Pressure measurement sheet set, pressure measurement sheet, dispersion liquid

By using a combination of microcapsules with glass transition temperatures above 150°C in the sheet set for pressure measurement, the precision of pressure measurement in high temperature environment is solved, and the effect of accurately measuring pressure distribution at high temperature is achieved.

CN114026401BActive Publication Date: 2024-11-26FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080045067.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2020-06-23
Publication Date
2024-11-26
Estimated Expiration
2040-06-23

AI Technical Summary

Technical Problem

In high temperature environments, existing pressure measurement sheets also produce color outside the pressurized area, and the pressure distribution cannot be accurately measured.

Method used

The pressure measurement sheet group containing microcapsules containing chromogens and color developer is adopted. The capsule wall of the microcapsules is composed of polyurea, polyurethane urea and polyurethane, and the glass transition temperature is set to 150°C or above, combined with The resin formed by polyisocyanate A and polyisocyanate B with 3 functions and above ensures that the chromogen does not leak at high temperatures.

Benefits of technology

The pressure distribution can be measured accurately in high temperature environments, mainly in the pressurized area, avoiding unnecessary color growth and improving measurement accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114026401B_ABST
    Figure CN114026401B_ABST
Patent Text Reader

Abstract

The present invention provides a pressure measurement sheet set, a pressure measurement sheet, and a dispersion liquid capable of measuring pressure distribution even when used in a high temperature environment. The pressure measurement sheet set of the present invention comprises: a first sheet having a first layer including microcapsules containing a color former; and a second sheet having a second layer including a color former, wherein the capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea, and polyurethane, and the glass transition temperature of the capsule wall is 150° C. or higher or the capsule wall does not show a glass transition temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a pressure measurement sheet set, a pressure measurement sheet and a dispersion liquid. Background Art

[0002] In recent years, the need to measure pressure distribution has tended to increase due to the higher functionality and higher definition of products.

[0003] For example, Patent Document 1 proposes a pressure measurement sheet using microcapsules containing an electron-donating leuco dye precursor.

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-019949 Summary of the invention

[0007] Technical issues to be solved by the invention

[0008] On the other hand, in various compression bonding operations under high temperature environments such as thermocompression bonding of integrated circuits and wiring in printed circuit boards, it is desired to measure precise pressure distribution in order to improve profitability.

[0009] The present inventors measured pressure distribution in a high temperature environment (180° C. or higher) using the pressure measurement sheet described in Patent Document 1 and found that color development also occurred outside the pressurized region, making it impossible to measure precise pressure distribution.

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a measuring sheet set and a pressure measuring sheet capable of measuring pressure of pressure distribution even when used in a high temperature environment.

[0011] Another object of the present invention is to provide a dispersion liquid.

[0012] Means for solving technical problems

[0013] As a result of intensive studies on the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by the following configuration.

[0014] (1) A pressure measurement sheet set comprising:

[0015] a first sheet having a first layer including microcapsules containing a coloring agent; and

[0016] a second sheet having a second layer containing a developer,

[0017] The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane,

[0018] The glass transition temperature of the capsule wall is 150° C. or higher or the capsule wall does not show a glass transition temperature.

[0019] (2) The pressure measurement sheet set according to (1), wherein:

[0020] The resin is formed using trifunctional or higher polyisocyanate A and polyisocyanate B.

[0021] The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule,

[0022] The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

[0023] (3) The pressure measurement sheet set according to (2), wherein:

[0024] The mass ratio of polyisocyanate A to polyisocyanate B is 98 / 2 to 20 / 80.

[0025] (4) The pressure measurement sheet set according to any one of (1) to (3), wherein:

[0026] The resin has a polymethylene polyphenyl structure.

[0027] (5) The pressure measurement sheet set according to any one of (1) to (4), wherein:

[0028] The molecular weight of the coloring agent is 550 or more.

[0029] (6) The pressure measurement sheet set according to any one of (1) to (5), wherein:

[0030] The microcapsule satisfies the relationship of formula (1) described later.

[0031] (7) The pressure measurement sheet set according to any one of (1) to (6), wherein:

[0032] The number average wall thickness of the microcapsules is 0.2 μm or more.

[0033] (8) A pressure measuring sheet comprising:

[0034] The first layer comprises microcapsules containing a coloring agent; and

[0035] a second layer disposed on the first layer and comprising a developer,

[0036] The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane,

[0037] The glass transition temperature of the capsule wall is 150° C. or higher or the capsule wall does not show a glass transition temperature.

[0038] (9) The pressure measurement sheet according to (8), wherein:

[0039] The resin is formed using trifunctional or higher polyisocyanate A and polyisocyanate B.

[0040] The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule,

[0041] The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

[0042] (10) The pressure measurement sheet according to (9), wherein:

[0043] The mass ratio of polyisocyanate A to polyisocyanate B is 98 / 2 to 20 / 80.

[0044] (11) The pressure measurement sheet according to any one of (8) to (10), wherein:

[0045] The resin has a polymethylene polyphenyl structure.

[0046] (12) The pressure measurement sheet according to any one of (8) to (11), wherein:

[0047] The molecular weight of the coloring agent is 550 or more.

[0048] (13) The pressure measurement sheet according to any one of (8) to (12), wherein:

[0049] The microcapsule satisfies the relationship of formula (1) described later.

[0050] (14) The pressure measurement sheet according to any one of (8) to (13), wherein:

[0051] The number average wall thickness of the microcapsules is 0.2 μm or more.

[0052] (15) A dispersion liquid for forming a layer used in combination with a layer containing a color developer for pressure measurement, and comprising microcapsules containing a color developer, wherein:

[0053] The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane,

[0054] The glass transition temperature of the capsule wall is 150° C. or higher or the capsule wall does not show a glass transition temperature.

[0055] (16) The dispersion according to (15), wherein

[0056] The resin is formed using trifunctional or higher polyisocyanate A and polyisocyanate B.

[0057] The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule,

[0058] The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

[0059] (17) The dispersion according to (15) or (16), wherein

[0060] The molecular weight of the coloring agent is 550 or more.

[0061] (18) A dispersion liquid for forming a layer for pressure measurement, comprising microcapsules containing a color former and a developer, wherein:

[0062] The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane,

[0063] The glass transition temperature of the capsule wall is 150° C. or higher or the capsule wall does not show a glass transition temperature.

[0064] (19) The dispersion according to (18), wherein

[0065] The resin is formed using trifunctional or higher polyisocyanate A and polyisocyanate B.

[0066] The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule,

[0067] The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

[0068] (20) The dispersion according to (18) or (19), wherein

[0069] The molecular weight of the coloring agent is 550 or more.

[0070] Effects of the Invention

[0071] According to the present invention, it is possible to provide a pressure measurement sheet set and a pressure measurement sheet capable of measuring pressure distribution even when used in a high-temperature environment.

[0072] Furthermore, according to the present invention, a dispersion liquid can also be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 This is a cross-sectional view of one embodiment of a pressure measurement sheet set.

[0074] Figure 2 This is a diagram for explaining the usage of the pressure measurement sheet set.

[0075] Figure 3 This is a cross-sectional view of one embodiment of a pressure measurement sheet. DETAILED DESCRIPTION

[0076] Hereinafter, the present invention will be described in detail.

[0077] In addition, in this specification, the numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0078] Furthermore, in the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. Furthermore, in the numerical ranges recorded in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the value shown in the embodiments.

[0079] The various components described below may be used alone or in combination of two or more. For example, the polyisocyanate described below may be used alone or in combination of two or more.

[0080] The characteristic features of the pressure measurement sheet set and the pressure measurement sheet of the present invention include using microcapsules containing a coloring agent and having a capsule wall of the microcapsule having a glass transition temperature of 150° C. or higher or having no glass transition temperature.

[0081] As described above, the inventors of the present invention used a conventional pressure measurement sheet to measure pressure distribution in a high temperature environment. As a result, they first discovered that coloring also occurred outside the pressurized area, making it impossible to measure precise pressure distribution. Furthermore, as a result of studying the cause of this problem, they discovered that the coloring agent in the microcapsule leaked in a high temperature environment, and a coloring reaction occurred between the coloring agent and the developer, causing coloring to occur in an unpressurized area. In response to the above problem, the inventors of the present invention suppressed the leakage of the coloring agent by setting the glass transition temperature of the capsule wall of the microcapsule to 150°C or above or by not causing the capsule wall to show a glass transition temperature. As a result, they discovered that coloring occurred mainly in the pressurized area, and that pressure distribution could be measured in a high temperature environment.

[0082] <<First Embodiment>>

[0083] Figure 1 This is a cross-sectional view of one embodiment of a pressure measurement sheet set.

[0084] The pressure measurement sheet set 10 comprises a first sheet 16 and a second sheet 22 , wherein the first sheet 16 has a first support 12 and a first layer 14 including predetermined microcapsules 13 arranged on the first support 12 , and the second sheet 22 has a second support 18 and a second layer 20 including a color developer arranged on the second support 18 .

[0085] like Figure 2 As shown, when the pressure measurement sheet set 10 is used, the first sheet 16 and the second sheet 22 are stacked so that the first layer 14 in the first sheet 16 and the second layer 20 in the second sheet 22 face each other. By applying pressure from at least one of the first support 12 side of the first sheet 16 and the second support 18 side of the second sheet 22 in the obtained stacked body, the microcapsules 13 are ruptured in the pressurized area, and the coloring agent contained in the microcapsules 13 comes out of the microcapsules 13 and reacts with the coloring agent in the second layer 20. As a result, coloring is developed in the pressurized area.

[0086] As described later, the first sheet 16 may have only the first layer 14 and may not have the first support 12 . Furthermore, the second sheet 22 may have only the second layer 20 and may not have the second support 18 .

[0087] In addition, Figure 1 In the embodiment, the first support 12 and the first layer 14 are directly stacked, but the present invention is not limited to this embodiment. As described later, another layer (for example, an easy-adhesion layer) may be arranged between the first support 12 and the first layer 14. Figure 1In the embodiment, the second support 18 and the second layer 20 are directly stacked, but the present invention is not limited to this embodiment, and as described later, another layer (for example, an easy-adhesion layer) may be arranged between the second support 18 and the second layer 20.

[0088] Hereinafter, the structures of the first sheet 16 and the second sheet 22 constituting the pressure measurement sheet set 10 will be described in detail.

[0089] <1st sheet>

[0090] Figure 1 The first sheet 16 described in has a first support 12 and a first layer 14 including microcapsules containing a color developer.

[0091] Hereinafter, each component will be described in detail.

[0092] (First Support Body)

[0093] The first support is a member for supporting the first layer. In addition, when the first layer itself can be handled, the first sheet may not have the first support.

[0094] The first support may be in any shape of a sheet, a film, or a plate.

[0095] Examples of the first support include paper, plastic film, and synthetic paper.

[0096] Examples of the paper include premium paper, mid-grade paper, groundwood paper, neutral paper, acid paper, recycled paper, coated paper, machine-coated paper, coated paper, cast-coated paper, micro-coated paper, transparent paper, and recycled paper.

[0097] Examples of the plastic film include polyester films such as polyethylene terephthalate films, cellulose derivative films such as cellulose triacetate, polyolefin films such as polypropylene and polyethylene, and polystyrene films.

[0098] Examples of synthetic paper include synthetic paper (Yupo, etc.) obtained by biaxially stretching polypropylene or polyethylene terephthalate to form a plurality of micropores, synthetic paper made from synthetic fibers such as polyethylene, polypropylene, polyethylene terephthalate and polyamide, and synthetic paper in which these are layered on a portion, one side or both sides of the paper.

[0099] Among them, from the viewpoint of further increasing the color development density due to pressurization, a plastic film or a synthetic paper is preferred, and a plastic film is more preferred.

[0100] The thickness of the first support is not particularly limited, but is preferably 10 to 200 μm.

[0101] (1st floor)

[0102] The first layer contains microcapsules containing a colorant.

[0103] As described above, the characteristic features of the present invention include that the capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane, and the capsule wall has a glass transition temperature of 150° C. or higher or does not have a glass transition temperature.

[0104] Hereinafter, first, the materials constituting the microcapsules will be described in detail.

[0105] The microcapsule generally has a core and a capsule wall for containing a core material (inclusion (also referred to as inclusion component)) constituting the core.

[0106] In the present invention, the microcapsule contains a coloring agent as a core material (internal component). Since the coloring agent is contained in the microcapsule, the coloring agent can exist stably until the microcapsule is ruptured by applying pressure.

[0107] Microcapsules have a capsule wall containing a core material.

[0108] The capsule wall in the microcapsule contains at least one resin selected from the group consisting of polyurea, polyurethaneurea, and polyurethane (hereinafter, also simply referred to as “specific resin”).

[0109] The capsule wall of the microcapsule is preferably substantially composed of a resin (preferably a specific resin). Substantially composed of a resin means that the content of the resin relative to the total mass of the capsule wall is 90% by mass or more, preferably 100% by mass. That is, the capsule wall of the microcapsule is preferably composed of a resin.

[0110] In addition, the polyurethane is preferably a polymer having a plurality of urethane bonds, and is a reaction product of raw materials including a polyol and a polyisocyanate.

[0111] Furthermore, polyurea is preferably a polymer having a plurality of urea bonds, and is a reaction product formed from raw materials including polyamines and polyisocyanates. In addition, in the case where a part of polyisocyanate reacts with water to form polyamines, polyurea can also be synthesized using polyisocyanates instead of polyamines.

[0112] Furthermore, polyurethane urea is preferably a polymer having a urethane bond and a urea bond, and is a reaction product formed from raw materials including polyols, polyamines and polyisocyanates. In addition, when polyols and polyisocyanates are reacted, a part of the polyisocyanates reacts with water to form polyamines, and as a result, polyurethane urea can be obtained.

[0113] The polyisocyanate is a compound having two or more isocyanate groups, and examples thereof include aromatic polyisocyanates and aliphatic polyisocyanates. From the viewpoint of being able to introduce an aromatic ring group into the capsule wall of the microcapsule, aromatic polyisocyanates are preferred.

[0114] Examples of the aromatic polyisocyanate include aromatic diisocyanates, such as m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-toluene diisocyanate, 2,4-toluene diisocyanate, naphthalene-1,4-diisocyanate, diphenylmethane-4,4′-diisocyanate, 3,3′-dimethoxy-biphenyl diisocyanate, 3,3′-dimethyldiphenylmethane-4,4′-diisocyanate, xylylene-1,4-diisocyanate, xylylene-1,3-diisocyanate, 4-chloroxylylene-1,3-diisocyanate, 2-methylxylylene-1,3-diisocyanate, 4,4′-diphenylpropane diisocyanate, and 4,4′-diphenylhexafluoropropane diisocyanate.

[0115] Examples of the aliphatic polyisocyanate include aliphatic diisocyanates, such as trimethylene diisocyanate, hexamethylene diisocyanate, propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, cyclohexylene-1,2-diisocyanate, cyclohexylene-1,3-diisocyanate, cyclohexylene-1,4-diisocyanate, dicyclohexylmethane-4,4′-diisocyanate, 1,4-bis(isocyanatemethyl)cyclohexane, 1,3-bis(isocyanatemethyl)cyclohexane, isophorone diisocyanate, lysine diisocyanate, and hydrogenated xylylene diisocyanate.

[0116] In addition, although bifunctional aromatic polyisocyanates and aliphatic polyisocyanates are exemplified above, trifunctional or higher-functional polyisocyanates (for example, trifunctional triisocyanates and tetrafunctional tetraisocyanates) may also be mentioned as the polyisocyanates.

[0117] More specifically, examples of the polyisocyanate include a biuret form or an isocyanate form which is a trimer of the above-mentioned bifunctional polyisocyanate, an adduct (adduct) of a polyol such as trimethylolpropane and a bifunctional polyisocyanate, a formalin condensate of phenylisocyanate, a polyisocyanate having a polymerizable group such as methacryloyloxyethyl isocyanate, and lysine triisocyanate.

[0118] Polyisocyanate is described in “Handbook of Polyurethane Resins” (edited by Keiji Iwata, published by NIKKAN KOGYOSHIMBUN, Ltd. (1987)).

[0119] Among them, as one of the preferred aspects of the polyisocyanate, trifunctional or higher-functional polyisocyanates are preferred.

[0120] Examples of trifunctional or higher-functional polyisocyanates include trifunctional or higher-functional aromatic polyisocyanates and trifunctional or higher-functional aliphatic polyisocyanates.

[0121] As the trifunctional or higher polyisocyanate, an adduct (adduct) of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule (for example, a trifunctional or higher polyol, a polyamine, or a polythiol, etc.), that is, a trifunctional or higher polyisocyanate (an adduct-type trifunctional or higher polyisocyanate) and a trimer (biuret-type or isocyanurate-type) of an aromatic diisocyanate or an alicyclic diisocyanate are also preferred, and a trifunctional or higher polyisocyanate as the above-mentioned adduct (adduct) is more preferred.

[0122] The trifunctional or higher polyisocyanate as the above-mentioned adduct is preferably an adduct of an aromatic diisocyanate or an alicyclic diisocyanate with a polyol having three or more hydroxyl groups in one molecule, i.e. a trifunctional or higher polyisocyanate, and more preferably an adduct of an aromatic diisocyanate or an alicyclic diisocyanate with a polyol having three or more hydroxyl groups in one molecule, i.e. a trifunctional polyisocyanate.

[0123] As the adduct, an adduct obtained using an aromatic diisocyanate is preferably used from the viewpoint that pressure distribution in a high temperature environment can be measured more satisfactorily (hereinafter also referred to as “the viewpoint that the effect of the present invention is more excellent”).

[0124] As the polyol, for example, a trifunctional or higher-functional low-molecular polyol described below is preferred, and trimethylolpropane is more preferred.

[0125] Examples of the addition-type trifunctional or higher-functional polyisocyanates include TAKENATE (registered trademark) D-102, D-103, D-103H, D-103M2, P49-75S, D-110N, D-120N, D-140N, and D-160N (manufactured by Mitsui Chemicals, Inc.), DESMODULE (registered trademark) L75 and UL57SP (manufactured by Sumika Bayer Urethane Co., Ltd.), CORONATE (registered trademark) HL, HX, and L (manufactured by Nippon Polyurethane Industry Co., Ltd.), P301-75E (manufactured by Asahi Kasei Corporation), and BURNOCK (registered trademark) D-750 (manufactured by DIC Corporation).

[0126] Among them, as the addition type trifunctional or higher functional polyisocyanate, for example, TAKENATE (registered trademark) D-110N, D-120N, D-140N, D-160N (manufactured by Mitsui Chemicals, Inc.) or BURNOCK (registered trademark) D-750 manufactured by DIC CORPORATION is preferred.

[0127] Examples of the isocyanurate type trifunctional or higher-functional polyisocyanates include TAKENATE (registered trademark) D-127N, D-170N, D-170HN, D-172N, D-177N, and D-204 (manufactured by Mitsui Chemicals, Inc.), SUMIDURN 3300, DESMODULE (registered trademark) N3600, N3900, and Z4470BA (manufactured by Sumika Bayer Urethane Co., Ltd.), CORONATE (registered trademark) HX and HK (manufactured by Nippon Polyurethane Industry Co., Ltd.), and Duranate (registered trademark) TPA-100, TKA-100, TSA-100, TSS-100, TLA-100, and TSE-100 (manufactured by Asahi Kasei Corporation).

[0128] Examples of biuret-type trifunctional or higher-functional polyisocyanates include TAKENATE (registered trademark) D-165N and NP1100 (manufactured by Mitsui Chemicals, Inc.), DESMODULE (registered trademark) N3200 (manufactured by Sumika Bayer Urethane Co., Ltd.), and Duranate (registered trademark) 24A-100 (manufactured by Asahi Kasei Corporation).

[0129] Furthermore, as the polyisocyanate, polymethylene polyphenyl polyisocyanate is also preferred.

[0130] As the polymethylene polyphenyl polyisocyanate, a compound represented by the formula (X) is preferred.

[0131] [Chemical formula 1]

[0132]

[0133] In formula (X), n represents the number of repeating units. The number of repeating units represents an integer of 1 or more, and n is preferably an integer of 1 to 10, more preferably an integer of 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0134] Examples of the polyisocyanate containing polymethylene polyphenyl polyisocyanate include MILLIONATE MR-100, MILLIONATE MR-200, MILLIONATE MR-400 (manufactured by TOSOH Corporation), WANNATE PM-200, WANNATE PM-400 (manufactured by Wanhua Chemical (Japan) Co., Ltd.), COSMONATE M-50, COSMONATE M-100, COSMONATEM-200, COSMONATE M-300 (manufactured by Mitsui Chemicals, Inc.), and BORONATE M-595 (manufactured by Dow Chemical Japan).

[0135] Polyol refers to a compound having two or more hydroxyl groups, and examples thereof include low molecular weight polyols (e.g., aliphatic polyols, aromatic polyols), polyvinyl alcohol, polyether polyols, polyester polyols, polylactone polyols, castor oil polyols, polyolefin polyols and hydroxyl-containing amine compounds.

[0136] The low molecular weight polyol refers to a polyol having a molecular weight of 400 or less, and examples thereof include bifunctional low molecular weight polyols such as ethylene glycol, diethylene glycol and propylene glycol, and trifunctional or higher low molecular weight polyols such as glycerol, trimethylolpropane, hexanetriol, pentaerythritol and sorbitol.

[0137] In addition, examples of hydroxyl-containing amine compounds include amino alcohols, such as alkoxylated derivatives of amino compounds. Examples of amino alcohols include N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine and N,N,N',N'-tetrakis[2-hydroxyethyl]ethylenediamine, which are propylene oxide or ethylene oxide adducts of amino compounds such as ethylenediamine.

[0138] Polyamine refers to a compound having two or more amino groups (primary or secondary amino groups), and examples thereof include aliphatic polyamines such as diethylenetriamine, triethylenetetramine, 1,3-propylenediamine and hexamethylenediamine; epoxy adducts of aliphatic polyamines; alicyclic polyamines such as piperazine; and heterocyclic diamines such as 3,9-bis-aminopropyl-2,4,8,10-tetraoxospiro-(5,5)undecane.

[0139] Among them, the resin contained in the capsule wall is preferably formed using an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule, that is, a trifunctional or higher-functional polyisocyanate A (hereinafter also referred to as "polyisocyanate A") and a polyisocyanate B selected from the group consisting of an aromatic diisocyanate and a polymethylene polyphenyl polyisocyanate (hereinafter also referred to as "polyisocyanate B").

[0140] That is, the capsule wall is preferably a capsule wall composed of the above-mentioned resin (at least one resin selected from the group consisting of polyurea, polyurethane urea, and polyurethane) formed using the above-mentioned polyisocyanate A and polyisocyanate B.

[0141] By using the above-mentioned polyisocyanate A and polyisocyanate B, the effect of the present invention is more excellent. In addition, the temperature dependence of color development is also small. In addition, the temperature dependence of color development refers to a characteristic that indicates the difference in the degree of color development based on the temperature when pressure is applied to the pressure measuring sheet set (or the pressure measuring sheet described later). More specifically, when the heating temperature is changed within the range of high temperature conditions (above 180°C) using the pressure measuring sheet set (or the pressure measuring sheet described later) and the degree of color development is observed, when the difference in the degree of color development is large, it can be said that the temperature dependence of color development is large.

[0142] In addition, as polyisocyanate B, aromatic diisocyanate may be used alone, polymethylene polyphenyl polyisocyanate may be used alone, or both may be used in mixture. Among them, as polyisocyanate B, a mixture of aromatic diisocyanate and polymethylene polyphenyl polyisocyanate is preferred.

[0143] In the mixture, the mass ratio of polymethylene polyphenyl polyisocyanate to aromatic diisocyanate (mass of polymethylene polyphenyl polyisocyanate / mass of aromatic diisocyanate) is not particularly limited, but is preferably 0.1 to 10, more preferably 0.5 to 2, and further preferably 0.75 to 1.5.

[0144] The viscosity of the polyisocyanate B is not particularly limited, but is preferably 100 to 1000 mPa·s from the viewpoint of achieving more excellent effects of the present invention.

[0145] In addition, the above-mentioned viscosity is the viscosity at 25°C.

[0146] When polyisocyanate A and polyisocyanate B are used simultaneously, the mass ratio of polyisocyanate A to polyisocyanate B (mass of polyisocyanate A / mass of polyisocyanate B) is not particularly limited, but is preferably 98 / 2 to 20 / 80, more preferably 80 / 20 to 20 / 80, and further preferably 80 / 20 to 45 / 55.

[0147] When the mass ratio is within the above range, the effect of the present invention is more excellent and the temperature dependence of color development is also small.

[0148] Furthermore, from the viewpoint of achieving more excellent effects of the present invention, it is preferred that the resin has a polymethylene polyphenyl structure. That is, it is preferred that the resin has a polymethylene polyphenyl structure as a partial structure.

[0149] The polymethylene polyphenyl structure is derived from the structure of polymethylene polyphenyl polyisocyanate, and more specifically, is a structure represented by the following formula.

[0150] [Chemical formula 2]

[0151]

[0152] In the formula, n represents the number of repeating units. The number of repeating units represents an integer of 1 or more, and n is preferably an integer of 1 to 10, and more preferably an integer of 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0153] The glass transition temperature of the capsule wall of the microcapsule is 150° C. or higher, or the capsule wall does not show a glass transition temperature. That is, the glass transition temperature of the material constituting the capsule wall of the microcapsule is 150° C. or higher, or the material constituting the capsule wall of the microcapsule does not show a glass transition temperature.

[0154] In addition, when the capsule wall of the microcapsule shows a glass transition temperature, from the viewpoint of more excellent effects of the present invention, the temperature is preferably 160° C. or higher, more preferably 180° C. or higher, and further preferably 200° C. or higher. When the capsule wall of the microcapsule shows a glass transition temperature, the upper limit of the temperature is not particularly limited, but is usually below the thermal decomposition temperature of the capsule wall of the microcapsule, and is usually 250° C. or lower.

[0155] Among them, from the viewpoint of achieving more excellent effects of the present invention, it is preferred that the capsule wall of the microcapsule does not exhibit a glass transition temperature.

[0156] In addition, the fact that the capsule wall of the microcapsule does not show a glass transition temperature means that the capsule wall of the microcapsule (the material constituting the capsule wall of the microcapsule) does not show a glass transition temperature until the temperature from 25°C to the temperature (thermal decomposition temperature - 5°C) at which 5°C is subtracted from the thermal decomposition temperature of the capsule wall described later. That is, the glass transition temperature does not show in the range from "25°C" to "(thermal decomposition temperature (°C) - 5°C)".

[0157] There is no particular limitation on the method for making the glass transition temperature of the capsule wall of the microcapsule be above 150°C or the capsule wall not exhibiting a glass transition temperature, and it can be adjusted by appropriately selecting the raw materials used in the manufacture of the microcapsules. For example, polyurea has the property of exhibiting a high glass transition temperature, so a method of forming the capsule wall with polyurea can be cited. In addition, a method of increasing the crosslinking density in the material constituting the capsule wall can also be cited. In addition, a method of introducing an aromatic ring group (for example, a benzene ring group) into the material constituting the capsule wall can also be cited.

[0158] The glass transition temperature of the capsule wall is measured as follows.

[0159] Prepare 50 sheets of the first layer (microcapsule layer) of 1 cm in length and 1 cm in width, immerse all of them in 10 ml of water and let stand for 24 hours to obtain an aqueous dispersion of microcapsules. Alternatively, when the first sheet includes the first support, 50 sheets of the first sheet of 1 cm in length and 1 cm in width may be prepared and immersed.

[0160] The obtained aqueous dispersion of microcapsules was centrifuged at 15000 rpm for 30 minutes to separate microcapsules. Ethyl acetate was added to the separated microcapsules and further stirred at 25°C for 24 hours. Thereafter, the obtained solution was filtered and the obtained residue was vacuum dried at 60°C for 48 hours to obtain microcapsules containing nothing inside (hereinafter also referred to as "measurement material"). That is, the capsule wall material of the microcapsule to be measured for the glass transition temperature was obtained.

[0161] Next, the thermal decomposition temperature of the obtained measurement material was measured using a thermogravimetric differential thermal analyzer TG-DTA (device name: DTG-60, Shimadzu Corporation). In addition, the thermal decomposition temperature refers to the temperature at which the measurement material is heated from room temperature at a constant heating rate (10°C / min) and the mass of the measurement material before heating is reduced by 5% by mass as the thermal decomposition temperature (°C) in a thermogravimetric analysis (TGA) in an atmospheric environment.

[0162] Next, the glass transition temperature of the measured material was measured using a differential scanning calorimeter DSC (device name: DSC-60a Plus, Shimadzu Corporation) and a closed pan at a heating rate of 5°C / min in the range of 25°C to (thermal decomposition temperature (°C) - 5°C). As the glass transition temperature of the capsule wall of the microcapsule, the value at the time of the second week of heating was used.

[0163] The particle size of the microcapsule is not particularly limited, but is preferably 1 to 80 μm, more preferably 5 to 70 μm, and even more preferably 10 to 50 μm in terms of volume-based median diameter (D50).

[0164] The volume-based median diameter of the microcapsules can be controlled by adjusting the production conditions of the microcapsules and the like.

[0165] The volume-based median diameter of microcapsules refers to the diameter at which the volume of the particles on the larger diameter side and the larger diameter side are equal when the entire microcapsule is divided into two using the particle diameter at which the cumulative volume is 50% as the threshold value. That is, the median diameter corresponds to the so-called D50.

[0166] The value is calculated by photographing the surface of the first layer of the first sheet having the first layer containing microcapsules at 1000 times magnification using an optical microscope, and measuring the sizes of all microcapsules within a range of 500 μm×500 μm.

[0167] The number average wall thickness of the microcapsules (the number average wall thickness of the capsule wall of the microcapsules) is not particularly limited, and is preferably 0.01 to 2 μm, and more preferably 0.05 to 1 μm. Among them, from the viewpoint of the better effect of the present invention, as the lower limit, it is preferably 0.2 μm or more, and more preferably 0.3 μm or more. And, from the viewpoint of the better effect of the present invention, it is further preferably 0.2 to 2 μm, and particularly preferably 0.3 to 1 μm.

[0168] In addition, the wall thickness of the microcapsule refers to the thickness (μm) of the capsule wall of the capsule particles forming the microcapsule, and the number average wall thickness refers to the average value of the thickness (μm) of each capsule wall of 5 microcapsules obtained by scanning electron microscopy (SEM). More specifically, a cross-sectional slice of the first sheet having the first layer containing microcapsules is prepared, and the cross section is observed at 200 times by SEM, and on the basis of selecting any 5 microcapsules having a particle size in the range of (the value of the median particle size based on the volume of the microcapsule)×0.9 to (the value of the median particle size based on the volume of the microcapsule)×1.1, the cross-section of each selected microcapsule is observed at 15000 times, and the thickness of the capsule wall is obtained and the average value is calculated.

[0169] The ratio (δ / Dm) of the number average wall thickness δ of the microcapsules to the volume-based median diameter (Dm) of the microcapsules is not particularly limited, but is often 0.005 or more. From the viewpoint of achieving more excellent effects of the present invention, it is preferred that the relationship of formula (1) is satisfied.

[0170] Formula (1) δ / Dm>0.010

[0171] That is, the above ratio (δ / Dm) is preferably greater than 0.010. Furthermore, the above ratio (δ / Dm) is preferably 0.015 or more. The upper limit is not particularly limited, but is preferably 0.100 or less, and more preferably 0.050 or less.

[0172] When the microcapsules satisfy the relationship of the above formula (1), the balance between the size of the capsule and the thickness of the capsule wall is good, and there is less concern about leakage of the contents of the microcapsules in a high temperature environment.

[0173] The coloring agent is contained in the microcapsules.

[0174] The coloring agent refers to a compound that develops color from a colorless state by contact with a color developer described later. As the coloring agent, an electron donating dye precursor (precursor of a color-developing dye) is preferred. That is, as the coloring agent, an electron donating colorless dye is preferred.

[0175] The coloring agent can be a coloring agent known in the application of pressure-sensitive carbon paper or thermal recording paper. Examples of the coloring agent include triphenylmethanephthalide compounds, fluoran compounds, phenothiazine compounds, indolylphthalide compounds, azaindolylphthalide compounds, colorless golden amine compounds, rhodamine lactam compounds, triphenylmethane compounds, diphenylmethane compounds, triazene compounds, spiropyran compounds, and fluorene compounds.

[0176] For details of the above compounds, reference can be made to the description of Japanese Patent Application Laid-Open No. 5-257272.

[0177] The coloring agent may be used alone or in combination of two or more.

[0178] The molecular weight of the coloring agent is not particularly limited, and is generally 300 or more. Among them, from the viewpoint of more excellent effects of the present invention, it is preferably 420 or more, more preferably 550 or more, and further preferably 610 or more. The upper limit is not particularly limited, but is preferably 1000 or less. By using a coloring agent with a large molecular weight, unnecessary outflow of the coloring agent at high temperature can be suppressed.

[0179] When two or more coloring agents are used in combination, the coloring agent having a molecular weight of 550 or more is preferably 50 to 100% by mass, more preferably 75 to 100% by mass, and even more preferably 90 to 100% by mass relative to all the coloring agents. In addition, from the viewpoint of achieving a more excellent effect of the present invention, the coloring agent having a molecular weight of 610 or more is preferably 50 to 100% by mass, more preferably 75 to 100% by mass, and even more preferably 90 to 100% by mass relative to all the coloring agents.

[0180] The molar absorption coefficient (ε) of the pigment (corresponding to the pigment that develops color) (hereinafter also referred to as "specific pigment") obtained by contacting the color former with the color developer described later is not particularly limited, but is preferably 10,000 mol / L. -1 cm -1 L or more, more preferably 15000 mol-1 cm -1 ·L or more, more preferably 25000 mol -1 cm -1 The upper limit of the molar absorption coefficient (ε) is not particularly limited, but is usually 50,000 mol -1 cm -1 ·L or less.

[0181] Preferred examples of the coloring agent include 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide (ε=61000), 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-n-octyl-2-methylindol-3-yl)phthalide (ε=40000), 3-[2,2-bis(1-ethyl-2-methylindol-3-yl)vinyl]-3-(4-diethylaminophenyl)-phthalide (ε=40000), 9-[ethyl(3-methylbutyl)amino]spiro[12H-benzo[a]xanthene-12,1'(3'H)isobenzofuran]-3'-one (ε=34000), 2-anilino-6- Dibutylamino-3-methylfluoran (ε=22000), 6-diethylamino-3-methyl-2-(2,6-thiocyano)-fluoran (ε=19000), 2-(2-chloroanilino)-6-dibutylaminofluoran (ε=21000), 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophthalide (ε=16000), 2-anilino-6-diethylamino-3-methylfluoran (ε=16000), 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindol-1,9'-xanthene]-3-one, 6'-(diethylamino)-1',3'-dimethylfluoran and 3,3-bis(2-methyl-1-octyl-3-indolyl)phthalide, etc.

[0182] In addition, the above ε represents the molar absorption coefficient of each compound after color development.

[0183] The molar absorption coefficient (ε) can be calculated from the absorbance when the specific pigment is dissolved in 95 mass % acetic acid aqueous solution. Specifically, in a 95 mass % acetic acid aqueous solution of a specific pigment whose concentration is adjusted in a manner such that the absorbance is below 1.0, the length of the measurement cell is set to Acm, the concentration of the specific pigment is set to Bmol / L, and the absorbance is set to C, and can be calculated by the following formula.

[0184] Molar absorptivity (ε) = C / (A×B)

[0185] [Other ingredients]

[0186] The microcapsules may contain other ingredients besides the above-mentioned coloring agents.

[0187] For example, the microcapsules preferably contain a solvent.

[0188] The solvent is not particularly limited, and examples thereof include alkylnaphthalene compounds such as diisopropylnaphthalene, diarylalkane compounds such as 1-phenyl-1-xylylethane, alkylbiphenyl compounds such as isopropylbiphenyl, triarylmethane compounds, alkylbenzene compounds, benzylnaphthalene compounds, diarylalkylene compounds and arylindanes; aromatic hydrocarbons such as dibutyl phthalate and isoparaffins; natural animal and plant oils such as soybean oil, corn oil, cottonseed oil, rapeseed oil, olive oil, coconut oil, castor oil and fish oil, and high-boiling-point fractions of natural products such as mineral oils.

[0189] The solvent may be used alone or in combination of two or more.

[0190] When the solvent is contained in the microcapsules, the mass ratio of the solvent to the color former (mass of the solvent / mass of the color former) is preferably in the range of 98 / 2 to 30 / 70, more preferably in the range of 97 / 3 to 40 / 60, from the viewpoint of color development.

[0191] The microcapsule may contain, in addition to the above-mentioned components, one or more additives such as ultraviolet absorbers, light stabilizers, antioxidants, paraffin waxes, and deodorants as necessary.

[0192] [Method for producing microcapsules]

[0193] The method for producing the microcapsules containing the coloring agent is not particularly limited, and examples thereof include known methods such as interfacial polymerization, internal polymerization, phase separation, external polymerization, and coacervation. Among them, interfacial polymerization is preferred.

[0194] As the interfacial polymerization method, preferably, there is an interfacial polymerization method which includes a step of dispersing an oil phase containing a coloring agent and a capsule wall material (for example, a raw material containing at least one selected from the group consisting of polyisocyanate, polyol and polyamine. In addition, when polyamine is produced in the reaction system by reacting polyisocyanate with water, polyol and polyamine may not be used.) in an aqueous phase containing an emulsifier to prepare an emulsion (emulsification step) and a step of polymerizing the capsule wall material at the interface between the oil phase and the aqueous phase to form a capsule wall and form microcapsules containing the coloring agent (encapsulation step).

[0195] The mass ratio of the total amount of polyol and polyamine to the amount of polyisocyanate in the raw materials (total amount of polyol and polyamine / amount of polyisocyanate) is not particularly limited, but is preferably 0.1 / 99.9 to 30 / 70, and more preferably 1 / 99 to 25 / 75.

[0196] Moreover, as mentioned above, as a polyisocyanate, you may use together the said polyisocyanate A and polyisocyanate B. When using both together, the preferable range of the mixing ratio of both is as mentioned above.

[0197] In addition, the type of the emulsifier used in the emulsification step is not particularly limited, and examples thereof include a dispersant and a surfactant.

[0198] As a dispersant, polyvinyl alcohol is mentioned, for example.

[0199] The first layer comprises the above-mentioned microcapsules.

[0200] The content of the microcapsules in the first layer is not particularly limited, but is preferably 50 to 90% by mass, more preferably 55 to 85% by mass, and even more preferably 55 to 80% by mass based on the total mass of the first layer from the viewpoint of achieving more excellent effects of the present invention.

[0201] The content of the coloring agent in the first layer is not particularly limited, but is preferably 0.1 to 10 g / m 2 , more preferably 0.1 to 4 g / m 2 .

[0202] The first layer may contain other components in addition to the above-mentioned microcapsules.

[0203] Examples of other components include polymer binders, inorganic fillers (eg, colloidal silica), fluorescent whitening agents, defoaming agents, penetrants, ultraviolet absorbers, surfactants, and preservatives.

[0204] As the polymer binder, for example, synthetic polymers or natural polymers such as styrene-butadiene copolymer, polyvinyl acetate, polyacrylate, polyvinyl alcohol, polyacrylic acid, maleic anhydride-styrene copolymer, starch, casein, gum arabic, gelatin, carboxymethyl cellulose or its salt and methyl cellulose can be mentioned. One type of the polymer binder can be used alone, or two or more types can be used simultaneously.

[0205] The content of the polymer binder is not particularly limited, but is preferably 0 to 50% by mass relative to the total mass of the first layer from the viewpoint of achieving a more excellent effect of the present invention. From the viewpoint of being suitable for a low pressure region of 10 MPa or less, it is preferably 0.1 to 20% by mass, and more preferably 0.2 to 10% by mass.

[0206] Examples of the surfactant include anionic surfactants, nonionic surfactants, and cationic surfactants. From the viewpoint of maintaining the dispersibility of the microcapsules, anionic surfactants and nonionic surfactants are preferred.

[0207] Examples of the surfactant include fluorine-based surfactants, silicone-based surfactants, and hydrocarbon-based surfactants. From the viewpoint of maintaining coating properties and dispersibility of microcapsules, hydrocarbon-based surfactants are preferred.

[0208] The content of the surfactant is not particularly limited, but is preferably 0.01 to 10% by mass, more preferably 0.1 to 5% by mass, based on the total mass of the first layer from the viewpoint of achieving more excellent effects of the present invention.

[0209] Preferably, the inorganic filler is introduced after the first sheet and the second sheet are stacked and heated and pressure-measured to facilitate separation of the two. From the viewpoint of facilitating separation of the first sheet and the second sheet, the inorganic filler is preferably silica particles or alumina particles.

[0210] The median particle size of the inorganic filler is preferably 0.001 to 1 μm, more preferably 0.005 to 0.1 μm, and even more preferably 0.005 to 0.05 μm.

[0211] The content of the inorganic filler is preferably 1 to 50% by mass, more preferably 3 to 30% by mass, and even more preferably 5 to 20% by mass, based on the total mass of the first layer.

[0212] The thickness of the first layer is not particularly limited, but from the perspective of being suitable for low-pressure areas below 20 MPa, it is preferably 0.01 to 5 μm, and more preferably 0.02 to 3 μm. The thickness of the first layer refers to the thickness of the microcapsules excluding the microcapsules exposed from the surface of the layer when the diameter of the microcapsules is greater than the layer thickness. If the thickness of the first layer is within the above range, when the first layer-forming composition containing the microcapsules is applied and then dried, the aggregation of the microcapsules can be suppressed, and the capsules can be adjusted to rupture at the desired pressure. From the perspective of being suitable for low-pressure areas below 20 MPa, the thickness of the first layer is preferably 50% or less, and more preferably 25% or less, relative to the median particle size of the microcapsules. The thinner the thickness of the first layer is relative to the microcapsules, the easier it is to rupture, so it can be adjusted according to the measured pressure band.

[0213] And, the mass per unit area of ​​the first layer (g / m 2 ) is not particularly limited, but is preferably 0.5 to 20 g / m 2 .

[0214] [Method for forming the first layer]

[0215] The method for forming the first layer is not particularly limited, and a known method may be used.

[0216] For example, there can be mentioned a method in which a first layer-forming composition containing microcapsules is applied onto a first support and then dried as necessary.

[0217] The first layer forming composition preferably contains at least microcapsules and a solvent. Alternatively, a microcapsule dispersion obtained by the above-mentioned interfacial polymerization method may be used as the first layer forming composition.

[0218] The first layer forming composition may contain other components that can be contained in the above-mentioned first layer.

[0219] The method for coating the first layer forming composition is not particularly limited. Examples of the coater used for coating include an air knife coater, a rod coater, a rod coater, a curtain coater, a gravure coater, an extrusion coater, a die coater, a slide bead coater, and a knife coater.

[0220] After the first layer-forming composition is applied onto the first support, the coating film may be dried as necessary. Examples of the drying treatment include heating treatment.

[0221] In addition, the method of forming the first layer on the first support is described above, but it is not limited to the above method. For example, the first sheet consisting of the first layer can be formed by forming the first layer on a temporary support and then peeling the temporary support.

[0222] The temporary support is not particularly limited as long as it is a releasable support.

[0223] (Other parts)

[0224] The first sheet may have other members in addition to the above-mentioned first support and first layer.

[0225] For example, the first sheet may include an easily adhesive layer between the first support and the first layer for improving the adhesion between the two.

[0226] The easy-adhesion layer may be a layer containing a urethane polymer, blocked isocyanate, or the like.

[0227] The thickness of the easy-adhesion layer is not particularly limited, but is preferably 0.005 to 0.2 μm, and more preferably 0.01 to 0.1 μm.

[0228] <Second Sheet>

[0229] Figure 1 The second sheet 22 described in has a second support 18 and a second layer 20 including a color developer disposed on the second support 18 .

[0230] Hereinafter, each component will be described in detail.

[0231] (Second Support Body)

[0232] The second support is a member for supporting the second layer. In addition, when the second layer itself can be processed, the second sheet may not have the second support.

[0233] The configuration of the second support is the same as that of the first support described above, and therefore description thereof will be omitted.

[0234] (Layer 2)

[0235] The second layer is a layer containing a color developer.

[0236] The color developer is a compound that has no color-developing function itself but has the property of causing the color-developing agent to develop color when in contact with the color-developing agent. The color developer is preferably an electron-accepting compound.

[0237] Examples of the color developer include inorganic compounds and organic compounds, of which inorganic compounds that are difficult to decompose at high temperatures are preferred from the viewpoint of achieving more excellent effects of the present invention.

[0238] Examples of the inorganic compound include clay substances such as acidic clay, activated clay, attapulgite, zeolite, bentonite, and kaolin.

[0239] Examples of the organic compound include metal salts of aromatic carboxylic acids, metal salts of phenol formaldehyde resins and carboxylated terpene phenol resins, and the like.

[0240] Among them, the color developer is preferably acidic clay, activated clay, zeolite, kaolin, metal salts of aromatic carboxylic acids or metal salts of carboxylated terpene-phenol resins, and more preferably acidic clay, activated clay, kaolin or metal salts of aromatic carboxylic acids.

[0241] Preferred metal salts of aromatic carboxylic acids are 3,5-di-t-butylsalicylic acid, 3,5-di-t-octylsalicylic acid, 3,5-di-t-nonylsalicylic acid, 3,5-di-t-dodecanoic acid, 3-methyl-5-t-dodecanoic acid, 3-t-dodecanoic acid, 5-t-dodecanoic acid, 5-cyclohexylsalicylic acid, 3,5-bis(α,α-dimethylbenzyl)salicylic acid, 3-methyl-5-(α-methylbenzyl)salicylic acid, 3-(α,α-dimethylbenzyl)salicylic acid, salicylic acid, 3-(α,α-dimethylbenzyl)-6-methylsalicylic acid, 3-(α-methylbenzyl)-5-(α,α-dimethylbenzyl)salicylic acid, 3-(α,α-dimethylbenzyl)-6-ethylsalicylic acid, 3-phenyl-5-(α,α-dimethylbenzyl)salicylic acid, carboxyl-modified terpene-phenol resin, salicylic acid resin obtained by reacting 3,5-bis(α-methylbenzyl)salicylic acid with benzyl chloride, etc., zinc salts, nickel salts, aluminum salts or calcium salts, etc.

[0242] The content of the color developer in the second layer is not particularly limited, but is preferably 20 to 95% by mass, more preferably 30 to 90% by mass, based on the total mass of the second layer from the viewpoint of achieving more excellent effects of the present invention.

[0243] The color developer may be used alone or in combination of two or more.

[0244] The content of the color developer in the second layer is not particularly limited, but is preferably 0.1 to 30 g / m 2 When the developer is an inorganic compound, the content of the developer is preferably 3 to 20 g / m 2 , more preferably 5 to 15 g / m 2 When the developer is an organic compound, the content of the developer is preferably 0.1 to 5 g / m 2 , more preferably 0.2 to 3 g / m 2 .

[0245] The second layer may contain other components in addition to the above-mentioned developer.

[0246] Examples of other components include polymer binders, pigments, fluorescent whitening agents, defoaming agents, penetrants, ultraviolet absorbers, surfactants, and preservatives.

[0247] Examples of the polymer binder include synthetic polymers or natural polymers such as styrene-butadiene copolymers, polyvinyl acetate, polyacrylate, polyvinyl alcohol, polyacrylic acid, maleic anhydride-styrene copolymers, starch, casein, gum arabic, gelatin, carboxymethyl cellulose, and methyl cellulose.

[0248] Examples of the pigment include heavy calcium carbonate, light calcium carbonate, talc, and titanium dioxide.

[0249] The thickness of the second layer is not particularly limited, but is preferably 1 to 50 μm, more preferably 2 to 30 μm, from the viewpoint of achieving more excellent effects of the present invention.

[0250] And, the mass per unit area of ​​the second layer (g / m 2 ) is not particularly limited, but is preferably 0.5 to 30 g / m 2 .

[0251] [Method for forming the second layer]

[0252] The method for forming the second layer is not particularly limited, and a known method may be used.

[0253] For example, there can be mentioned a method in which a second layer-forming composition containing a color developer is applied onto the second support and then subjected to a drying treatment as necessary.

[0254] The second layer forming composition may be a dispersion obtained by dispersing the developer in water or the like. When the developer is an inorganic compound, the developer dispersion may be prepared by mechanically dispersing the inorganic compound in water. When the developer is an organic compound, the developer dispersion may be prepared by mechanically dispersing the organic compound in water or dissolving it in an organic solvent.

[0255] The second layer forming composition may contain other components that can be contained in the above-mentioned second layer.

[0256] The method of applying the second layer forming composition is not particularly limited, and an example includes a method using the same coater used when applying the above-mentioned first layer forming composition.

[0257] After the second layer-forming composition is applied onto the second support, the coating film may be dried as necessary. Examples of the drying treatment include heating treatment.

[0258] In addition, the method of forming the second layer on the second support is described above, but it is not limited to the above method. For example, the second layer may be formed on a temporary support and then the temporary support may be peeled off to form a second sheet composed of the second layer.

[0259] The temporary support is not particularly limited as long as it is a releasable support.

[0260] (Other parts)

[0261] The second sheet may have other members in addition to the above-mentioned second support and second layer.

[0262] For example, the second sheet may include an easily adhesive layer between the second support and the second layer for improving the adhesion between the two.

[0263] The aspect of the easy-adhesion layer may be the aspect of the easy-adhesion layer which the above-mentioned 1st sheet|seat may have.

[0264] As described above, the first sheet and the second sheet are stacked so that the first layer of the first sheet and the second layer of the second sheet face each other to obtain a stacked body, and the stacked body is pressurized for use.

[0265] In addition, when the pressure measurement sheet set is small, the color density difference obtained by the following color density difference measurement 1 is preferably 0.25 or less, more preferably 0.20 or less, and further preferably 0.10 or less. The lower limit is not particularly limited, but is usually 0.01 or more.

[0266] Color density difference measurement 1: The first sheet and the second sheet are stacked in a manner such that the first layer of the first sheet and the second layer of the second sheet are opposed to each other to obtain a stacked body, and the difference in optical density of the stacked body before and after heating the stacked body at 220°C for 2 minutes in a non-pressurized state is taken as the color density difference.

[0267] In the color density difference measurement 1, as described above, the laminate is subjected to a heat treatment under the prescribed conditions. In addition, the above measurement is performed in a non-pressurized state. The non-pressurized state refers to a state in which no pressure is applied to the laminate (a state in which no pressure is applied). Furthermore, when heating at 220°C, the laminate at room temperature (about 23°C) is heated to the above-described prescribed temperature.

[0268] When the value of the color development density difference measurement 1 is within the above range, it is preferred from the viewpoint of at least one of obtaining a more excellent effect of the present invention and reducing the temperature dependency of color development.

[0269] As a method for measuring the optical density, X-rite eXact (manufactured by X-Rite) was used to measure without a filter and at a concentration state of ISO state T, D50 / 2°. As the optical density, the value of OD (optical density) was adopted. In addition, when measuring, OD was measured in each mode of CMYK (C: Cyan, M: Magenta, Y: Yellow, K: Black), and the optical density showing the highest OD was selected.

[0270] <<Second Embodiment>>

[0271] Figure 3 This is a cross-sectional view of one embodiment of a pressure measurement sheet.

[0272] The pressure measurement sheet 30 includes a support 32 , a second layer 20 containing a color developer, and a first layer 14 containing predetermined microcapsules 13 in this order.

[0273] When the pressure measurement sheet 30 is used, by applying pressure from at least one of the support body 32 side and the first layer 14 side, the microcapsules 13 are ruptured in the pressurized area, and the coloring agent contained in the microcapsules 13 comes out of the microcapsules 13 and reacts with the coloring agent in the second layer 20. As a result, color is developed in the pressurized area.

[0274] As will be described later, the pressure measurement sheet 30 only needs to include the first layer 14 and the second layer 20 , and may not include the support 32 .

[0275] In addition, Figure 3In the embodiment, the support 32 and the second layer 20 are directly stacked, but the present invention is not limited to this embodiment, and as described later, another layer (for example, an easy-adhesion layer) may be disposed between the support 32 and the second layer 20.

[0276] And, in Figure 3 , a pressure measuring sheet 30 including a support 32, a second layer 20, and a first layer 14 in this order is disclosed. However, the present invention is not limited to this embodiment, and a pressure measuring sheet including a support 32, a first layer 14, and a second layer 20 in this order may also be used.

[0277] The first layer 14 and the second layer 20 in the pressure measurement sheet 30 are the same as the first layer 14 and the second layer 20 described in the first embodiment, and thus description thereof is omitted.

[0278] Hereinafter, the support body 32 will be mainly described in detail.

[0279] (Supporting body)

[0280] The support is a member for supporting the first layer and the second layer. In addition, when the laminate of the first layer and the second layer can be handled by itself, the pressure measurement sheet may not have a support.

[0281] A preferred embodiment of the support body is the same as the preferred embodiment of the first support body described above, and therefore the description thereof is omitted.

[0282] (Method for manufacturing pressure measuring sheet)

[0283] The method for producing the pressure measurement sheet is not particularly limited, and a known method may be used.

[0284] For example, the following method can be mentioned: after forming the second layer on the support, a composition for forming the second layer containing a color developer is applied to the support and dried as needed, and then a composition for forming the first layer containing microcapsules is further applied to the second layer and dried as needed to form the first layer.

[0285] The method for forming the first layer using the first layer forming composition is as described in the first embodiment. Furthermore, the method for forming the second layer using the second layer forming composition is also as described in the first embodiment.

[0286] (Other parts)

[0287] The pressure measurement sheet may include other members in addition to the support body, the second layer, and the first layer.

[0288] For example, the pressure measurement sheet may include an easy-adhesion layer between the support and the second layer for improving the adhesion between the two.

[0289] The aspect of the easy-adhesion layer may be the aspect of the easy-adhesion layer which the above-mentioned 1st sheet|seat may have.

[0290] As described above, the pressure measurement sheet is used by applying pressure to the surface thereof.

[0291] In the pressure measurement sheet, the color density difference determined by the following color density difference measurement 2 is preferably 0.25 or less, more preferably 0.20 or less, and even more preferably 0.10 or less. The lower limit is not particularly limited, but is usually 0.01 or more.

[0292] Color density difference measurement 2: The difference in optical density of the pressure measurement sheet before and after the pressure measurement sheet was heated at 220° C. for 2 minutes in a non-pressurized state was taken as the color density difference.

[0293] As described above, in the color density difference measurement 2, the pressure measurement sheet is subjected to a heating treatment under the prescribed conditions. In addition, the measurement is performed in a non-pressurized state. The non-pressurized state refers to a state in which no pressure is applied to the pressure measurement sheet (a state in which no pressure is applied). Furthermore, when heating at 220°C, the laminate at room temperature (about 23°C) is heated to the prescribed temperature.

[0294] When the value of the color development density difference measurement 2 is within the above range, it is preferred from the viewpoint of at least one of the viewpoint that a more excellent effect of the present invention is obtained and the viewpoint that the temperature dependency of color development is smaller.

[0295] As a method for measuring the optical density, X-rite eXact (manufactured by X-Rite) was used to measure without a filter and at a concentration state of ISO state T, D50 / 2°. As the optical density, the value of OD (optical density) was adopted. In addition, when measuring, OD was measured in each mode of CMYK (C: Cyan, M: Magenta, Y: Yellow, K: Black), and the optical density showing the highest OD was selected.

[0296] The pressure measuring sheet set and the pressure measuring sheet of the present invention can be used for various purposes, such as verification or management of various manufacturing processes including high temperature pressing in the process. For example, the pressure distribution confirmation in the stacking process in the field of batteries (lithium-ion batteries, fuel cells), the pressure distribution confirmation in the stacking process in the field of printed circuit boards (FPC (Flexible Printed Circuits, flexible printed circuits), BWB (Back Wiring Board)), the pressure distribution confirmation in the hot pressing process such as ACF (Anisotropic Conductive Film) bonding and lamination of the wiring extraction part, and the pressure distribution confirmation of the mold fastening part, etc.

[0297] The pressure distribution can be confirmed by visual observation, and a pressure image analysis system (FPD-8010, manufactured by FUJIFILM Corporation) can also be used.

[0298] The pressure measurement sheet set and the pressure measurement sheet can be used in a wide range of pressure ranges. Specifically, they are preferably used in a range of 0.05 to 20 MPa, and more preferably in a range of 0.5 to 10 MPa.

[0299] The usable temperature range is room temperature, but preferably 160°C or higher, more preferably 180 to 240°C. When used at 240°C or higher, the temperature applied to the pressure measurement sheet set (the first sheet and the second sheet) and the pressure measurement sheet can be appropriately reduced by using a protective sheet. Examples of the protective sheet include a Teflon (registered trademark) sheet and a Kapton film, which are highly heat-resistant sheets.

[0300] <<Third Embodiment>>

[0301] As a third embodiment of the present invention, there is a dispersion liquid (hereinafter also referred to as “first dispersion liquid”) which is used to form a layer used in combination with a layer containing a color developer for pressure measurement and contains microcapsules containing a color developer.

[0302] The first dispersion contains microcapsules containing a coloring agent, wherein the capsule wall of the microcapsules contains at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane, and the capsule wall has a glass transition temperature of 150° C. or higher or has no glass transition temperature.

[0303] Examples of the first dispersion include the above-mentioned first layer-forming composition.

[0304] As an aspect of the microcapsules contained in the first dispersion, an aspect of the microcapsules contained in the first layer forming composition can be mentioned.

[0305] The first dispersion generally contains a solvent. The type of the solvent contained in the first dispersion is not particularly limited, and examples thereof include water and organic solvents.

[0306] The first dispersion is used to form a layer for pressure measurement (corresponding to the first layer described above) similarly to the first layer-forming composition.

[0307] The first dispersion liquid may be used in combination with a dispersion liquid used to form a layer containing a color developer (hereinafter, also simply referred to as "second dispersion liquid"). That is, the first dispersion liquid and the second dispersion liquid may be used as a set.

[0308] Examples of the second dispersion include the above-mentioned second layer-forming composition.

[0309] As an aspect of the color developer contained in the second dispersion, the aspect of the color developer contained in the second layer forming composition can be mentioned.

[0310] The second dispersion generally contains a solvent. The type of the solvent contained in the second dispersion is not particularly limited, and examples thereof include water and organic solvents.

[0311] The first dispersion can also be applied to an object that is difficult to measure pressure in a sheet such as a pressure measurement sheet set or a pressure measurement sheet. More specifically, a required amount of the first dispersion is applied to an area where pressure measurement of the pressure measurement object is required, and a layer containing the microcapsules is formed in the area, without being affected by the surface shape of the pressure measurement object, thereby enabling pressure measurement. In particular, it can be preferably applied to a case where pressure is measured on a curved surface. More specifically, the first dispersion is applied to a curved surface to form a layer containing microcapsules, thereby enabling pressure measurement.

[0312] In addition, as described above, the layer formed of the first dispersion is used in combination with the layer containing the developer for pressure measurement. Therefore, as in the case of using the first dispersion, a required amount of the second dispersion is applied to a region where pressure measurement of the pressure measurement object is required, and the layer containing the developer is disposed adjacent to the layer containing the microcapsules, thereby enabling pressure measurement.

[0313] In addition, the layer containing microcapsules and the layer containing the developer are usually stacked and arranged in the area where the pressure measurement object needs to be measured, but either layer may be arranged on the side of the pressure measurement object. In other words, either the first dispersion or the second dispersion may be applied first in the area where the pressure measurement object needs to be measured.

[0314] The method of applying the first dispersion liquid and the second dispersion liquid is not particularly limited, and examples thereof include roll coating, spray coating, brush coating, and dip coating.

[0315] The first dispersion liquid and the second dispersion liquid may be applied directly to the measurement surface of the measurement object, or may be applied via a film, paper, or the like.

[0316] The application amount of the first dispersion and the second dispersion can be set according to the measurement purpose, but from the viewpoint of obtaining good color development and color development distribution, it is preferably 2 to 40 g / m2 in terms of solid content. 2 .

[0317] <<Fourth Embodiment>>

[0318] As a fourth embodiment of the present invention, there is mentioned a dispersion liquid containing microcapsules containing a color former and a color developer (hereinafter, also simply referred to as "third dispersion liquid"), and this dispersion liquid is used to form a layer for pressure measurement.

[0319] The third dispersion contains microcapsules containing a color former and a developer, wherein the capsule wall of the microcapsules contains at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane, and the capsule wall has a glass transition temperature of 150° C. or higher or has no glass transition temperature.

[0320] As an aspect of the microcapsules contained in the third dispersion, the aspect of the microcapsules contained in the first layer forming composition can be mentioned.

[0321] As an aspect of the color developer contained in the third dispersion, the aspect of the color developer contained in the second layer forming composition can be mentioned.

[0322] The third dispersion generally contains a solvent. The type of the solvent contained in the first dispersion is not particularly limited, and examples thereof include water and organic solvents.

[0323] The third dispersion may be a mixture of the above-mentioned first layer forming composition with a color developer, or a mixture of the above-mentioned second layer forming composition with the first layer forming composition.

[0324] Since the third dispersion liquid contains microcapsules containing a color former and a color developer, the pressure measurement is performed only on the layer formed by applying the third dispersion liquid.

[0325] That is, like the first dispersion and the second dispersion, the third dispersion can also be applied to an object that is difficult to measure pressure in a sheet such as a pressure measurement sheet set or a pressure measurement sheet. More specifically, the pressure measurement can be performed by applying a required amount of the third dispersion to an area where pressure measurement of the pressure measurement object is required and forming a layer in the area without being affected by the surface shape of the pressure measurement object.

[0326] Examples of the coating method and coating conditions of the third dispersion include the coating method and coating conditions of the above-mentioned first dispersion and second dispersion.

[0327] The first dispersion liquid, the second dispersion liquid, and the third dispersion liquid described above can be used for various purposes.

[0328] For example, the following can be mentioned: confirmation of pressure distribution in the forming process of various components, main bodies, etc. or the assembly process of components in the manufacture of vehicles such as automobiles or aircraft, confirmation of pressure distribution in the assembly process of building materials, confirmation of pressure distribution in processes such as curved surface processing of electronic products, confirmation of impact force applied to goods accompanying transportation, confirmation of each mold in the manufacture of metal products, confirmation of each mold during the molding process of resin products, confirmation of pressure distribution in the tableting of pharmaceutical tablets, confirmation of pressure distribution on the surface of furniture such as sofa seats, confirmation of grip force applied to stationery, etc., confirmation of pressure on stationery, confirmation of impact force applied to sports equipment such as balls made of elastic materials, and confirmation of the gap (clearance) between upper and lower teeth in dental products.

[0329] [Example]

[0330] The present invention will be further described below by way of examples. The present invention is not limited to the following examples unless it deviates from the gist thereof.

[0331] <Example 1>

[0332] (Preparation of Microcapsules)

[0333] The following compound (A) (molecular weight: 623) (6.8 parts by mass) as a coloring agent was dissolved in linear alkylbenzene (ENEOS Corporation, grade olefin L) (52 parts by mass) to obtain solution A. Next, synthetic isoparaffin (Idemitsu Kosan Co., Ltd., IP solvent 1620) (14 parts by mass) was added to the stirred solution A to obtain solution B. In addition, trimethylolpropane adduct of toluene diisocyanate (DIC CORPORATION, BURNOCK D-750) (13.9 parts by mass) (solid content mass: 10.4 parts by mass) dissolved in 2-butanone (10 parts by mass) was added to the stirred solution B to obtain solution C. In addition, BURNOCK D-750 was a solution having a homopolymer concentration of 75% by mass.

[0334] Furthermore, the above solution C was added to a solution of polyvinyl alcohol (PVA-217E, Kuraray Co., Ltd.) (7.8 parts by mass) dissolved in water (130 parts by mass) to perform emulsification dispersion. Water (230 parts by mass) was added to the emulsified solution after emulsification dispersion, and the mixture was heated to 70° C. while stirring, stirred for 1 hour, and then cooled. In addition, water was added to adjust the concentration, and a microcapsule solution containing a coloring agent having a solid content concentration of 19.6% by mass was obtained.

[0335] Furthermore, as shown in the following structural formula, the BURNOCK D-750 corresponds to an adduct of an aromatic diisocyanate and trimethylolpropane, that is, a trifunctional polyisocyanate.

[0336] [Chemical formula 3]

[0337]

[0338] Compound (A) (hereinafter, refer to the structural formula)

[0339] [Chemical formula 4]

[0340]

[0341] The volume-based median diameter of the microcapsules containing the coloring agent was 20 μm, the number-average wall thickness was 0.44 μm, and δ / Dm was 0.022. The glass transition temperature of the capsule wall of the microcapsules was 150°C.

[0342] As described below, after preparing the first sheet having the first layer containing microcapsules, the surface of the first layer was photographed at 1000 times with an optical microscope, and the sizes of all microcapsules in the range of 500 um×500 μm were measured to calculate the median diameter (Dm).

[0343] Regarding the number average wall thickness, as described later, after preparing the first sheet having the first layer containing microcapsules, a cross-sectional slice of the first sheet having the first layer containing microcapsules is prepared, and the cross-section is observed by SEM at 200 times. Based on the selection of any five microcapsules having a particle size in the range of (the value of the median particle size based on the volume of the microcapsules) × 0.9 to (the value of the median particle size based on the volume of the microcapsules) × 1.1, the cross-sections of the selected microcapsules are observed, the thickness of the capsule wall is determined, and the average value is calculated.

[0344] And, the glass transition temperature was measured by the following method.

[0345] First, as described later, after preparing the first sheet having the first layer containing microcapsules, cut it into 50 pieces of 1 cm in length and 1 cm in width, and immerse all of them in 10 ml of water and let it stand for 24 hours. That is, prepare the first sheet having the first layer of 50 pieces of 1 cm in length and 1 cm in width, immerse all of them in 10 ml of water and let it stand for 24 hours, and obtain an aqueous dispersion of microcapsules. The obtained aqueous dispersion of microcapsules was centrifuged at 15000 rpm for 30 minutes, and the microcapsules were separated. Ethyl acetate was added to the separated microcapsules, and further stirred at 25°C for 24 hours. After that, the obtained solution was filtered, and the obtained residue was vacuum dried at 60°C for 48 hours, thereby obtaining microcapsules that do not contain anything inside (hereinafter, also referred to as "measurement material"). Next, the thermal decomposition temperature of the obtained measurement material was measured using a thermogravimetric differential thermal analyzer TG-DTA (device name: DTG-60, Shimadzu Corporation). In addition, as the thermal decomposition temperature, the temperature at which the measured material is heated from room temperature at a constant heating rate (10°C / min) and the mass of the measured material before heating is reduced by 5% by mass is taken as the thermal decomposition temperature (°C) in the thermogravimetric analysis (TGA) in the atmospheric environment. Next, the glass transition temperature of the measured material was measured using a differential scanning calorimeter DSC (device name: DSC-60a Plus, Shimadzu Corporation) and a closed pan at a heating rate of 5°C / min in the range of 25°C to (thermal decomposition temperature -5°C). As the glass transition temperature of the capsule wall of the microcapsule, the value at the second week of heating was used.

[0346] (Preparation of the first sheet)

[0347] A microcapsule liquid containing a coloring agent (43 parts by mass), water (15 parts by mass), colloidal silica (Nissan Chemical Corporation SNOWTEX (registered trademark) 30, solid content concentration 30% by mass) (4.3 parts by mass), a 10% by mass aqueous solution of carboxymethylcellulose Na (DKS Co. Ltd., CELLOGEN 5A) (4.3 parts by mass), a 1% by mass aqueous solution of carboxymethylcellulose Na (DKS Co. Ltd., CELLOGEN EP) (10 parts by mass), a 15% by mass aqueous solution of sodium alkylbenzene sulfonate (DKS Co. Ltd., NEOGENT) (0.3 parts by mass), and a 1% by mass aqueous solution of NOIGEN LP70 (DKS Co. Ltd.) (1.0 parts by mass) were mixed and stirred for 2 hours to obtain a composition for forming the first layer.

[0348] The obtained first layer forming composition was applied on a 75 μm thick polyethylene terephthalate sheet with an easy-adhesion layer (TOYOBO CO., LTD., COSMOSHINE (registered trademark) A4300) by a bar coater so that the mass after drying would be 4.5 g / m 2 , and dried to form the first layer, thereby producing the first sheet.

[0349] (Preparation of the Second Sheet)

[0350] Using mixed sand, sulfuric acid-treated activated clay (200 parts by mass) as a color developer, sodium hexametaphosphate (1 part by mass), a 10% by mass aqueous solution of sodium hydroxide (30 parts by mass), and water (290 parts by mass) were dispersed so that the average particle size of all particles became 2 μm, thereby preparing a dispersion liquid.

[0351] Next, a 19 mass % aqueous dispersion (180 mass parts) of NIPOL LX-814 (Zeon Corporation), a 3.3 mass % aqueous solution (220 mass parts) of POLYMARON 482 (ARAKAWA CHEMICAL INDUSTRIES, LTD.), a 1 mass % aqueous solution (80 mass parts) of carboxymethylcellulose Na (DKS Co. Ltd., CELLOGEN EP), a 15 mass % aqueous solution (4.7 mass parts) of sodium alkylbenzene sulfonate (DKS Co. Ltd., NEOGEN T), and a 1 mass % aqueous solution (70 mass parts) of NOIGEN LP70 (DKS Co. Ltd.) were mixed with the prepared dispersion to prepare a coating solution containing a color developer.

[0352] The coating solution containing the developer was applied on a polyethylene terephthalate sheet having a thickness of 75 μm so that the coating amount of the same volume component became 12.0 g / m 2 , and dried to form a second layer, thereby obtaining a second sheet.

[0353] <Example 2>

[0354] Instead of trimethylolpropane adduct of toluene diisocyanate (DIC CORPORATION, BURNOCK D-750) (13.9 parts by mass), trimethylolpropane adduct of toluene diisocyanate (DIC CORPORATION, BURNOCK D-750) (13.2 parts by mass) (solid content mass: 9.9 parts by mass) and polyisocyanate B (TOSOH Corporation, MILLIONATE MR-200) (0.5 parts by mass) were used. The first sheet and the second sheet were prepared in the same order as in Example 1, except that the above-mentioned materials were replaced with trimethylolpropane adduct of toluene diisocyanate (DIC CORPORATION, BURNOCK D-750) (13.9 parts by mass).

[0355] In Example 2, the total solid content of the trimethylolpropane adduct of tolylene diisocyanate and the polymethylene polyphenyl polyisocyanate was 10.4 parts by mass.

[0356] Furthermore, MILLIONATE MR-200 used as the above-mentioned polyisocyanate B corresponds to a mixture of diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate (corresponding to the compound represented by formula (X)).

[0357] <Examples 3 to 5>

[0358] The first sheet and the second sheet were prepared in the same procedure as in Example 2 except that the total amount of the trimethylolpropane adduct of toluene diisocyanate and the polyisocyanate B was the same as in Example 2 (10.4 parts by mass) and the mixing mass ratio of the two was as shown in Table 1.

[0359] <Example 6>

[0360] Instead of the trimethylolpropane adduct of toluene diisocyanate (DIC CORPORATION, BURNOCK D-750), as shown in Table 1, a trimethylolpropane adduct of 1,3-bis(isocyanate methyl)cyclohexane (Mitsui Chemicals, Inc., TAKENATED-120N) was used, and the mixing mass ratio with polyisocyanate B was adjusted as shown in Table 1. Except for this, the first sheet and the second sheet were prepared in the same order as in Example 4.

[0361] As shown in the following structural formula, the above-mentioned TAKENATED-120N corresponds to an adduct of an alicyclic diisocyanate and trimethylolpropane, that is, a trifunctional polyisocyanate.

[0362] [Chemical formula 5]

[0363]

[0364] <Examples 7 to 8>

[0365] The first sheet and the second sheet were produced in the same procedure as in Example 4 except that MILLIONATE MR-100 or MILLIONATE MR-400 was used instead of MILLIONATE MR-200.

[0366] In addition, the above-mentioned MILLIONATE MR-100 and the above-mentioned MILLIONATE MR-400 correspond to a mixture of diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate (corresponding to the compound represented by formula (X)).

[0367] <Examples 9 to 12>

[0368] The first sheet and the second sheet were prepared in the same procedure as in Example 4 except that compounds (B) to (E) were used as shown in Table 1 instead of compound (A).

[0369] In addition, compounds (B) to (E) are as follows.

[0370] [Chemical formula 6]

[0371]

[0372] <Examples 13 to 16>

[0373] The first sheet and the second sheet were prepared in the same procedure as in Example 4 except that the amount of the solid content of the polyisocyanate used was changed to that described in "Polyisocyanate solid content (parts by mass)" in Table 1.

[0374] In addition, the solid content usage-amount means the solid content total mass of the trimethylolpropane adduct of tolylene diisocyanate and polyisocyanate B.

[0375] <Comparative Example 1>

[0376] According to the procedure described in Example 1 of Patent Document 1, a first sheet (electron donating leuco dye sheet) and a second sheet (developer sheet) were produced.

[0377] Table 1 shows the median particle size, δ / Dm, and glass transition temperature of the capsule wall of the microcapsule in each of the Examples and Comparative Examples.

[0378] In addition, the thermal decomposition temperature of the capsule wall of the microcapsule produced in each example was about 250°C.

[0379] Then, the color density difference was determined according to the procedure of the color density difference measurement 1. The results are summarized in Table 1.

[0380] <Evaluation>

[0381] (Pressure distribution measurement)

[0382] The first sheet and the second sheet prepared in each example and comparative example were cut into a size of 5 cm×5 cm, and the first sheet and the second sheet were overlapped with the surface of the first layer of the first sheet and the surface of the second layer of the second sheet in contact with each other to obtain a laminated body.

[0383] Next, a hot press having two upper and lower heating platforms was prepared, the heating platforms were separated from each other, a ring-shaped SUS substrate with a width of 5 mm was arranged on the lower platform, and the laminate was arranged in a manner covering the SUS substrate. After that, the SUS substrate and the laminate were sandwiched between two heating platforms heated to 220° C. and pressurized at 2.0 MPa for 2 minutes. After the pressurization was completed, the shape of the color development area of ​​the obtained laminate was observed and evaluated according to the following criteria.

[0384] "5": There is no sparseness or density of color development, and the shape of the color development area can be recognized very well as being a ring shape similar to that of the SUS substrate.

[0385] "4": The density of color development is very small, but the shape of the color development area can be well recognized as a ring shape similar to that of the SUS substrate.

[0386] "3": There are sparse and dense areas of color development, but the shape of the color development area can be sufficiently recognized as a ring shape.

[0387] "2": Due to the density of the color development, there is a ring-shaped portion where the color development area cannot be recognized.

[0388] "1": The density of the color development is very large, and the shape of the color development area is almost unrecognizable as a ring shape.

[0389] (Evaluation of color development temperature dependence)

[0390] According to the same procedure as described above (pressure distribution measurement), two laminated bodies composed of the first sheet and the second sheet produced in each of the examples and comparative examples were prepared.

[0391] Next, a heat press having two upper and lower heating carriers was prepared, the heating carriers were separated from each other, and the laminate was placed on the lower carrier. After that, the laminate was sandwiched between two heating carriers heated to 200°C and pressed at 2.0 MPa for 2 minutes. After heating, the optical density A of the color development area of ​​the laminate was measured.

[0392] The laminate was pressed in the same manner as above except that the temperature of the heating stage was changed to 180° C. After the heating was completed, the optical density B of the color development region of the laminate was measured.

[0393] Next, the difference between the optical density A and the optical density B (optical density A-optical density B) was determined and evaluated according to the following criteria: The smaller the difference, the smaller the difference in the degree of color development due to temperature.

[0394] "4": The above difference is 0.3 or less.

[0395] "3": The above difference is greater than 0.3 and less than 0.4.

[0396] "2": The above difference is greater than 0.4 and less than 0.5.

[0397] "1": the above difference is greater than 0.5.

[0398] In addition, as a method for measuring the optical density, X-rite eXact (manufactured by X-Rite) was used to measure without a filter and at a concentration state of ISO state T, D50 / 2°. As the optical density, the value of OD was used. In addition, when measuring, OD was measured in each mode of CMYK (C: Cyan, M: Magenta, Y: Yellow, K: Black), and the optical density showing the highest OD was selected.

[0399] In Table 1, "polyisocyanate A" corresponds to an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule, i.e., a trifunctional or higher polyisocyanate, and "polyisocyanate B" corresponds to a mixture of diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate (corresponding to the compound represented by formula (X)).

[0400] In Table 1, “mass ratio (A / B)” indicates the mass ratio of the mass of polyisocyanate A to the mass of polyisocyanate B.

[0401] In Table 1, "polyisocyanate solid content (parts by mass)" indicates the total amount of the solid content mass of polyisocyanate A and the solid content mass of polyisocyanate B.

[0402] In Table 1, the "Type" column of the "Color Forming Agent" column shows the above-mentioned compounds (A) to (E), respectively, and the "Molecular Weight" column shows the molecular weight of each compound.

[0403] In Table 1, the column "Particle size (μm)" shows the volume-based median particle size (μm) of the microcapsule.

[0404] In Table 1, "δ / Dm" represents "δ / Dm" in the above formula (1), δ represents the number average wall thickness (μm) of the microcapsules, and Dm represents the volume-based median diameter (μm) of the microcapsules.

[0405] In Table 1, the column "Glass transition temperature (° C.)" indicates the glass transition temperature of the capsule wall in the microcapsule.

[0406] In Table 1, "None" in the "Glass transition temperature" column means that the glass transition temperature did not appear in the above measurement. That is, it means that the capsule wall of the microcapsule does not show a glass transition temperature in the range of "25°C" to "(thermal decomposition temperature (°C) - 5°C)".

[0407] In Table 1, the column "Color density difference" shows the color density difference obtained by the color density difference measurement 1 described above.

[0408] [Table 1]

[0409]

[0410] As shown in Table 1, it was confirmed that when the pressure measurement sheet set of the present invention was used, the desired effect was obtained.

[0411] Among them, from the comparison of Examples 2 to 5, it was confirmed that when the mass ratio of polyisocyanate A to polyisocyanate B was 80 / 20 to 20 / 80 (preferably 80 / 20 to 45 / 55), more excellent effects were achieved.

[0412] Furthermore, from the comparison between Examples 4 and 6, it was confirmed that a more preferable effect can be obtained by using an adduct obtained using an aromatic diisocyanate.

[0413] Furthermore, from the comparison between Example 4 and Examples 9 to 12, it was confirmed that when the molecular weight of the color former is 420 or more (preferably 550 or more), the effect is more excellent.

[0414] Furthermore, from the comparison between Example 4 and Examples 13 to 16, it was confirmed that when δ / Dm was larger than 0.010 (preferably 0.015 or larger), the effect was more excellent.

[0415] In addition, although the above description shows a method of using a pressure measurement sheet set having a first sheet and a second sheet, a pressure measurement sheet having a second layer and a first layer stacked in sequence on a support was prepared, and the same test as above was performed, and the same result as that of each embodiment was obtained. For example, the second layer and the first layer prepared in the above embodiment 4 were sequentially arranged on a polyethylene terephthalate sheet with an easy-adhesion layer (TOYOBO CO., LTD., COSMOSHINE (registered trademark) A4300), and a pressure measurement sheet having a support, a second layer, and a first layer in sequence was prepared, and the above (pressure distribution measurement) and (color development temperature dependence evaluation) were performed, and the same result as that of embodiment 4 was obtained.

[0416] <Example 17>

[0417] The pressure measurement solution set was spray-coated on the curved surface member, and color development evaluation was performed.

[0418] Specifically, the microcapsule liquid containing the color former prepared in Example 2 was prepared as the first dispersion liquid, and the dispersion liquid containing the color developer prepared in Example 2 was prepared as the second dispersion liquid.

[0419] A metal plate (10 cm×10 cm) made of stainless steel (SUS304) heated to 180° C. was spray-coated with the first dispersion, and then spray-coated with the second dispersion. The same metal plate was placed on the coated surface so as to cover the coated area, and pressurized at a pressure of 2.0 MPa for 2 minutes using a press machine (product name: H1F35-1, manufactured by Komatsu Ltd.). After the pressurization was completed, the metal plate placed on the upper part was removed, and the color development and color distribution of the coated area were confirmed by visual observation, and it was confirmed that the color was developed at a sufficient concentration that could be visually recognized.

[0420] <Example 18>

[0421] As a result of color development evaluation carried out in the same manner as in Example 17 except that the first dispersion liquid and the second dispersion liquid were mixed in advance, it was confirmed that color development occurred at a concentration sufficient to be visually recognized, as in Example 17.

[0422] Explanation of symbols

[0423] 10 - sheet group for pressure measurement, 12 - first support, 13 - microcapsule, 14 - first layer, 16 - first sheet, 18 - second support, 20 - second layer, 22 - second sheet, 30 - sheet for pressure measurement, 32 - support.

Claims

1. A pressure measurement sheet set, comprising: a first sheet having a first layer including microcapsules containing a coloring agent; and a second sheet having a second layer containing a developer, The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane, wherein the resin has a polymethylene polyphenyl structure. The glass transition temperature of the capsule wall is above 160° C. or the capsule wall does not show a glass transition temperature, The microcapsules satisfy the relationship of formula (1), Formula (1) δ / Dm>0.010 δ represents the number average wall thickness of the microcapsules, in μm, and Dm represents the volume-based median particle size of the microcapsules, in μm.

2. The pressure measurement sheet set according to claim 1, wherein: The resin is formed using a trifunctional or higher-functional polyisocyanate A and a polyisocyanate B. The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule. The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

3. The pressure measurement sheet set according to claim 2, wherein: The mass ratio of the polyisocyanate A to the polyisocyanate B is 95 / 5 to 50 / 50.

4. The pressure measurement sheet set according to claim 1 or 2, wherein: The molecular weight of the coloring agent is 550 or more.

5. The pressure measurement sheet set according to claim 1 or 2, wherein: The number average wall thickness of the microcapsules is greater than 0.2 μm.

6. A pressure measuring sheet, comprising: The first layer comprises microcapsules containing a coloring agent; and a second layer disposed on the first layer and comprising a color developer, The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane, wherein the resin has a polymethylene polyphenyl structure. The glass transition temperature of the capsule wall is above 160° C. or the capsule wall does not show a glass transition temperature, The microcapsules satisfy the relationship of formula (1), Formula (1) δ / Dm>0.010 δ represents the number average wall thickness of the microcapsules, in μm, and Dm represents the volume-based median particle size of the microcapsules, in μm.

7. The pressure measuring sheet according to claim 6, wherein: The resin is formed using a trifunctional or higher-functional polyisocyanate A and a polyisocyanate B. The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule. The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

8. The pressure measuring sheet according to claim 7, wherein: The mass ratio of the polyisocyanate A to the polyisocyanate B is 95 / 5 to 50 / 50.

9. The pressure measuring sheet according to claim 6 or 7, wherein: The molecular weight of the coloring agent is 550 or more.

10. The pressure measuring sheet according to claim 6 or 7, wherein: The number average wall thickness of the microcapsules is greater than 0.2 μm.

11. A dispersion liquid for forming a layer used in combination with a layer containing a color developer for pressure measurement, comprising microcapsules containing a color developer, wherein: The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane, wherein the resin has a polymethylene polyphenyl structure. The glass transition temperature of the capsule wall is above 160° C. or the capsule wall does not show a glass transition temperature, The microcapsules satisfy the relationship of formula (1), Formula (1) δ / Dm>0.010 δ represents the number average wall thickness of the microcapsules, in μm, and Dm represents the volume-based median particle size of the microcapsules, in μm.

12. The dispersion according to claim 11, wherein The resin is formed using a trifunctional or higher-functional polyisocyanate A and a polyisocyanate B. The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule. The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

13. The dispersion according to claim 11 or 12, wherein The molecular weight of the coloring agent is 550 or more.

14. A dispersion liquid for forming a layer for pressure measurement, comprising microcapsules containing a color former and a developer, wherein: The capsule wall of the microcapsule comprises at least one resin selected from the group consisting of polyurea, polyurethaneurea and polyurethane, wherein the resin has a polymethylene polyphenyl structure. The glass transition temperature of the capsule wall is above 160° C. or the capsule wall does not show a glass transition temperature, The microcapsules satisfy the relationship of formula (1), Formula (1) δ / Dm>0.010 δ represents the number average wall thickness of the microcapsules, in μm, and Dm represents the volume-based median particle size of the microcapsules, in μm.

15. The dispersion according to claim 14, wherein The resin is formed using a trifunctional or higher-functional polyisocyanate A and a polyisocyanate B. The trifunctional or higher-functional polyisocyanate A is an adduct of an aromatic diisocyanate or an alicyclic diisocyanate and a compound having three or more active hydrogen groups in one molecule. The polyisocyanate B is selected from the group consisting of aromatic diisocyanates and polymethylene polyphenyl polyisocyanates.

16. The dispersion according to claim 14 or 15, wherein The molecular weight of the coloring agent is 550 or more.