Magnetic sensor array having a TMR stack including two free layers
By using synthetic antiferromagnetic free layer and new magnetic layer structure in TMR sensors, the reliability and performance differences caused by TMR sensor manufacturing methods are solved, and the sensitivity and manufacturing efficiency of the magnetic field sensor of Wheatstone bridge are improved.
Patent Information
- Application Number
- CN202080007007.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-30
- Filing Date
- 2020-03-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-03-31
AI Technical Summary
The manufacturing methods of existing TMR sensors lead to differences in reliability and performance, affecting magnetoresistive response, and the sensitivity of sensors to be used in Wheatstone bridges is limited.
Four identical TMR sensors using synthetic antiferromagnetic free layer as the top layer, by removing the spacer layer and the second magnetic layer, a new magnetic layer is formed so that its thickness is basically the same as the combination of the original layer, and in the exposed first A new magnetic layer is deposited on a magnetic layer to create a TMR sensor with different resistance characteristics.
It achieves high reliability and performance consistency of TMR sensors, improves the sensitivity of the magnetic field sensor of the Wheatstone bridge, increases the output voltage, and improves manufacturing efficiency.
Smart Images

Figure CN113196079B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. application 16 / 730,746, filed on December 30, 2019, which claims priority to and the benefit of U.S. Provisional Patent Application Serial No. 62 / 891,153, filed on August 23, 2019, both of which are hereby incorporated by reference into this document. Background Art Technical Field
[0004] Embodiments of the present disclosure generally relate to Wheatstone bridge arrays and methods of making the same.
[0005] Description of Related Art
[0006] A Wheatstone bridge is a circuit used to measure unknown resistance by balancing two legs of a bridge circuit, one of which contains the unknown component. The Wheatstone circuit provides extremely accurate measurements compared to a simple voltage divider.
[0007] The Wheatstone bridge includes multiple resistors and, more recently, magnetic materials such as magnetic sensors. Magnetic sensors may include Hall effect magnetic sensors, anisotropic magnetoresistive sensors (AMR), giant magnetoresistive (GMR) sensors, and tunnel magnetoresistive (TMR) sensors. Compared to other magnetic sensors, TMR sensors have very high sensitivity.
[0008] The reliability and performance of a TMR sensor determines the magnetoresistive response. Various factors affect the reliability and performance of a TMR sensor, such as the material of the TMR sensor and, more importantly, the method of manufacturing the TMR sensor. For example, while two different TMR sensors can be manufactured using exactly the same material, the TMR sensors will have different reliability and performance due to different manufacturing processes.
[0009] Therefore, there is a need in the art for TMR sensors and methods of manufacturing the same that achieve good reliability and performance. Summary of the invention
[0010] The present disclosure as a whole relates to a Wheatstone bridge array including TMR sensors and a method for manufacturing the same. In the Wheatstone bridge array, there are four different TMR sensors. These TMR sensors are all manufactured simultaneously to produce four identical TMR sensors with a synthetic antiferromagnetic free layer as a top layer. These synthetic antiferromagnetic free layers include a first magnetic layer, a spacer layer, and a second magnetic layer. After forming the four identical TMR sensors, the spacer layer and the second magnetic layer are removed from two TMR sensors. After removing the spacer layer and the second magnetic layer, a new magnetic layer is formed on the now exposed first magnetic layer so that the new magnetic layer has substantially the same thickness as the combination of the spacer layer and the second magnetic layer.
[0011] In one embodiment, a TMR sensor device includes: a first TMR sensor; and a second TMR sensor, wherein the second TMR sensor includes two different magnetic layers disposed in contact with each other.
[0012] In another embodiment, a TMR sensor device includes: a first TMR sensor, wherein the first TMR sensor includes a free layer; and a second TMR sensor, wherein the second TMR sensor includes a free layer different from the free layer of the first TMR sensor.
[0013] In another embodiment, a method of manufacturing a TMR sensor device includes: manufacturing a first TMR sensor and a second TMR sensor; removing a first layer from the second TMR sensor; removing a second layer from the second TMR sensor to expose a free magnetic layer; and depositing a magnetic layer on the exposed free magnetic layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Thus, a detailed understanding of the manner in which the above-described features of the present disclosure are understood, a more particular description of the present disclosure, the above brief overview, may be obtained by reference to the embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the drawings illustrate only typical embodiments of the present disclosure and are therefore not to be considered limiting of its scope, as the present disclosure may admit to other equally effective embodiments.
[0015] Figure 1 is a schematic diagram of a Wheatstone bridge array design.
[0016] Figures 2A to 2K is a schematic diagram of two TMR sensors at various stages of fabrication.
[0017] Figure 3 To show Figures 2A to 2K Flowchart of a method of making a TMR sensor.
[0018] Figure 4 It is shown Figure 2KA graph of the simulation results of the TMR sensor.
[0019] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. It is contemplated that elements disclosed in one embodiment may be beneficially utilized on other embodiments without specific recitation. DETAILED DESCRIPTION
[0020] Hereinafter, reference is made to the embodiments of the present disclosure. However, it should be understood that the present disclosure is not limited to the embodiments specifically described. On the contrary, any combination of the following features and elements (whether or not related to different embodiments) is considered to realize and practice the present disclosure. In addition, although the embodiments of the present disclosure can achieve advantages that are superior to other possible solutions and / or superior to the prior art, whether a specific advantage is achieved by a given embodiment is not a limitation to the present disclosure. Therefore, the following aspects, features, embodiments and advantages are merely illustrative, and are not considered to be elements or limitations of the appended claims, unless explicitly stated in the claims. Similarly, reference to "the present disclosure" should not be interpreted as a summary of any inventive subject matter disclosed herein, and should not be considered to be elements or limitations of the appended claims, unless explicitly stated in the claims.
[0021] The present disclosure as a whole relates to a Wheatstone bridge array including TMR sensors and a method for manufacturing the same. In the Wheatstone bridge array, there are four different TMR sensors. These TMR sensors are all manufactured simultaneously to produce four identical TMR sensors with a synthetic antiferromagnetic free layer as a top layer. These synthetic antiferromagnetic free layers include a first magnetic layer, a spacer layer, and a second magnetic layer. After forming the four identical TMR sensors, the spacer layer and the second magnetic layer are removed from two TMR sensors. After removing the spacer layer and the second magnetic layer, a new magnetic layer is formed on the now exposed first magnetic layer so that the new magnetic layer has substantially the same thickness as the combination of the spacer layer and the second magnetic layer.
[0022] Figure 1 is a schematic diagram of a Wheatstone bridge array 100 design. The array 100 includes a bias source 102, a first resistor 104, a second resistor 106, a third resistor 108, a fourth resistor 110, a first sensor output pad 112, a second sensor output pad 114, and a ground connection 116. A bias voltage is applied across the array from the bias source 102 to the ground connection 116. The first sensor output pad 112 and the second sensor output pad 114 sense the output of the applied voltage. Any temperature changes from the resistors 104, 106, 108, 110 can be offset.
[0023] As discussed herein, resistors 104, 106, 108, 110 each comprise a TMR sensor. In one embodiment, each TMR sensor is unique and different, such that resistors 104, 106, 108, 110 have different resistances. In another embodiment, the TMR sensors are the same, but resistors 104, 106, 108, 110 are different. In yet another embodiment, resistors 104, 110 are identical to one another (because the TMR sensors comprising resistors 104, 110 are identical to one another), and resistors 106, 108 are identical to one another (because the TMR sensors comprising resistors 106, 108 are identical to one another) but are different from resistors 104, 110. For the TMR sensors in array 100, the RA of array 100 is about 100 ohms / square micrometer.
[0024] Typical magnetic field sensors use MR (magnetoresistive) devices in a Wheatstone bridge circuit. This sensor requires the MR devices to be varied differently in the bridge. As discussed in this article, a new approach to making magnetic field sensors is to make two different TMR films in the same layer. The reliability and performance of the TMR film determines the magnetoresistive response. In this way, combining the characteristics of different TMR films, a perfect Wheatstone bridge design for a magnetic field sensor can be made.
[0025] about Figure 1 If the free layer of the TMR sensor including resistors 104, 106, 108, 110 has a long axis that is +45° or -45° to the pinned layer magnetization direction, then due to shape anisotropy, the free layer easy magnetization axis is constrained to be along the long axis, and the magnetization direction can be set by the Ampere field from the setting line current as shown in the simplified diagram, especially when there is a setting line orthogonal to the long axis of the free layer on the top of the free layer.
[0026] When a magnetic field is applied along the Y axis, resistors 110 and 104 increase as the field increases, while resistors 106 and 108 decrease as the field increases. This different response implements a Wheatstone bridge, and the sensor sensitivity is proportional to the output voltage, which is proportional to the difference between resistor 110 (or resistor 104) and resistor 106 (or resistor 108). However, in use, due to the 45° free layer or pinned layer initial state, only half of the magnetoresistance change is used. If the free layer to pinned layer initial state can be 90° and still have two different magnetoresistance changes, the sensor sensitivity can be increased by two times.
[0027] If the free layer and the pinned layer are orthogonal, the pinned layer magnetization direction is set by the magnetic annealing direction. Typically, resistors 104, 106, 108, 110 are made of the same TMR film and undergo the same process, so all have the same pinned layer direction. Each device can operate at a full MR ratio, but all devices respond to external fields in the same way, so there is no output voltage at all. A simple way to solve this problem is to shield resistors 106 and 108 by covering them with a thick NiFe film so that resistors 106 and 108 will not respond to the magnetic field. Alternatively, resistors 106 and 108 can be replaced by constant resistors. However, this half-bridge sensing scheme will also reduce the output voltage and therefore limit the sensitivity.
[0028] Figures 2A to 2K is a schematic diagram of two TMR sensors 200, 250 at various stages of fabrication. The TMR sensors 200, 250 each include a seed layer 202, 252, which is to be formed on a bottom lead (not shown). In one embodiment, the seed layer 202, 252 comprises a conductive material such as ruthenium, and has a thickness between about 10 angstroms and about 100 angstroms, and is deposited by well-known deposition methods such as electroplating, chemical plating, or sputtering. In addition, it should be understood that while ruthenium has been exemplified as the seed layer 202, 252 material, other materials are also contemplated, and the embodiments discussed herein are not limited to the use of ruthenium for the seed layer 202, 252. In addition, the seed layers 202, 252 are deposited simultaneously.
[0029] like Figure 2A As shown, then, an antiferromagnetic (AFM) layer 204, 254 is disposed on the seed layer 204, 254. Suitable materials for the AFM layer 204, 254 include IrMn or PtMn with a thickness between about 40 angstroms and about 500 angstroms. The AFM layer 204, 254 can be formed by a well-known deposition method (such as sputtering). In addition, it should be understood that although IrMn and PtMn have been exemplified as AFM layer 204, 254 materials, other materials are also contemplated, and the embodiments discussed herein are not limited to using IrMn or PtMn for the AFM layer 204, 404. In addition, the AMF layer 204, 254 is deposited simultaneously.
[0030] like Figure 2BAs shown, the pinning layer 206, 256 is disposed on the AFM layer 204, 254. Suitable materials for the pinning layer 206, 256 include CoFe or Co / CoFe / Co multilayer stacks having a thickness between about 20 angstroms and about 30 angstroms. The pinning layer 206, 256 can be formed by a well-known deposition method (such as sputtering). In addition, it should be understood that although CoFe or Co / CoFe / Co has been exemplified as the pinning layer 206, 256 material, other materials are also contemplated, and the embodiments discussed herein are not limited to using CoFe or Co / CoFe / Co for the pinning layer 206, 256. In addition, the pinning layers 206, 256 are deposited simultaneously.
[0031] like Figure 2C As shown, the spacer layer 208, 258 is disposed on the pinned layer 206, 256. Suitable materials for the spacer layer 208, 258 include Ru with a thickness between about 4 angstroms and about 10 angstroms. The spacer layer 208, 258 can be formed by a well-known deposition method (such as sputtering). In addition, it should be understood that although ruthenium has been exemplified as the spacer layer 208, 258 material, other materials are also contemplated, and the embodiments discussed herein are not limited to the use of ruthenium for the spacer layer 208, 258. In addition, the spacer layers 208, 258 are deposited simultaneously.
[0032] like Figure 2D As shown, reference layers 210, 260 are disposed on spacer layers 208, 258. Suitable materials for reference layers 210, 260 include CoFe / Ta / CoFeB / CoFe as a multilayer stack. The CoFe layer may have a thickness between about 8 angstroms and about 10 angstroms. The Ta layer may have a thickness between about 0.5 angstroms and about 2 angstroms. The CoFeB layer may have a thickness between about 10 angstroms and about 15 angstroms. The second CoFe layer may have a thickness between about 3 angstroms and about 10 angstroms. The reference layers 210, 260 may be formed by well-known deposition methods such as sputtering. In addition, it should be understood that although CoFe / Ta / CoFeB / CoFe has been exemplified as reference layer 210, 260 materials, other materials are also contemplated, and the embodiments discussed herein are not limited to using CoFe / Ta / CoFeB / CoFe for reference layers 210, 260. In addition, the reference layers 210, 260 are deposited simultaneously.
[0033] like Figure 2E As shown, barrier layers 212, 262 are disposed on reference layers 210, 260. Suitable materials for barrier layers 212, 262 include MgO having a thickness between about 10 angstroms and about 20 angstroms. It should be understood that while MgO is illustrated as barrier layers 212, 262, other insulating materials are also contemplated. In addition, barrier layers 212, 262, 252 are deposited simultaneously.
[0034] like Figure 2F As shown, the first free layer 214, 264 is disposed on the barrier layer 212, 262. Suitable materials for the first free layer 214, 264 include CoFe / CoFeB / Ta / NiFe multilayer stacks. The CoFe layer may have a thickness between about 3 angstroms and about 10 angstroms. The CoFeB layer may have a thickness between about 10 angstroms and about 20 angstroms. The Ta layer may have a thickness between about 0.5 angstroms and about 2 angstroms. The NiFe layer may have a thickness between about 3 angstroms and about 300 angstroms, such as between about 3 angstroms and about 10 angstroms or between about 10 angstroms and about 300 angstroms. The first free layer 214, 264 can be formed by a well-known deposition method (such as sputtering). In addition, it should be understood that although CoFe / CoFeB / Ta / NiFe has been exemplified as the first free layer 214, 264 material, other materials are also contemplated, and the embodiments discussed herein are not limited to using CoFe / CoFeB / Ta / NiFe for the first free layer 214, 264. Additionally, the first free layers 214, 216, 252 are deposited simultaneously.
[0035] like Figure 2G As shown, additional spacer layers 216, 266 are then formed on the first free layers 214, 264. In one embodiment, the spacer layers 216, 266 are a multilayer structure comprising Co / Ru / Co. It should be understood that the spacer layer 416 can be a single layer or other multilayer stack including a first magnetic layer, a non-magnetic conductive layer, and a second magnetic layer. In embodiments where the spacer layers 216, 266 are Co / Ru / Co, the first Co layer can have a thickness between about 3 angstroms to about 6 angstroms, the Ru layer can have a thickness between about 6 angstroms and about 10 angstroms, and the second Co layer can have a thickness between about 3 angstroms to about 6 angstroms. The Co layer is used to enhance synthetic antiferromagnetic (SAF) coupling. The spacer layers 216, 266 can be formed by a well-known deposition method (such as sputtering). In addition, the spacer layers 216, 266 are deposited simultaneously.
[0036] like Figure 2HAs shown, a second free layer 218, 268 is then formed on the spacer layer 216, 266. Suitable materials for the second free layer 218, 268 include NiFe. The NiFe layer may have a thickness between about 100 angstroms and about 300 angstroms, such as between about 100 angstroms and about 200 angstroms (the magnetic moment of the second free layer 218, 268 is greater than the magnetic moment of the first free layer 214, 264) or between about 200 angstroms and about 300 angstroms. The second free layer 218, 268 may be formed by a well-known deposition method (such as sputtering). It should be understood that although NiFe has been exemplified as the second free layer 218, 268 material, other materials are also contemplated, and the embodiments discussed herein are not limited to using NiFe for the second free layer 218, 268. In addition, the second free layer 218, 268 is deposited simultaneously. The first free layer 214 , 264 together with the spacer layer 216 , 266 and the second free layer 218 , 268 collectively form an unbalanced synthetic AFM structure.
[0037] At this point, TMR sensors 200, 250 are identical and have been manufactured at the same time. Therefore, TMR sensors 200, 250 are formed only once, with both sensors 200, 250 having the same RA and the same TMR. For a Wheatstone bridge array, all sensors cannot be identical. Instead, resistors 104, 110 are identical to each other, and resistors 106, 108 are identical to each other and different from resistors 104, 110. In order to make the resistors different, additional processing is required for both of resistors 106, 108. TMR sensor 250 will represent resistors 106, 108 that have undergone additional processing.
[0038] like Fig.2I As shown, the second free layer 268 is removed from the TMR sensor 250, while the second free layer 218 is retained for the TMR sensor 200. The second free layer 268 is removed by a well-known process such as ion milling to expose the underlying spacer layer 266. For the TMR sensor 250, Fig.2I The resulting structure shown does not have the second free layer 268, but instead has an exposed spacer layer 266. The TMR sensor 200 is unchanged and still has the second free layer 218. The TMR sensor 200 is masked during the removal process so that no material is removed from the TMR sensor 200.
[0039] Afterwards, if Figure 2J As shown, the spacer layer 266 is removed from the TMR sensor 250. No material is removed from the TMR sensor 200. Again, the TMR sensor 200 is masked during the removal process. The spacer layer 266 can be removed by a well-known process such as ion milling to expose the first free layer 264 below. For the TMR sensor 250, Figure 2JThe resulting structure shown in FIG. 2 has no second free layer 268 and no spacer layer 266, but has an exposed first free layer 264. The TMR sensor 200 is unchanged and still has both the second free layer 218 and the spacer layer 216. It should be understood that while the spacer layer 266 removal and the second free layer 268 removal have been discussed as two separate processes, one continuous process may be used to remove both the second free layer 268 and the spacer layer 266.
[0040] Then, if Figure 2K As shown, another magnetic layer 270 is deposited on the exposed first free layer 264 of TMR 250. Another magnetic layer 270 is substantially the same in composition as the second free layer 218, 268, but will have a thickness substantially equal to the total thickness of the spacer layer 216, 266 and the second free layer 218, 268. Suitable materials for the second magnetic layer 270 include NiFe having a total thickness between about 100 angstroms and about 350 angstroms. The NiFe layer may have a thickness between about 100 angstroms and about 300 angstroms, such as between about 100 angstroms and about 200 angstroms or between about 200 angstroms and about 300 angstroms. The second free layer 218, 268 can be formed by well-known deposition methods (such as sputtering or ion beam deposition). It should be understood that although NiFe has been exemplified as the second free layer 218, 268 material, other materials are also contemplated, and the embodiments discussed herein are not limited to using NiFe for the second free layer 218, 268.
[0041] After forming the second magnetic layer 270, a capping layer may be formed over the second free layer 218 and the second magnetic layer 270. The resulting TMR sensor 200, 250 is then annealed in a magnetic oven at a temperature between about 250 degrees Celsius and about 300 degrees Celsius and a magnetic field between about 10,000 Oe and about 50,000 Oe. It should be understood that while the annealing has been discussed as occurring after depositing the second magnetic layer 270, it is contemplated that the annealing may also occur after depositing the second free layer 218, 268. The second magnetic layer 270 has a greater magnetic moment than the first free layer 214, 264. It should be understood that the second magnetic layer 270 has a thickness greater than the thickness of the first free layer 264. In the TMR sensor 250, the second magnetic layer 270 is ferromagnetically coupled to the first free layer 264 in the TMR 250, and the first free layer 264 will provide a magnetoresistance with opposite magnetic directions under the same bias field. The hard magnetic bias field H bias is shown by arrow 272. After annealing, the pinned layers 206, 256 are pinned in the -Z direction. When the hard magnetic bias field is applied, the reference layers 210, 260 have a magnetic moment in the +Z direction, and the first free layer 214 of the TMR sensor 200 has a magnetic moment shown by arrow 276, which is antiparallel to the magnetic moment of the first free layer 264 of the TMR sensor 250 shown by arrow 278. In addition, under the applied hard magnetic bias, the second free layer 218 and the second magnetic layer 270 have parallel magnetic moments shown by arrows 274, 280. As shown in FIG. Figure 2K As shown, under the same hard magnetic bias field, the magnetic moment of the first free layer 214 is antiparallel to the magnetic moment of the second free layer 218 , while the magnetic moment of the first free layer 264 is parallel to the magnetic moment of the second magnetic layer 270 .
[0042] Figure 3 To show Figures 2A to 2K Flowchart of a method 300 of manufacturing a TMR sensor. In step 302, a plurality of TMR sensors are formed. Then in step 304, a top layer of at least one TMR sensor is removed by a process such as ion milling or etching. Then in step 306, another layer is removed from the same TMR sensor from which the top layer was previously removed by a process such as ion milling. Then in step 308, a magnetic layer is formed in the location of the removed top layer and another layer by a process such as ion beam deposition or sputtering.
[0043] Figure 4 It is shown Figure 2K The curve diagram of the simulation results of the TMR sensor. Figure 4 As shown, film A, which is equivalent to TMR sensor 200, and film B, which is equivalent to TMR sensor 250, have substantially opposite magnetoresistances under an applied magnetic field.
[0044] In one embodiment, a TMR sensor device includes: a first TMR sensor; and a second TMR sensor, wherein the second TMR sensor includes two different magnetic layers arranged in contact with each other. The first TMR sensor has a top layer of magnetic material and a layer in contact with the top layer, wherein the second TMR sensor includes a top layer of magnetic material having a thickness substantially equal to the thickness of the top layer of magnetic material of the first TMR sensor and the layer in contact with the top layer of magnetic material of the first TMR sensor. The first TMR sensor has a first free magnetic layer, a spacer layer arranged on the first free magnetic layer, and a second free magnetic layer arranged on the spacer layer, wherein the first free magnetic layer and the second free magnetic layer are magnetically coupled in antiparallel. The second TMR sensor includes a first free magnetic layer and a second free magnetic layer arranged on the first free magnetic layer, wherein the first free magnetic layer and the second free magnetic layer are magnetically coupled in parallel. The second free magnetic layer of the second TMR sensor is thicker than the first free magnetic layer of the second TMR sensor. The array also includes: a third TMR sensor; and a fourth TMR sensor, wherein the first TMR sensor and the third TMR sensor are substantially identical. The fourth TMR sensor and the second TMR sensor are substantially identical.
[0045] In another embodiment, a TMR sensor device includes: a first TMR sensor, wherein the first TMR sensor includes a free layer; and a second TMR sensor, wherein the second TMR sensor includes a free layer different from the free layer of the first TMR sensor. The first TMR sensor includes an unbalanced synthetic antiferromagnetic free layer. The free layer of the second TMR sensor is a multilayer structure. The free layer of the second TMR sensor includes a first magnetic layer and a second magnetic layer disposed on the first magnetic layer. The first magnetic layer and the second magnetic layer are magnetically coupled in parallel. The bottom layer of the unbalanced synthetic antiferromagnetic free layer of the first TMR sensor is substantially the same as the first magnetic layer of the free layer of the second TMR sensor.
[0046] In another embodiment, a method of manufacturing a TMR sensor device includes: manufacturing a first TMR sensor and a second TMR sensor; removing a first layer from the second TMR sensor; removing the second layer from the second TMR sensor to expose a free magnetic layer; depositing a magnetic layer on the exposed free magnetic layer. Before removing the first layer from the second TMR sensor, the first TMR sensor and the second TMR sensor are substantially identical. The magnetic layer has a thickness substantially equal to a thickness of the first layer and the second layer combined. Removing the first layer of the second TMR sensor includes ion milling the first layer. Removing the second layer of the second TMR sensor includes ion milling the second layer. Depositing the magnetic layer is performed by an ion beam deposition process. Depositing the magnetic layer is performed by a sputtering process.
[0047] In one embodiment, the TMR sensor is used in a camera that operates as a single-axis sensor. Examples of such sensors are found in U.S. Patent Application Publication 2019 / 0020822 A1, which is incorporated herein by reference. However, it is expected that the TMR sensor can be used as a two-dimensional or even three-dimensional sensor. In addition, it is expected that the TMR sensor can be integrated and used in inertial measurement unit technologies other than cameras, such as wearable devices, compasses, and MEMS devices. In addition, the TMR sensor can be operated as a position sensor, a bridge angle sensor, a magnetic switch, a current sensor, or a combination thereof. The TMR sensor can be used to focus a camera, such as a smartphone camera, by using the TMR sensor as a position and angle sensor. In addition, the TMR sensor can also be used as a switch, current and angle sensor in the automotive industry to replace the current Hall sensor, anisotropic magnetoresistive (AMR) sensor, and giant magnetoresistive (GMR) sensor. TMR sensors can also be used as position and angle sensors in drones and robotics industries. Medical devices can also use TMR sensors to control the flow of infusion systems, and endoscope camera sensors can also be used. Thus, the TMR sensors discussed herein have applications far beyond smartphone cameras, and therefore should not be limited to use as sensors for smartphone cameras. Furthermore, the TMR sensors need not be arranged in a Wheatstone bridge arrangement, but can be arranged in any number of ways.
[0048] By forming the TMR sensor simultaneously and then changing the top two layers, only one anneal is required, and manufacturing throughput is greatly increased.
[0049] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be envisaged without departing from the basic scope of the present disclosure, and the scope of the present disclosure is determined by the appended claims.
Claims
1. A tunnel magnetoresistance sensor device, i.e., a TMR sensor device, comprising: a first TMR sensor, wherein the first TMR sensor has a first free magnetic layer, a spacer layer disposed on the first free magnetic layer, and a second free magnetic layer disposed on the spacer layer, wherein the first free magnetic layer and the second free magnetic layer are magnetically coupled in an antiparallel manner; and a second TMR sensor, wherein the second TMR sensor comprises two different free magnetic layers arranged in contact with each other, The two different free magnetic layers of the second TMR sensor include a first free magnetic layer and a second free magnetic layer arranged on the first free magnetic layer, the first free magnetic layer of the second TMR sensor and the second free magnetic layer of the second TMR sensor are magnetically coupled in parallel, and the second free magnetic layer of the second TMR sensor is thicker than the first free magnetic layer of the second TMR sensor. 2 . The TMR sensor device of claim 1 , wherein a thickness of the second free magnetic layer of the second TMR sensor is equal to a thickness of the second free magnetic layer of the first TMR sensor and a thickness of the spacer layer of the first TMR sensor.
3. The TMR sensor device according to claim 1, further comprising: The third TMR sensor; and A fourth TMR sensor, wherein the first TMR sensor and the third TMR sensor are the same. 4 . The TMR sensor device of claim 3 , wherein the fourth TMR sensor and the second TMR sensor are identical.
5. The TMR sensor device according to claim 1: wherein the first free magnetic layer of the first TMR sensor has a first magnetic moment and the second free magnetic layer of the first TMR sensor has a second magnetic moment, the second magnetic moment being antiparallel to the first magnetic moment; and Wherein when a hard bias is applied to the TMR sensor device, the two different free magnetic layers of the second TMR sensor provide a magnetoresistance having a magnetic direction opposite to the magnetic direction provided by the first free magnetic layer and the second free magnetic layer of the first TMR sensor. 6 . The TMR sensor device of claim 2 , wherein the first free magnetic layer of the first TMR sensor together with the spacer layer and the second free magnetic layer of the first TMR sensor collectively form an unbalanced synthetic antiferromagnetic structure. 7 . The TMR sensor device of claim 6 , wherein the first free magnetic layer of the unbalanced synthetic antiferromagnetic structure of the first TMR sensor is the same as the first free magnetic layer of the second TMR sensor.
8. A method of manufacturing a tunnel magnetoresistive sensor device, i.e., a TMR sensor device, the method comprising: fabricating a first TMR sensor and a second TMR sensor, each sensor having a respective first free magnetic layer, a spacer layer disposed on the first free magnetic layer, and a second free magnetic layer disposed on the spacer layer; removing the second free magnetic layer from the second TMR sensor; removing the spacer layer from the second TMR sensor to expose the first free magnetic layer of the second TMR sensor; as well as depositing another second magnetic layer on the exposed first free magnetic layer, The first free magnetic layer and the another second magnetic layer of the second TMR sensor are magnetically coupled in parallel, and the another second magnetic layer is thicker than the first free magnetic layer of the second TMR sensor. 9 . The method of claim 8 , wherein the first TMR sensor and the second TMR sensor are identical before removing the second free magnetic layer from the second TMR sensor. 10 . The method of claim 8 , wherein a thickness of the another second magnetic layer is equal to a thickness of a combination of the second magnetic layer and the spacer layer of the second TMR sensor. 11 . The method of claim 8 , wherein removing the second magnetic layer of the second TMR sensor comprises ion milling the second magnetic layer. 12 . The method of claim 11 , wherein removing the spacer layer of the second TMR sensor comprises ion milling the spacer layer.
13. The method of claim 8, wherein depositing the another second magnetic layer is performed by an ion beam deposition process. The method of claim 8 , wherein depositing the another second magnetic layer is performed by a sputtering process.