A method for doping single crystal silicon and a method for manufacturing single crystal silicon

By dynamically adjusting the crucible speed and heater power during the growth of single crystal silicon, controlling the volatility and concentration of dopants, the problem of uneven resistivity distribution of single crystal silicon is solved, and the uniformity and pass rate of the product are improved. Reduced costs.

CN113622017BActive Publication Date: 2024-11-19ORDOS LONGJI SILICON MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202010388875.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-09
Publication Date
2024-11-19
Estimated Expiration
2040-05-09

AI Technical Summary

Technical Problem

The head and tail resistivity distribution of existing single crystal silicon is uneven, resulting in low product pass rate and high cost.

Method used

By dynamically adjusting the crucible speed and heater power during the growth of single crystal silicon, controlling the volatility and concentration of dopants, ensuring the consistency of the weight of silicon material, and gradually adding the preset speed and power difference within the threshold range. Dopant to grow uniformly single crystal silicon.

Benefits of technology

It effectively solves the problem of uneven resistivity distribution of single crystal silicon, improves the head and tail resistivity uniformity of single crystal silicon, improves product qualification rate and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113622017B_ABST
    Figure CN113622017B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention provides a method for doping single crystal silicon and a method for manufacturing single crystal silicon, the method comprising: adding silicon material and a first weight of dopant into a crucible to grow a first single crystal silicon; after the end stage of the growth of the first single crystal silicon is completed, adjusting the speed of the crucible according to a preset speed, and adjusting the power of the heater according to a preset power, wherein the absolute value of the difference between the preset speed and the speed of the crucible in the seeding stage is less than or equal to a first threshold, and the absolute value of the difference between the preset power and the power of the heater in the seeding stage is less than or equal to a second threshold; adding a second weight of dopant into the crucible to grow a second single crystal silicon; wherein, during the growth of the first single crystal silicon and the second single crystal silicon, dynamically adding silicon material into the crucible so that the weight of the silicon material in the crucible at any time is the preset weight. The method of the embodiment of the present invention can effectively control the amount of dopant, improve the utilization efficiency of dopant, and solve the problem of uneven resistivity distribution at the head and tail of single crystal silicon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar photovoltaic technology, and in particular to a single crystal silicon doping method and a single crystal silicon manufacturing method. Background Art

[0002] Monocrystalline silicon is the most basic material for preparing solar cells. The performance of solar cells mainly depends on the quality of monocrystalline silicon, and resistivity is an important parameter reflecting the quality of monocrystalline silicon.

[0003] At present, the resistivity of single crystal silicon is mainly controlled by doping a certain amount of impurities during the growth process of single crystal silicon. Since doping with gallium during the preparation of single crystal silicon can improve the overall performance of solar cells, especially making solar cells have excellent performance in terms of conversion efficiency, service life and resistance to harsh environments, doping with gallium is gradually applied to the production and preparation of single crystal silicon. However, since the segregation coefficient of gallium is too small and the melting point of gallium is low, it is difficult to control the doping concentration. As a result, it is difficult to control the resistivity of single crystal silicon during the growth process of single crystal silicon, which can easily lead to uneven resistivity distribution at the head and tail of single crystal silicon, making the proportion of qualified resistivity in the entire single crystal silicon rod unsatisfactory, which is not conducive to improving the qualified rate of finished products, resulting in a high average cost of the product. Summary of the invention

[0004] The embodiments of the present invention provide a single crystal silicon doping method and a single crystal silicon manufacturing method to solve the problem of uneven resistivity distribution at the head and tail of the existing single crystal silicon.

[0005] In order to solve the above problem, the present invention is achieved as follows:

[0006] In a first aspect, an embodiment of the present invention provides a method for doping single crystal silicon, the method comprising:

[0007] Adding silicon material and a first weight of dopant into a crucible to grow a first silicon single crystal;

[0008] After the final stage of the growth of the first silicon monocrystalline is completed, the rotation speed of the crucible is adjusted according to a preset rotation speed, and the power of the heater is adjusted according to a preset power, wherein the absolute value of the difference between the preset rotation speed and the rotation speed of the crucible in the seeding stage is less than or equal to a first threshold, and the absolute value of the difference between the preset power and the power of the heater in the seeding stage is less than or equal to a second threshold;

[0009] adding a second weight of the dopant into the crucible to grow a second silicon single crystal;

[0010] During the growth of the first silicon single crystal and the second silicon single crystal, the silicon material is dynamically added into the crucible so that the weight of the silicon material in the crucible at any moment is a preset weight.

[0011] Optionally, the step of adding the silicon material and the first weight of the dopant into the crucible before growing the first silicon single crystal comprises:

[0012] determining a target resistivity of the first silicon single crystal;

[0013] A first weight of the dopant required for the first single silicon crystal is calculated.

[0014] Optionally, the step of adding the second weight of the dopant into the crucible before growing the second silicon single crystal comprises:

[0015] determining a target resistivity of the second single crystal silicon;

[0016] calculating a second weight of the dopant required for the second single silicon crystal; and

[0017] Outside the single crystal furnace, adding a second weight of the dopant into a doping device;

[0018] The step of adding a second weight of the dopant into the crucible to grow a second silicon single crystal comprises:

[0019] placing the doping device into the single crystal furnace;

[0020] adjusting the opening size of the doping device;

[0021] The dopant is added into the crucible through the opening to grow a second silicon single crystal.

[0022] Optionally, after adding the second weight of the dopant into the crucible and growing the second silicon single crystal, the method further comprises:

[0023] After the end stage of the growth of the second silicon single crystal is completed, adjusting the rotation speed of the crucible according to the preset rotation speed, and adjusting the power of the heater according to the preset power;

[0024] A third weight of the dopant is added into the crucible, and another second silicon single crystal is grown until the amount of the second silicon single crystal reaches a preset amount.

[0025] Optionally, the step of adding the third weight of the dopant into the crucible before growing the next second silicon single crystal comprises:

[0026] determining a target resistivity of a next strand of the second single crystal silicon;

[0027] calculating a third weight of the dopant required for a next strand of the second single crystal silicon;

[0028] Outside the single crystal furnace, a third weight of the dopant is added into the doping device.

[0029] Optionally, the first threshold is 3r / min, and the second threshold is 5kw.

[0030] Optionally, the crucible comprises an inner crucible and an outer crucible;

[0031] The step of adding the silicon material and the first weight of the dopant into the crucible to grow the first silicon single crystal comprises: adding the silicon material and the first weight of the dopant between the inner crucible and the outer crucible or into the inner crucible to grow the first silicon single crystal;

[0032] The dynamically adding the silicon material into the crucible during the growth of the first silicon single crystal and the second silicon single crystal comprises: dynamically adding the silicon material between the inner crucible and the outer crucible through a feeding device during the growth of the first silicon single crystal and the second silicon single crystal.

[0033] Optionally, the dopant is gallium or a gallium-containing compound.

[0034] In a second aspect, an embodiment of the present invention further provides a method for manufacturing single crystal silicon, the method comprising any one of the single crystal silicon doping methods described above.

[0035] Optionally, adding the silicon material and the first weight of the dopant into a crucible to grow a first silicon single crystal comprises:

[0036] Adding silicon material and a first weight of a dopant into an inner crucible, and heating to melt the silicon material and the dopant;

[0037] Immersing the seed crystal in molten silicon, and lifting the seed crystal at a preset speed to reduce the diameter of the crystal;

[0038] When the diameter of the crystal is reduced to a first preset diameter, slowing down the growth rate to increase the diameter of the crystal;

[0039] When the diameter of the silicon single crystal reaches a second preset diameter, the growth speed is maintained unchanged and the single crystal is grown to a preset length;

[0040] After the final stage of cooling treatment, the first single crystal silicon is obtained.

[0041] In an embodiment of the present invention, silicon material and a first weight of dopant are added to a crucible to grow a first silicon single crystal; after the end stage of the growth of the first silicon single crystal is completed, the speed of the crucible is adjusted according to a preset speed, and the power of the heater is adjusted according to a preset power, wherein the absolute value of the difference between the preset speed and the speed of the crucible in the seeding stage is less than or equal to a first threshold, and the absolute value of the difference between the preset power and the power of the heater in the seeding stage is less than or equal to a second threshold; a second weight of dopant is added to the crucible to grow a second silicon single crystal; wherein, during the growth of the first silicon single crystal and the second silicon single crystal, silicon material is dynamically added to the crucible so that the weight of the silicon material in the crucible at any time is the preset weight. After the end stage of the growth of the previous silicon single crystal is completed, the crucible speed and the heater power are adjusted to ensure that the volatilization amount of the dopant is consistent in each stage of pulling a silicon single crystal, and the dopant required for growing the next silicon single crystal is added to the crucible at one time, and the weight of the silicon material in the crucible is ensured to be unchanged before doping. In this way, the amount of dopant can be effectively controlled, and the volatilization amount and doping concentration of the dopant can be controlled during the growth of the next single crystal silicon, thereby ensuring that the resistivity distribution at the head and tail of the single crystal silicon is uniform, which can effectively solve the problem of uneven resistivity distribution at the head and tail of existing single crystal silicon. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0043] Figure 1 A flow chart showing a single crystal silicon doping method according to the first embodiment of the present invention;

[0044] Figure 2 A schematic diagram showing the working principle of single crystal silicon doping according to an embodiment of the present invention;

[0045] Figure 3 A flow chart showing a single crystal silicon doping method according to a second embodiment of the present invention;

[0046] Figure 4 A flow chart showing a single crystal silicon doping method according to a third embodiment of the present invention.

[0047] Description of reference numerals:

[0048] 10-single crystal furnace, 11-crucible, 111-outer crucible, 112-inner crucible, 12-isolating valve, 20-feeding device, 21-material containing part, 22-feeding channel, 30-doping device, 31-cylinder bottom, 32-cylinder body. DETAILED DESCRIPTION

[0049] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0050] It should be understood that the references to "one embodiment" or "an embodiment" throughout the specification mean that the specific features, structures, or characteristics associated with the embodiment are included in at least one embodiment of the present invention. Therefore, the references to "in one embodiment" or "in an embodiment" appearing throughout the specification do not necessarily refer to the same embodiment. In addition, these specific features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.

[0051] In various embodiments of the present invention, it should be understood that the size of the serial numbers of the following processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.

[0052] Embodiment 1

[0053] Reference Figure 1 , shows a flow chart of a single crystal silicon doping method according to an embodiment of the present invention, which may specifically include the following steps:

[0054] Step 101: Add silicon material and a first weight of dopant into a crucible to grow a first silicon single crystal.

[0055] In the embodiment of the present invention, the silicon material may be native polycrystalline silicon material, etc., and the embodiment of the present invention does not limit this. In order to ensure the resistivity of single crystal silicon, it is necessary to dope the single crystal silicon, and the type of dopant can be determined according to the conductivity type of the target single crystal silicon. For example, when the conductivity type of the target single crystal silicon is P-type, trace amounts of Group IIIA elements such as gallium, boron, aluminum, etc. can be doped; when the conductive type of the target single crystal silicon is N-type, trace amounts of Group VA elements such as phosphorus, antimony, arsenic, etc. can be doped. It can be understood that the first weight of the dopant is the weight of the dopant required to grow the first single crystal silicon, and the first weight of the dopant can be calculated based on the target resistivity of the first single crystal silicon.

[0056] In the embodiment of the present invention, Figure 2As shown, the silicon material and the first weight of the dopant are added to the crucible, and the dopant can be first added to the silicon material, and then the doped silicon material is put into the crucible 11 to grow the first single crystal silicon. It can be understood that the weight of the silicon material added to the crucible 11 this time can be the weight of the silicon material required to grow the first single crystal silicon, or the weight of the silicon material required to grow multiple single crystal silicon. The single crystal silicon in the embodiment of the present invention can be grown by the Czochralski method, and the embodiment of the present invention does not limit this.

[0057] In addition, in an embodiment of the present invention, the crucible 11 may include an inner crucible 112 and an outer crucible 111. Optionally, when growing the first single crystal silicon, before the single crystal furnace is heated, the temperature in the furnace is relatively low and the dopant is not easy to volatilize. Therefore, the silicon material and the dopant can be added between the inner crucible 112 and the outer crucible 111, or added to the inner crucible 112. Both adding positions are acceptable.

[0058] Step 102, after the final stage of the growth of the first single crystal silicon is completed, the rotation speed of the crucible is adjusted according to a preset rotation speed, and the power of the heater is adjusted according to a preset power, wherein the absolute value of the difference between the preset rotation speed and the rotation speed of the crucible in the crystal initiation stage is less than or equal to a first threshold, and the absolute value of the difference between the preset power and the power of the heater in the crystal initiation stage is less than or equal to a second threshold.

[0059] In an embodiment of the present invention, after the end stage of the growth of the first single silicon crystal is completed, the speed of the crucible is adjusted according to the preset speed, and the power of the heater is adjusted according to the preset power, wherein the absolute value of the difference between the preset speed and the speed of the crucible in the seeding stage is less than or equal to the first threshold, and the absolute value of the difference between the preset power and the power of the heater in the seeding stage is less than or equal to the second threshold. After adjusting the speed of the crucible and the power of the heater, the crucible can be rotated at the preset speed and the heater can work at the preset power, so that the temperature of the silicon melt in the crucible 11 can be kept constant, so that the volatilization amount of the dopant in the silicon melt is equal in the same time period, which is beneficial to the uniformity of the resistivity distribution of the head and tail of each single silicon crystal.

[0060] Step 103, adding a second weight of the dopant into the crucible 11 to grow a second silicon single crystal; wherein, during the growth of the first silicon single crystal and the second silicon single crystal, the silicon material is dynamically added into the crucible 11 so that the weight of the silicon material in the crucible 11 at any moment is a preset weight.

[0061] In the embodiment of the present invention, after the crucible rotation speed and the heater power are adjusted, a second weight of dopant is added to the crucible 11. The second weight of dopant can be calculated based on the target resistivity of the second single crystal silicon, and the second weight of dopant can be calculated at the end of the growth of the first single crystal silicon, so that the second weight of dopant can be added to the crucible 11 in time after the end of the growth of the first single crystal silicon. Figure 2 As shown, the second weight of dopant can be added to the doping device 30 outside the single crystal furnace 10. After the doping device 30 is placed in the single crystal furnace 10, the dopant enters the inner crucible 11 from the doping device 30. At this time, the silicon material required for growing the second single crystal silicon still enters the crucible 11 from the feeding channel 22 of the feeding device 20 to grow the second single crystal silicon. Since the dopant required for the subsequent growth of the second single crystal silicon is added from the top of the single crystal furnace 10 through the single crystal furnace doping device 30, the dopant gradually approaches the high temperature area at the bottom of the furnace from the low temperature area at the top of the furnace, rather than directly approaching the high temperature silicon melt. The dopant is less affected by the thermal convection of the silicon melt, and its volatilization amount is small. Therefore, the influence of thermal convection on the resistivity consistency of the single crystal silicon can be reduced. It can be understood that the first single crystal silicon can be the first single crystal silicon grown, and the second single crystal silicon can be the single crystal silicon grown in the subsequent process. In terms of the parameter performance of the target resistivity and target growth length of the single crystal silicon, the first single crystal silicon can be the same as the second single crystal silicon, or the first single crystal silicon can be different from the second single crystal silicon. Among them, during the growth process of the first silicon single crystal and the second silicon single crystal, the liquid level of the silicon melt in the crucible 11 will be lowered due to the continuous growth of the silicon single crystal. Therefore, silicon material can be added to the crucible 11 in real time through the feeding device 20 while the silicon single crystal is pulled, so as to ensure that the amount of silicon material in the crucible 11 before each doping is a preset weight. It can be understood that the preset weight is the weight of the silicon material required for pulling the first silicon single crystal or the second silicon single crystal, that is, the amount of silicon material in the crucible 11 can be kept unchanged. Specifically, in the process of replenishing silicon material, since there are continuously growing single crystal silicon rods in the area of ​​the inner crucible, in order to avoid the added material interfering with the growth of the silicon rods, the silicon material is replenished between the inner crucible and the outer crucible through the feeding device 20, and then automatically flows into the inner crucible.

[0062] Specifically, taking the dopant gallium as an example, since gallium is in solid state when the temperature is less than 25°C, weighing the solid gallium can effectively control the doping amount of gallium. Since the segregation coefficient of gallium is small and it is difficult to control the doping concentration, after the end stage of the growth of the first single crystal silicon is completed, the rotation speed of the crucible and the power of the heater can be adjusted, and then the gallium required for the second single crystal silicon can be added to the crucible at one time, so that the temperature of the molten silicon in the crucible remains unchanged, so that the volatilization amount of gallium in the molten silicon in the same time period is equal. Of course, the dopant in the embodiment of the present invention can also be a gallium-containing compound, which is not limited in the embodiment of the present invention. Therefore, the embodiment of the present invention can not only improve the utilization rate of the dopant, but also improve the uniformity of the resistivity distribution of single crystal silicon, thereby effectively solving the problem of uneven resistivity distribution of existing single crystal silicon. In addition, after the end stage of the growth of the first single crystal silicon is completed in the embodiment of the present invention, the dopant required for the second single crystal silicon is added to the crucible at one time, so that the single crystal silicon doping method of the embodiment of the present invention has fewer process steps and strong operability.

[0063] In an embodiment of the present invention, silicon material and a first weight of dopant are added to a crucible to grow a first silicon single crystal; after the end stage of the growth of the first silicon single crystal is completed, the speed of the crucible is adjusted according to a preset speed, and the power of the heater is adjusted according to a preset power, wherein the absolute value of the difference between the preset speed and the speed of the crucible in the seeding stage is less than or equal to a first threshold, and the absolute value of the difference between the preset power and the power of the heater in the seeding stage is less than or equal to a second threshold; a second weight of dopant is added to the crucible to grow a second silicon single crystal; wherein, during the growth of the first silicon single crystal and the second silicon single crystal, silicon material is dynamically added to the crucible so that the weight of the silicon material in the crucible at any time is the preset weight. After the end stage of the growth of the previous silicon single crystal is completed, the crucible speed and the heater power are adjusted to ensure that the volatilization amount of the dopant is consistent in each stage of pulling a silicon single crystal, and the dopant required for growing the next silicon single crystal is added to the crucible at one time, and the weight of the silicon material in the crucible is ensured to be unchanged before doping. In this way, the amount of dopant can be effectively controlled, and the volatilization amount and doping concentration of the dopant can be controlled during the growth of the next single crystal silicon, thereby ensuring that the resistivity distribution at the head and tail of the single crystal silicon is uniform, which can effectively solve the problem of uneven resistivity distribution at the head and tail of existing single crystal silicon.

[0064] Embodiment 2

[0065] Reference Figure 3 , shows a flow chart of a single crystal silicon doping method according to the second embodiment of the present invention, which may specifically include the following steps:

[0066] Step 201, determining a target resistivity of the first single crystal silicon.

[0067] In an embodiment of the present invention, determining the target resistivity of the first single crystal silicon includes determining the conductivity type and the target resistivity value of the first single crystal silicon. The conductivity type and the target resistivity value of the single crystal silicon will directly affect the conductivity of the single crystal silicon, so when the single crystal silicon is used to make a solar cell, it will affect the performance of the solar cell. Its conductivity type can be P-type or N-type. The majority carriers in P-type single crystal silicon are mainly holes in the single crystal silicon. The more such impurities are doped into the single crystal silicon, the higher the hole concentration, and the stronger the conductivity of the single crystal silicon; the majority carriers in N-type single crystal silicon are mainly free electrons in the single crystal silicon. The more such impurities are doped into the single crystal silicon, the higher the concentration of free electrons, and the stronger the conductivity of the single crystal silicon. The target resistivity of the first single crystal silicon can be determined according to the requirements in the actual application. In actual applications, the required resistivity value of the single crystal silicon is generally low, and the embodiment of the present invention does not require this.

[0068] Step 202: Calculate a first weight of the dopant required for the first single crystal silicon.

[0069] In the embodiment of the present invention, the first weight of the dopant required to grow a single crystal silicon can be calculated according to formula (1):

[0070]

[0071] Among them, C S represents the target dopant concentration, K0 represents the segregation coefficient of the dopant, W represents the charge amount, d represents the silicon density, M represents the atomic weight of the doping element, and N0 represents the Avogadro constant. In practical applications, if the target resistivity value of single crystal silicon is known, the target dopant concentration value C can be obtained by consulting the relationship table corresponding to the resistivity and impurity concentration value. S After determining the type of dopant, the atomic weight M of the doping element can be obtained according to the periodic table. The segregation coefficient K0 of the dopant can be obtained by consulting the chemical properties of the doping element. The silicon density d is taken as a constant of 2.33 g / cm 3 , Avogadro constant N0 is taken as 6.02*10 23 The charge amount W is the weight of silicon material added to grow single crystal silicon. When the charge amount W and the target resistivity are known, the first weight of the dopant required to grow the first single crystal silicon can be calculated by formula (1).

[0072] Step 203: Add silicon material and a first weight of dopant into a crucible to grow a first silicon single crystal.

[0073] In the embodiment of the present invention, step 203 may refer to the above step 101, and will not be described again here to avoid repetition.

[0074] Step 204: determine a target resistivity of the second single crystal silicon.

[0075] Step 205: Calculate a second weight of the dopant required for the second single crystal silicon.

[0076] In the embodiment of the present invention, step 204 can refer to the above step 201, and step 205 can refer to the above step 202, which will not be repeated here. It should be noted that step 204 and step 205 can be performed in the final stage of the first single crystal silicon growth, and the embodiment of the present invention does not limit this.

[0077] Step 206: Add a second weight of the dopant into a doping device outside the single crystal furnace.

[0078] In an embodiment of the present invention, a second weight of dopant is added to the doping device outside the single crystal furnace, and the doping amount of the dopant can be effectively controlled. Taking gallium as an example, gallium is solid below 25°C. When the ambient temperature is below 25°C outside the single crystal furnace, the solid gallium is easy to weigh and easy to load into the doping device. The required gallium can be accurately weighed, and the loss of gallium during the loading process can be reduced, so that the doping amount of gallium can be effectively controlled. It can be understood that step 206 can also be performed in the final stage of the growth of the first single crystal silicon to ensure that after the final stage of the growth of the first single crystal silicon is completed, the dopant can be added to the crucible in time to grow the second single crystal silicon, so that the resistivity distribution of the second single crystal silicon can be more uniform, and the embodiment of the present invention does not limit this.

[0079] Step 207, after the final stage of the growth of the first silicon single crystal is completed, adjusting the rotation speed of the crucible according to a preset rotation speed, and adjusting the power of the heater according to a preset power;

[0080] Among them, the first threshold is 3r / min, and the second threshold is 5kw.

[0081] In an embodiment of the present invention, after the end stage of the growth of the first single crystal silicon is completed, the speed of the crucible is adjusted according to the preset speed, and the power of the heater is adjusted according to the preset power, wherein the range of the preset speed can be within ±3r / min of the speed of the crucible in the seeding stage, that is, the maximum value of the preset speed can be the speed of the crucible in the seeding stage plus 3r / min, and the minimum value of the preset speed can be the speed of the crucible in the seeding stage minus 3r / min; the range of the preset power can be within ±5kw of the power of the heater in the seeding stage, that is, the maximum value of the preset power can be the power of the heater in the seeding stage plus 5kw, and the minimum value of the preset power can be the power of the heater in the seeding stage minus 5kw. After adjusting the speed of the crucible and the power of the heater, the crucible can be rotated at the preset speed and the heater can be operated at the preset power, thereby keeping the temperature of the silicon melt in the crucible unchanged, so that the volatilization amount of the dopant in the silicon melt is equal in the same time period, thereby ensuring the uniformity of the resistivity distribution of the head and tail of each single crystal silicon.

[0082] Step 208, placing the doping device 30 into the single crystal furnace 10, adjusting the size of the opening of the doping device 30, and adding the dopant into the crucible 11 through the opening to grow a second silicon single crystal.

[0083] In the embodiment of the present invention, after adjusting the rotation speed of the crucible 11 and the power of the heater, Figure 2 As shown, the doping device 30 includes a cylinder bottom 31 and a cylinder body 32 that are movably connected. The doping device 30 is placed in the single crystal furnace 10. The doping device 30 can be connected to the single crystal furnace 10. At this time, the cylinder bottom 31 and the cylinder body 32 of the doping device 30 are separated to form an opening. The size of the opening of the doping device 30 is adjusted, and the dopant enters the crucible 11 from the opening to grow the second single crystal silicon. In the single crystal furnace 10, as the temperature rises, the dopant undergoes a melting process and gradually changes from a solid state to a liquid state. As the temperature further rises, the dopant may undergo a vaporization process and gradually change from a liquid state to a gaseous state and volatilize. When the rotation speed of the crucible 11 and the power of the heater are kept constant, the volatilization amount of the dopant in the same time is equal, which can effectively control the volatilization amount of the dopant, and then control the uniformity of the resistivity distribution of the single crystal silicon. At this time, the dopant is directly added into the crucible 11 , and silicon material required for growing the second silicon single crystal may also be added into the crucible 11 through the feeding channel 22 of the feeding device 20 , which is not limited in this embodiment of the present invention.

[0084] Of course, in an embodiment of the present invention, silicon material can also be added to the crucible in real time through the feeding device 20 during the growth process of the first silicon monocrystalline and the second silicon monocrystalline, so that the weight of the silicon material in the crucible 11 at any time is a preset weight, thereby ensuring that the amount of silicon material in the crucible 11 remains unchanged before each doping.

[0085] Embodiment 3

[0086] Reference Figure 4 , shows a flow chart of a single crystal silicon doping method according to Embodiment 3 of the present invention, which may specifically include the following steps:

[0087] Step 301: Add silicon material and a first weight of dopant into a crucible to grow a first silicon single crystal.

[0088] Step 302, after the final stage of the growth of the first silicon single crystal is completed, adjusting the rotation speed of the crucible according to a preset rotation speed, and adjusting the power of the heater according to a preset power;

[0089] Step 303: Add a second weight of the dopant into the crucible to grow a second silicon single crystal.

[0090] In the embodiment of the present invention, step 301 may refer to the above step 101, step 302 may refer to the above step 102, and step 303 may refer to the above step 103. To avoid repetition, they are not described again here.

[0091] Step 304, after the final stage of the growth of the second silicon single crystal is completed, adjusting the rotation speed of the crucible according to a preset rotation speed, and adjusting the power of the heater according to a preset power;

[0092] Step 305: Add a third weight of the dopant into the crucible, and grow another second silicon single crystal until the amount of the second silicon single crystal reaches a preset amount.

[0093] Step 306, ending doping.

[0094] In an embodiment of the present invention, the preset number is the number of second single crystal silicon that needs to be grown in the whole process of growing single crystal silicon, which is preset by a person skilled in the art. When the number of the second single crystal silicon that has been grown is less than the preset number, the second single crystal silicon needs to continue to grow, so it is necessary to perform steps 304 and 305, that is, after the end stage of the growth of the second single crystal silicon is completed, the speed of the crucible is adjusted according to the preset speed, and the power of the heater is adjusted according to the preset power, and the third weight of the dopant is added to the crucible to grow the next second single crystal silicon, until the number of the second single crystal silicon reaches the preset number, then there is no need to grow the second single crystal silicon, so that steps 304 and 305 are ended, and step 306 can be executed to end the doping, and the whole process of single crystal silicon growth is ended. It can be understood that the third weight of the dopant can be calculated based on the target resistivity of the next second single crystal silicon. In an embodiment of the present invention, when the number of the second single crystal silicon does not reach the preset number, steps 304 and 305 need to be performed in a loop until the number of the second single crystal silicon reaches the preset number, and the loop ends. Among them, step 304 and step 305 can be executed once, or can be executed multiple times in a loop, which is not limited in the embodiment of the present invention.

[0095] Specifically, when the number of second silicon monocrystals grown is less than the preset number and before the final stage of the growth of the second silicon monocrystal is completed, the target resistivity of the next second silicon monocrystal can be determined, the third weight of the dopant required for the next second silicon monocrystal is calculated, and the third weight of the dopant is added to the doping device outside the single crystal furnace. This step can refer to the above steps 204, 205 and 206, which will not be repeated here. It can be understood that the second silicon monocrystal actually refers to the silicon monocrystal other than the first silicon monocrystal. Therefore, the specifications, dimensions, target resistivity and other parameters of each silicon monocrystal in the second silicon monocrystal can be the same or different, and the embodiment of the present invention does not limit this. After the final stage of the growth of the second silicon monocrystal is completed, the rotation speed of the crucible can be adjusted according to the preset rotation speed, and the power of the heater can be adjusted according to the preset power. This step can refer to the above step 207, which will not be repeated here. A third weight of dopant is added into the crucible to grow a second silicon single crystal. The doping device containing the third weight of dopant is placed into the single crystal furnace to grow the second silicon single crystal. This step can refer to the above step 208 and will not be repeated here.

[0096] In the embodiment of the present invention, the dopant is optionally gallium. In P-type monocrystalline silicon, the performance of the monocrystalline silicon grown by doping with gallium is better than that grown by doping with other dopants, and the solar cell using this monocrystalline silicon has excellent performance in terms of conversion efficiency, service life, and resistance to harsh environments, thereby improving the uniformity of the resistivity distribution of the monocrystalline silicon doped with gallium, and further improving the performance of the solar cell.

[0097] Embodiment 4

[0098] The embodiment of the present invention further provides a method for manufacturing single crystal silicon. The method for manufacturing single crystal silicon of the present invention is described below in conjunction with an example of an actual production process:

[0099] 200 kg of silicon material is put into a 28-inch hot field to produce 6 single crystal silicon. When the target resistivity of the 6 single crystal silicon is the same: the target resistivity of each single crystal silicon is 0.6 Ω·cm. When the target resistivity of the 6 single crystal silicon is not exactly the same, the target resistivity of each single crystal silicon is between 0.5 Ω·cm and 0.7 Ω·cm, for example: the target resistivity of the first single crystal silicon is 0.5 Ω·cm; the target resistivity of the second single crystal silicon is 0.7 Ω·cm, and the target resistivity of the subsequent single crystal silicon is between 0.5 Ω·cm and 0.7 Ω·cm.

[0100] The dopant used in the production process is high-purity gallium. When the target resistivity of the six silicon single crystals is the same, the dopant content required for each single crystal is the same, which is 2g. When the target resistivity of the six silicon single crystals is not exactly the same, the dopant content required for each single crystal is not exactly the same. For example, it is calculated that the doping amount required for the first single crystal is 1.9g, and the doping amount required for the second single crystal is 2.1g. In the seeding stage of the crystal pulling process, the crucible speed is controlled to 9r / min, and the power of the heater is the seeding power.

[0101] However, in the actual crystal pulling process, the concentration of dopants is difficult to control, resulting in inconsistent resistivity at the head and tail of each single crystal silicon, with a large difference. For example, the resistivity of the head of single crystal silicon produced by the existing production process is 0.4Ω·cm, and the resistivity of the tail is 1.0Ω·cm, with a resistivity difference of 2.5 times between the head and tail.

[0102] The specific operation method of the embodiment of the present invention is as follows:

[0103] 1. Cleaning device.

[0104] 2. Calculate the amount of silicon material required to grow 6 single crystal silicon and the amount of doping required to grow the first single crystal silicon. Weigh 200 kg of silicon material and 2 g of dopant.

[0105] 3. After the thermal field is cleaned, the silicon material and dopant are passed through Figure 2 The feeding device 20 shown is added into the inner crucible of the high-purity quartz crucible, the heat field and the single crystal furnace are closed, vacuum is drawn, and after verifying that the vacuum leak rate meets the production requirements, the silicon material and the dopant are heated and melted.

[0106] 4. Adjust the crucible speed to 9r / min and the heater power to 60kw during the seeding stage.

[0107] 5. Immerse the seed crystal in the molten silicon and lift the seed crystal at a preset speed to reduce the diameter of the crystal. This process is the necking stage. After the seed crystal is immersed in the molten silicon, the seed crystal is quickly pulled up to form an inverted cone-shaped crystal with a large top and a small bottom at the bottom of the seed crystal to prevent the dislocation in the seed crystal from extending into the crystal.

[0108] 6. When the diameter of the crystal is reduced to the first preset diameter, the growth rate is slowed down to increase the diameter of the crystalline silicon. This process is the shoulder release stage. When the neck is reduced to the first preset diameter, it can be considered that the dislocation in the seed crystal will no longer affect the quality of the crystal. Therefore, it is necessary to slow down the growth rate to increase the diameter of the crystalline silicon so that the diameter gradually increases to the designed size.

[0109] 7. When the diameter of the silicon monocrystalline reaches the second preset diameter, the growth rate is maintained unchanged and it grows to the preset length. This process is the isodiameter growth stage. When the diameter of the silicon monocrystalline grows to the second preset diameter, it can be considered to have grown to the designed size. Therefore, it is necessary to maintain the growth rate and keep the diameter unchanged. As the silicon monocrystalline is pulled, it continues to grow to the designed preset length.

[0110] 8. After the finishing stage cooling treatment, the first single crystal silicon is obtained. The single crystal silicon grown to a preset length is subjected to the finishing treatment of reducing its diameter, and the temperature is lowered at the same time, and it is taken out of the single crystal furnace to obtain the first single crystal silicon.

[0111] 9. Before the final stage of the growth of the first silicon single crystal is completed, calculate the doping dosage required for the growth of the second silicon single crystal and weigh 2g of dopant.

[0112] 10. After the doping device is cleaned, add the dopant outside the single crystal furnace. Figure 2 In the doping device 30 shown.

[0113] 11. During the growth of the first silicon single crystal, silicon material is added between the inner crucible and the outer crucible in real time through the feeding device 20 so that the weight of the silicon material in the crucible is 200 kg at any time.

[0114] 12. After the final stage of the growth of the first silicon single crystal is completed, the crucible rotation speed is adjusted to within the range of 6 r / min to 12 r / min, and the heater power is adjusted to within the range of 55 kw to 65 kw.

[0115] 13. Place the doping device 30 into the single crystal furnace, adjust the size of the opening of the doping device 30, and add the dopant into the inner crucible through the opening.

[0116] 14. Referring to the above method, after the final stage of the growth of the previous silicon single crystal is completed, the crucible speed and the heater power are adjusted, and then the doping device 30 is added with dopants to generate other silicon single crystals until the number of silicon single crystals meets the preset number. For example, the first silicon single crystal can be the first silicon single crystal in the entire manufacturing process, and the second silicon single crystal can be the silicon single crystal manufactured after the first silicon single crystal is generated. In the process of continuous manufacturing of several second silicon single crystals, the crucible speed and the heater power can be adjusted after the final stage of the previous second silicon single crystal is completed, and then doping is performed to generate other second silicon single crystals.

[0117] 15. Test the resistivity of the generated single crystal silicon.

[0118] When the target resistivity of the six silicon monocrystals is the same, the head resistivity of each silicon monocrystal is 0.5Ω·cm, and the tail resistivity of each silicon monocrystal is 0.7Ω·cm. It can be seen that the ratio between the head resistivity and the tail resistivity is reduced to 1.4 times. Compared with the traditional process, the resistivity of each silicon monocrystal is significantly improved.

[0119] When the target resistivity of the six single crystal silicon strands is not exactly the same, the head resistivity of the first single crystal silicon strand is 0.6Ω·cm, and the tail resistivity is 0.7Ω·cm. It can be seen that the ratio between the head resistivity and the tail resistivity of the first single crystal silicon strand is reduced to 1.16 times, and the resistivity of the single crystal silicon strand is significantly improved compared to the traditional process. The resistivity improvement effect of the second and third single crystal silicon strands is similar.

[0120] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0121] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for doping single crystal silicon, characterized in that: The method comprises: Adding silicon material and a first weight of a dopant into a crucible to grow a first silicon single crystal; After the final stage of the growth of the first silicon monocrystalline is completed, the rotation speed of the crucible is adjusted according to a preset rotation speed, and the power of the heater is adjusted according to a preset power, wherein the absolute value of the difference between the preset rotation speed and the rotation speed of the crucible in the seeding stage is less than or equal to a first threshold, and the absolute value of the difference between the preset power and the power of the heater in the seeding stage is less than or equal to a second threshold; adding a second weight of the dopant into the crucible to grow a second silicon single crystal; During the growth of the first silicon single crystal and the second silicon single crystal, the silicon material is dynamically added into the crucible so that the weight of the silicon material in the crucible at any moment is a preset weight.

2. The method for doping single crystal silicon according to claim 1, characterized in that: The step of adding silicon material and a first weight of dopant into a crucible before growing a first silicon single crystal comprises: determining a target resistivity of the first silicon single crystal; A first weight of the dopant required for the first single silicon crystal is calculated.

3. The method for doping single crystal silicon according to claim 1 or 2, characterized in that: The step of adding the second weight of the dopant into the crucible before growing the second silicon single crystal comprises: determining a target resistivity of the second single crystal silicon; calculating a second weight of the dopant required for the second single silicon crystal; and Outside the single crystal furnace, adding a second weight of the dopant into a doping device; The step of adding a second weight of the dopant into the crucible to grow a second silicon single crystal comprises: placing the doping device into the single crystal furnace; adjusting the opening size of the doping device; and The dopant is added into the crucible through the opening to grow a second silicon single crystal.

4. The method for doping single crystal silicon according to claim 1, characterized in that: After adding the second weight of the dopant into the crucible and growing the second silicon single crystal, the method comprises: After the end stage of the growth of the second silicon single crystal is completed, adjusting the rotation speed of the crucible according to the preset rotation speed, and adjusting the power of the heater according to the preset power; A third weight of the dopant is added into the crucible, and another second silicon single crystal is grown until the amount of the second silicon single crystal reaches a preset amount.

5. The method for doping single crystal silicon according to claim 4, characterized in that: The step of adding the third weight of the dopant into the crucible before growing the next second silicon single crystal comprises: determining a target resistivity of a next strand of the second single crystal silicon; calculating a third weight of the dopant required for a next strand of the second single crystal silicon; Outside the single crystal furnace, a third weight of the dopant is added into the doping device.

6. The method for doping single crystal silicon according to claim 1, characterized in that: The first threshold is 3r / min, and the second threshold is 5kw.

7. The method for doping single crystal silicon according to claim 1, characterized in that: The crucible comprises an inner crucible and an outer crucible; The step of adding the silicon material and the first weight of the dopant into the crucible to grow the first silicon single crystal comprises: adding the silicon material and the first weight of the dopant between the inner crucible and the outer crucible or into the inner crucible to grow the first silicon single crystal; The dynamically adding the silicon material into the crucible during the growth of the first silicon single crystal and the second silicon single crystal comprises: dynamically adding the silicon material between the inner crucible and the outer crucible through a feeding device during the growth of the first silicon single crystal and the second silicon single crystal.

8. The method for doping single crystal silicon according to claim 1, characterized in that: The dopant is gallium or a gallium-containing compound.

9. A method for manufacturing single crystal silicon, characterized in that: The method comprises the single crystal silicon doping method according to any one of claims 1 to 8.

10. The method for manufacturing single crystal silicon according to claim 9, characterized in that: The step of adding silicon material and a first weight of a dopant into a crucible to grow a first silicon single crystal comprises: Adding silicon material and a first weight of a dopant into an inner crucible, and heating to melt the silicon material and the dopant; Immersing the seed crystal in molten silicon, and lifting the seed crystal at a preset speed to reduce the diameter of the crystal; When the diameter of the crystal is reduced to a first preset diameter, slowing down the growth rate to increase the diameter of the crystal; When the diameter of the silicon single crystal reaches a second preset diameter, the growth speed is maintained unchanged and the single crystal is grown to a preset length; After the final stage of cooling treatment, the first single crystal silicon is obtained.

Citation Information

Patent Citations

  • Growth device, growth furnace and preparation method of yttrium lithium fluoride laser crystals

    CN104674344A

  • Pulling of single crystal

    JP1997255479A

  • Method for regulating specific resistance of single crystal silicon and apparatus for producing single crystal silicon

    JP1998029894A

  • Sb-DOPED SILICON SINGLE CRYSTAL AND GROWING METHODTHEREOF

    KR1020070066326A

  • Continuous production method for crystalline silicon and production apparatus for the same