A secondary battery

By using polyethylene glycol additives modified with phosphorus-containing groups in secondary batteries, a stable solid-state interface film is formed, which solves the problem of unstable interface films of secondary batteries under high temperature conditions and improves the cycle life and high temperature of the battery. performance.

CN114094182BActive Publication Date: 2024-10-18ZHUHAI COSMX BATTERY CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202111295014.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-03
Publication Date
2024-10-18
Estimated Expiration
2041-11-03

AI Technical Summary

Technical Problem

Under high-temperature conditions in secondary batteries, the interface film on the surface of the positive and negative electrodes is unstable, resulting in rapid degradation of battery performance. It is difficult to effectively improve the stability and high-temperature performance of the solid interface film with existing technology.

Method used

Polyethylene glycol modified with phosphorus-containing groups is introduced as an additive in secondary batteries. By mixing with the negative electrode current collector and electrolyte, a stable solid-state interface film is formed to improve lithium ion conductivity and battery cycle performance.

Benefits of technology

It significantly reduces the increase in internal resistance during battery cycling, extends the cycle life, improves the high-temperature performance of the battery, and forms a solid interface film with higher conductivity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0003336228640000021
    Figure BDA0003336228640000021
  • Figure BDA0003336228640000041
    Figure BDA0003336228640000041
Patent Text Reader

Abstract

The present invention discloses a secondary battery, the secondary battery includes an additive, the additive includes polyethylene glycol modified by a phosphorus-containing group. The additive can form a film on the surface of the negative electrode, can effectively improve the negative electrode interface film components during the negative electrode cycle, reduce the degree of increase in internal resistance during the cycle, and improve the cycle life. The additive of the present invention can also participate in the film-forming reaction of the negative electrode, form a solid interface film of a certain molecular weight on the surface of the negative electrode, can improve the composition of the solid interface film on the surface of the negative electrode, increase the content of high molecular components in the solid interface film, improve the conduction of electrons and lithium ions inside the negative electrode sheet of the secondary battery, improve the lithium ion dynamics inside the negative electrode sheet, and improve the battery cycle performance. Compared with conventional solid interface films, the solid interface film formed by the present invention has higher lithium ion conductivity, higher molecular weight, and higher stability, which is mainly reflected in the secondary battery with lower battery internal resistance, longer cycle life and better high temperature performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a secondary battery containing additives. Background Art

[0002] Secondary batteries are currently widely used in energy storage, power tools and digital products, including water power, thermal power, wind power, solar power stations, power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. During the charging and discharging process of secondary batteries, an interface film will be formed on the surface of the positive and negative electrodes in the secondary battery, and the composition of the interface film will directly affect the battery performance.

[0003] As the application of secondary batteries expands, higher requirements are placed on the performance of secondary batteries, especially high-temperature performance. When the secondary battery is at high temperature, the interface film components on the positive and negative surfaces are unstable, which will cause the interface film components to continuously dissolve and generate, thereby causing the electrolyte to be continuously consumed, causing the battery's internal resistance to continue to increase and the battery's performance to decay rapidly. How to improve the stability of the solid-state interface film of secondary batteries and enhance the high-temperature performance of batteries is an important development direction for the industry. Summary of the invention

[0004] In order to improve the problem of poor stability of the interface film formed in the existing secondary battery, the present invention provides a secondary battery, in particular a secondary battery containing an additive, the addition of the additive can effectively improve the stability of the interface film in the secondary battery and enhance the cycle performance of the secondary battery.

[0005] The object of the present invention is achieved through the following technical solutions:

[0006] A secondary battery comprises an additive, wherein the additive comprises polyethylene glycol modified with a phosphorus-containing group.

[0007] Wherein, the phosphorus-containing group-modified polyethylene glycol is selected from at least one of the compounds shown in the following formula 1:

[0008]

[0009] In Formula 1, n is the degree of polymerization; R1 and R'1 are end-capping groups, and at least one of R1 and R'1 includes at least one phosphorus-containing functional group; and R and R' are connecting groups.

[0010] Wherein, in Formula 1, the phosphorus-containing functional group includes -PO4R2R3 -PR4R5 -(P=R6)R7R8 At least one of the following, wherein R2 to R8 are organic functional groups.

[0011] Wherein, the number average molecular weight of the compound represented by Formula 1 is 200 to 30,000.

[0012] Wherein, the compound represented by formula 1 is selected from phospholipid-polyethylene glycol-thiol, phospholipid-polyethylene glycol-hydroxyl, distearoyl phosphatidyl acetamide-polyethylene glycol-amine, active ester-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-maleimide, fluorescein-polyethylene glycol-phospholipid, distearoyl phosphatidylethanolamine-polyethylene glycol-N-hydroxysuccinimide, amino-polyethylene glycol-phospholipid, eight-arm polyethylene glycol-phospholipid, phospholipid-polyethylene glycol polylactic acid-glycolic acid copolymer, linear peptide RGD-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-octreotide, phospholipid-polyethylene glycol-mannose, distearoyl phosphatidylethanolamine-polyethylene glycol, four-arm polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-targeted transmembrane Peptide TAT, phospholipid-PEG-polycaprolactone, carboxyl-PEG-phospholipid, phospholipid-PEG-amino, silicon-PEG-phospholipid, methoxy-PEG-phospholipid, phospholipid-PEG-silicon, phospholipid-PEG-active ester, phospholipid-PEG-rhodamine B, phospholipid-PEG-cyclic peptide RGD, phospholipid-PEG-biotin, azide-PEG-phospholipid, phospholipid-PEG-carboxyl, phospholipid-PEG-CY5, peptide SP94-PEG-phospholipid, phospholipid-PEG-estrogen, four-arm PEG-distearic acid acylphosphatidylethanolamine, phospholipid-PEG-polyethylene glycol imine, phospholipid-PEG-phospholipid, phospholipid-PEG-substrate Amino tert-butyloxycarbonyl, phospholipid-polyethylene glycol-diphenylcyclooctyne, phospholipid-polyethylene glycol-polyaspartic acid benzyl ester, phospholipid-polyethylene glycol-folic acid, phospholipid-polyethylene glycol-polyglutamic acid, phospholipid-polyethylene glycol-cholesterol, phospholipid-polyethylene glycol-lactide-glycolide copolymer, phospholipid-polyethylene glycol-progesterone, indocyanine-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-biotin, six-arm polyethylene glycol-distearic acid acylphosphatidylethanolamine, polylysine-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-rhodamine B, phospholipid-polyethylene glycol-peptide, phospholipid-polyethylene glycol-triphenylphosphine, phospholipid-polyethylene glycol-polyaspartic acid, dimerized trimethylene carbonate-polyethylene glycol, methotrexate-polyethylene glycol At least one of alcohol-distearoylphosphatidylethanolamine, triphenyl phosphate-polyethylene glycol-distearoylphosphatidylethanolamine, galactose-polyethylene glycol-phospholipids, acrylate-polyethylene glycol-phospholipids, acrylamide-polyethylene glycol-phospholipids, dansylamide-polyethylene glycol-phospholipids, cholesterol-polyethylene glycol-phospholipids, p-toluenesulfonate-polyethylene glycol-phospholipids, dopamine-polyethylene glycol-phospholipids, dimercaptopyridine-polyethylene glycol-phospholipids, mannose-polyethylene glycol-phospholipids, alkynyl-polyethylene glycol-phospholipids, cyclooctyne-polyethylene glycol-phospholipids, epoxy-polyethylene glycol-phospholipids, methacrylate-polyethylene glycol-phospholipids, nitrophenyl carbonate-polyethylene glycol-phospholipids, and lipoic acid-polyethylene glycol-phospholipids.

[0013] Wherein, the secondary battery comprises a negative electrode sheet, and the negative electrode sheet comprises the additive.

[0014] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector, and the negative electrode active material layer comprises a negative electrode active material, a conductive agent, a binder and the above-mentioned additives.

[0015] Wherein, the secondary battery comprises an electrolyte, and the electrolyte comprises the additive.

[0016] Wherein, the electrolyte includes a non-aqueous organic solvent, a lithium salt and the above-mentioned additives.

[0017] Wherein, the content of the additive accounts for 0.01-5wt% of the total mass of the electrolyte.

[0018] Beneficial effects of the present invention:

[0019] The present invention provides a secondary battery, in particular a secondary battery containing an additive, wherein the additive (at least one of the compounds shown in Formula 1) can be fully mixed with other components during the preparation process of the negative electrode sheet of the secondary battery and / or during the preparation process of the electrolyte due to its small molecular weight and short polymer chain segment, and the additive is in a viscous liquid, semi-solid or solid state at room temperature, and it can fully contact each component and immerse in the internal pores of the negative electrode sheet. The additive of the present invention can form a film on the surface of the negative electrode, can effectively improve the negative electrode interface film components during the negative electrode cycle process, reduce the degree of increase in internal resistance during the cycle process, and improve the cycle life. The additive of the present invention can also participate in the film-forming reaction of the negative electrode, form a solid interface film of a certain molecular weight on the surface of the negative electrode, can improve the composition of the solid interface film on the surface of the negative electrode, increase the content of the polymer component in the solid interface film, improve the conduction of electrons and lithium ions inside the negative electrode sheet of the secondary battery, improve the lithium ion dynamics inside the negative electrode sheet, and improve the battery cycle performance. Compared with conventional solid interface films, the solid interface film formed by the present invention has higher lithium ion conductivity, higher molecular weight, and higher stability, which is mainly reflected in secondary batteries as lower battery internal resistance, longer cycle life, and better high-temperature performance. DETAILED DESCRIPTION

[0020] <Additives>

[0021] As mentioned above, the present invention provides a secondary battery, wherein the secondary battery comprises an additive, wherein the additive comprises polyethylene glycol modified with a phosphorus-containing group.

[0022] In one embodiment of the present invention, the phosphorus-containing group-modified polyethylene glycol is selected from at least one of the compounds shown in the following formula 1:

[0023]

[0024] In Formula 1, n is the degree of polymerization; R1 and R'1 are end-capping groups, and at least one of R1 and R'1 includes at least one phosphorus-containing functional group; and R and R' are connecting groups.

[0025] In one embodiment of the present invention, in Formula 1, the phosphorus-containing functional group includes -PO4R2R3 -PR4R5 -(P=R6)R7R8 At least one of the following, wherein R2 to R8 are organic functional groups.

[0026] In one embodiment of the present invention, in Formula 1, n is an integer between 2 and 680.

[0027] In one embodiment of the present invention, in Formula 1, the linking group may or may not be present. If present, R and R' are organic functional groups.

[0028] In one embodiment of the present invention, the number average molecular weight of the compound represented by Formula 1 is 200 to 30,000, preferably 300 to 10,000.

[0029] The phosphorus-containing functional group of the present invention can undergo electrochemical polymerization under low potential conditions to form a stable interface film on the negative electrode surface, effectively reducing the occurrence of side reactions on the negative electrode surface, reducing the increase in internal resistance during battery cycling, and improving battery cycling performance.

[0030] In one embodiment of the present invention, the compound represented by formula 1 is selected from phospholipid-polyethylene glycol-thiol, phospholipid-polyethylene glycol-hydroxyl, distearoyl phosphatidyl acetamide-polyethylene glycol-amine, active ester-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-maleimide, fluorescein-polyethylene glycol-phospholipid, distearoyl phosphatidylethanolamine-polyethylene glycol-N-hydroxysuccinimide, amino-polyethylene glycol-phospholipid, eight-arm polyethylene glycol-phospholipid, phospholipid-polyethylene glycol polylactic acid-glycolic acid copolymer, linear peptide RGD-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-octreotide, phospholipid-polyethylene glycol-mannose, distearoyl phosphatidylethanolamine-polyethylene glycol, four-arm polyethylene glycol-phospholipid, phospholipid-polyethylene glycol Alcohol-targeted cell-penetrating peptide TAT, phospholipid-PEG-polycaprolactone, carboxyl-PEG-phospholipid, phospholipid-PEG-amino, silicon-PEG-phospholipid, methoxy-PEG-phospholipid, phospholipid-PEG-silicon, phospholipid-PEG-active ester, phospholipid-PEG-rhodamine B, phospholipid-PEG-cyclic peptide RGD, phospholipid-PEG-biotin, azide-PEG-phospholipid, phospholipid-PEG-carboxyl, phospholipid-PEG-CY5, peptide SP94-PEG-phospholipid, phospholipid-PEG-estrogen, four-arm PEG-distearic acid acyl phosphatidylethanolamine, phospholipid-PEG-polyethylene glycol-polyethylene imine, phospholipid-PEG-phospholipid, phospholipid-PEG-ethylene glycol diol-imino tert-butyloxycarbonyl, phospholipid-polyethylene glycol-diphenylcyclooctyne, phospholipid-polyethylene glycol-polyaspartic acid benzyl ester, phospholipid-polyethylene glycol-folic acid, phospholipid-polyethylene glycol-polyglutamic acid, phospholipid-polyethylene glycol-cholesterol, phospholipid-polyethylene glycol-lactide-glycolide copolymer, phospholipid-polyethylene glycol-progesterone, indocyanine-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-biotin, six-arm polyethylene glycol-distearic acid acyl phosphatidylethanolamine, polylysine-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-rhodamine B, phospholipid-polyethylene glycol-peptide, phospholipid-polyethylene glycol-triphenylphosphine, phospholipid-polyethylene glycol-polyaspartic acid, dimer trimethylene carbonate-polyethylene glycol, methotrexate-poly At least one of ethylene glycol-distearoylphosphatidylethanolamine, triphenyl phosphate-polyethylene glycol-distearoylphosphatidylethanolamine, galactose-polyethylene glycol-phospholipids, acrylate-polyethylene glycol-phospholipids, acrylamide-polyethylene glycol-phospholipids, dansylamide-polyethylene glycol-phospholipids, cholesterol-polyethylene glycol-phospholipids, p-toluenesulfonate-polyethylene glycol-phospholipids, dopamine-polyethylene glycol-phospholipids, dimercaptopyridine-polyethylene glycol-phospholipids, mannose-polyethylene glycol-phospholipids, alkynyl-polyethylene glycol-phospholipids, cyclooctyne-polyethylene glycol-phospholipids, epoxy-polyethylene glycol-phospholipids, methacrylate-polyethylene glycol-phospholipids, nitrophenyl carbonate-polyethylene glycol-phospholipids, and lipoic acid-polyethylene glycol-phospholipids.

[0031] In the present invention, the phosphorus-containing group-modified polyethylene glycol can be prepared by conventional methods in the art, or purchased through commercial channels.

[0032] <Negative electrode>

[0033] In one embodiment of the present invention, the secondary battery includes a negative electrode sheet, and the negative electrode sheet includes the above-mentioned additive.

[0034] Specifically, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector, and the negative electrode active material layer includes a negative electrode active material, a conductive agent, a binder and the above-mentioned additives.

[0035] At this time, the phosphorus-containing functional groups in the additive represented by Formula 1 of the present invention undergo electrochemical polymerization under low potential conditions to form a stable solid interface film on the negative electrode surface, effectively reducing side reactions on the negative electrode surface, reducing the increase in internal resistance during battery cycling, and improving battery cycling performance.

[0036] In one embodiment of the present invention, the negative electrode active material layer includes the following components in percentage by weight: 75-98.5 wt % of negative electrode active material, 0.5-15 wt % of conductive agent, 0.999-8 wt % of binder, and 0.001-2 wt % of additives.

[0037] Exemplarily, the mass percentage of the negative electrode active material content of the total mass of the negative electrode active material layer is 75wt%, 76wt%, 77wt%, 78wt%, 79wt%, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%, 95wt%, 96wt%, 97wt% or 98.5wt%.

[0038] Exemplarily, the content of the conductive agent is 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt% of the total mass of the negative electrode active material layer.

[0039] Exemplarily, the mass percentage of the additive in the total mass of the negative electrode active material layer is 0.001 wt%, 0.05 wt%, 0.1 wt%, 0.15 wt%, 0.25 wt%, 0.55 wt%, 0.65 wt%, 0.70 wt%, 0.75 wt%, 0.85 wt%, 0.90 wt%, 1.0 wt%, 1.2 wt%, 1.5 wt% or 2 wt%. When the content of the additive is greater than 2 wt%, the content of the additive is too high, which will cause the additive to aggregate on the surface of the negative electrode active material, resulting in low capacity of the electrode sheet and poor lithium-ion conduction network inside the electrode sheet, affecting the battery performance and not meeting the application conditions; when the content of the additive is less than 0.001 wt%, the content of the additive is too low, the film-forming property is poor, and the structure of the solid electrolyte interphase film formed on the surface of the negative electrode is unstable, reducing the battery performance.

[0040] Exemplarily, the mass percentage of the binder in the total mass of the negative electrode active material layer is 0.999 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt% or 8 wt%.

[0041] In one aspect of the present invention, the negative electrode active material is selected from silicon-based materials and / or carbon-based materials and / or other negative electrode materials.

[0042] Among them, the carbon-based material is selected from at least one of artificial graphite, natural graphite, hard carbon, soft carbon, mesophase microspheres, fullerenes, and graphene.

[0043] Among them, the silicon-based material is selected from at least one of nano-silicon, SiOx (0 < x < 2), aluminum-silicon alloy, magnesium-silicon alloy, boron-silicon alloy, phosphorus-silicon alloy, and lithium-silicon alloy.

[0044] Among them, the other negative electrode materials are selected from at least one of lithium metal, boron and its derivatives (such as boron powder, boron oxide), aluminum and its derivatives (such as aluminum powder, lithium-aluminum alloy), magnesium and its derivatives (such as magnesium, magnesium-aluminum alloy), bismuth and its derivatives (such as bismuth, lithium-bismuth alloy), nickel and its derivatives (such as nickel, lithium-nickel alloy, nickel nitride lithium), silver and its derivatives (such as silver powder, lithium-silver alloy), zinc and its derivatives (such as zinc powder, zinc-lithium alloy, zinc nitride), titanium and its derivatives (such as titanium powder, lithium titanate, titanium dioxide, lithium-titanium alloy, etc.), gallium and its derivatives (such as gallium, lithium-gallium alloy), indium and its derivatives (such as indium powder, lithium-indium alloy), tin and its derivatives (such as tin powder, stannous oxide, tin oxide, tin sulfate), lithium nitride, and copper nitride.

[0045] In one aspect of the present invention, the conductive agent includes one or several of conductive carbon black, Ketjen black, conductive fiber, conductive polymer, acetylene black, carbon nanotube, graphene, flake graphite, conductive oxide, and metal particles.

[0046] In one embodiment of the present invention, the binder is selected from at least one of polyvinylidene fluoride and its copolymer derivatives, polytetrafluoroethylene and its copolymer derivatives, polyacrylic acid and its copolymer derivatives, polyvinyl alcohol and its copolymer derivatives, polystyrene-butadiene rubber and its copolymer derivatives, polyimide and its copolymer derivatives, polyethyleneimine and its copolymer derivatives, polyacrylate and its copolymer derivatives, and sodium carboxymethyl cellulose and its copolymer derivatives.

[0047] In one embodiment of the present invention, the single-sided surface density of the negative electrode sheet is 1 to 25 mg / cm 2 .

[0048] In one embodiment of the present invention, the thickness of the negative electrode active material layer (the thickness of the single-sided negative electrode active material layer after rolling) is 10μm to 150μm, preferably 30μm to 100μm, such as 10μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm or 150μm.

[0049] <Method for preparing negative electrode sheet>

[0050] The present invention also provides a method for preparing the negative electrode sheet, the method comprising the following steps:

[0051] The solvent, the negative electrode active material, the conductive agent, the binder and at least one compound represented by Formula 1 are uniformly mixed to prepare a negative electrode slurry; the negative electrode slurry is coated on the surface of the negative electrode current collector and dried to prepare the negative electrode sheet.

[0052] In one embodiment of the present invention, the negative electrode slurry contains 100-300 parts by mass of a solvent, 75-98.5 parts by mass of a negative electrode active material, 0.5-15 parts by mass of a conductive agent, 0.001-2 parts by mass of at least one compound represented by Formula 1, and 0.999-10 parts by mass of a binder.

[0053] In one embodiment of the present invention, the solvent is selected from at least one of water, acetonitrile, benzene, toluene, xylene, acetone, tetrahydrofuran, hydrofluoroether, and N-methylpyrrolidone.

[0054] In one embodiment of the present invention, the negative electrode slurry is preferably sieved, for example, sieved through a 200-mesh sieve.

[0055] In one embodiment of the present invention, the temperature of the drying treatment is 70 to 110° C., and the time of the drying treatment is 12 to 36 hours.

[0056] <Electrolyte>

[0057] In one embodiment of the present invention, the secondary battery includes an electrolyte, and the electrolyte includes the above-mentioned additive.

[0058] Specifically, the electrolyte includes a non-aqueous organic solvent, a lithium salt and the above-mentioned additives.

[0059] At this time, the phosphorus-containing functional groups in the additive represented by Formula 1 of the present invention undergo electrochemical polymerization under low potential conditions to form a stable solid interface film on the negative electrode surface, effectively reducing the occurrence of side reactions on the negative electrode surface, reducing the increase in internal resistance during battery cycling, and improving battery cycling performance.

[0060] In one embodiment of the present invention, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorooxalatoborate), lithium bis(fluorobis(oxalatophosphate), lithium tetrafluorooxalatophosphate, lithium difluorophosphate, lithium perchlorate, lithium bis(fluorosulfonamide), and lithium bis(trifluoromethylsulfonylimide).

[0061] In one embodiment of the present invention, the content of the lithium salt accounts for 10 to 20wt% of the total mass of the electrolyte, for example, 10wt%, 11wt%, 12wt%, 12.5wt%, 13wt%, 13.5wt%, 14wt%, 14.5wt%, 15wt%, 15.5wt%, 16wt%, 16.5wt%, 17wt%, 17.5wt%, 18wt%, 19wt% or 20wt%.

[0062] In one embodiment of the present invention, the non-aqueous organic solvent is selected from a mixture of at least one cyclic carbonate and at least one linear carbonate and linear carboxylic acid ester in any proportion.

[0063] Preferably, the cyclic carbonate is selected from at least one of ethylene carbonate and propylene carbonate, the linear carbonate is selected from at least one of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate, and the linear carboxylic acid ester is selected from at least one of ethyl propionate, propyl propionate and propyl acetate.

[0064] In one embodiment of the present invention, in the electrolyte, based on 100 wt% of the total mass, the mass fraction of the cyclic carbonate is 10-50 wt%, and the mass fraction of the linear carbonate and / or linear carboxylate is 50-90 wt%.

[0065] In one embodiment of the present invention, the content of the additive is 0.01-5wt% of the total mass of the electrolyte, for example, 0.1wt%, 0.15wt%, 0.25wt%, 0.55wt%, 0.65wt%, 0.70wt%, 0.75wt%, 0.85wt%, 0.90wt%, 1.0wt%, 1.2wt%, 1.5wt%, 2wt%, 3wt%, 4wt% or 5wt%; when the content of the additive is higher than 5wt%, the excess additive It will increase the viscosity of the electrolyte, resulting in poor wettability of the electrolyte. At the same time, a large amount of additives are complexed on the surface of the negative electrode, which will prevent lithium ions from being deintercalated from the negative electrode active material into the electrolyte. Therefore, it has a large impedance R solid interface, which can easily lead to a large impedance of the solid electrolyte membrane on the surface of the negative electrode, and there is a great resistance to the deintercalation of lithium ions at the negative electrode interface, resulting in rapid performance degradation; when the content of the additive is lower than 0.01wt%, the additive content is too little to form a stable solid interface film, resulting in rapid battery performance degradation.

[0066] <Method for preparing electrolyte solution>

[0067] The present invention also provides a method for preparing the above electrolyte, the method comprising the following steps:

[0068] The electrolyte is prepared by mixing a non-aqueous organic solvent, a lithium salt and the above-mentioned additives.

[0069] Exemplarily, the method comprises the following steps:

[0070] In an argon atmosphere glove box with a water content of <10 ppm, a non-aqueous organic solvent, a lithium salt and an additive are uniformly mixed in a certain mass ratio to obtain an electrolyte.

[0071] The present invention will be described in further detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0072] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0073] Example 1

[0074] 1) Preparation of positive electrode:

[0075] 95g of positive electrode active material lithium cobalt oxide, 2g of binder polyvinylidene fluoride (PVDF), 2g of conductive agent conductive carbon black, and 1g of conductive agent carbon nanotube are mixed, and 200g of N-methylpyrrolidone (NMP) is added, and stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 12μm; after drying at 100℃ for 36 hours, a vacuum treatment is performed to obtain a pole piece, and the pole piece is rolled and cut to obtain a positive electrode sheet;

[0076] 2) Preparation of negative electrode sheet:

[0077] 75g of silicon dioxide, 5g of conductive agent single-walled carbon nanotube (SWCNT), 10g of conductive agent conductive carbon black (SP), 2g of carboxyl polyethylene glycol phospholipid, 4g of binder sodium carboxymethyl cellulose (CMC), 4g of binder styrene butadiene rubber (SBR), and 300g of deionized water are prepared into a slurry by a wet process, and coated on the surface of the negative electrode current collector copper foil, and dried, rolled and die-cut to obtain a negative electrode sheet;

[0078] 3) Preparation of electrolyte:

[0079] In a glove box filled with argon gas and with a qualified water and oxygen content, ethylene carbonate, propylene carbonate, diethyl carbonate, and n-propyl propionate were mixed in a mass ratio of 20:10:15:55, and then 1 mol / L of fully dried lithium hexafluorophosphate (LiPF6) was quickly added thereto and stirred to prepare an electrolyte;

[0080] 4) Preparation of lithium-ion batteries

[0081] The positive electrode sheet and the negative electrode sheet obtained above are used to prepare a lithium-ion battery cell, and after liquid injection, packaging and welding, a lithium-ion battery is obtained.

[0082] Comparative Example 1.1

[0083] The specific process of Comparative Example 1.1 refers to Example 1, the main difference is that in Comparative Example 1.1, polyethylene glycol of the same mass and molecular weight as carboxyl polyethylene glycol phospholipid is added, and other conditions are consistent with Example 1.

[0084] Comparative Example 1.2

[0085] The specific process of Comparative Example 1.2 is referred to Example 1, the main difference is that no carboxyl polyethylene glycol phospholipid is added in Comparative Example 1.2, and other conditions are consistent with Example 1.

[0086] The specific processes of Examples 2-6 and other comparative examples refer to Example 1, with the main differences being the process conditions of the positive electrode sheet, the content of each component, and the type of material of each component. For specific details, see Tables 1 and 2.

[0087] Table 1 Composition of negative electrode sheets of embodiments and comparative examples

[0088]

[0089]

[0090] Table 2 Composition of negative electrode sheets of embodiments and comparative examples

[0091]

[0092]

[0093] The performance of the batteries prepared in the above examples and comparative examples was tested:

[0094] (1) Battery internal resistance AC impedance test method: The AC impedance test of 50% SOC lithium-ion battery was performed using Metrohm PGSTAT302N chemical workstation in the range of 100KHz-0.1mHz and 25°C. The test results are listed in Table 3.

[0095] Table 3 Battery internal resistance AC impedance test results of the embodiment and comparative example

[0096]

[0097] The internal resistance test results during the battery cycle show that the lithium-ion battery prepared by the embodiment of the present invention has a smaller internal resistance than the lithium-ion battery prepared by the comparative example when the battery is cycled 100 times, 300 times, 500 times, and 700 times. The main reason is that the additive in the present invention can form a solid interface film on the surface of the negative electrode. The solid interface film is different from the solid interface film on the surface of the conventional negative electrode and has the characteristics of high-speed lithium conduction. The formed interface film can quickly conduct lithium ions, so the lithium-ion battery prepared by it has a lower internal resistance during the cycle. The internal resistance of the lithium-ion battery increases slightly during the cycle, and it has certain application potential.

[0098] (2) Battery cycle performance test method: The lithium-ion battery was subjected to a charge and discharge cycle test on a blue battery charge and discharge test cabinet. The test conditions were 25°C and 0.5C / 0.5C charge and discharge. The test results are listed in Table 4.

[0099] Table 4 Battery cycle performance test results of the embodiments and comparative examples

[0100]

[0101] The test results of the cycle performance of the embodiments and the comparative examples show that the lithium ion battery prepared by the present invention has a higher capacity retention rate when the battery is cycled 100 times, 300 times, 500 times, and 700 times compared with the lithium ion battery prepared by the comparative example. The main reason is that the additive in the present invention can form a solid interface film on the surface of the negative electrode. The solid interface film is different from the solid interface film on the surface of the conventional negative electrode. The solid interface film prepared by the present invention has the characteristics of good stability and high-speed lithium conduction. The solid interface film on the surface of the conventional negative electrode is formed in the first battery cycle. As the lithium ions react at the negative electrode, the solid interface film is constantly dissolved and regenerated. In the solid interface film on the surface of the conventional negative electrode, some solid interface components will dissolve, and more new interfaces will be generated. The new interface consumes electrolyte and lithium salt, which will reduce the battery performance. In the present invention, due to the addition of additives, a more stable solid interface film with higher lithium conduction performance is formed on the surface of the negative electrode material, which can improve the battery cycle performance.

[0102] The test results of the cyclic charge and discharge performance of the embodiments and the comparative examples show that the battery of the present invention has a small internal resistance and a higher capacity retention rate during the cycle process.

[0103] Example 7

[0104] 1) Preparation of positive electrode:

[0105] 97g of positive electrode active material lithium cobalt oxide, 1g of binder polyvinylidene fluoride (PVDF), 1g of conductive agent conductive carbon black, and 1g of conductive agent carbon nanotube are mixed, and 150g of N-methylpyrrolidone (NMP) is added, and stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 12μm; after drying at 100℃ for 36 hours, a pole piece is obtained after vacuum treatment, and the pole piece is rolled and cut to obtain a positive electrode sheet;

[0106] 2) Preparation of negative electrode sheet:

[0107] 3g of silicon dioxide, 90g of graphite, 1g of conductive agent single-walled carbon nanotube (SWCNT), 2g of conductive agent conductive carbon black (SP), 2g of binder sodium carboxymethyl cellulose (CMC), 2g of binder styrene-butadiene rubber (SBR), and 200g of deionized water are prepared into a slurry by a wet process, and coated on the surface of the negative electrode current collector copper foil, and dried, rolled and die-cut to obtain a negative electrode sheet;

[0108] 3) Preparation of electrolyte:

[0109] In a glove box filled with argon gas and with a qualified water and oxygen content, 25 g of ethylene carbonate, 15 g of propylene carbonate, 10 g of diethyl carbonate, and 50 g of n-propyl propionate were mixed evenly according to a certain proportion, 0.1 g of phospholipid polyethylene glycol maleimide after sufficient drying was added and mixed evenly, and then 1.10 mol / L of fully dried lithium hexafluorophosphate (LiPF6) was quickly added thereto, and the electrolyte was prepared by stirring evenly;

[0110] 4) Preparation of lithium-ion batteries

[0111] The positive electrode sheet and the negative electrode sheet obtained above are used to prepare a lithium-ion battery cell, and after liquid injection, packaging and welding, a lithium-ion battery is obtained.

[0112] Comparative Example 7.1

[0113] The specific process of Comparative Example 7.1 refers to Example 7, the main difference is that in Comparative Example 7.1, polyethylene glycol maleimide of the same mass and molecular weight as the phospholipid polyethylene glycol maleimide is added, and other conditions are consistent with Example 7.

[0114] Comparative Example 7.2

[0115] The specific process of Comparative Example 7.2 refers to Example 7, the main difference is that phospholipid polyethylene glycol maleimide is not added in Comparative Example 7.2, and other conditions are consistent with Example 7.

[0116] The specific processes of Examples 8-12 and other comparative examples refer to Example 7, the main difference is the electrolyte formula, and the specific details are shown in Tables 5 and 6.

[0117] Table 5 Composition of the electrolyte of the embodiment and the comparative example

[0118]

[0119]

[0120] Table 6 Composition of electrolytes of Examples and Comparative Examples

[0121] Serial number additive Serial number additive Example 7 Phospholipid Polyethylene Glycol Maleimide Example 10 Azide-PEG-phospholipids Comparative Example 7.1 Polyethylene glycol maleimide Comparative Example 10.1 Polyethylene glycol azide Comparative Example 7.2 ----- Comparative Example 10.2 ---- Example 8 Methoxypolyethylene glycol phospholipids Embodiment 11 Pyridine-PEG-1,1-dithiocyanate Comparative Example 8.1 Methoxypolyethylene glycol Comparative Example 11.1 Polyethylene glycol dithiopyridine Comparative Example 8.2 ---- Comparative Example 11.2 --- Example 9 Phospholipid Polyethylene Glycol Amino Example 12 Polyethylene glycol methacrylate phospholipids Comparative Example 9.1 Polyethylene glycol amino Comparative Example 12.1 Polyethylene glycol methacrylate Comparative Example 9.2 ---- Comparative Example 12.2 ----

[0122] The performance of the batteries prepared in the above examples and comparative examples was tested:

[0123] (1) Battery internal resistance AC impedance test method: The AC impedance test of 50% SOC lithium-ion battery was performed using a Metrohm PGSTAT302N chemical workstation in the range of 100 kHz-0.1 mHz and 25°C. The test results are listed in Table 7.

[0124] Table 7 Battery internal resistance AC impedance test results of the embodiment and comparative example

[0125]

[0126]

[0127] The internal resistance test results during the battery cycle show that the internal resistance of the lithium-ion battery prepared in the embodiment of the present invention is lower than that of the lithium-ion battery prepared in the comparative example during the cycle. The main reason is that the additive of the present invention can form an interface film on the surface of the negative electrode of the battery. Compared with the interface film formed on the surface of the conventional negative electrode, the interface film has the characteristics of high-speed lithium conduction and can quickly conduct lithium ions. Therefore, the lithium-ion battery prepared by the additive has lower internal resistance during the cycle and has certain application prospects.

[0128] (2) Battery cycle performance test method: The lithium-ion battery was subjected to a charge and discharge cycle test on a blue battery charge and discharge test cabinet. The test conditions were 25°C and 0.5C / 0.5C charge and discharge. The test results are listed in Table 8.

[0129] Table 8 Battery cycle performance test results of the embodiments and comparative examples

[0130]

[0131]

[0132] The test results of the cycle performance of the embodiment and the comparative example show that the capacity retention rate of the lithium-ion battery prepared in the embodiment of the present invention is higher than that of the lithium-ion battery prepared in the comparative example during the cycle. The main reason is that the additive of the present invention can form an interface film on the surface of the negative electrode. The solid interface film of the present invention is different from the interface film on the surface of the conventional negative electrode, and has the characteristics of good stability and high-speed lithium conduction. The conventional interface film on the surface of the negative electrode is formed during the first charge and discharge process of the lithium-ion battery. During the charge and discharge process of the lithium-ion battery, part of the interface film will dissolve and continue to generate. The components of the interface film generation need to consume electrolyte and lithium salt. The continuous consumption of electrolyte and lithium salt will cause the internal resistance of the battery to increase and the cycle performance to deteriorate. In the present invention, due to the addition of additives, it can form an interface film with better stability and higher lithium conductivity on the surface of the negative electrode, which can improve the lithium ion conduction performance inside the battery pole piece and enhance the battery cycle performance.

[0133] The test results of the cyclic charge and discharge performance of the embodiments and the comparative examples show that the lithium ion battery prepared by the electrolyte of the present invention has advantages in internal resistance and cycle performance compared with the comparative examples.

[0134] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A secondary battery, comprising a negative electrode sheet, wherein the negative electrode sheet comprises an additive and a negative electrode active material, wherein the additive comprises polyethylene glycol modified with a phosphorus-containing group, and the polyethylene glycol modified with a phosphorus-containing group is selected from at least one of the compounds shown in the following formula 1: Formula 1 In Formula 1, n is the degree of polymerization; R1 and R'1 are end-capping groups, and at least one of R1 and R'1 includes at least one phosphorus-containing functional group; R and R' are linking groups; The number-average molecular weight of the compound represented by Formula 1 is 200 to 30,000; The phosphorus-containing functional group includes at least one of -PO4R2R3, -PR4R5, and -(P=R6)R7R8, wherein: R2 to R8 are organic functional groups; The negative electrode active material is selected from silicon-based materials; alternatively, the negative electrode active material is selected from silicon-based materials and carbon-based materials; the silicon-based materials are selected from at least one of nano-silicon, SiOx where 0 < x < 2, aluminum-silicon alloy, magnesium-silicon alloy, boron-silicon alloy, phosphorus-silicon alloy, and lithium-silicon alloy; The mass of the additive accounts for 0.001 to 2 wt% of the total mass of the negative electrode active material layer; The single surface density of the negative electrode sheet is 1-25 mg / cm 2 .

2. The secondary battery according to claim 1, wherein The compound represented by formula 1 is selected from phospholipid-polyethylene glycol-thiol, phospholipid-polyethylene glycol-hydroxyl, distearoyl phosphatidyl acetamide-polyethylene glycol-amine, active ester-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-maleimide, fluorescein-polyethylene glycol-phospholipid, distearoyl phosphatidylethanolamine-polyethylene glycol-N-hydroxysuccinimide, amino-polyethylene glycol-phospholipid, eight-arm polyethylene glycol-phospholipid, phospholipid-polyethylene glycol polylactic acid-glycolic acid copolymer, linear peptide RGD-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-octreotide, phospholipid-polyethylene glycol-mannose, distearoyl phosphatidylethanolamine-polyethylene glycol, four-arm polyethylene glycol -Phospholipids, phospholipid-PEG-targeted cell-penetrating peptide TAT, phospholipid-PEG-polycaprolactone, carboxyl-PEG-phospholipids, phospholipid-PEG-amino, silicon-PEG-phospholipids, methoxy-PEG-phospholipids, phospholipid-PEG-silicon, phospholipid-PEG-rhodamine B, phospholipid-PEG-cyclic peptide RGD, phospholipid-PEG-biotin, azide-PEG-phospholipids, phospholipid-PEG-carboxyl, phospholipid-PEG-CY5, targeting peptide SP94-PEG-phospholipids, phospholipid-PEG-estrogen, four-arm PEG-distearic acid acylphosphatidylethanolamine, phospholipid-PEG-poly Ethylenimine, phospholipid-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-imino-tert-butyloxycarbonyl, phospholipid-polyethylene glycol-diphenylcyclooctyne, phospholipid-polyethylene glycol-polyaspartic acid benzyl ester, phospholipid-polyethylene glycol-folic acid, phospholipid-polyethylene glycol-polyglutamic acid, phospholipid-polyethylene glycol-cholesterol, phospholipid-polyethylene glycol-lactide-glycolide copolymer, phospholipid-polyethylene glycol-progesterone, indocyanine-polyethylene glycol-phospholipid, six-arm polyethylene glycol-distearic acid acylphosphatidylethanolamine, polylysine-polyethylene glycol-phospholipid, phospholipid-polyethylene glycol-peptide, phospholipid-polyethylene glycol-triphenylphosphine, phospholipid-polyethylene glycol-polyaspartic acid, methotrexate - At least one of polyethylene glycol-distearoylphosphatidylethanolamine, triphenyl phosphate-polyethylene glycol-distearoylphosphatidylethanolamine, galactose-polyethylene glycol-phospholipids, acrylate-polyethylene glycol-phospholipids, acrylamide-polyethylene glycol-phospholipids, dansylamide-polyethylene glycol-phospholipids, p-toluenesulfonate-polyethylene glycol-phospholipids, dopamine-polyethylene glycol-phospholipids, dimercaptopyridine-polyethylene glycol-phospholipids, alkynyl-polyethylene glycol-phospholipids, cyclooctyne-polyethylene glycol-phospholipids, epoxy-polyethylene glycol-phospholipids, methacrylate-polyethylene glycol-phospholipids, nitrophenyl carbonate-polyethylene glycol-phospholipids, and lipoic acid-polyethylene glycol-phospholipids.

3. The secondary battery according to claim 1, wherein The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer coated on one side or both sides of the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material, a conductive agent, a binder and the additive.

4. The secondary battery according to any one of claims 1 to 3, wherein: The secondary battery includes an electrolyte, and the electrolyte includes the additive.

5. The secondary battery according to claim 4, wherein: The electrolyte also includes a non-aqueous organic solvent and a lithium salt.

6. The secondary battery according to claim 4, wherein The content of the additive accounts for 0.01-5wt% of the total mass of the electrolyte.

Citation Information

Patent Citations

  • Method for modifying air stability phospholipid membrane on solid surface

    CN101955377A

  • Lithium ion secondary battery electrolyte

    CN103887563A

  • Lithium secondary battery and method for producing same

    CN104011925A

  • Preparation method of negative electrode of lithium manganate battery

    CN107749459A

  • Method for preparing negative electrode paste of lithium ion batteries