Separator, electrochemical device and electronic device including the separator
By setting a positive electrode diaphragm, negative electrode diaphragm and insulating layer on the lithium-ion battery separator, ensuring the consistency of compaction density in the electrode area and the AC Overhang area, the problems of insufficient working voltage and high self-discharge rate of lithium-ion batteries are solved, and the problem of high self-discharge rate of lithium-ion batteries is improved. Energy density and safety.
Patent Information
- Application Number
- CN202080030670.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-06-30
AI Technical Summary
The working voltage of lithium-ion batteries is difficult to exceed 5V, which limits its application in high voltage application scenarios. The series connection method leads to a reduction in energy density, resulting in self-discharge rate and safety problems.
A partition is designed, including a partition substrate, a positive electrode diaphragm, an anodized electrode diaphragm and an insulating layer. The insulating layer covers the negative electrode diaphragm to ensure the consistency of compaction density in the electrode area and the AC Overhang area, reduce edge discounts and damage, and improve Charge and discharge rate and safety.
It improves the energy density of lithium-ion batteries, reduces the self-discharge rate and safety risks, and enhances the performance and safety of electrochemical devices.
Smart Images

Figure CN114026722B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemistry, and in particular to a separator, an electrochemical device and an electronic device comprising the separator. Background Art
[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight, and are widely used in the field of consumer electronics. With the rapid development of electric vehicles and mobile electronic devices, people's performance requirements for lithium-ion batteries are also getting higher and higher. For example, lithium-ion batteries are required to have higher energy density, safety, and cycle performance.
[0003] However, lithium-ion batteries are limited by their inherent electrochemical system, and the operating voltage of a single battery is usually difficult to exceed 5 V. However, in the actual use of lithium-ion batteries, there are many demands for high-voltage application scenarios, such as electric vehicles (EVs) and energy storage systems (ESSs).
[0004] In order to increase the output voltage of lithium-ion batteries, the existing technology usually connects multiple lithium-ion batteries in series through external wires. However, due to the difference in capacity between individual lithium-ion batteries, this series connection method results in a low overall energy density (ED) of the lithium-ion batteries after the series connection, which limits the application scope of lithium-ion batteries. Summary of the invention
[0005] The purpose of the present application is to provide a separator, an electrochemical device and an electronic device including the separator, so as to improve the energy density of a lithium-ion battery. The specific technical solution is as follows:
[0006] A first aspect of the present application provides a separator, comprising a separator substrate, a positive electrode membrane, a negative electrode membrane and an insulating layer;
[0007] Wherein, the positive electrode membrane and the negative electrode membrane are respectively located on two sides of the separator substrate;
[0008] The insulating layer is arranged on the separator substrate, and the insulating layer is arranged on the periphery of the positive electrode membrane;
[0009] The area surrounded by the orthographic projection of the outer edge of the insulating layer on the separator substrate covers the orthographic projection of the negative electrode membrane on the separator substrate.
[0010] In one embodiment of the present application, a negative electrode membrane region exists on the other side of the separator substrate opposite to the positive electrode membrane region; and a negative electrode membrane region exists at least partially on the other side of the separator substrate opposite to the insulating layer region.
[0011] In one embodiment of the present application, there is a gap between the positive electrode diaphragm area and the insulating layer area. On the one hand, the gap can provide a buffer space for the electrode to be immersed in the electrolyte and for the change in the volume of the positive electrode material during the charging and discharging process; on the other hand, the gap also provides a channel for the electrolyte to penetrate into the positive electrode diaphragm from the side, which can increase the charging and discharging rate.
[0012] In one embodiment of the present application, the positive projection of the geometric center of the positive electrode diaphragm on the separator substrate coincides with the positive projection of the geometric center of the negative electrode diaphragm on the separator substrate, and the length from the geometric center to the outer edge of the positive electrode diaphragm in the divergent direction is L1; along the same divergent direction, the length from the outer edge of the positive electrode diaphragm to the outer edge of the insulating layer is D, and the length from the geometric center to the outer edge of the negative electrode diaphragm is L2, satisfying the following geometric relationship:
[0013] L1 <L2,L1+D≥L2。
[0014] In one embodiment of the present application, the positive electrode diaphragm and the negative electrode diaphragm are rectangular in shape, the orthographic projection of the geometric center of the positive electrode diaphragm on the separator substrate coincides with the orthographic projection of the geometric center of the negative electrode diaphragm on the separator substrate, and the positive electrode diaphragm, the negative electrode diaphragm, and the insulating layer satisfy the following geometric relationship:
[0015]
[0016] Among them, Lx1 is the length of the positive electrode diaphragm, Ly1 is the width of the positive electrode diaphragm, Lx2 is the length of the negative electrode diaphragm, Ly2 is the width of the negative electrode diaphragm, Dx is the width of the insulating layer extending along the long side direction of the positive electrode diaphragm, and Dy is the width of the insulating layer extending along the short side direction of the positive electrode diaphragm.
[0017] In one embodiment of the present application, the portion of the insulating layer extending along the long side direction of the positive electrode diaphragm includes a first portion and a second portion, and the widths of the first portion and the second portion are the same or different; the portion of the insulating layer extending along the short side direction of the positive electrode diaphragm includes a third portion and a fourth portion, and the widths of the third portion and the fourth portion are the same or different.
[0018] In one embodiment of the present application, the electronic resistivity of the insulating layer is greater than 10 7 Ω·m.
[0019] In one embodiment of the present application, 0mm≤L1+D-L2≤4.5mm.
[0020] In one embodiment of the present application, 0.5 mm ≤ D ≤ 5 mm.
[0021] In one embodiment of the present application, the separator satisfies at least one of the following features:
[0022] (a) The electronic resistivity of the insulating layer is greater than 10 10 Ω·m;
[0023] (b) 1mm≤L1+D-L2≤2.5mm;
[0024] (c)1.5mm≤D≤3mm.
[0025] In one embodiment of the present application, the partition further includes a sealing layer, and the sealing layer is located around the partition. The distance between the insulating layer and the sealing layer is D3, 0mm≤D3≤20mm.
[0026] In one embodiment of the present application, 2mm≤D3≤5mm.
[0027] In one embodiment of the present application, the insulating layer comprises ceramic particles, the average particle size of the ceramic particles is 10 nm to 20 μm, the porosity of the insulating layer is 10% to 60%, and the average pore size of the insulating layer is 20 nm to 50 μm.
[0028] In one embodiment of the present application, the insulating layer satisfies at least one of the following features:
[0029] (a) the average particle size of the insulating ceramic particles is 100 nm to 10 μm;
[0030] (b) the porosity of the insulating layer is 20% to 40%;
[0031] (c) The average pore size of the insulating layer is 200 nm to 20 μm.
[0032] In one embodiment of the present application, the insulating layer further includes an adhesive, and the adhesive accounts for 5% to 40% of the mass of the insulating layer.
[0033] In one embodiment of the present application, the adhesive includes at least one of polyamide, polyurethane, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, acrylate, polyvinylidene fluoride or polyvinylidene fluoride-hexafluoropropylene copolymer.
[0034] In one embodiment of the present application, the insulating layer includes at least one of HfO2, SrTiO3, SnO2, CeO2, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, boehmite, magnesium hydroxide, aluminum hydroxide, lithium phosphate, lithium titanium phosphate, lithium aluminum titanium phosphate, lithium lanthanum titanate, lithium germanium thiophosphate, lithium nitride, SiS2 glass, P2S5 glass, Li2O, LiF, LiOH, Li2CO3, LiAlO2, lithium germanium phosphosulfur ceramics or garnet ceramics.
[0035] A second aspect of the present application provides an electrochemical device, comprising the separator described in any of the above embodiments.
[0036] In one embodiment of the present application, the electrochemical device includes at least two electrode assemblies, the separator is sealed and connected to the outer package, and independently sealed chambers are formed on both sides of the separator, each of which contains an electrode assembly and an electrolyte.
[0037] The second aspect of the present application provides an electronic device, comprising the electrochemical device described in the third aspect of the present application.
[0038] The present application provides a separator, an electrochemical device and an electronic device including the separator. By arranging a positive electrode membrane and a negative electrode membrane on a separator substrate, the content of active materials in the electrochemical device can be increased, thereby improving the energy density of the electrochemical device. In addition, by arranging an insulating layer on the periphery of the positive electrode membrane, and making the area surrounded by the orthographic projection of the outer edge of the insulating layer on the separator substrate cover the orthographic projection of the negative electrode membrane on the separator substrate, after the separator is cold-pressed, the negative electrode over-positive region (AC Overhang) on the negative electrode membrane side is consistent with the compaction density of the electrode region, which, on the one hand, eliminates the local lithium precipitation phenomenon in the low compaction density region due to inconsistent compaction density, and on the other hand, reduces the occurrence of folding and damage of the separator edge, thereby improving the self-discharge performance and safety of the electrochemical device. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions of the present application and the prior art, the following briefly introduces the drawings required for use in the embodiments and the prior art. Obviously, the drawings described below are only some embodiments of the present application, and a person skilled in the art can also obtain other technical solutions based on these drawings.
[0040] Figure 1 This is a schematic diagram of the structure of a partition in one embodiment of the present application;
[0041] Figure 2 A top view of a partition in one embodiment of the present application;
[0042] Figure 3 A bottom view of a partition in one embodiment of the present application;
[0043] Figure 4 It is a schematic diagram of the structure of an electrochemical device in one embodiment of the present application. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solutions, and advantages of the present application more clearly understood, the present application is further described in detail with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. All other technical solutions obtained based on the embodiments in the present application belong to the scope of protection of the present application.
[0045] It should be noted that in the specific embodiments of the present application, a lithium-ion battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium-ion battery.
[0046] The prior art also generally adopts a single lithium-ion battery formed by connecting multiple electrochemical units in series, thereby increasing the output voltage of the lithium-ion battery. The pole piece used in this lithium-ion battery is a bipolar pole piece, wherein one side of the bipolar pole piece is coated with a positive electrode active material, and the other side is coated with a negative electrode active material. For the safety of lithium-ion batteries, the coating area of the negative electrode active material is generally larger than the coating area of the positive electrode active material, thereby avoiding the lithium precipitation problem caused by the fact that the negative electrode side active material at the local edge of the lithium-ion battery is less than the positive electrode side active material. However, the above-mentioned bipolar pole piece is a double-sided heterogeneous pole piece. In the cold pressing process, since it is necessary to cold press both sides of the above-mentioned bipolar pole piece simultaneously, at this time, on the outer side of the positive electrode active material coating area, at the edge position corresponding to the negative electrode active material coating area (AC Overhang area, or negative electrode over positive area), due to the inconsistent total thickness of the pole piece, the following problems are prone to occur:
[0047] 1) The edge of the positive electrode active material coating area and the corresponding negative electrode active material coating area will be folded and powdered after cold pressing, which will lead to local lithium deposition at the edge of the bipolar pole piece and abnormal self-discharge rate of lithium-ion batteries.
[0048] 2) The negative electrode super positive electrode area in the negative electrode active material coating area has a lower compaction density than other areas after cold pressing, which makes the local potential of the low compaction density area low, and it is easy to cause local lithium precipitation during the cycle process, resulting in a decrease in the cycle capacity retention rate of the lithium-ion battery;
[0049] 3) The current collector at the edge of the positive electrode active material coating area is prone to creases after cold pressing, which reduces the mechanical strength of the current collector and affects the safety of the lithium-ion battery.
[0050] In view of this, the present application provides a partition, Figure 1 This is a schematic diagram of the structure of a partition in one embodiment of the present application. Figure 2 This is a top view of a partition in one embodiment of the present application, such as Figure 1 and Figure 2 As shown, the separator includes a separator substrate 101, a positive electrode diaphragm 102, a negative electrode diaphragm 103 and an insulating layer 104, wherein the positive electrode diaphragm 102 and the negative electrode diaphragm 103 are respectively located on the two sides of the separator substrate 101; the insulating layer 104 is arranged on the separator substrate 101, and the insulating layer 104 is arranged on the periphery of the positive electrode diaphragm 102; the area surrounded by the orthographic projection of the outer edge of the insulating layer 104 on the separator substrate 101 covers the orthographic projection of the negative electrode diaphragm 103 on the separator substrate 101, which can make the ACOverhang area on the negative electrode diaphragm 103 side consistent with the compaction density of the electrode area, thereby eliminating the local lithium precipitation phenomenon in the low compaction density area due to the inconsistent compaction density of the electrode area on the one hand, and reducing the occurrence of folding and damage of the separator edge on the other hand, thereby reducing the self-discharge rate and safety of the lithium-ion battery.
[0051] from Figure 1 It can be seen that the length of the positive electrode membrane 102 is shorter than that of the negative electrode membrane 103 , because the coating area of the negative electrode active material is usually larger than the coating area of the positive electrode active material to improve the safety of the lithium-ion battery.
[0052] In one embodiment of the present application, reference Figure 1 , there is a negative electrode membrane area on the other side of the separator substrate 101 opposite to the positive electrode membrane area 102, that is, Figure 1 The other side of the separator substrate 101 opposite to the insulating layer 104 region at least partially has a negative electrode membrane region, that is, Figure 1 By making the insulating layer 104 extend beyond the AC Overhang region on the opposite side, the compaction density of the pole piece region and the AC Overhang region can be made consistent during cold pressing.
[0053] Furthermore, although the insulating layer 104 exceeds the AC Overhang area on the opposite side, since the insulating layer 104 itself is insulated, even if the insulating layer 104 is folded and powdered after cold pressing, it will not cause local lithium deposition at the edge of the anode, and will not affect the self-discharge performance and safety of the lithium-ion battery.
[0054] In one embodiment of the present application, the orthographic projection of the geometric center of the positive electrode diaphragm 102 on the separator substrate 101 coincides with the orthographic projection of the geometric center of the negative electrode diaphragm 103 on the separator substrate 101 at point O, and the length from the geometric center to the outer edge of the positive electrode diaphragm 102 in the divergent direction is L1, that is, the distance from the geometric center to the outer edge of the positive electrode diaphragm 102 is L1; along the same divergent direction, the length from the outer edge of the positive electrode diaphragm to the outer edge of the insulating layer is D, and the length from the geometric center to the outer edge of the negative electrode diaphragm is L2, that is, the distance from the geometric center to the outer edge of the negative electrode diaphragm 103 is L2, satisfying the following geometric relationship:
[0055] L1 <L2,L1+D≥L2。
[0056] It is understandable that when describing the relationship between L1, L2, and D, the same divergence direction may mean divergence along the long sides of the positive and negative electrode membranes at the same time, or divergence along the short sides of the positive and negative electrode membranes at the same time. For the convenience of description, the direction of divergence along the long sides of the positive and negative electrode membranes is defined as the X direction, and the direction of divergence along the short sides of the positive and negative electrode membranes is defined as the Y direction. Accordingly, Dx and Dy are used to distinguish D along different divergence directions respectively;
[0057] use Distinguish L1 along different divergent directions;
[0058] use L2 along different divergent directions are distinguished, wherein Lx1 is the length of the positive electrode membrane, Ly1 is the width of the positive electrode membrane, Lx2 is the length of the negative electrode membrane, and Ly2 is the width of the negative electrode membrane.
[0059] In one embodiment of the present application, when 0 mm ≤ L1 + D - L2 ≤ 4.5 mm, preferably 1 mm ≤ L1 + D - L2 ≤ 2.5 mm, the performance of the lithium ion battery is better.
[0060] In one embodiment of the present application, when 0.5 mm ≤ D ≤ 5 mm, preferably 1.5 mm ≤ D ≤ 3 mm, the performance of the lithium ion battery is better.
[0061] In one embodiment of the present application, Figure 2-3 As shown, the positive electrode membrane 102 and the negative electrode membrane 103 are rectangular in shape, and the orthographic projection of the geometric center of the positive electrode membrane 102 on the separator substrate 101 coincides with the orthographic projection of the geometric center of the negative electrode membrane 103 on the separator substrate 101 at point O.
[0062] A rectangular coordinate system can be established in the length direction and width direction of the separator, wherein the X direction represents the length direction of the separator and the Y direction represents the width direction of the separator. Then, the positive electrode membrane 102, the negative electrode membrane 103, and the insulating layer 104 satisfy the following geometric relationship:
[0063]
[0064] Among them, Lx1 is the length of the positive electrode diaphragm 102, Ly1 is the width of the positive electrode diaphragm 102, Lx2 is the length of the negative electrode diaphragm 103, Ly2 is the width of the negative electrode diaphragm 103, Dx is the width of the portion of the insulating layer 104 extending along the long side direction of the positive electrode diaphragm 102, and Dy is the width of the portion of the insulating layer 104 extending along the short side direction of the positive electrode diaphragm 102.
[0065] The inventors found that when the positive electrode diaphragm 102, the negative electrode diaphragm 103 and the insulating layer 104 satisfy the above-mentioned geometric relationship, the compaction density of the AC Overhang area on the negative electrode diaphragm 103 side can be made consistent with that of the electrode area, thereby, on the one hand, eliminating the local lithium precipitation phenomenon in the low compaction density area caused by the inconsistent compaction density of the electrode area, and on the other hand, reducing the occurrence of folding and breakage of the separator edge, thereby reducing the self-discharge rate and safety of the lithium-ion battery.
[0066] In one embodiment of the present application, Figure 2 As shown, the portion of the insulating layer 104 extending along the long side direction of the positive electrode diaphragm 102 includes a first portion 1 and a second portion 2, and the portion of the insulating layer 104 extending along the short side direction of the positive electrode diaphragm 102 includes a third portion 3 and a fourth portion 4. The width Dx of the first portion 1 and the second portion 2 may be the same or different; the width Dy of the third portion 3 and the fourth portion 4 may be the same or different, as long as the purpose of the invention of this application can be achieved.
[0067] The present application has no special restrictions on the separator substrate 101, as long as the purpose of the invention of the present application can be achieved. For example, the separator substrate 101 may include a polymer material layer, and the two sides of the polymer material layer may be plated with different metals to form a metal layer, such as a first metal M, including at least one of Cu, Ni, Ti, Ag, Au, Pt, stainless steel or its alloy, and the other side is plated with a second metal N, including at least one of Al, Ni, Ti, Ag, Au, Pt, stainless steel or its alloy, for carrying different active materials respectively. Conductive materials such as graphite, conductive carbon fiber, etc. may be added to the polymer material layer, so that the polymer material layer is electronically conductive and ionically insulated. The first metal M and the second metal N may be the same or different, but should be compatible with the active material coated on its surface and have corresponding anti-oxidation or anti-reduction properties. In addition, the present application has no particular limitation on the thickness of the separator substrate 101. For example, the thickness of the polymer material layer may be 5 μm to 500 μm, the thickness of the first metal M may be 0.95 μm to 800 μm, and the thickness of the second metal N may be 0.95 μm to 200 μm.
[0068] Alternatively, the separator substrate 101 may also be a metal plate, the metal plate may include at least one of Ni, Ti, Ag, Au, Pt, and stainless steel, and the thickness of the metal plate may be 10 μm to 200 μm.
[0069] Furthermore, the present application has no particular limitation on the polymer material used for the polymer material layer, as long as the purpose of the invention of the present application can be achieved. For example, the polymer material layer may include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyetheretherketone, polyimide, polyamide, polyethylene glycol, polyamideimide, polycarbonate, cyclic polyolefin, polyphenylene sulfide, polyvinyl acetate, polytetrafluoroethylene, polymethylene naphthalene, polyvinylidene fluoride, polyethylene naphthalate, polypropylene carbonate, poly(vinylidene fluoride-hexafluoropropylene), poly(vinylidene fluoride-co-chlorotrifluoroethylene), silicone resin, vinylon, polypropylene, polyethylene, polyvinyl chloride, polystyrene, polyether nitrile, polyurethane, polyphenylene ether, polysulfone or at least one of the derivatives of the above substances.
[0070] In the present application, the positive electrode membrane 102 may contain positive electrode active materials, and the negative electrode membrane 103 may contain negative electrode active materials. Alternatively, the positive electrode membrane 102 may be formed by directly coating the positive electrode active materials on the separator substrate 101, and the negative electrode membrane 103 may be formed by directly coating the negative electrode active materials on the separator substrate 101.
[0071] In one embodiment of the present application, the electronic resistivity of the insulating layer 104 is greater than 107 Ω·m, preferably greater than 10 10 Ω·m, without being limited to any theory, when the electronic resistivity of the insulating layer 104 is larger, the insulating performance of the insulating layer 104 is better.
[0072] In one embodiment of the present application, when Lithium-ion batteries perform better.
[0073] In one embodiment of the present application, further, when Lithium-ion batteries perform better.
[0074] In one embodiment of the present application, since the insulating material in the insulating layer 104 itself does not participate in the electrochemical reaction, by making 0.5mm≤Dx≤5mm, 0.5mm≤Dy≤5mm, the width of the insulating layer in the X direction and the Y direction are controlled respectively, thereby controlling the amount of insulating material added. While achieving the purpose of the invention of the present application, too much inactive material will not be introduced into the lithium-ion battery, thereby achieving the effect of improving the energy density of the lithium-ion battery.
[0075] In one embodiment of the present application, Dx is preferably: 1.5 mm ≤ Dx ≤ 3 mm; Dy is preferably: 1.5 mm ≤ Dy ≤ 3 mm, which can further improve the performance of the lithium-ion battery.
[0076] The present application has no particular limitation on the thickness of the insulating layer 104, as long as the purpose of the invention of the present application is achieved. For example, the thickness of the insulating layer 104 can be set according to the thickness of the positive electrode diaphragm 102, so that the thickness of the insulating layer 104 and the positive electrode diaphragm 102 can be kept consistent after cold pressing, so that the compaction density of the AC Overhang area and the electrode area of the negative electrode diaphragm 103 on the opposite side can be more consistent after cold pressing.
[0077] Furthermore, the present application has no particular restrictions on the insulating material used for the insulating layer 104, as long as the purpose of the invention of the present application is achieved. For example, the insulating layer may include at least one of HfO2, SrTiO3, SnO2, CeO2, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, boehmite, magnesium hydroxide, and aluminum hydroxide, or a material having the ability to conduct lithium ions, such as lithium phosphate (Li3PO4), lithium titanium phosphate, lithium aluminum titanium phosphate, lithium lanthanum titanate, lithium germanium thiophosphate, lithium nitride, SiS2 glass, P2S5 glass, Li2O, LiF, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2 ceramics or garnet ceramics.
[0078] Among them, the general formula of lithium titanium phosphate can be (Li x Ti y (PO4)3, where 0 < x < 2 and 0 < y < 3;
[0079] The general formula of lithium aluminum titanium phosphate can be (Li x Al y Ti z (PO4)3, where 0 < x < 2, 0 < y < 1, and 0 < z < 3;
[0080] The general formula of lithium lanthanum titanate can be Li x La y TiO3, where 0 < x < 2 and 0 < y < 3;
[0081] The general formula of lithium germanium thiophosphate can be Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1, and 0 < w < 5;
[0082] The general formula of lithium nitride can be Li x N y , where 0 < x < 4, and 0 < y < 2;
[0083] The general formula of SiS2 glass can be Li x Si y S z , where 0 ≤ x < 3, 0 < y < 2, and 0 < z < 4;
[0084] The general formula of P2S5 glass can be Li x P y S z , where 0 ≤ x < 3, 0 < y < 3, and 0 < z < 7;
[0085] The general formula of lithium germanium phosphorus sulfur ceramic can be Li2O - Al2O3 - SiO2 - P2O5 - TiO2 - GeO2;
[0086] The general formula of garnet ceramic is Li3 + xLa3M2O 12 , where 0 ≤ x ≤ 5, and M includes at least one of Te, Nb, or Zr.
[0087] In one embodiment of the present application, such as Figure 1 and Figure 2As shown, the partition may further include a sealing layer 105, which is located around the partition to improve the packaging effect. The distance between the insulating layer 104 and the sealing layer 105 is D3, 0≤D3≤20mm, preferably 2≤D3≤5mm, which can make the lithium-ion battery have a better sealing effect, reduce the self-discharge rate of the lithium-ion battery, and thus improve the self-discharge performance of the lithium-ion battery.
[0088] The present application has no particular limitation on the material used for the sealing layer 105 as long as the purpose of the invention of the present application can be achieved. For example, the sealing layer 105 may include at least one of polypropylene, polyester plastic or para-hydroxybenzaldehyde (PHBA).
[0089] In one embodiment of the present application, the insulating layer 104 includes ceramic particles, and the ceramic particles have excellent insulating properties, wherein the average particle size of the ceramic particles is 10nm to 20μm, preferably 100nm to 10μm; the porosity of the insulating layer is 10% to 60%, preferably 20% to 40%; the average pore size of the insulating layer is 20nm to 50μm, preferably 200nm to 20μm.
[0090] In one embodiment of the present application, the insulating layer also includes an adhesive, which can make the insulating ceramic particles in the insulating layer more firmly connected and reduce the powder loss of the insulating layer during cold pressing. The adhesive usually accounts for 5% to 40% of the mass of the insulating layer, ensuring that the insulating layer has good insulating and mechanical properties.
[0091] The present application has no particular limitation on the adhesive, as long as the purpose of the invention of the present application can be achieved. For example, the adhesive may include at least one of polyamide, polyurethane, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, acrylate, polyvinylidene fluoride or polyvinylidene fluoride-hexafluoropropylene copolymer.
[0092] The present application has no particular limitation on the preparation method of the insulating layer, as long as the purpose of the invention of the present application can be achieved. For example, it can be achieved by various methods such as slurry coating, glue coating, 3D printing, etc.
[0093] The present application provides a separator, which is provided with an insulating layer on the outer side of a positive electrode diaphragm, and the area surrounded by the orthographic projection of the outer edge of the insulating layer on the separator substrate covers the orthographic projection of the negative electrode diaphragm on the separator substrate. After the separator is cold pressed, the AC Overhang area on the negative electrode diaphragm side is consistent with the compaction density of the electrode area. On the one hand, the local lithium precipitation phenomenon in the low compaction density area caused by inconsistent compaction density is eliminated, and on the other hand, the occurrence of folding and damage of the separator edge is reduced. When it is used as a electrode, the self-discharge performance and safety of the electrochemical device are improved.
[0094] The present application also provides an electrochemical device, which includes at least one separator as described in any of the above embodiments of the present application.
[0095] In one embodiment of the present application, the electrochemical device includes at least two electrode assemblies, wherein the separator is sealed and connected to the outer package, and independent sealed chambers are formed on both sides of the separator, each of which contains an electrode assembly and an electrolyte to form an independent electrochemical unit. Active materials of opposite polarities are coated on both sides of the separator.
[0096] Figure 4 This is a schematic diagram of the structure of an electrochemical device in one embodiment of the present application, such as Figure 4 As shown, the separator separates the electrochemical device into two electrode assemblies, namely a first electrode assembly 300 and a second electrode assembly 400. The first electrode assembly 300 is Figure 4 The second electrode assembly 400 includes a positive electrode sheet 301, a positive electrode active material layer 302, and a first separator 303 from bottom to top; Figure 4 The electrochemical device includes a negative electrode sheet 401, a negative electrode active material layer 402, and a second separator 403 from top to bottom. The negative electrode sheet 103 of the separator substrate 101 is adjacent to the positive electrode active material layer 302 of the first electrode assembly 300, and the positive electrode sheet 102 of the separator substrate 101 is adjacent to the negative electrode active material layer 402 of the second electrode assembly 400. In addition, the electrochemical device can also be sealed by the sealing layer 105, so that the electrochemical device forms two independent chamber structures, and the two chambers correspond to the first electrode assembly 300 and the second electrode assembly 400, respectively.
[0097] In one embodiment, two adjacent electrode assemblies may each lead out a tab, and the tabs of the two electrode assemblies have opposite polarities. For example, when the side of the separator adjacent to the first electrode assembly is a positive electrode membrane, and the side adjacent to the second electrode assembly is a negative electrode membrane, the first electrode assembly leads out a negative electrode tab, and the second electrode assembly leads out a positive electrode tab. At this time, the output voltage between the two tabs is the sum of the output voltages of the two electrochemical units.
[0098] In one embodiment, two adjacent electrode assemblies can each lead out two tabs. For example, when the side of the separator adjacent to the first electrode assembly is a positive electrode membrane and the side adjacent to the second electrode assembly is a negative electrode membrane, the positive tab of the first electrode assembly and the negative tab of the second electrode assembly are connected in series, the negative tab of the first electrode assembly and the positive tab of the second electrode assembly are output tabs, and the output voltage is the sum of the output voltages of the two electrochemical units. At this time, the separator acts as a bipolar pole piece, so that there is an internal series connection through the separator and an external series connection through the tabs between the two adjacent electrochemical units.
[0099] In one embodiment, when the separator is used as a bipolar pole piece, a pole ear can be led out from the separator to monitor the working state of the lithium-ion battery.
[0100] In one embodiment of the present application, the separator substrate of the separator may include a primer layer between the separator substrate and the positive electrode membrane or the negative electrode membrane, and the primer layer is used to improve the bonding performance between the separator substrate and the active material. The primer layer is usually obtained by coating a slurry formed by mixing conductive carbon black, styrene-butadiene rubber and deionized water on the separator substrate and drying it, and the primer layers on both sides of the separator substrate may be the same or different.
[0101] There is no particular limitation on the positive electrode sheet in the present application, as long as the purpose of the present application can be achieved. For example, the positive electrode sheet generally comprises a positive current collector and a positive active material. Among them, the positive current collector is not particularly limited, and can be any positive current collector known in the art, such as aluminum foil, aluminum alloy foil or composite current collector. The positive active material is not particularly limited, and can be any positive active material in the prior art, and the active material includes at least one of NCM811, NCM622, NCM523, NCM111, NCA, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium iron manganese phosphate or lithium titanate.
[0102] There is no particular limitation on the negative electrode plate in the present application, as long as the purpose of the present application can be achieved. For example, the negative electrode plate generally comprises a negative electrode current collector and a negative electrode active material layer. Among them, the negative electrode current collector is not particularly limited, and any negative electrode current collector known in the art can be used, such as copper foil, aluminum foil, aluminum alloy foil, and composite current collector. The negative electrode active material layer includes a negative electrode active material, and the negative electrode active material is not particularly limited, and any negative electrode active material known in the art can be used. For example, it can include at least one of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon, hard carbon, silicon, silicon carbon, lithium titanate, etc.
[0103] The electrolyte in the present application is not particularly limited, and any electrolyte known in the art can be used, for example, it can be any one of a gel state, a solid state and a liquid state. For example, a liquid electrolyte can include a lithium salt and a non-aqueous solvent.
[0104] The lithium salt is not particularly limited, and any lithium salt known in the art can be used, as long as the purpose of the present application can be achieved. For example, the lithium salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), bistrifluoromethanesulfonyl imide lithium LiN(CF3SO2)2 (LiTFSI), bis(fluorosulfonyl)imide lithium Li(N(SO2F)2)(LiFSI), lithium bis(oxalate borate) LiB(C2O4)2 (LiBOB) or lithium difluorooxalate borate LiBF2(C2O4) (LiDFOB). For example, the lithium salt may be selected from LiPF6.
[0105] The non-aqueous solvent is not particularly limited as long as the purpose of the present application can be achieved. For example, the non-aqueous solvent may include at least one of a carbonate compound, a carboxylate compound, an ether compound, a nitrile compound or other organic solvents.
[0106] For example, the carbonate compound may include at least one of diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate.
[0107] The separator in the present application is not particularly limited. For example, the separator includes a polymer or an inorganic substance formed of a material stable to the electrolyte of the present application.
[0108] For example, the diaphragm may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, a film or a composite film having a structure, and the material of the substrate layer may be selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Optionally, a polypropylene film, a polyethylene film, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric or a polypropylene-polyethylene-polypropylene composite film may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance.
[0109] For example, the inorganic layer includes inorganic particles and a binder, and the inorganic particles are not particularly limited, for example, they can be selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is not particularly limited, for example, it can be selected from one or more combinations of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene).
[0110] The present application provides an electrochemical device, in which the separator used is provided with an insulating layer on the outer side of the positive electrode diaphragm, and the area surrounded by the orthographic projection of the outer edge of the insulating layer on the separator substrate covers the orthographic projection of the negative electrode diaphragm on the separator substrate. After the separator is cold-pressed, the AC Overhang area on the negative electrode diaphragm side is consistent with the compaction density of the electrode area. On the one hand, the local lithium precipitation phenomenon in the low compaction density area caused by inconsistent compaction density is eliminated, and on the other hand, the occurrence of folding and damage of the separator edge is reduced. When it is used as a electrode, the self-discharge performance and safety of the electrochemical device are improved.
[0111] The present application also provides an electronic device, which includes the electrochemical device provided in the embodiments of the present application.
[0112] The electrode assembly of the present application is not particularly limited, and any electrode assembly of the prior art can be used as long as the purpose of the present application can be achieved, for example, a laminated electrode assembly or a wound electrode assembly can be used. The electrode assembly generally includes a positive electrode sheet, a negative electrode sheet and a separator.
[0113] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on weight.
[0114] Example 1
[0115] <Preparation of separator>
[0116] Preparation of insulating layer slurry: boehmite and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 95:5, and then dispersed in a mixed solvent consisting of DMF and acetone, and stirred evenly to obtain an insulating layer slurry with a solid content of 40%. The volume ratio of DMF and acetone in the mixed solvent was 7:3.
[0117] Prepare positive electrode slurry: Mix the positive electrode active material lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and PVDF in a weight ratio of 97.5:1.0:1.5, then add NMP as a solvent, prepare a slurry with a solid content of 75%, and stir evenly.
[0118] Preparation of negative electrode slurry: negative electrode active material graphite (Graphite), conductive carbon black (Super P), styrene-butadiene rubber (SBR) were mixed in a weight ratio of 96:1.5:2.5, and then deionized water was added as a solvent to prepare a slurry with a solid content of 70%, and stirred evenly.
[0119] Preparation of positive electrode membrane: A commercially available stainless steel separator substrate with a thickness of 20 μm was selected, and a layer of positive electrode slurry was first coated on one side of the stainless steel separator substrate, and dried at 90°C for 1 hour to obtain a positive electrode membrane, wherein the thickness of the positive electrode membrane was 110 μm, the length of the positive electrode membrane Lx1 was 40 mm, and the width of the positive electrode membrane Ly1 was 34 mm.
[0120] Preparation of insulating layer: a layer of insulating layer slurry was prepared around the positive electrode membrane using a glue coating machine and dried at 90°C for 1 hour to obtain an insulating layer with a thickness of 100 μm and a width Dx and Dy of 5 mm respectively;
[0121] Preparation of negative electrode membrane: A layer of negative electrode slurry is coated on the other side of the stainless steel separator substrate and dried at 110°C for 1 hour to obtain a negative electrode membrane, wherein the thickness of the negative electrode membrane is 130 μm, the length of the negative electrode membrane Lx2 is 46 mm, and the width of the negative electrode membrane Ly2 is 40 mm. and 2mm respectively.
[0122] Preparation of separator: The stainless steel separator substrate after double-sided coating was cold-pressed by a cold pressing roller to obtain a separator with a thickness of 230 μm.
[0123] <Preparation of negative electrode sheet>
[0124] The negative electrode active material graphite, conductive carbon black (Super P), and styrene-butadiene rubber (SBR) were mixed in a weight ratio of 96:1.5:2.5, and then deionized water was added as a solvent to prepare a slurry with a solid content of 70%, and stirred evenly. The slurry was evenly coated on one surface of a copper foil with a thickness of 10 μm, and dried at 110°C to obtain a negative electrode sheet with a single-sided negative electrode active material layer coated with a coating thickness of 150 μm, and then the above coating steps were repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a double-sided negative electrode active material layer coated. The negative electrode sheet was cut into a specification of 41 mm × 61 mm for standby use.
[0125] <Preparation of positive electrode sheet>
[0126] The positive electrode active materials lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and PVDF are mixed in a weight ratio of 97.5:1.0:1.5, and then NMP is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and dried at 90°C to obtain a positive electrode sheet with a coating thickness of 100μm, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 38mm×58mm for standby use.
[0127] <Preparation of Electrolyte>
[0128] In a dry argon atmosphere, organic solvents ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of 30:50:20, and then lithium hexafluorophosphate (LiPF6) is added to the organic solvent to dissolve and mix evenly to obtain an electrolyte, wherein the molar concentration of LiPF6 in the electrolyte is 1.15 mol / L.
[0129] <Preparation of Electrode Assembly>
[0130] <Preparation of First Electrode Assembly>
[0131] A polyethylene (PE) film with a thickness of 15 μm is selected as a separator, a positive electrode sheet is placed on each side of the negative electrode sheet, and a separator is placed between the positive electrode sheet and the negative electrode sheet to form a stack, and then the four corners of the entire stack structure are fixed to obtain a first electrode assembly. The first electrode assembly has two tabs, one positive electrode tab and one negative electrode tab.
[0132] <Preparation of Second Electrode Assembly>
[0133] The second electrode assembly is prepared by the same method as the first electrode assembly. The second electrode assembly also has two tabs, one positive tab and one negative tab.
[0134] <Assembly of Electrode Assembly>
[0135] Place the aluminum-plastic film with a thickness of 90 μm with the pit surface facing upward, put the first electrode assembly into the pit of the aluminum-plastic film, make the positive electrode sheet of the first electrode assembly face upward, and then place the negative electrode sheet of the separator downward on the first electrode assembly, make the positive electrode sheet of the first electrode assembly correspond to the negative electrode sheet of the separator, and press them to obtain the first assembly.
[0136] For the first assembly, the positive electrode film of its separator is facing upward, and the negative electrode sheet of the second electrode assembly is facing downward, and placed on the electrode sheet, so that the negative electrode sheet of the second electrode assembly corresponds to the positive electrode film of the separator, and then another aluminum-plastic film with a thickness of 90 μm is formed with a pit face downward and covers the second electrode assembly, and then the two aluminum-plastic films are heat-sealed by hot pressing, so that the first electrode assembly and the second electrode assembly are separated by the separator to obtain an assembled electrode assembly. The assembled electrode assembly has two independent chambers, wherein the first electrode assembly corresponds to the first chamber, and the second electrode assembly corresponds to the second chamber, and the positive and negative pole ears of the first electrode assembly and the second electrode assembly are both led out of the packaging bag.
[0137] <Electrode assembly injection packaging>
[0138] The electrolyte is injected into the two chambers of the assembled electrode assembly respectively and then packaged. At this time, the first electrode assembly becomes the first electrochemical unit, the second electrode assembly becomes the second electrochemical unit, and the positive electrode tab of the first electrochemical unit is connected in series with the negative electrode tab of the second electrochemical unit to obtain a series lithium-ion battery. There is no ion exchange between the two chambers of the series lithium-ion battery.
[0139] When charging and discharging the series-connected lithium-ion battery, the negative electrode tab of the first electrochemical unit and the positive electrode tab of the second electrochemical unit are connected. In addition, the series-connected tabs can be retained as voltage monitoring electrodes for the series-connected lithium-ion battery, or the series-connected tabs can be insulated and wrapped in the series-connected lithium-ion battery.
[0140] Example 2
[0141] In addition to the insulating layer, the electronic resistivity is 2.70×10 10 , except that Al2O3 is selected as the insulating ceramic material, the rest is the same as that of Example 1.
[0142] Example 3
[0143] In addition to the insulating layer, the electronic resistivity is 3.50×10 13Other than that, the rest is the same as Example 2.
[0144] Example 4
[0145] In addition to the insulating layer, the electronic resistivity is 3.60×10 13 , Dx and Dy are 2mm, and Except that they are 0 mm respectively, the rest are the same as those in Example 2.
[0146] Example 5
[0147] In addition to the insulating layer, the electronic resistivity is 3.30×10 13 , Dx and Dy are 0.5mm, and Except that they are 0 mm respectively, the rest are the same as those in Example 2.
[0148] Example 6
[0149] In addition to the insulating layer, the electronic resistivity is 3.40×10 13 , Dx and Dy are 2mm, and Except that they are 1 mm respectively, the rest is the same as in Example 2.
[0150] Example 7
[0151] In addition to the insulating layer, the electronic resistivity is 3.40×10 13 , and Except that they are 4.5 mm respectively, the rest are the same as in Example 2.
[0152] Example 8
[0153] In addition to the insulating layer, the electronic resistivity is 3.50×10 13 , Dx and Dy are 2mm, and Except that D1 and D2 are 1 mm respectively, the rest are the same as those in Example 2.
[0154] Example 9
[0155] In addition to the insulating layer, the electronic resistivity is 3.40×10 13 Except that D3 is 3 mm, the rest is the same as Example 8.
[0156] Example 10
[0157] In addition to the insulating layer, the electronic resistivity is 3.30×10 13 Except that D3 is 20 mm, the rest is the same as Example 8.
[0158] Embodiment 11
[0159] In addition to the insulating layer, the electronic resistivity is 5.70×10 9 , except that the insulating ceramic material is ZnO, the rest is the same as Example 9.
[0160] Example 12
[0161] In addition to the insulating layer, the electronic resistivity is 8.30×10 12 Except that the insulating ceramic material is Al2O3 and the adhesive is polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), the rest is the same as Example 11.
[0162] Example 13
[0163] The above process is the same as that of Example 9 except that the average particle size of the insulating ceramic particles is 15 μm and the average pore size of the insulating layer is 50 μm.
[0164] Embodiment 14
[0165] The same as Example 13 except that the porosity of the insulating layer is 30%.
[0166] Embodiment 15
[0167] In addition to the insulating layer, the electronic resistivity is 3.50×10 13 Except that the average particle size of the insulating ceramic particles is 5 μm and the average pore size of the insulating layer is 15 μm, the rest is the same as Example 14.
[0168] Comparative Example 1
[0169] <Preparation of negative electrode sheet>
[0170] The negative electrode active material graphite, conductive carbon black (Super P), and styrene-butadiene rubber (SBR) were mixed in a weight ratio of 96:1.5:2.5, and then deionized water was added as a solvent to prepare a slurry with a solid content of 70%, and stirred evenly. The slurry was evenly coated on one surface of a copper foil with a thickness of 10 μm, and dried at 110°C to obtain a negative electrode sheet with a single-sided negative electrode active material layer coated with a coating thickness of 150 μm, and then the above coating steps were repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a double-sided negative electrode active material layer coated. The negative electrode sheet was cut into a specification of 41 mm × 61 mm for standby use.
[0171] <Preparation of positive electrode sheet>
[0172] The positive electrode active materials lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and PVDF are mixed in a weight ratio of 97.5:1.0:1.5, and then NMP is added as a solvent to prepare a slurry with a solid content of 75%, and stirred evenly. The slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and dried at 90°C to obtain a positive electrode sheet with a coating thickness of 100μm, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet coated with a positive electrode active material layer on both sides. The positive electrode sheet is cut into a specification of 38mm×58mm for standby use.
[0173] <Preparation of Electrolyte>
[0174] In a dry argon atmosphere, organic solvents ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of 30:50:20, and then lithium hexafluorophosphate (LiPF6) is added to the organic solvent to dissolve and mix evenly to obtain an electrolyte, wherein the molar concentration of LiPF6 in the electrolyte is 1.15 mol / L.
[0175] <Preparation of electrochemical cell>
[0176] The negative electrode sheet and the positive electrode sheet are stacked together to form a laminate, and a polyethylene (PE) film with a thickness of 15 μm is selected as an isolation film between the positive and negative electrode sheets. The four corners of the entire laminate structure are then fixed with tape and placed in an aluminum-plastic film. After top and side sealing, electrolyte injection and packaging, an electrochemical unit is obtained.
[0177] At least two electrochemical units are prepared in the same manner, which are respectively used as the first electrochemical unit and the second electrochemical unit.
[0178] <Preparation of tandem lithium-ion batteries>
[0179] The negative electrode of the first electrochemical unit and the positive electrode of the second electrochemical unit are connected in series through a wire to obtain a series-connected lithium-ion battery.
[0180] Comparative Example 2
[0181] Except that the separator between the first electrode assembly and the second electrode assembly is a stainless steel foil separator, the rest is the same as Example 1. The thickness of the stainless steel foil is about 20 μm.
[0182] Comparative Example 3
[0183] Except that the separator does not contain an insulating layer, the rest is the same as Example 1.
[0184] <Performance Test>
[0185] The series-connected lithium-ion batteries prepared in each embodiment and each comparative example were tested using the following method:
[0186] 01C discharge energy density test:
[0187] First charge to 8.90V at 0.5C, then charge to 0.025C at a constant voltage, let stand for 5 minutes, then discharge to 6.0V at 0.1C, record its discharge capacity, and then calculate 01C discharge energy density according to the following formula: Energy density (Wh / kg) = discharge capacity (Wh) / electrochemical device weight (kg).
[0188] Cycle test:
[0189] The test temperature is 25°C. The battery is charged to 8.90V at a constant current of 0.5C and then charged to 0.025C at a constant voltage. After standing for 5 minutes, the battery is discharged to 6.0V at 0.5C. The capacity obtained in this step is taken as the initial capacity. After 50 cycles of 0.5C charge / 0.5C discharge, the ratio of the capacity of the lithium-ion battery to the initial capacity is calculated.
[0190] Drop test:
[0191] 1) Drop the lithium-ion battery sample freely from a height of 1.5 meters onto a smooth marble surface;
[0192] 2) Check the damage of the positive electrode edge separator of the lithium-ion battery after falling;
[0193] 3) Test 20 groups of samples and record the number of damaged samples.
[0194] Self-discharge performance test:
[0195] After testing the capacity of the lithium-ion battery, let it stand at room temperature for 48 hours, and measure its voltage as V1; after letting the lithium-ion battery stand for another 48 hours, measure its voltage V2; then the K value used to represent the self-discharge performance of the lithium-ion battery is calculated according to the following formula: K = (V1-V2) / 48, unit mV / h.
[0196] Table 1 Test parameters and corresponding experimental results of various embodiments and comparative examples
[0197]
[0198]
[0199] It can be seen from Examples 1 to 15 and Comparative Examples 1 to 2 that the discharge energy density of the lithium-ion battery having the bipolar separator of the present application is significantly improved.
[0200] It can be seen from Examples 1 to 15 and Comparative Example 3 that the cycle capacity retention rate of the lithium ion battery having the bipolar separator of the present application is improved.
[0201] It can be seen from Examples 1 to 15 and Comparative Example 3 that the lithium-ion battery having the bipolar separator of the present application is less likely to be damaged at the folded portion of the positive electrode edge separator after a drop test, thereby improving the safety of the lithium-ion battery.
[0202] It can be seen from Examples 1 to 15 and Comparative Examples 1 to 3 that the self-discharge of the lithium-ion battery having the bipolar separator of the present application is greatly improved.
[0203] It can be seen from Examples 1 to 3 that the cycle capacity retention rate of the lithium-ion battery increases with the increase of the electronic resistivity of the insulating layer, and the self-discharge condition improves with the increase of the electronic resistivity of the insulating layer.
[0204] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. An electrochemical device, comprising a separator, a first laminated electrode assembly, a second laminated electrode assembly and an outer package, wherein the separator is sealed and connected to the outer package, and a first sealed chamber and a second sealed chamber are formed on both sides of the separator, respectively, wherein the first sealed chamber contains the first laminated electrode assembly and an electrolyte, and the second sealed chamber contains the second laminated electrode assembly and an electrolyte; the separator comprises a separator substrate, a positive electrode membrane, a negative electrode membrane and an insulating layer; in, The positive electrode membrane and the negative electrode membrane are respectively located on two sides of the separator substrate; The insulating layer is arranged on the separator substrate, and the insulating layer is arranged on the periphery of the positive electrode membrane; The area surrounded by the orthographic projection of the outer edge of the insulating layer on the separator substrate covers the orthographic projection of the negative electrode membrane on the separator substrate; The positive electrode sheet of the first stacked-sheet electrode assembly is adjacent to the negative electrode sheet of the separator, and the negative electrode sheet of the second stacked-sheet electrode assembly is adjacent to the positive electrode sheet of the separator; The positive electrode tab and the negative electrode tab of the first stacked electrode assembly are both led out of the outer package, and the positive electrode tab and the negative electrode tab of the second stacked electrode assembly are both led out of the outer package; The positive electrode tab of the first stacked electrode assembly is connected in series with the negative electrode tab of the second stacked electrode assembly; There is a negative electrode diaphragm region on the other side of the separator substrate directly opposite to the positive electrode diaphragm region; there is at least partially a negative electrode diaphragm region on the other side of the separator substrate directly opposite to the insulating layer region; the positive electrode diaphragm geometric center projection on the separator substrate coincides with the negative electrode diaphragm geometric center projection on the separator substrate, and the length from the geometric center to the outer edge of the positive electrode diaphragm in the divergent direction is L1; along the same divergent direction, the length from the outer edge of the positive electrode diaphragm to the outer edge of the insulating layer is D, and the length from the geometric center to the outer edge of the negative electrode diaphragm is L2, satisfying the following geometric relationship: L1 <L2,L1+D≥L2,0.5mm≤D≤5mm; The partition further includes a sealing layer, and the sealing layer is located around the partition. The distance between the insulating layer and the sealing layer is D3, 0mm≤D3≤20mm.
2. The electrochemical device according to claim 1, wherein: The positive electrode membrane and the negative electrode membrane are rectangular in shape, and the positive electrode membrane, the negative electrode membrane, and the insulating layer satisfy the following geometric relationship: Lx1 <Lx2,Ly1<Ly2, Among them, Lx1 is the length of the positive electrode diaphragm, Ly1 is the width of the positive electrode diaphragm, Lx2 is the length of the negative electrode diaphragm, Ly2 is the width of the negative electrode diaphragm, Dx is the width of the insulating layer extending along the long side direction of the positive electrode diaphragm, and Dy is the width of the insulating layer extending along the short side direction of the positive electrode diaphragm.
3. The electrochemical device according to claim 1, wherein The electronic resistivity of the insulating layer is greater than 10 7 Ω·m.
4. The electrochemical device according to claim 1, wherein 0mm≤L1+D-L2≤4.5mm.
5. The electrochemical device according to claim 1, wherein The separator meets at least one of the following characteristics: (a) The electronic resistivity of the insulating layer is greater than 10 10 Ω·m; (b) 1mm≤L1+D-L2≤2.5mm; (c)1.5mm≤D≤3mm.
6. The electrochemical device according to claim 1, wherein 2mm≤D3≤5mm.
7. The electrochemical device according to claim 1, wherein: The insulating layer comprises ceramic particles, the average particle size of the ceramic particles is 10 nm to 20 μm, the porosity of the insulating layer is 10% to 60%, and the average pore size of the insulating layer is 20 nm to 50 μm.
8. The electrochemical device according to claim 7, wherein: The insulating layer satisfies at least one of the following characteristics: (a) the average particle size of the ceramic particles is 100 nm to 10 μm; (b) the porosity of the insulating layer is 20% to 40%; (c) The average pore size of the insulating layer is 200 nm to 20 μm.
9. The electrochemical device according to claim 1, wherein: The insulating layer also includes an adhesive, and the adhesive accounts for 5% to 40% of the mass of the insulating layer.
10. The electrochemical device according to claim 9, wherein: The adhesive includes at least one of polyamide, polyurethane, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, acrylate, polyvinylidene fluoride or polyvinylidene fluoride-hexafluoropropylene copolymer.
11. The electrochemical device according to claim 1, wherein the insulating layer comprises at least one of HfO2, SrTiO3, SnO2, CeO2, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, boehmite, magnesium hydroxide, aluminum hydroxide, lithium phosphate, lithium titanium phosphate, lithium aluminum titanium phosphate, lithium lanthanum titanate, lithium germanium thiophosphate, lithium nitride, SiS2 glass, P2S5 glass, Li2O, LiF, LiOH, Li2CO3, LiAlO2, lithium germanium phosphosulfur ceramics or garnet ceramics.
12. An electronic device comprising the electrochemical device according to any one of claims 1 to 11.