disclosure. Fig.24As shown, the main structure of the display substrate of this exemplary embodiment is similar to that of the above-mentioned embodiment, including a driving circuit layer 101 and a light-emitting structure layer 102 arranged in the light-emitting region A, and a sensing circuit layer 201 and an optoelectronic structure layer 202 arranged in the sensing region B. The driving circuit layer 101 and the sensing circuit layer 201 contain transistors and an impurity absorption layer 100. The atomic ratio of silicon element to nitrogen element in the impurity absorption layer 100 is 1:5 to 1:35. The impurity absorption layer is configured to reduce the penetration of hydrogen element, oxygen element and metal element into the transistors in the driving circuit layer 101 and the sensing circuit layer 201 to ensure the normal electrical characteristics of the transistors, thereby avoiding a large number of bright spots on the display substrate and improving the yield rate. Different from the above-mentioned embodiment, the sensing region B of this exemplary embodiment is provided with a flat island 20.
[0181] In an exemplary embodiment, the driving circuit layer 101 of the light-emitting region A may include: a first blocking layer arranged on a substrate, an impurity absorption layer 100 covering the first blocking layer, a first insulating layer 11 arranged on a side of the impurity absorption layer 100 away from the substrate, a first active layer arranged on a side of the first insulating layer 11 away from the substrate, a second insulating layer 12 arranged on a side of the first active layer away from the substrate, a first gate electrode arranged on a side of the second insulating layer 12 away from the substrate, a third insulating layer 13 covering the first gate electrode, a first source electrode and a first drain electrode arranged on a side of the third insulating layer 13 away from the substrate, and a fourth insulating layer 14 covering the first source electrode and the first drain electrode.
[0182] In an exemplary embodiment, the sensing circuit layer 201 of the sensing region B may include: a second blocking layer disposed on the substrate, an impurity absorption layer 100 covering the second blocking layer, a first insulating layer 11 disposed on a side of the impurity absorption layer 100 away from the substrate, a second active layer disposed on a side of the first insulating layer 11 away from the substrate, a second insulating layer 12 disposed on a side of the second active layer away from the substrate, a second gate electrode disposed on a side of the second insulating layer 12 away from the substrate, a third insulating layer 13 covering the second gate electrode, a second source electrode and a second drain electrode disposed on a side of the third insulating layer 13 away from the substrate, a fourth insulating layer 14 covering the second source electrode and the second drain electrode, and a flat island 20 disposed on a side of the fourth insulating layer 14 away from the substrate.
[0183] The preparation process of the display substrate of this exemplary embodiment is similar to that of the above-mentioned embodiment, except that, on the substrate formed with the third metal layer pattern, a fourth insulating film is first deposited, and then an organic material film is coated on the fourth insulating film, and the above film is patterned by a gray tone mask patterning process to form a fourth insulating layer 14 pattern covering the third metal layer, and a flat island 20 pattern arranged on the fourth insulating layer 14, a fourth via hole is formed in the light emitting region A, the fourth insulating layer 14 in the fourth via hole is removed, and the surface of the first drain electrode is exposed, and a fifth via hole is formed in the sensing region B, and the flat island 20 and the fourth insulating layer 14 in the fifth via hole are removed, and the surface of the second drain electrode is exposed. Then, a fourth metal layer pattern is formed, and the fourth metal layer pattern at least includes a connecting electrode 61 located in the light emitting region A and a first electrode 71 located in the sensing region B, the connecting electrode 61 is arranged on the fourth insulating layer 14, and is connected to the first drain electrode of the first transistor 110 through the fourth via hole, and the first electrode 71 is arranged on the flat island 20, and is connected to the second drain electrode of the second transistor 210 through the fifth via hole.
[0184] Fig.25 Schematic diagram of a top view of a flat island and a photodiode according to an exemplary embodiment of the present disclosure. Fig.26 for Fig.25 The cross-sectional view along the AA axis only illustrates the flat island and the photodiode portion of the display substrate, and does not illustrate other film structures of the display substrate. Fig.25 As shown, in a plane parallel to the substrate, the shape of the flat island 20 may be a rectangle, the long side of the rectangle extends along a first direction X, the short side of the rectangle extends along a second direction Y, and the second direction Y intersects the first direction X. In an exemplary embodiment, the first direction X may be an extension direction of the first scan signal line, and the second direction Y may be perpendicular to the first direction X. The shape of the first electrode 71 may be a rectangle, which is similar to the shape of the flat island 20, the area of the first electrode 71 may be less than or equal to the area of the flat island 20, and the orthographic projection of the first electrode 71 on the substrate may be within the range of the orthographic projection of the flat island 20 on the substrate. The shape of the second electrode 75 may be a rectangle, which is similar to the shape of the first electrode 71, the area of the second electrode 75 may be less than or equal to the area of the first electrode 71, and the orthographic projection of the first electrode 71 on the substrate may be within the range of the orthographic projection of the first electrode 71 on the substrate. As shown Fig.26 As shown, in a plane perpendicular to the substrate, the first electrode 71 is arranged on one side of the third direction Z of the flat island 20, the first doped layer 72 is arranged on one side of the third direction Z of the first electrode 71, the intrinsic layer 73 is arranged on one side of the third direction Z of the first doped layer 72, the second doped layer 74 is arranged on one side of the third direction Z of the intrinsic layer 73, and the second electrode 75 is arranged on one side of the third direction Z of the second doped layer 74, and the third direction Z is the direction away from the substrate.
[0185] In an exemplary embodiment, the shapes of the flat island 20 , the first electrode 71 , and the second electrode 75 may be other shapes as long as they conform to the aforementioned projection relationship, which is not limited in the present disclosure.
[0186] In an exemplary embodiment, in the second direction Y, the width of the flat island 20 may be greater than the width of the first electrode 71, and the orthographic projection of the edge of the first electrode 71 on the substrate is located within the range of the orthographic projection of the edge of the flat island 20 on the substrate. In an exemplary embodiment, the first distance L1 between the edge of the first electrode 71 and the edge of the flat island 20 may be approximately 2 μm to 4 μm. For example, the first distance L1 may be approximately 3 μm.
[0187] In an exemplary embodiment, in the second direction Y, the width of the first electrode 71 may be greater than the width of the first doping layer 72, and the orthographic projection of the edge of the first doping layer 72 on the substrate is located within the range of the orthographic projection of the edge of the first electrode 71 on the substrate. In an exemplary embodiment, the second distance L2 between the edge of the first doping layer 72 and the edge of the first electrode 71 may be approximately 1 μm to 3 μm. For example, the second distance L2 may be approximately 2 μm.
[0188] In an exemplary embodiment, in the second direction Y, the width of the first doping layer 72 may be greater than the width of the second electrode 75, and the orthographic projection of the edge of the second electrode 75 on the substrate is located within the range of the orthographic projection of the edge of the first doping layer 72 on the substrate. In an exemplary embodiment, the third distance L3 between the edge of the second electrode 75 and the edge of the first doping layer 72 may be approximately 0.5 μm to 2.5 μm. For example, the third distance L3 may be approximately 1.5 μm.
[0189] In an exemplary embodiment, the distance between the edge of the second electrode 75 and the edge of the first electrode 71 (second distance L2+third distance L3) may be about 1.5 μm to 5.5 μm. For example, the sum of the second distance L2 and the third distance L3 may be about 3.5 μm.
[0190] like Fig.24 As shown, combined with Figures 5 to 18 , the exemplary embodiment of the present disclosure shows that the substrate may include:
[0191] Base 10;
[0192] A first metal layer is disposed on the substrate 10, and the first metal layer at least includes a first shielding layer 31 located in the light emitting area A and a second shielding layer 41 located in the sensing area B;
[0193] An impurity absorption layer 100 covering the first metal layer;
[0194] A first insulating layer 11 covering the impurity absorption layer 100;
[0195] A semiconductor layer disposed on a side of the first insulating layer 11 away from the substrate, the semiconductor layer at least comprising a first active layer 32 located in the light emitting region A and a second active layer 42 located in the sensing region B;
[0196] A second insulating layer 12 is disposed on the semiconductor layer, and a second metal layer is disposed on the second insulating layer 12, wherein the second metal layer at least includes a first gate electrode 33 located in the light emitting region A and a second gate electrode 43 located in the sensing region B;
[0197] The third insulating layer 13 covering the second metal layer, the third insulating layer 13 in the light emitting area A is provided with a first via hole K1 exposing the first shielding layer 31 and a second via hole K2 exposing the first active layer 32, and the third insulating layer 13 in the sensing area B is provided with a third via hole K3 exposing the second active layer 42;
[0198] A third metal layer is provided on the third insulating layer 13, the third metal layer at least includes a first source electrode 34 and a first drain electrode 35 located in the light emitting region A, and a second source electrode 44 and a second drain electrode 45 located in the sensing region B, the first source electrode 34 is connected to the first shielding layer 31 through a first via hole K1, the first source electrode 34 and the first drain electrode 35 are respectively connected to the first active layer 32 through a second via hole K2, and the second source electrode 44 and the second drain electrode 45 are respectively connected to the second active layer 42 through a third via hole K3;
[0199] A fourth insulating layer 14 covering the third metal layer and a flat island 20 disposed on the fourth insulating layer 14, the flat island 20 is located in the sensing region B, the light emitting region A is provided with a fourth via hole K4 exposing the first drain electrode 35, and the sensing region B is provided with a fifth via hole K5 exposing the second drain electrode 45;
[0200] A fourth metal layer is disposed on the fourth insulating layer 14 and the first planar layer 18, the fourth metal layer at least comprising a connecting electrode 61 located in the light emitting region A and disposed on the fourth insulating layer 14, and a first electrode 71 located in the sensing region B and disposed on the first planar layer 18, the connecting electrode 61 is connected to the first drain electrode 35 through a fourth via hole K4, and the first electrode 71 is connected to the second drain electrode 45 through a fifth via hole K5;
[0201] The fifth insulating layer 15 covers the fourth metal layer and the flat island 20 , and the sensing region B is provided with a sixth via hole K6 exposing the first electrode 71 ;
[0202] A first doped layer 72, an intrinsic layer 73, a second doped layer 74 and a second electrode 75 disposed on the first electrode 71;
[0203] a sixth insulating layer 16 covering the photodiode;
[0204] The second planar layer 19 covers the sixth insulating layer 16 , the light emitting region A is provided with a seventh via hole K7 exposing the connecting electrode 61 , and the sensing region B is provided with an eighth via hole K8 exposing the second electrode 75 ;
[0205] A second conductive layer disposed on the second flat layer 19, the second conductive layer at least comprising an anode 81 and an electrode lead 91, the anode 81 is connected to the connection electrode 61 through a seventh via hole K7, and the electrode lead 91 is connected to the second electrode 75 through an eighth via hole K8;
[0206] A pixel definition layer 82 covering the second conductive layer, a first pixel opening V1 exposing the anode 81 is provided in the light emitting region A, and a second pixel opening V2 exposing the anode 81 is provided in the sensing region B;
[0207] An organic light emitting layer 83 is disposed on the pixel definition layer 82, and the organic light emitting layer 83 is connected to the anode 81 through the first pixel opening V1 and the second pixel opening V2;
[0208] The cathode 84 is disposed on the organic light emitting layer 83 , and is connected to the organic light emitting layer 83 .
[0209] The exemplary embodiments of the present disclosure can not only achieve the same technical effects as the aforementioned embodiments, including effectively reducing the penetration of hydrogen, oxygen and metal elements into the active layer of the transistor and reducing the overall negative bias of the first transistor, but can also further reduce the influence of hydrogen on the active layer of the transistor. In a display substrate, a first flat layer that is laid flat on the entire surface is usually provided on the fourth insulating layer, that is, the first flat layer covers the entire substrate, and only vias are provided at corresponding positions. The inventors of the present application have found that since the first flat layer of organic material (such as resin) itself contains a large amount of hydrogen, the hydrogen elements in the photodiode preparation process and the hydrogen elements in the first flat layer itself will penetrate downward together, and the amount of hydrogen penetration is large, which has a greater impact on the active layer. The exemplary embodiment of the present disclosure arranges an island-shaped flat island on the fourth insulating layer, and the flat island is arranged in the sensing area B. Due to the reduction in the area of the flat island, not only the amount of hydrogen elements in the organic material is reduced as a whole, but also the release space of the hydrogen elements is increased. In the subsequent baking, the flat island has a larger space to release the hydrogen elements therein, and a large amount of hydrogen elements contained in it and hydrogen elements in the photodiode preparation process are released, which effectively reduces the amount of hydrogen elements penetrating downward, and effectively reduces the impact on the active layer. Since the first electrode is arranged on the side of the flat island away from the substrate, the first distance between the edge of the first electrode and the edge of the flat island is about 2μm to 4μm, so the first electrode of the metal material can effectively reduce most of the hydrogen elements in the preparation from entering the flat island, further reducing the hydrogen content in the flat island, further reducing the amount of hydrogen elements penetrating downward, and further reducing the impact on the active layer.
[0210] Fig. 27 FIG. 2 is a schematic cross-sectional structure diagram of another display substrate according to an exemplary embodiment of the present disclosure. Fig. 27 As shown, the main structure of the display substrate of this exemplary embodiment is similar to that of the above-mentioned embodiment, including a driving circuit layer 101 and a light-emitting structure layer 102 arranged in the light-emitting region A, and a sensing circuit layer 201 and an optoelectronic structure layer 202 arranged in the sensing region B. The driving circuit layer 101 and the sensing circuit layer 201 contain transistors and an impurity absorption layer 100. The atomic ratio of silicon element to nitrogen element in the impurity absorption layer 100 is 1:5 to 1:35, and the atomic ratio of silicon element to hydrogen element is 1:5 to 1:30. The impurity absorption layer is configured to reduce the penetration of hydrogen element, oxygen element and metal element into the transistors in the driving circuit layer 101 and the sensing circuit layer 201, so as to ensure the normal electrical characteristics of the transistors, thereby avoiding a large number of bright spots on the display substrate and improving the yield rate. Different from the above-mentioned embodiment, a color filter layer 85 is provided in the light-emitting structure layer 102 of this exemplary embodiment.
[0211] In an exemplary embodiment, the light-emitting structure layer 102 may include an anode 81, a pixel definition layer 82, an organic light-emitting layer 83, a cathode 84 and a color filter layer 85. The structures of the anode 81, the pixel definition layer 82, the organic light-emitting layer 83 and the cathode 84 are similar to those of the aforementioned embodiments. The color filter layer 85 may be arranged on the side of the sixth insulating layer 16 away from the substrate, and the second flat layer 19 covers the color filter layer 85.
[0212] In an exemplary embodiment, the organic light-emitting layers of different sub-pixels may emit the same color light, such as white light or blue light. In an exemplary embodiment, the hole injection layer, hole transport layer, electron blocking layer, light-emitting layer, hole blocking layer, electron transport layer and electron injection layer of all sub-pixels may be a common layer connected together, and the organic light-emitting layer may be formed by open mask evaporation or by inkjet process.
[0213] In an exemplary embodiment, the color filter layer 85 is configured to filter or convert the light emitted by the organic light emitting layer into corresponding color light, and the color filter layers of different sub-pixels can filter or convert light of different colors, such as red light, green light and blue light. For example, the color filter layer in the sub-pixel that filters out or converts red light can use a red color filter or a red quantum dot material, the color filter layer in the sub-pixel that filters out or converts green light can use a green color filter or a green quantum dot material, and the color filter layer in the sub-pixel that filters out or converts blue light can use a blue color filter or a blue quantum dot material. After the light emitted by the organic light emitting layer in the first pixel opening area passes through the color filter layer, it is filtered out or converted into the corresponding color light, and is emitted from the side of the substrate away from the driving circuit layer to realize image display.
[0214] The preparation process of the display substrate of this exemplary embodiment is similar to that of the aforementioned embodiment, except that after the sixth insulating film covering the PIN photodiode is deposited, a color filter layer 85 is formed on the sixth insulating film in the light emitting area A, and then a flat film is coated, and the flat film covers the color filter layer 85. Then, patterning is performed through a patterning process to form a pattern of the sixth insulating layer 16 covering the PIN photodiode, a pattern of the color filter layer 85 disposed on the sixth insulating layer 16, and a pattern of the second flat layer 19 covering the color filter layer 85 and the sixth insulating layer 16.
[0215] The structure and preparation process shown in the present disclosure are merely exemplary illustrations. The display substrate of the present disclosure can be applied to other display devices having pixel driving circuits, such as quantum dot displays, etc., which are not limited in the present disclosure. In an exemplary embodiment, the corresponding structure can be changed and the patterning process can be increased or decreased according to actual needs. For example, a plurality of impurity absorption layers can be provided, and the impurity absorption layers can be provided simultaneously on the side of the active layer away from the substrate and on the side of the active layer close to the substrate. For another example, the impurity absorption layer can be patterned to form an impurity absorption island, and the position of the impurity absorption island corresponds to the position of the active layer, etc. For another example, the display substrate can be a top-emitting display substrate, which is not limited in the present disclosure.
[0216] The present disclosure also provides a method for preparing a display substrate. In an exemplary embodiment, the preparation method may include:
[0217] A circuit layer is formed on a substrate; the circuit layer includes at least one impurity absorption layer and at least one transistor, the transistor includes an active layer, and at least one insulating layer is provided between the impurity absorption layer and the active layer; the atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:5 to 1:35;
[0218] A light-emitting structure layer and a photoelectric structure layer are formed on the circuit layer.
[0219] In an exemplary embodiment, forming a circuit layer on a substrate may include:
[0220] forming a first metal layer on a substrate;
[0221] depositing an impurity absorbing film on a side of the first metal layer away from the substrate, and performing plasma treatment on the impurity absorbing film to form an impurity absorbing layer covering the first metal layer;
[0222] forming a first insulating layer on a side of the impurity absorption layer away from the substrate;
[0223] A first transistor and a second transistor are formed on a side of the first insulating layer away from the substrate.
[0224] In an exemplary embodiment, depositing the impurity absorbing film may include: using chemical vapor deposition to deposit a film with a thickness of 500 W to 1200 W at a deposition power of 330° C. to 450° C. and a deposition pressure of 1000 mT to 1800 mT. to The impurity absorption film is made of any one or more of the following materials: silicon nitride, silicon oxynitride and aluminum silicon nitride.
[0225] In an exemplary embodiment, performing plasma treatment on the impurity absorption film may include performing plasma treatment on the impurity absorption film using nitrous oxide at a plasma power of 600 W to 1500 W and a plasma pressure of 600 mT to 2000 mT.
[0226] The present disclosure provides a method for preparing a display substrate. By setting an impurity absorption layer, the impurity absorption layer is set between the metal layer and the buffer layer, which can effectively reduce the penetration of hydrogen, oxygen and metal elements into the active layer of the transistor, effectively ensure the electrical stability of the transistor, effectively ensure the uniformity of the electrical characteristics of the transistor, effectively avoid the appearance of a large number of bright spots on the display substrate, improve the yield rate, and improve the display effect. The method for preparing the display substrate of the exemplary embodiment of the present disclosure has a simple process and good process compatibility, which is conducive to ensuring display uniformity and reducing production costs.
[0227] The present disclosure also provides a display device, including the display substrate of the above embodiment. The display device can be any product or component with a display function, such as a mobile phone, a tablet computer, a television, a monitor, a notebook computer, a digital photo frame or a navigator.
[0228] Although the embodiments disclosed in the present disclosure are as above, the contents described are only embodiments adopted to facilitate understanding of the present disclosure and are not intended to limit the present disclosure. Any technician in the field to which the present disclosure belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the present disclosure, but the scope of patent protection of this application shall still be subject to the scope defined in the attached claims.
Claims
1. A display substrate, It is characterized in that The invention comprises a circuit layer arranged on a substrate, and a light emitting structure layer and a photoelectric structure layer arranged on a side of the circuit layer away from the substrate, wherein the circuit layer comprises at least one impurity absorption layer and at least one transistor, the transistor comprises an active layer, and at least one insulating layer is arranged between the impurity absorption layer and the active layer; the atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:5 to 1:35; The display substrate comprises a light-emitting area and a sensing area; the circuit layer comprises a driving circuit layer arranged in the light-emitting area and a sensing circuit layer arranged in the sensing area, the driving circuit layer comprises a first transistor, the sensing circuit layer comprises a second transistor, the light-emitting structure layer is arranged on a side of the driving circuit layer away from the substrate, and the photoelectric structure layer is arranged on a side of the sensing circuit layer away from the substrate; the light-emitting structure layer comprises an anode, an organic light-emitting layer and a cathode; the photoelectric structure layer comprises a photodiode and an electrode lead; the anode and the electrode lead are arranged on the same layer; The driving circuit layer includes: a first blocking layer arranged on the substrate, an impurity absorption layer arranged on a side of the first blocking layer away from the substrate, a first insulating layer arranged on a side of the impurity absorption layer away from the substrate, and a first transistor arranged on a side of the first insulating layer away from the substrate; the sensing circuit layer includes: a second blocking layer arranged on the substrate, an impurity absorption layer arranged on a side of the second blocking layer away from the substrate, a first insulating layer arranged on a side of the impurity absorption layer away from the substrate, and a second transistor arranged on a side of the first insulating layer away from the substrate.
2. The display substrate according to claim 1, It is characterized in that The atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:10 to 1:
25.
3. The display substrate according to claim 1, It is characterized in that The atomic ratio of silicon element to hydrogen element in the impurity absorption layer is 1:5 to 1:
30.
4. The display substrate according to claim 3, It is characterized in that The atomic ratio of silicon element to hydrogen element in the impurity absorption layer is 1:5 to 1:
15.
5. The display substrate according to claim 1, It is characterized in that The material of the impurity absorption layer includes any one or more of the following: silicon nitride, silicon oxynitride and aluminum silicon nitride.
6. The display substrate according to claim 1, It is characterized in that The thickness of the impurity absorption layer is to The photodiode has a thickness of 0.8 μm to 1.2 μm.
7. The display substrate according to claim 1, It is characterized in that The first transistor includes: a first active layer arranged on a side of the first insulating layer away from the substrate, a second insulating layer arranged on a side of the first active layer away from the substrate, a first gate electrode arranged on a side of the second insulating layer away from the substrate, a third insulating layer arranged on a side of the first gate electrode away from the substrate, a first source electrode and a first drain electrode arranged on a side of the third insulating layer away from the substrate, and the first source electrode is connected to the first blocking layer through a via; the second active layer of the second transistor is arranged on the same layer as the first active layer, the second gate electrode of the second transistor is arranged on the same layer as the first gate electrode, and the second source electrode and the second drain electrode of the second transistor are arranged on the same layer as the first source electrode and the first drain electrode.
8. The display substrate according to claim 1, It is characterized in that The sensing circuit layer further includes: a fourth insulating layer disposed on a side of the second transistor away from the substrate, a flat island disposed on a side of the fourth insulating layer away from the substrate, the flat island disposed in the sensing region, and the photodiode disposed on a side of the flat island away from the substrate.
9. The display substrate according to claim 8, It is characterized in that The photodiode comprises a first electrode arranged on a side of the flat island away from the substrate, and a first doped layer, an intrinsic layer, a second doped layer and a second electrode arranged in sequence on the first electrode, the first electrode is connected to the second drain electrode of the second transistor through a via hole, and the second electrode is connected to the electrode lead through a via hole; the flat island, the first electrode and the second electrode are all rectangular with long sides extending along the first direction; In the second direction, the orthographic projection of the edge of the first electrode on the substrate is within the range of the orthographic projection of the edge of the flat island on the substrate, and a first distance between the edge of the first electrode and the edge of the flat island is 2 μm to 4 μm; The orthographic projection of the edge of the second electrode on the substrate is within the range of the orthographic projection of the edge of the first electrode on the substrate, and the distance between the edge of the second electrode and the edge of the first electrode is 1.5 μm to 5.5 μm; the second direction intersects the first direction.
10. A display device, It is characterized in that The display substrate comprises the display substrate as claimed in any one of claims 1 to 9.
11. A method for preparing a display substrate, It is characterized in that The display substrate comprises a light emitting area and a sensing area; the preparation method comprises: A circuit layer is formed on a substrate; the circuit layer includes at least one impurity absorption layer and at least one transistor, the transistor includes an active layer, and at least one insulating layer is arranged between the impurity absorption layer and the active layer; the atomic ratio of silicon element to nitrogen element in the impurity absorption layer is 1:5 to 1:35; the circuit layer includes a driving circuit layer arranged in the light emitting area and a sensing circuit layer arranged in the sensing area, the driving circuit layer includes a first transistor, the sensing circuit layer includes a second transistor, the driving circuit layer includes: a first shielding layer arranged on the substrate, an impurity absorption layer arranged on a side of the first shielding layer away from the substrate, a first insulating layer arranged on a side of the impurity absorption layer away from the substrate, and a first transistor arranged on a side of the first insulating layer away from the substrate; the sensing circuit layer includes: a second shielding layer arranged on the substrate, an impurity absorption layer arranged on a side of the second shielding layer away from the substrate, a first insulating layer arranged on a side of the impurity absorption layer away from the substrate, and a second transistor arranged on a side of the first insulating layer away from the substrate; A light-emitting structure layer and a photoelectric structure layer are formed on the circuit layer, wherein the light-emitting structure layer is arranged on the side of the driving circuit layer away from the substrate, and the photoelectric structure layer is arranged on the side of the sensing circuit layer away from the substrate; the light-emitting structure layer includes an anode, an organic light-emitting layer and a cathode; the photoelectric structure layer includes a photodiode and an electrode lead; the anode and the electrode lead are arranged on the same layer.
12. The preparation method according to claim 11, It is characterized in that A circuit layer is formed on a substrate, comprising: forming a first metal layer on a substrate; depositing an impurity absorbing film on a side of the first metal layer away from the substrate, and performing plasma treatment on the impurity absorbing film to form an impurity absorbing layer covering the first metal layer; forming a first insulating layer on a side of the impurity absorption layer away from the substrate; A first transistor and a second transistor are formed on a side of the first insulating layer away from the substrate.
13. The preparation method according to claim 12, It is characterized in that Depositing an impurity absorbing film, comprising: using a chemical vapor deposition method, at a deposition power of 500W to 1200W, a deposition temperature of 330°C to 450°C, and a deposition pressure of 1000mT to 1800mT, the deposition thickness is to The impurity absorption film is made of any one or more of the following materials: silicon nitride, silicon oxynitride and aluminum silicon nitride.
14. The preparation method according to claim 12, It is characterized in that The impurity absorption film is subjected to plasma treatment, comprising: using nitrous oxide to perform plasma treatment on the impurity absorption film at a plasma power of 600W to 1500W and a plasma pressure of 600mT to 2000mT.
Citation Information
Patent Citations
Display substrate, display panel and display substrate manufacturing method
CN109841632A
Display substrate and manufacturing method thereof
CN112331675A
Thin-film transistor array substrate, display device including the same, and method of manufacturing the thin-film transistor array substrate
US20150048320A1
Back plate and manufacturing method thereof
US20190067403A1
Pixel structure and display panel
US20190198585A1