A double-sided battery grid back panel glass assembly and preparation method thereof
By using specific formulas of EVA and POE film layers and grid backplane glass layers in double-sided photovoltaic modules, the problems of insufficient light utilization and weather resistance of photovoltaic modules are solved, and the power generation efficiency and weather resistance are improved.
Patent Information
- Application Number
- CN202110855294.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-07-28
AI Technical Summary
The existing double-sided photovoltaic modules have insufficient light utilization efficiency and weather resistance, especially in high temperature and high humidity environments, which affects power generation efficiency.
A double-sided battery grid backplane glass assembly is used, which is composed of a front encapsulation glass layer, an EVA film layer, a battery sheet layer, a POE film layer and a grid backplane glass layer. The EVA film layer and the POE film layer are added separately. Antioxidants, light stabilizers and UV absorbers, the grid backing glass layer has a glaze layer on the outside to increase reflectivity.
It improves the power generation efficiency and weather resistance of double-sided photovoltaic modules, enhances the weather resistance and light transmittance of EVA film layer and POE film layer, uses grid backplane glass to increase optical secondary reflection, and improves the power of photovoltaic modules output.
Smart Images

Figure CN113675286B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery assemblies, and more specifically, to a double-sided battery grid backplane glass assembly and a preparation method thereof. Background Art
[0002] Conventional photovoltaic modules can only receive sunlight on the front side to generate electricity, while bifacial photovoltaic modules, due to their special cell structure and transparent backplane material, can effectively use the received light on the back side to generate electricity in addition to the front side. These lights include reflected light from the ground, scattered light in the atmosphere, reflected light from dust in the air, reflected light from surrounding buildings, etc. The bifacial power generation characteristics of bifacial photovoltaic modules usually enable them to generate more electricity than conventional photovoltaic modules; nowadays, with advanced cell technology, the back side of solar cells does not need to be treated with aluminum back field, and there will be no performance loss, which creates conditions for bifacial cells. Under the same unit installed capacity, the power generation of bifacial photovoltaic systems far exceeds that of single-sided systems. Measurement results show that under the same unit installed capacity, the former generates 10% to 30% more power than the latter. Due to the growing demand for photovoltaic systems in areas such as deserts where the intensity of solar radiation and ground reflectivity are very high, bifacial power generation solutions are becoming more and more popular.
[0003] The back of a bifacial photovoltaic module can generate electricity using reflected light from the ground. The higher the ground reflectivity, the stronger the light received by the back of the battery, and the better the power generation effect. Common ground reflectivities are: 15%-25% for grass, 25%-35% for concrete, and 55%-75% for wet snow. The use of bifacial photovoltaic modules on grass can increase power generation by 8%-10%, and on snow can increase power generation by up to 30%. Its main purpose is to generate more electricity per unit area, improve power generation efficiency, and reduce costs and increase efficiency.
[0004] The existing double-sided photovoltaic modules have insufficient back light utilization effect, and the weather resistance of the photovoltaic modules is insufficient during use. The encapsulation film layer in the photovoltaic modules is prone to power attenuation in high temperature and high humidity environments, affecting the efficiency of the photovoltaic modules. Summary of the invention
[0005] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides a double-sided cell grid backplane glass assembly and a preparation method thereof. The problem to be solved by the present invention is: how to improve the efficiency of the double-sided photovoltaic assembly and improve the weather resistance of the photovoltaic assembly.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a double-sided battery grid backplane glass assembly, the double-sided battery assembly comprising a front encapsulation glass layer, an EVA film layer, a battery layer, a POE film layer and a grid backplane glass layer stacked in sequence, a glaze layer being arranged on the light-facing surface of the grid backplane glass layer, and an anti-reflection film being arranged on the surfaces of the battery layer in contact with the EVA film layer and the POE film layer.
[0007] In a preferred embodiment, the EVA film layer comprises the following raw materials in parts by weight: 60-90 parts of ethylene-vinyl acetate copolymer, 5-10 parts of polyolefin elastomer, 0.5-2.5 parts of modified phosphite antioxidant, 0.1-1 parts of light stabilizer, 0.2-0.8 parts of fluorescent brightener and 3-6 parts of first cross-linking agent; the POE film layer comprises the following raw materials in parts by weight: 75-90 parts of grafted modified POE resin, 0.5-3 parts of anti-aging additive, 0.5-1.5 parts of coupling agent, 1-3 parts of second cross-linking agent, 0.1-0.6 parts of ultraviolet absorber and 0.1-0.6 parts of antioxidant.
[0008] In a preferred embodiment, the EVA film layer comprises the following raw materials in parts by weight: 70-80 parts of ethylene-vinyl acetate copolymer, 7-9 parts of polyolefin elastomer, 1-2 parts of modified phosphite antioxidant, 0.4-0.6 parts of light stabilizer, 0.4-0.6 parts of fluorescent brightener and 4-5 parts of first cross-linking agent; the POE film layer comprises the following raw materials in parts by weight: 80-85 parts of grafted modified POE resin, 1.5-2 parts of anti-aging additive, 0.8-1.2 parts of coupling agent, 2-3 parts of second cross-linking agent, 0.2-0.4 parts of ultraviolet absorber and 0.2-0.4 parts of antioxidant.
[0009] In a preferred embodiment, the EVA film layer comprises the following raw materials in parts by weight: 75 parts of ethylene-vinyl acetate copolymer, 8 parts of polyolefin elastomer, 1.5 parts of modified phosphite antioxidant, 0.5 parts of light stabilizer, 0.5 parts of fluorescent brightener and 4.5 parts of first cross-linking agent; the POE film layer comprises the following raw materials in parts by weight: 82 parts of grafted modified POE resin, 1.8 parts of anti-aging additive, 1 part of coupling agent, 2.5 parts of second cross-linking agent, 0.3 parts of ultraviolet absorber and 0.3 parts of antioxidant.
[0010] In a preferred embodiment, the light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate or N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine; the fluorescent whitening agent is 2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene; the first crosslinking agent is a mixture of ethoxylated trimethylolpropane triacrylate and ethoxylated trimethylolpropane; the anti-aging agent is 2,2,6 , one of 6-tetramethyl-4-piperidinyl stearate, salicylic acid or 2-hydroxy-4-octyloxybenzophenone; the coupling agent is a silane coupling agent; the second cross-linking agent is a mixture of tert-butyl peroxide-2-ethylhexyl carbonate and triallyl isocyanurate; the ultraviolet absorber is 2-hydroxy-4-octyloxybenzophenone, and the antioxidant is 6-tert-butyl-4-methylphenol or bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide.
[0011] In a preferred embodiment, the reflectivity of the glaze layer is 85-95%, the weight ratio of ethoxylated trimethylolpropane triacrylate and ethoxylated trimethylolpropane in the first cross-linking agent is (3-5):1, the weight ratio of peroxy-2-ethylhexyl carbonate and triallyl isocyanurate in the second cross-linking agent is (2-4):1, and the grafted modified POE resin is maleic anhydride grafted modified POE resin.
[0012] The present invention also provides a method for preparing a double-sided battery grid backplane glass assembly, and the specific preparation steps are as follows:
[0013] Step 1: Preparation of EVA film layer, placing the weighed phosphite antioxidant in a reaction container for ultrasonic treatment, heating to 70-90°C, adding isooctyl alcohol, organic amine compound, polycarbodiimide and silane coupling agent to the reaction container, stirring for reaction for 30-50 minutes, keeping warm and standing for 2-4 hours, and then filtering, concentrating and crystallizing the filtrate, and drying to obtain a modified phosphite antioxidant, mixing the modified phosphite antioxidant with ethylene-vinyl acetate copolymer, polyolefin elastomer, light stabilizer, fluorescent brightener and first cross-linking agent, and then placing in a twin-screw extruder for heating and melting to extrude into a film, and then rolling the film, cooling and shaping, and winding to obtain an EVA film;
[0014] Step 2: Preparation of POE film layer: according to the above weight parts, the graft modified POE resin, anti-aging additive, coupling agent, second cross-linking agent, ultraviolet absorber and antioxidant are mixed and evenly mixed, and then placed in a twin-screw extruder to heat, melt and extrude into a film, and then the POE film is obtained by rolling, cooling and shaping, and winding;
[0015] Step 3: Use welding tape to weld the selected battery cells to form a battery cell layer, and then lay the front encapsulation glass layer, EVA film layer, battery cell layer, POE film layer and grid backplane glass layer in order. After laying, perform lamination. After lamination, use the frame to assemble and package to obtain a double-sided battery grid backplane glass assembly.
[0016] In a preferred embodiment, the amounts of isooctyl alcohol, organic amine compound, polycarbodiimide and silane coupling added in step 1 are respectively (10-15%), (8-15%), (5-8%) and (0.5-1.5%) of the total amount of phosphite antioxidant.
[0017] In a preferred embodiment, when selecting the battery cells in step 3, battery cells with qualified appearance, the same color and efficiency are selected for welding.
[0018] In a preferred embodiment, the double-sided battery grid backplane glass assembly packaged in step three is tested for electrical properties, weather resistance and anti-PID performance.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] 1. A double-sided battery grid backplane glass component prepared by the raw material formula of the present invention, wherein the EVA film layer adopts ethylene-vinyl acetate copolymer as a raw material, and is added with a polyolefin elastomer, a modified phosphite antioxidant, a light stabilizer, a fluorescent brightener and a first cross-linking agent, which can effectively improve the weather resistance and light transmittance of the EVA film layer, and the phosphite antioxidant improves the hydrolysis resistance and stability after modification. When the phosphite antioxidant is used in the EVA film layer, it can not only improve the weather resistance, but also has a good light transmittance, thereby improving the power of the photovoltaic component; the POE film layer adopts a grafted modified POE resin as a raw material, and is added with an anti-aging aid, a coupling agent, a second cross-linking agent, an ultraviolet absorber and an antioxidant. The POE resin has good ultraviolet light resistance and mechanical properties after being grafted and modified by maleic anhydride, and the anti-aging aid, the ultraviolet absorber and the antioxidant can make the POE film layer have good weather resistance;
[0021] 2. The back panel of the double-sided battery module of the present invention adopts a grid back panel glass. A grid is formed on the outer side of the back panel glass, and a glaze layer is arranged on the grid line. The glaze layer has a high reflectivity and can make full use of the blank area between the strings to increase the optical secondary reflection, so that the battery strings on both sides can receive more light radiation and increase the power of the photovoltaic module. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0023] Figure 1 is a schematic diagram of the cross-sectional structure of a double-sided battery assembly of the present invention;
[0024] Figure 2 It is a schematic diagram of the structure of the light-facing surface of the grid back panel glass layer of the present invention.
[0025] In the figure: 1 front encapsulation glass layer, 2 EVA film layer, 3 battery cell layer, 4 POE film layer, 5 grid back panel glass layer, 6 glaze layer, 7 anti-reflection film. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Embodiment 1:
[0028] See also Figure 1-2 As shown, the present invention provides a double-sided battery grid backplane glass assembly, the double-sided battery assembly includes a front encapsulation glass layer 1, an EVA film layer 2, a battery layer 3, a POE film layer 4 and a grid backplane glass layer 5 stacked in sequence, a glaze layer 6 is arranged on the light-facing surface of the grid backplane glass layer 5, and the surfaces of the battery layer 3 in contact with the EVA film layer 2 and the POE film layer 4 are all provided with anti-reflection films 7.
[0029] In a preferred embodiment, the EVA film layer 2 includes the following raw materials in parts by weight: 60 parts of ethylene-vinyl acetate copolymer, 5 parts of polyolefin elastomer, 0.5 parts of modified phosphite antioxidant, 0.1 parts of light stabilizer, 0.2 parts of fluorescent brightener and 3 parts of first cross-linking agent; the POE film layer 4 includes the following raw materials in parts by weight: 75 parts of grafted modified POE resin, 0.5 parts of anti-aging additive, 0.5 parts of coupling agent, 1 part of second cross-linking agent, 0.1 parts of ultraviolet absorber and 0.1 parts of antioxidant.
[0030] In a preferred embodiment, the light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate or N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine; the fluorescent whitening agent is 2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene; the first crosslinking agent is a mixture of ethoxylated trimethylolpropane triacrylate and ethoxylated trimethylolpropane; the anti-aging agent is 2,2,6 , one of 6-tetramethyl-4-piperidinyl stearate, salicylic acid or 2-hydroxy-4-octyloxybenzophenone; the coupling agent is a silane coupling agent; the second cross-linking agent is a mixture of tert-butyl peroxide-2-ethylhexyl carbonate and triallyl isocyanurate; the ultraviolet absorber is 2-hydroxy-4-octyloxybenzophenone, and the antioxidant is 6-tert-butyl-4-methylphenol or bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide.
[0031] In a preferred embodiment, the reflectivity of the glaze layer 6 is 85-95%, the weight ratio of ethoxylated trimethylolpropane triacrylate and ethoxylated trimethylolpropane in the first cross-linking agent is 4:1, the weight ratio of peroxy-2-ethylhexyl carbonate and triallyl isocyanurate in the second cross-linking agent is 3:1, and the grafted modified POE resin is maleic anhydride grafted modified POE resin.
[0032] The present invention also provides a method for preparing a double-sided battery grid backplane glass assembly, and the specific preparation steps are as follows:
[0033] Step 1: Preparation of EVA film layer, placing the weighed phosphite antioxidant in a reaction container for ultrasonic treatment, heating to 80°C, adding isooctyl alcohol, organic amine compound, polycarbodiimide and silane coupling agent into the reaction container, stirring for reaction for 40 minutes, keeping the temperature for 3 hours, and then filtering, concentrating and crystallizing the filtrate, and drying to obtain a modified phosphite antioxidant, mixing the modified phosphite antioxidant with ethylene-vinyl acetate copolymer, polyolefin elastomer, light stabilizer, fluorescent brightener and first cross-linking agent, and then placing in a twin-screw extruder for heating and melting to extrude into a film, and then rolling the film, cooling and shaping, and winding to obtain an EVA film;
[0034] Step 2: Preparation of POE film layer: according to the above weight parts, the graft modified POE resin, anti-aging additive, coupling agent, second cross-linking agent, ultraviolet absorber and antioxidant are mixed and evenly mixed, and then placed in a twin-screw extruder to heat, melt and extrude into a film, and then the POE film is obtained by rolling, cooling and shaping, and winding;
[0035] Step 3: Use welding tape to weld the selected battery cells to form a battery cell layer, and then lay the front encapsulation glass layer, EVA film layer, battery cell layer, POE film layer and grid backplane glass layer in order. After laying, perform lamination. After lamination, use the frame to assemble and package to obtain a double-sided battery grid backplane glass assembly.
[0036] In a preferred embodiment, the amounts of isooctyl alcohol, organic amine compound, polycarbodiimide and silane coupling added in step 1 are 13%, 9%, 7% and 1% of the total amount of the phosphite antioxidant, respectively.
[0037] In a preferred embodiment, when selecting the battery cells in step 3, battery cells with qualified appearance, the same color and efficiency are selected for welding.
[0038] In a preferred embodiment, the double-sided battery grid backplane glass assembly packaged in step three is tested for electrical properties, weather resistance and anti-PID performance.
[0039] Embodiment 2:
[0040] Different from Example 1, the present invention provides a double-sided battery grid backplane glass assembly, the EVA film layer 2 includes the following raw materials in parts by weight: 75 parts of ethylene-vinyl acetate copolymer, 8 parts of polyolefin elastomer, 1.5 parts of modified phosphite antioxidant, 0.5 parts of light stabilizer, 0.5 parts of fluorescent brightener and 4.5 parts of first cross-linking agent; the POE film layer 4 includes the following raw materials in parts by weight: 82 parts of grafted modified POE resin, 1.8 parts of anti-aging additive, 1 part of coupling agent, 2.5 parts of second cross-linking agent, 0.3 parts of ultraviolet absorber and 0.3 parts of antioxidant.
[0041] Embodiment 3:
[0042] Different from Examples 1-2, the present invention provides a double-sided battery grid backplane glass assembly, wherein the EVA film layer comprises the following raw materials in parts by weight: 90 parts of ethylene-vinyl acetate copolymer, 10 parts of polyolefin elastomer, 2.5 parts of modified phosphite antioxidant, 1 part of light stabilizer, 0.8 parts of fluorescent brightener and 6 parts of first cross-linking agent; the POE film layer comprises the following raw materials in parts by weight: 90 parts of grafted modified POE resin, 3 parts of anti-aging additive, 1.5 parts of coupling agent, 3 parts of second cross-linking agent, 0.6 parts of ultraviolet absorber and 0.6 parts of antioxidant.
[0043] Embodiment 4:
[0044] The present invention provides a double-sided battery grid backplane glass assembly, which comprises a front encapsulation glass layer 1, an EVA film layer 2, a battery layer 3, a POE film layer 4 and a grid backplane glass layer 5 stacked in sequence, a glaze layer 6 is arranged on the light-facing surface of the grid backplane glass layer 5, and an anti-reflection film 7 is arranged on the surfaces of the battery layer 3 that are in contact with the EVA film layer 2 and the POE film layer 4.
[0045] In a preferred embodiment, the EVA film layer 2 includes the following raw materials in parts by weight: 60 parts of ethylene-vinyl acetate copolymer, 5 parts of polyolefin elastomer, 0.5 parts of phosphite antioxidant, 0.1 parts of light stabilizer, 0.2 parts of fluorescent brightener and 3 parts of first cross-linking agent; the POE film layer 4 includes the following raw materials in parts by weight: 75 parts of grafted modified POE resin, 0.5 parts of anti-aging additive, 0.5 parts of coupling agent, 1 part of second cross-linking agent, 0.1 parts of ultraviolet absorber and 0.1 parts of antioxidant.
[0046] In a preferred embodiment, the light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate or N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine; the fluorescent whitening agent is 2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene; the first crosslinking agent is a mixture of ethoxylated trimethylolpropane triacrylate and ethoxylated trimethylolpropane; the anti-aging agent is 2,2,6 , one of 6-tetramethyl-4-piperidinyl stearate, salicylic acid or 2-hydroxy-4-octyloxybenzophenone; the coupling agent is a silane coupling agent; the second cross-linking agent is a mixture of tert-butyl peroxide-2-ethylhexyl carbonate and triallyl isocyanurate; the ultraviolet absorber is 2-hydroxy-4-octyloxybenzophenone, and the antioxidant is 6-tert-butyl-4-methylphenol or bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide.
[0047] In a preferred embodiment, the reflectivity of the glaze layer 6 is 85-95%, the weight ratio of ethoxylated trimethylolpropane triacrylate and ethoxylated trimethylolpropane in the first cross-linking agent is 4:1, the weight ratio of peroxy-2-ethylhexyl carbonate and triallyl isocyanurate in the second cross-linking agent is 3:1, and the grafted modified POE resin is maleic anhydride grafted modified POE resin.
[0048] The present invention also provides a method for preparing a double-sided battery grid backplane glass assembly, and the specific preparation steps are as follows:
[0049] Step 1: Preparation of EVA film layer, mixing phosphite antioxidant with ethylene-vinyl acetate copolymer, polyolefin elastomer, light stabilizer, fluorescent brightener and first cross-linking agent evenly, placing in a twin-screw extruder to heat and melt to extrude into a film, and then rolling, cooling and shaping, and winding to obtain EVA film;
[0050] Step 2: Preparation of POE film layer: according to the above weight parts, the graft modified POE resin, anti-aging additive, coupling agent, second cross-linking agent, ultraviolet absorber and antioxidant are mixed and evenly mixed, and then placed in a twin-screw extruder to heat, melt and extrude into a film, and then the POE film is obtained by rolling, cooling and shaping, and winding;
[0051] Step 3: Use welding tape to weld the selected battery cells to form a battery cell layer, and then lay the front encapsulation glass layer, EVA film layer, battery cell layer, POE film layer and grid backplane glass layer in order. After laying, perform lamination. After lamination, use the frame to assemble and package to obtain a double-sided battery grid backplane glass assembly.
[0052] In a preferred embodiment, when selecting the battery cells in step 3, battery cells with qualified appearance, the same color and efficiency are selected for welding.
[0053] In a preferred embodiment, the double-sided battery grid backplane glass assembly packaged in step three is tested for electrical properties, weather resistance and anti-PID performance.
[0054] The EVA films and POE films prepared in the above embodiments 1-4 were respectively taken as experimental group 1, experimental group 2, experimental group 3 and experimental group 4, and the EVA films and POE films prepared by traditional EVA resin and POE resin were used as the control group. The selected EVA films and POE films were respectively tested for UV aging resistance index and wet heat aging resistance index, and the comprehensive conversion rate and anti-PID performance of the double-sided photovoltaic modules made of the selected EVA films and POE films were tested (the back panels of the double-sided photovoltaic modules prepared by traditional EVA resin and POE resin are ordinary glass back panels). The test results are shown in Table 1:
[0055]
[0056] Table 1
[0057] As can be seen from Table 1, the double-sided battery grid backplane glass assembly of the present invention has a higher comprehensive conversion rate and better anti-PID performance than the traditional double-sided photovoltaic battery assembly. In addition, the EVA film and POE film used in the present invention have better UV resistance and moisture and heat resistance, thereby improving the weather resistance of the double-sided photovoltaic battery assembly. The double-sided battery grid backplane glass assembly prepared by the raw material formula of the present invention, the EVA film layer adopts ethylene-vinyl acetate copolymer as raw material, and is added with polyolefin elastomer, modified phosphite antioxidant, light stabilizer, fluorescent brightener and the first cross-linking agent, which can effectively improve the weather resistance and light transmittance of the EVA film layer. The phosphite antioxidant is modified to improve the hydrolysis resistance and stability. When the phosphite antioxidant is used in the EVA film layer, not only It can improve weather resistance and has good light transmittance, which increases the power of photovoltaic modules. The POE film layer uses grafted modified POE resin as raw material, and is added with anti-aging additives, coupling agents, second cross-linking agents, ultraviolet absorbers and antioxidants. The POE resin has good ultraviolet light resistance and mechanical properties after being grafted and modified by maleic anhydride. The anti-aging additives, ultraviolet absorbers and antioxidants can make the POE film layer have good weather resistance. The backplane of the double-sided battery module uses grid backplane glass, a grid is formed on the outer side of the backplane glass, and a glaze layer is arranged on the grid line. The glaze layer has a high reflectivity and can make full use of the blank area between the strings to increase optical secondary reflection, so that the battery strings on both sides can receive more light radiation and increase the power of the photovoltaic module.
[0058] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A double-sided cell grid backplane glass assembly, characterized in that: The double-sided battery grid backplane glass assembly comprises a front encapsulation glass layer (1), an EVA film layer (2), a battery layer (3), a POE film layer (4) and a grid backplane glass layer (5) which are stacked in sequence; a glaze layer (6) is provided on the light-facing surface of the grid backplane glass layer (5); and the surfaces of the battery layer (3) in contact with the EVA film layer (2) and the POE film layer (4) are both provided with an anti-reflection film (7); The EVA adhesive film layer (2) comprises the following raw materials in parts by weight: 60-90 parts of ethylene-vinyl acetate copolymer, 5-10 parts of polyolefin elastomer, 0.5-2.5 parts of modified phosphite antioxidant, 0.1-1 parts of light stabilizer, 0.2-0.8 parts of fluorescent brightener and 3-6 parts of first cross-linking agent; the POE adhesive film layer (4) comprises the following raw materials in parts by weight: 75-90 parts of grafted modified POE resin, 0.5-3 parts of anti-aging additive, 0.5-1.5 parts of coupling agent, 1-3 parts of second cross-linking agent, 0.1-0.6 parts of ultraviolet absorber and 0.1-0.6 parts of antioxidant; The preparation method of the double-sided battery grid backplane glass assembly has the following specific preparation steps: Step 1: Preparation of EVA film layer, placing the weighed phosphite antioxidant in a reaction container for ultrasonic treatment, heating to 70-90°C, adding isooctyl alcohol, organic amine compound, polycarbodiimide and silane coupling agent to the reaction container, stirring for reaction for 30-50 minutes, keeping warm and standing for 2-4 hours, and then filtering, concentrating and crystallizing the filtrate, and drying to obtain a modified phosphite antioxidant, mixing the modified phosphite antioxidant with ethylene-vinyl acetate copolymer, polyolefin elastomer, light stabilizer, fluorescent brightener and first cross-linking agent, and then placing in a twin-screw extruder for heating and melting to extrude into a film, and then rolling the film, cooling and shaping, and winding to obtain an EVA film; Step 2: Preparation of POE film layer: according to the above weight parts, the graft modified POE resin, anti-aging additive, coupling agent, second cross-linking agent, ultraviolet absorber and antioxidant are mixed and evenly mixed, and then placed in a twin-screw extruder to heat, melt and extrude into a film, and then the POE film is obtained by rolling, cooling and shaping, and winding; Step 3: The selected cells are welded with welding ribbons to form a cell layer, and then the front encapsulation glass layer, EVA film layer, cell layer, POE film layer and mesh backplane glass layer are laid in order, and after the laying is completed, lamination is performed, and after the lamination, the frame is used for assembly and packaging to obtain a double-sided cell mesh backplane glass assembly; The light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate or N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine; the fluorescent whitening agent is 2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene; the first crosslinking agent is a mixture of ethoxylated trimethylolpropane triacrylate and ethoxylated trimethylolpropane; the anti-aging aid is 2,2,6,6-tetramethyl -4-piperidinyl stearate, salicylic acid or 2-hydroxy-4-n-octyloxybenzophenone; the coupling agent is a silane coupling agent; the second cross-linking agent is a mixture of tert-butyl peroxide-2-ethylhexyl carbonate and triallyl isocyanurate; the ultraviolet absorber is 2-hydroxy-4-n-octyloxybenzophenone, and the antioxidant is 6-tert-butyl-4-methylphenol or bis(3,5-tert-butyl-4-hydroxyphenyl) sulfide; The reflectivity of the glaze layer (6) is 85-95%, the weight ratio of ethoxylated trimethylolpropane triacrylate to ethoxylated trimethylolpropane in the first crosslinking agent is (3-5):1, the weight ratio of peroxy-2-ethylhexyl carbonate to triallyl isocyanurate in the second crosslinking agent is (2-4):1, and the graft-modified POE resin is a maleic anhydride graft-modified POE resin; The amounts of isooctyl alcohol, organic amine compound, polycarbodiimide and silane coupling added in step 1 are respectively (10-15%), (8-15%), (5-8%) and (0.5-1.5%) of the total amount of phosphite antioxidant.
2. A double-sided cell grid backplane glass assembly according to claim 1, characterized in that: The EVA film layer (2) comprises the following raw materials in parts by weight: 70-80 parts of ethylene-vinyl acetate copolymer, 7-9 parts of polyolefin elastomer, 1-2 parts of modified phosphite antioxidant, 0.4-0.6 parts of light stabilizer, 0.4-0.6 parts of fluorescent brightener and 4-5 parts of first cross-linking agent; the POE film layer (4) comprises the following raw materials in parts by weight: 80-85 parts of grafted modified POE resin, 1.5-2 parts of anti-aging additive, 0.8-1.2 parts of coupling agent, 2-3 parts of second cross-linking agent, 0.2-0.4 parts of ultraviolet absorber and 0.2-0.4 parts of antioxidant.
3. The double-sided cell grid backplane glass assembly according to claim 1, characterized in that: The EVA film layer (2) comprises the following raw materials in parts by weight: 75 parts of ethylene-vinyl acetate copolymer, 8 parts of polyolefin elastomer, 1.5 parts of modified phosphite antioxidant, 0.5 parts of light stabilizer, 0.5 parts of fluorescent brightener and 4.5 parts of first cross-linking agent; the POE film layer (4) comprises the following raw materials in parts by weight: 82 parts of grafted modified POE resin, 1.8 parts of anti-aging additive, 1 part of coupling agent, 2.5 parts of second cross-linking agent, 0.3 parts of ultraviolet absorber and 0.3 parts of antioxidant.
4. The double-sided cell grid backplane glass assembly according to claim 1, characterized in that: When selecting the battery cells in step 3, select the battery cells with qualified appearance, the same color and the same efficiency for welding.
5. The double-sided cell grid backplane glass assembly according to claim 1, characterized in that: The double-sided battery grid backplane glass assembly packaged in step three is tested for electrical properties, weather resistance and PID resistance.
Citation Information
Patent Citations
EVA adhesive film and preparation method thereof
CN105111950A
Two-sided dual-glass photovoltaic module glass back plate and two-sided dual-glass photovoltaic component
CN107863407A
Anti-PID POE adhesive film special for photovoltaic double-glass assembly packaging and preparation method thereof