Positive electrode active material for lithium ion secondary battery and lithium ion secondary battery
By optimizing the material mass ratio and distribution of lithium, nickel, manganese, titanium and niobium in the lithium nickel manganese composite oxide, combined with STEM-EDX and laser diffraction scattering analysis, the problem of lithium nickel manganese composite oxide under high nickel ratio was solved. The problem of insufficient thermal stability has been solved, and a cathode active material with low cost, high thermal stability and low dissolved alkali content has been achieved, which is suitable for industrial-scale production.
Patent Information
- Application Number
- CN202080049430.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-07-08
- Filing Date
- 2020-06-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-06-30
AI Technical Summary
The existing lithium-nickel-manganese composite oxide cathode active material has insufficient thermal stability under high nickel ratios and high cost, and the existing technology cannot effectively combine the effects of niobium and titanium as dissimilar elements.
It adopts a lithium-nickel-manganese composite oxide with a hexagonal crystal layered structure, including lithium, nickel, manganese, titanium and niobium. Through specific material mass ratio and distribution, combined with analysis such as STEM-EDX and laser diffraction scattering method, niobium and niobium are optimized. The titanium is distributed to improve thermal stability and reduce the amount of dissolved alkali through water washing to prevent gelation.
A cathode active material with low cost, high thermal stability and low dissolved alkali content is realized, which is suitable for industrial-scale production and has both high battery capacity and output characteristics.
Smart Images

Figure CN114097114B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery and a lithium ion secondary battery. Background Art
[0002] In recent years, with the popularity of portable electronic devices such as mobile phones and notebook personal computers, there is a strong desire to develop small and lightweight non-aqueous electrolyte secondary batteries with high energy density and durability. In addition, as batteries for power tools and electric vehicles represented by hybrid vehicles, there is a strong desire to develop high-output secondary batteries.
[0003] As secondary batteries that meet such requirements, there are non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries. Lithium ion secondary batteries using lithium metal composite oxides with layered or spinel crystal structures as positive electrode active materials can obtain high voltages of 4V, and are therefore being promoted for practical use as batteries with high energy density.
[0004] As lithium metal composite oxides, lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel which is cheaper than cobalt, and lithium nickel cobalt manganese composite oxide (LiNiO2) have been proposed. 1 / 3 Co 1 / 3 Mn 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 O2) etc.
[0005] In addition, when a lithium ion secondary battery uses a non-aqueous electrolyte as a battery material, high thermal stability is required. For example, when a short circuit occurs inside the lithium ion secondary battery, heat is generated due to a rapid current, so higher thermal stability is required.
[0006] Therefore, attention has been paid to lithium nickel cobalt manganese composite oxides and lithium nickel manganese composite oxides having excellent thermal stability. Lithium nickel cobalt manganese composite oxides are layered compounds like lithium cobalt composite oxides and lithium nickel composite oxides, and materials having a composition ratio of 1:1:1 of nickel, cobalt and manganese at transition metal sites are called ternary positive electrode active materials.
[0007] In particular, in recent years, attention has been paid to ternary positive electrode active materials with the goal of high capacity, and positive electrode active materials with high nickel ratios (Hi-Ni positive electrode materials) that increase the nickel ratio of lithium nickel manganese composite oxides. However, the increase in battery capacity and the decrease in thermal stability caused by the nickel ratio are trade-offs, so positive electrode active materials with high performance (high cycle characteristics, high capacity, high output) as lithium ion secondary batteries and short circuit resistance and thermal stability are required.
[0008] In order to improve thermal stability, some technologies for adding niobium to lithium metal composite oxides have been proposed. For example, Patent Document 1 proposes a positive electrode active material for a non-aqueous secondary battery, which comprises a general formula: Li a Ni 1-x-y-z Co x M y Nb z O b (wherein M is one or more elements selected from the group consisting of Mn, Fe and Al, 1≤a≤1.1, 0.1≤x≤0.3, 0≤y≤0.1, 0.01≤z≤0.05, 2≤b≤2.2) A composition consisting of at least one compound containing lithium, nickel, cobalt, element M, niobium and oxygen. According to Patent Document 1, since the Li-Nb-O series compound present near the surface or inside the particle has high thermal stability, a positive electrode active material with high thermal stability and large discharge capacity can be obtained.
[0009] In addition, Patent Document 2 proposes a positive electrode active material for a non-aqueous electrolyte secondary battery, characterized in that it comprises a positive electrode active material having a general formula: Li x Ni 1-y-z MnCo y M z A lithium metal composite oxide powder represented by O2 (wherein 0.96≤x≤1.03, 0.05<y≤0.20, 0<z≤0.10, M is at least one metal element selected from the group consisting of V, Cr, Fe, and Mn), wherein the ratio of the sum of the atomic number of metal elements other than Li (i.e., the atomic number of Ni, Co, and M metal element) (Me) to the atomic number of Li (Li / Me) is 1.01 to 1.10, and when the positive electrode active material for a non-aqueous electrolyte secondary battery is immersed in water, the lithium dissolved into the water is less than 0.1wt%. According to Patent Document 2, a positive electrode active material for a non-aqueous electrolyte secondary battery with high capacity, excellent cycle characteristics, and low elution of alkali components can be obtained.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2002-151071
[0013] Patent Document 2: Japanese Patent No. 6201277
[0014] Patent Document 3: Japanese Patent Application Publication No. 2008-017729
[0015] Patent Document 4: Japanese Patent No. 4807467
[0016] Patent Document 5: Japanese Patent Application Publication No. 2006-147499
[0017] Patent Document 6: Japanese Patent Application Publication No. 2007-265784
[0018] Patent Document 7: Japanese Patent Application Publication No. 2008-257902 Summary of the invention
[0019] Problems to be solved by the invention
[0020] Although the above-mentioned Patent Document 1 states that the positive electrode active material described therein improves thermal stability by including niobium in a specific form, it is required to further improve the thermal stability of lithium nickel manganese composite oxides having a high nickel ratio. In addition, since niobium is expensive, a positive electrode active material capable of achieving high thermal stability at a lower cost is required.
[0021] In addition, the positive electrode active material described in the above patent document 2 can reduce the elution of alkali components and prevent gelation in the paste preparation for making battery plates by replacing a part of nickel with a specific transition metal and washing the calcined active material with water. However, the above patent document 2 does not record the effect of thermal stability at all.
[0022] The present invention is completed in view of these circumstances, and its purpose is to achieve higher thermal stability at low cost for a positive electrode active material containing a lithium nickel manganese composite oxide with a high nickel ratio, and to reduce the eluted alkali component to prevent gelation during paste preparation. In addition, the present invention aims to provide a method for easily producing such a positive electrode active material in industrial-scale production.
[0023] In order to obtain a positive electrode active material with high battery characteristics, for example, some technologies of adding titanium to lithium metal composite oxides have been proposed. According to Patent Documents 3 to 7, positive electrode active materials containing lithium nickel cobalt titanium composite oxides have good thermal stability and high battery capacity.
[0024] However, Patent Documents 1 to 7 do not describe at all the effects of containing niobium and titanium as different elements in combination in a lithium nickel manganese composite oxide.
[0025] Methods for solving problems
[0026] In a first embodiment of the present invention, a positive electrode active material for a lithium ion secondary battery is provided, which comprises a lithium nickel manganese composite oxide having a hexagonal layered structure and composed of secondary particles formed by agglomeration of a plurality of primary particles, wherein the metal elements constituting the lithium nickel manganese composite oxide comprise lithium (Li), nickel (Ni), manganese (Mn), cobalt (Co), titanium (Ti) and niobium (Nb) and optionally zirconium (Zr), and the mass ratio of the metal elements is Li:Ni:Mn:Co:Zr:Ti:Nb=a:b:c:d:e:f:g (wherein, 0.97≤a≤1.10, 0.80≤b≤0.88, 0.04≤c≤0.12, 0.04≤d≤0.10, 0≤e≤0.004, 0.003<f≤0.030, 0.001<g≤0.006, b+c+d+e+f+g=1) indicates that, in the mass ratio, (f+g)≤0.030 and f>g are satisfied, niobium is segregated at the grain boundaries between the primary particles of the lithium nickel manganese composite oxide, and the amount of lithium dissolved into water when immersed in water is less than 0.20 mass % relative to the total positive electrode active material.
[0027] In addition, the mass ratio of the metal elements can be represented by Li: Ni: Mn: Co: Zr: Ti: Nb = a: b: c: d: e: f: g (where 0.97 ≤ a ≤ 1.10, 0.80 ≤ b ≤ 0.88, 0.04 ≤ c ≤ 0.12, 0.04 ≤ d ≤ 0.10, 0 ≤ e ≤ 0.004, 0.003 < f ≤ 0.030, 0.003 ≤ g ≤ 0.006, b + c + d + e + f + g = 1). In addition, the amount of lithium dissolved into the water when immersed in water is preferably 0.10% by mass or less relative to the entire positive electrode active material. In addition, the niobium concentration at the grain boundary between the primary particles of the lithium nickel manganese composite oxide obtained by point analysis using STEM-EDX is preferably 1.3 times or more relative to the niobium concentration inside the primary particles. In addition, the titanium concentration of the grain boundary between the primary particles of the lithium nickel manganese composite oxide obtained by point analysis using STEM-EDX is preferably less than 1.3 times the titanium concentration inside the primary particles. In addition, the discrete index [(D90-D10) / Mv] representing the particle size calculated from D90 and D10 in the particle size distribution using the laser diffraction scattering method and the volume average particle size (Mv) is preferably 0.80 or more and 1.20 or less. In addition, the volume average particle size Mv is preferably 8 μm or more and 20 μm or less.
[0028] In a second aspect of the present invention, there is provided a lithium ion secondary battery comprising a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode contains the positive electrode active material for a lithium ion secondary battery.
[0029] Effects of the Invention
[0030] According to the present invention, a positive electrode active material that can achieve very high thermal stability at low cost and is not easily gelled during paste preparation can be provided. In addition, the present invention can easily produce such a positive electrode active material in industrial-scale production, and can be said to have great industrial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] [ Figure 1 ] Figure 1 This is a diagram showing an example of a method for producing a positive electrode active material according to this embodiment.
[0032] [ Figure 2 ] Figure 2 (A) and Figure 2 (B) is a diagram showing an example of a method for producing a nickel-manganese composite compound according to the present embodiment.
[0033] [ Figure 3 ] Figure 3 This is a schematic cross-sectional view of a button-type battery used in battery evaluation. DETAILED DESCRIPTION
[0034] Hereinafter, in this embodiment, a positive electrode active material for lithium ion secondary batteries and a method for producing the same, and a lithium ion secondary battery using the positive electrode active material will be described.
[0035] 1. Positive electrode active material for lithium-ion secondary batteries
[0036] The positive electrode active material for lithium ion secondary battery of the present embodiment (hereinafter also referred to as "positive electrode active material") includes a lithium nickel manganese composite oxide having a hexagonal layered structure and composed of secondary particles formed by agglomeration of a plurality of primary particles. The metal elements constituting the lithium nickel manganese composite oxide include lithium (Li), nickel (Ni), manganese (Mn), titanium (Ti) and niobium (Nb) and optionally include zirconium (Zr).
[0037] Lithium-ion secondary batteries require high thermal stability, especially when using flammable non-aqueous electrolytes as the constituent materials of lithium-ion secondary batteries. In addition, in lithium-ion secondary batteries, when a short circuit occurs between the positive electrode and the negative electrode in a charged state, the following chain reaction sometimes occurs: the positive electrode active material decomposes due to the large amount of heat generated by the rapid flow of current, and then generates heat. Therefore, by using a positive electrode active material with high structural stability in an overcharged state and not easy to decompose even at high temperatures, it is possible to suppress the release of oxygen caused by the thermal decomposition of the positive electrode active material and improve thermal stability.
[0038] The inventors of the present invention have conducted in-depth research and found that in lithium nickel manganese composite oxides used as positive electrode active materials, in particular, by combining specific amounts of titanium (Ti) and niobium (Nb) and containing them in a specific distribution, oxygen release during overcharge of the positive electrode active material is suppressed, and by washing the active material containing titanium and niobium with water to reduce the amount of dissolved alkali, high thermal stability and low amount of dissolved alkali can be achieved, thereby completing the present invention. The composition of the positive electrode active material of this embodiment is described in detail below.
[0039] [Lithium Nickel Manganese Composite Oxide]
[0040] The lithium nickel manganese composite oxide contained in the positive electrode active material is composed of secondary particles formed by agglomeration of a plurality of primary particles and has a hexagonal layered structure.
[0041] The metal elements constituting the lithium nickel manganese composite oxide include lithium (Li), nickel (Ni), manganese (Mn), cobalt (Co), titanium (Ti), and niobium (Nb), and optionally include zirconium (Zr).
[0042] The amount ratio (molar ratio) of the metal elements constituting the lithium nickel manganese composite oxide is represented by Li:Ni:Mn:Co:Zr:Ti:Nb=a:b:c:d:e:f:g (where 0.97≤a≤1.10, 0.80≤b≤0.88, 0.04≤c≤0.12, 0.04≤d≤0.10, 0≤e≤0.004, 0.003<f≤0.030, 0.001<g≤0.006, b+c+d+e+f+g=1). In addition, among the above amount ratios, f representing the amount ratio of titanium (Ti) and g representing the amount ratio of niobium (Nb) satisfy the relationship of (f+g)≤0.030 and f>g. The composition of each metal element is described below.
[0043] (lithium)
[0044] In the above-mentioned amount ratio, a representing the amount ratio of Li corresponds to the amount ratio (Li / Me) of Li to the above-mentioned metal elements Me (i.e., Ni, Mn, Co, Zr, Ti, and Nb) other than lithium. In addition, the range of a is 0.97≤a≤1.10, preferably 1.00≤a≤1.05. When the value of a is in the above-mentioned range, the reaction resistance of the positive electrode is reduced and the output of the battery can be increased. In addition, the range of a is preferably 1.00≤a≤1.03.
[0045] (nickel)
[0046] In the above-mentioned amount ratio, the range of b representing the amount ratio of Ni is 0.80≤b≤0.88, preferably 0.80≤b≤0.85, and more preferably 0.81≤b≤0.84. When the value of b is in the above-mentioned range, it is possible to have a high battery capacity and high thermal stability. On the other hand, when the value of b is less than 0.80, the battery capacity is reduced due to the reduction in the amount of transition metal that can be oxidized and reduced. In addition, when the value of b is greater than 0.88, thermal stability may be reduced.
[0047] (manganese)
[0048] In the above-mentioned amount ratio, the range of c representing the amount ratio of Mn is 0.04≤c≤0.12, preferably 0.06≤c≤0.12, and more preferably 0.07≤c≤0.11. When the value of c is in the above-mentioned range, it is possible to have a high battery capacity and high thermal stability. On the other hand, when the value of c is less than 0.04, the improvement effect of thermal stability is sometimes not obtained. In addition, when the value of c is greater than 0.12, the battery capacity is reduced. In addition, by including manganese in the above-mentioned range, the firing temperature can be increased in the firing step (S20) described later, and the dispersion of titanium and the like can be promoted.
[0049] (cobalt)
[0050] In the above-mentioned amount ratio, the range of d representing the amount ratio of Co is 0.04≤d≤0.10, preferably 0.04≤d≤0.08, and more preferably 0.04≤d≤0.07. When the value of d is in the above-mentioned range, it is possible to have high thermal stability and output characteristics. On the other hand, when the value of d is less than 0.04, the improvement effect of thermal stability and output characteristics is sometimes not obtained. In addition, when the value of d is greater than 0.10, the ratio of Ni and Mn is relatively reduced, resulting in a decrease in battery capacity.
[0051] (zirconium)
[0052] In the above-mentioned amount ratio, the range of e representing the amount ratio of Zr is 0≤e≤0.004, preferably ≤e≤0.0038, and more preferably 0≤e≤0.0035. The value of e may be 0 or greater than 0. When the value of e is greater than 0, the output characteristics and durability can be improved. On the other hand, when the value of e is greater than 0.004, the ratio of Ni to Mn is relatively reduced, resulting in a decrease in battery capacity.
[0053] (titanium)
[0054] In the above-mentioned amount ratio, the range of f representing the amount ratio of Ti is 0.003<f≤0.030, preferably 0.010≤f≤0.030, and more preferably 0.020≤f≤0.030. When titanium is included in the above-mentioned range together with niobium, compared with the case where each element is included alone, oxygen release can be suppressed when used in the positive electrode of a secondary battery, thereby obtaining high thermal stability. On the other hand, when the value of f is less than 0.003, the effect of improving thermal stability is not sufficient. In addition, when the value of f is greater than 0.030, the ratio of Ni and Mn is relatively reduced, or the crystal structure is unstable and cation mixing is prone to occur, so the battery capacity is greatly reduced.
[0055] (niobium)
[0056] In the above-mentioned amount ratio, the range of g representing the amount ratio of Nb is 0.001<g≤0.006, preferably 0.003≤g≤0.006, and may be 0.003≤g≤0.005. By including niobium in the above-mentioned range together with titanium, even if the niobium content is small, oxygen release can be suppressed when used in the positive electrode of a secondary battery, and high thermal stability is obtained.
[0057] In addition, in the above-mentioned amount ratio, the sum (f+g) of the amount ratio of titanium (f) and the amount ratio of niobium (g) is 0.030 or less. When f+g is within the above-mentioned range, high thermal stability can be achieved while obtaining a higher battery capacity.
[0058] In addition, in the above-mentioned amount ratio, the amount ratio (g) of niobium is smaller than the amount ratio (f) of titanium (f) (f>g), preferably f≥2g, more preferably f≥3g, and further preferably f≥4g. Niobium is a more expensive element than titanium, so by making the content less than titanium, the manufacturing cost can be reduced, and by combining with titanium, high thermal stability can be achieved.
[0059] It should be noted that the composition of the lithium nickel manganese composite oxide can be measured by quantitative analysis using inductively coupled plasma (ICP) emission spectrometry.
[0060] (Distribution of Niobium)
[0061] Niobium (Nb) contained in the lithium nickel manganese composite oxide of the present embodiment is preferably segregated at the grain boundaries between primary particles. The segregation of niobium can be confirmed, for example, by performing surface analysis / line analysis of the composition of the primary particle cross section using energy dispersive X-ray spectroscopy (STEM-EDX) using a scanning transmission electron microscope, thereby detecting the concentration of niobium at the grain boundaries between primary particles. It should be noted that a portion of niobium may be present inside the primary particles.
[0062] The niobium concentration at the grain boundary between primary particles determined by STEM-EDX is preferably 1.3 times or more, more preferably 1.5 times or more, the niobium concentration inside the primary particles. The upper limit of the niobium concentration is not particularly limited, and is, for example, 5 times or less.
[0063] The concentration of niobium inside the primary particles or at the grain boundaries can be confirmed by performing surface analysis, line analysis, and point analysis on the composition of the cross sections of a plurality of secondary particles using STEM-EDX measurement.
[0064] For example, the niobium concentration at the grain boundary between primary particles can be obtained as follows: 20 regions including the grain boundary between primary particles (e.g., a 130 nm × 130 nm region, a region included in a region where the grain boundary crosses the region) are randomly selected from the cross-sections of a plurality of secondary particles, the composition of each region is confirmed by point analysis, and the average value thereof is calculated. In addition, when measuring the niobium concentration in primary particles, the niobium concentration can also be obtained as follows: 20 internal regions in primary particles (e.g., a 130 nm × 130 nm region, a region not including the grain boundary) are randomly selected, the composition of each region is confirmed by point analysis, and the average value thereof is calculated.
[0065] (Distribution of Titanium)
[0066] The distribution of titanium (Ti) contained in the lithium nickel manganese composite oxide of the present embodiment is not particularly limited, and it may be present in at least one of the interior of the primary particle and the grain boundary, or it may be solid-dissolved in the interior of the primary particle. From the viewpoint of increasing the battery capacity in the secondary battery, it is preferably solid-dissolved. Here, solid-dissolved titanium means, for example, that titanium is detected inside the primary particle by surface analysis of the cross section of the secondary particle using STEM-EDX, and no concentration of titanium at the interface of the primary particle is confirmed, and titanium is preferably detected on the entire surface inside the primary particle.
[0067] For example, the titanium concentration at the grain boundary between primary particles obtained by STEM-EDX is preferably less than 1.3 times, may be less than 1.2 times, or may be less than 1.0 times relative to the titanium concentration inside the primary particles. In addition, the titanium concentration at the grain boundary between primary particles may be more than 0.8 times and less than 1.2 times relative to the titanium concentration inside the primary particles, and may be more than 0.9 and less than 1.1 times. It should be noted that the titanium concentration can be measured by surface analysis of STEM-EDX, etc., similarly to the above-mentioned niobium concentration.
[0068] In the lithium nickel manganese composite oxide of this embodiment, the distribution of metal elements other than niobium (Nb) and titanium (Ti) is not particularly limited. For example, Ni, Mn and Co are preferably detected over the entire surface of the interior of the plurality of primary particles constituting the secondary particles.
[0069] [Volume average particle size (Mv)]
[0070] The volume average particle size (Mv) of the positive electrode active material of this embodiment is preferably 8 μm or more and 20 μm or less, and more preferably 10 μm or more and 17 μm or less. When the volume average particle size Mv is within the above range, when the positive electrode active material is used for the positive electrode of a secondary battery, it can have both high output characteristics and battery capacity, as well as high filling property in the positive electrode.
[0071] On the other hand, when the volume average particle size Mv is less than 8 μm, high filling property in the positive electrode cannot be obtained sometimes. In addition, if the volume average particle size (Mv) is greater than 20 μm, high output characteristics and battery capacity cannot be obtained sometimes. It should be noted that the average particle size can be obtained, for example, by the volume integral value measured by a laser diffraction scattering particle size distribution meter.
[0072] [(D90-D10) / Mv] (Dispersion Index)
[0073] The positive electrode active material of this embodiment is preferably calculated from D90 and D10 in the particle size distribution obtained by laser diffraction scattering method and the volume average particle size (Mv) [(D90-D10) / Mv] is greater than 0.80 and less than 1.20. In addition, [(D90-D10) / Mv] represents the discrete index of the particle size of the particles constituting the positive electrode active material. It should be noted that the meanings of D90, D10 and Mv are the particle size (D90) when the volume integral of the particle amount in the particle size distribution curve is 90%, the particle size (D10) when it is 10%, and the volume average particle size (Mv), respectively.
[0074] When the particle size distribution of the particles constituting the positive electrode active material becomes a wide range, there will be many tiny particles with a particle size smaller than the volume average particle size (Mv) and coarse particles with a particle size larger than the average particle size. Therefore, when the discrete index is in the above range, the tiny particles and coarse particles are mixed together and the packing density becomes higher, which can increase the energy density per unit volume. The method for manufacturing the positive electrode active material having the above discrete index is not limited, for example, it can be obtained by a continuous crystallization method to prepare the nickel-manganese composite compound used in the mixing step (S10) described later.
[0075] On the other hand, when the discrete index of the positive electrode active material is less than 0.80, the volume energy density sometimes decreases. The upper limit of the discrete index is not particularly limited, for example, about 1.20. It should be noted that in the calcination step (S20) described later, if the calcination temperature is greater than 1000°C, the discrete index of the particle size is sometimes greater than 1.20. In this case, sometimes when the positive electrode active material is formed, the specific surface area decreases and the resistance of the positive electrode increases, thereby reducing the battery capacity.
[0076] [Amount of dissolved lithium]
[0077] The positive electrode active material of this embodiment can improve the crystallinity of the positive electrode active material and the discharge capacity by reducing the amount of eluted lithium to a specific amount, and can also suppress the gelation of the positive electrode mixture paste when manufacturing the electrode plate of the secondary battery.
[0078] In the positive electrode active material of the present embodiment, the amount of lithium dissolved into water when immersed in water (dissolved lithium amount) is less than 0.20 mass % relative to the positive electrode active material as a whole, preferably less than 0.10 mass %, and more preferably less than 0.08 mass %. In addition, the lower limit of the amount of dissolved lithium is not particularly limited, for example, it is more than 0.01 mass %. When the amount of dissolved lithium is within the above range, the remaining lithium in the lithium nickel manganese composite oxide can be drawn out to suppress the occurrence of gelation of the positive electrode mixture paste, etc. It should be noted that when the amount of dissolved lithium is less than 0.01 mass %, lithium is sometimes excessively drawn out of the lithium nickel manganese composite oxide during water washing, and sometimes the battery characteristics are reduced. In addition, the amount of dissolved lithium can be less than 0.06 mass %.
[0079] It should be noted that the amount of dissolved lithium can be measured as follows: 2g of positive electrode active material is taken, put into 125ml of pure water at room temperature stirred by a stirrer, and titrated with an aqueous solution of HCl immediately after the positive electrode active material is put in. During titration, the Warder method is used to evaluate, and the amount of lithium hydroxide (LiOH) and the amount of lithium carbonate (Li2CO3) are calculated, and the sum of these lithium amounts is calculated as dissolved lithium. In addition, the amount of dissolved lithium can be adjusted to the above range, for example, by washing the lithium nickel manganese composite oxide obtained after calcination.
[0080] [Specific surface area]
[0081] Furthermore, the specific surface area of the positive electrode active material of the present embodiment measured by the BET method is preferably 0.4 m 2 / g above 2.0m 2 When the specific surface area is within the above range, the number of points where Li ions enter and exit during charge and discharge reactions increases, so the specific surface area is less than 0.4 m 2 / g can improve the battery capacity. On the other hand, in the positive electrode active material with a high nickel ratio, if the specific surface area is greater than 2.0m 2 / g, even if the water washing step (S30) described later is performed to remove the dissolved alkali components on the surface of the particles, it may sometimes react with the moisture in the atmosphere to increase the alkali components derived from the lithium dissolved from the surface of the particles. When such a positive electrode active material is used to make a positive electrode composite paste, the positive electrode composite paste may sometimes gel and make it difficult to make a positive electrode. In addition, the upper limit of the specific surface area of the positive electrode active material can be, for example, 1.5m 2For example, by performing the water washing step (S30) and the drying step (S40) described later, the specific surface area of the lithium nickel manganese composite oxide can be increased compared to that before water washing.
[0082] [Maximum oxygen production peak temperature]
[0083] The maximum oxygen generation peak temperature of the positive electrode active material of this embodiment when heated in an overcharged state is preferably 250°C or more. The upper limit of the maximum oxygen generation peak temperature when heated is not particularly limited, and is about 300°C or less. It should be noted that the maximum oxygen generation peak temperature can be measured using the method described in the examples. In addition, the maximum oxygen generation peak temperature refers to the temperature at which the oxygen generated when heated reaches a maximum and largest peak.
[0084] [Maximum oxygen release rate]
[0085] The positive electrode active material of this embodiment is expected to have a low maximum oxygen release rate when the temperature is increased in an overcharged state. Regarding the maximum oxygen release rate, when the positive electrode active material manufactured under the same conditions except that titanium and niobium are not added and the sintering temperature is adjusted according to the composition is set to 100%, it is preferably 60% or less, and more preferably 50% or less. The lower limit of the maximum oxygen release rate when the temperature is increased is not particularly limited, and it is a degree of more than 0.1%. It should be noted that the maximum oxygen release rate can be determined by the method described in the embodiment. In addition, the maximum oxygen release rate refers to the weight reduction rate at the time when the absolute value of the value after differentiating the weight reduction during heating by time is the largest. It should be noted that the sintering temperature adjusted according to the composition refers to the temperature range in which the discharge capacity reaches the highest in the composition (that is, the temperature range in which the crystallinity is sufficiently high). Generally, there is a tendency to become higher as the amount of added elements increases.
[0086] [Thermal runaway temperature]
[0087] The lithium-ion battery using the positive electrode active material of the present embodiment is expected to have a high thermal runaway temperature measured by an accelerated rate calorimeter (ARC) in a charged state. Regarding the thermal runaway temperature, the thermal runaway starting temperature of the positive electrode active material manufactured under the same conditions except that titanium and niobium are not added and the firing temperature is adjusted according to the composition is used as a reference, preferably above +8°C, more preferably above +10°C. The upper limit of the thermal runaway temperature is not particularly limited. It should be noted that the thermal runaway temperature can be measured using the method described in the examples. In addition, the thermal runaway temperature refers to the temperature at which the heat generation rate becomes greater than 10°C / min in the ARC measurement.
[0088] 2. Method for producing positive electrode active material for lithium ion secondary battery
[0089] Figure 1 , Figure 2 (A) and Figure 2 (B) is a diagram showing an example of a method for manufacturing a positive electrode active material for a lithium ion secondary battery according to the present embodiment (hereinafter also referred to as a “method for manufacturing a positive electrode active material”). The obtained positive electrode active material comprises a lithium nickel manganese composite oxide composed of secondary particles formed by agglomeration of a plurality of primary particles. In addition, by the above-mentioned manufacturing method, a positive electrode active material comprising the above-mentioned lithium nickel manganese composite oxide can be easily obtained on an industrial scale. It should be noted that the following description is an example of a manufacturing method according to the present embodiment and is not limited to the manufacturing method.
[0090] like Figure 1 As shown, the manufacturing method of this embodiment comprises: a mixing step (S10) of mixing at least a nickel-manganese composite compound, a titanium compound, a niobium compound and a lithium compound to obtain a mixture; a calcining step (S20) of calcining the mixture to obtain a lithium nickel-manganese composite oxide; a washing step (S30) of washing the lithium nickel-manganese composite oxide obtained after calcining; and a drying step (S40) of drying the lithium nickel-manganese composite oxide after washing.
[0091] In addition, the nickel-manganese composite compound used in the mixing step (S10) is, for example, Figure 2 (A) and Figure 2 The product shown in (B) can be obtained by a method comprising a crystallization step (S1) and / or a heat treatment step (S2). Each step will be described in detail below.
[0092] [Mixing step (S10)]
[0093] like Figure 1 As shown, the mixing step (S10) is a step of mixing the nickel-manganese composite compound, the titanium compound, the niobium compound and the lithium compound to obtain a mixture. In addition, a zirconium compound is also mixed as needed. The titanium compound, the niobium compound, the lithium compound and the zirconium compound as needed can be added and mixed, for example, in the form of powder (solid phase). The following describes each material.
[0094] (Nickel-manganese complex compound)
[0095] The nickel-manganese composite compound used in the mixing step (S10) can be obtained by a known method. The content (composition) of the metals (Ni, Mn, Co, etc.) in the nickel-manganese composite compound is also substantially maintained in the lithium nickel-manganese composite oxide particles, so the content of each metal is preferably in the same range as the content in the above-mentioned lithium nickel-manganese composite oxide. It should be noted that the nickel-manganese composite compound used in this embodiment may contain a small amount of elements other than the above-mentioned metal elements (Ni, Mn, Co, etc.), hydrogen and oxygen within a range that does not impair the effect of the present invention.
[0096] The nickel-manganese composite compound can be a hydroxide or an oxide. As a method for manufacturing the nickel-manganese composite hydroxide, for example, a method for neutralizing and crystallizing using an aqueous solution of a metal salt and an alkaline solution can be cited. In addition, the nickel-manganese composite compound can be heat-treated to remove the moisture of the nickel-manganese composite compound, or a part or all of the nickel-manganese composite compound can be made into a nickel-manganese composite oxide. Their manufacturing methods can be obtained, for example, by referring to the method described in Patent Document 2, etc.
[0097] (Titanium compounds)
[0098] As the titanium compound, a known compound containing titanium can be used. In addition, the titanium compound can be used alone or in combination of two or more.
[0099] Among them, compounds containing titanium and oxygen are preferred from the viewpoint of ease of acquisition and avoiding impurities from being mixed into the lithium nickel manganese composite oxide. It should be noted that when impurities are mixed into the lithium nickel manganese composite oxide, the thermal stability, battery capacity and cycle characteristics of the obtained secondary battery may be reduced.
[0100] (Niobium compounds)
[0101] As the niobium compound, a known compound containing niobium can be used. Among them, from the viewpoint of easy acquisition and avoiding impurities from being mixed into the lithium nickel manganese composite oxide, the niobium compound is preferably a compound containing niobium and oxygen. It should be noted that when impurities are mixed into the lithium nickel manganese composite oxide, the thermal stability, battery capacity, and cycle characteristics of the obtained secondary battery may be reduced.
[0102] (Lithium compounds)
[0103] The lithium compound is not particularly limited, and known lithium-containing compounds can be used, for example, lithium carbonate, lithium hydroxide, lithium nitrate or a mixture thereof can be used. Among them, lithium carbonate, lithium hydroxide or a mixture thereof is preferably used from the viewpoint that the influence of residual impurities is small and the mixture is dissolved at the calcination temperature.
[0104] (Hybrid Method)
[0105] The mixing method of the nickel-manganese composite compound, lithium compound, titanium compound, niobium compound and zirconium compound as required is not particularly limited, as long as the particles are fully mixed to such an extent that the skeletons of these particles are not destroyed. As a mixing method, for example, a general mixer can be used for mixing, for example, a vibrating mixer, a Lodige mixer, a Julia mixer, a V-type blender, etc. can be used for mixing. It should be noted that the titanium mixture is preferably fully mixed before the calcining process described later. In the case of insufficient mixing, sometimes the atomic % ratio (Li / Me, equivalent to a in the mass ratio) of Li and the metal element Me other than Li (Me=Ni+Mn+element M+Ti+Nb in this embodiment) between each particle of the positive electrode active material is deviated, and problems such as failure to obtain sufficient battery characteristics may occur.
[0106] The lithium compounds are mixed in such a way that the Li / Me in the mixture becomes the same as the Li / Me of the target positive electrode active material. This is because the molar ratio of Li / Me and each metal element does not change before and after the sintering process (S20), so the Li / Me of the mixture in the mixing process (S10) is the Li / Me of the lithium nickel manganese composite oxide after sintering. It should be noted that when the subsequent water washing process (S30) is implemented, a part of the remaining lithium component present on the surface of the active material will dissolve in water, so the Li / Me ratio may be reduced compared to the active material after the sintering process (S20). The reduction in the Li / Me ratio varies according to the composition, physical properties, and water washing conditions of the positive electrode active material. In an example of the manufacturing method of this embodiment, it is reduced by about 0.02 due to the water washing process (S30).
[0107] It should be noted that the content (ratio) of niobium (Nb) and titanium (Ti) in the mixture is also roughly maintained in the lithium nickel manganese composite oxide, so the mixing amount of the niobium compound and the titanium compound is preferably in the same range as the content of niobium and titanium in the above-mentioned lithium nickel manganese composite oxide.
[0108] [Firing step (S20)]
[0109] The calcining step ( S20 ) is a step of calcining the mixture obtained in the mixing step ( S10 ) to obtain a lithium nickel manganese composite oxide.
[0110] If the mixture is fired, the lithium in the lithium compound diffuses in the nickel-manganese composite compound, thereby forming a lithium-nickel-manganese composite oxide composed of particles with a polycrystalline structure. The lithium compound melts at the temperature during firing, penetrates into the nickel-manganese composite compound to form a lithium-nickel-manganese composite oxide. The lithium compound melts at the temperature during firing, penetrates into the nickel-manganese composite compound to form a lithium-nickel-manganese composite oxide. At this time, niobium and titanium contained in the lithium mixture also penetrate into the interior of the secondary particles together with the molten lithium compound. For primary particles, if there are grain boundaries, etc., it is believed that penetration will also occur. Below, the firing conditions are described in detail, and according to the mass ratio of the metal elements contained in the lithium-nickel-manganese composite oxide, adjustments are made within the range of each firing condition described below to optimize the battery characteristics.
[0111] The calcination atmosphere is preferably an oxidizing atmosphere, and more preferably an oxygen concentration higher than that of the air. By using an oxidizing atmosphere, a positive electrode active material having both battery characteristics and thermal stability can be obtained while maintaining a high battery capacity and improving thermal stability.
[0112] The firing temperature is 760°C to 1000°C in an oxidizing atmosphere, preferably 760°C to 950°C. When firing at the above temperature, melting of the lithium compound occurs, promoting the penetration and diffusion of titanium. In addition, the mixture can increase the firing temperature by containing manganese. By increasing the firing temperature, the diffusion of titanium and niobium can be promoted. Furthermore, the crystallinity of the lithium nickel manganese composite oxide becomes higher, which can further increase the battery capacity.
[0113] On the other hand, when the calcination temperature is less than 760°C, the diffusion of lithium, titanium, and manganese into the nickel-manganese composite compound will not proceed sufficiently, and the remaining lithium and unreacted particles will remain, or the crystal structure will not be neat enough, resulting in the problem that sufficient battery characteristics cannot be obtained. In addition, when the calcination temperature is greater than 1000°C, sintering occurs violently between the particles of the formed lithium-nickel-manganese composite oxide, and abnormal particle growth may occur. If abnormal particle growth occurs, the following problems will arise: the particles after calcination will become coarse, and the filling property will be reduced when the positive electrode active material is formed. In addition, the reaction resistance will increase due to the disorder of the crystal structure, and the discharge capacity will decrease.
[0114] The firing time is preferably set to at least 3 hours, more preferably 6 hours or more and 24 hours or less. When the firing time is less than 3 hours, it is possible not to fully generate the lithium nickel manganese composite oxide. In addition, the furnace used in the firing is not particularly limited, as long as the titanium mixture can be fired in an oxygen stream, preferably an electric furnace that does not generate gas, and any of a batch or continuous furnace can be used.
[0115] [Water washing (S30)]
[0116] The water washing step ( S30 ) is a step of mixing the lithium nickel manganese composite oxide obtained in the calcining step ( S20 ) with water and stirring (hereinafter referred to as “water stirring”), followed by solid-liquid separation.
[0117] The manufacturing method of this embodiment is provided with a water washing step (S30) and a drying step (S40) described later, so that the crystallinity of the positive electrode active material is improved and the discharge capacity is improved. Although the details are not clear, it is believed that, for example, when lithium in the positive electrode active material is extracted by water stirring, the disorder of the atomic arrangement is alleviated and the crystallinity of the positive electrode active material is improved, showing a high discharge capacity. In addition, by dissolving the remaining lithium component on the surface in water and removing it by utilizing the water washing step (S30), the gelation of the positive electrode composite paste when making the plate of the secondary battery can be suppressed.
[0118] The amount of water mixed in the water washing process (S30) is preferably 50 parts by mass or more and 200 parts by mass or less relative to 150 parts by mass of the lithium nickel manganese composite oxide. When the mixing ratio of water is more than 200 parts by mass, excessive lithium will be drawn out from the positive electrode active material, which may cause a decrease in battery capacity and an increase in reaction resistance. On the other hand, when the mixing ratio of water is less than 50 parts by mass, the effect of improving crystallinity and the removal of residual lithium components will be insufficient, which may cause a decrease in battery capacity and gelation of the positive electrode composite paste. In addition, the amount of water mixed in the water washing process (S30) can be 50 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the lithium nickel manganese composite oxide.
[0119] The time for washing with water is not particularly limited, and is, for example, about 1 minute to 2 hours, or 5 minutes to 50 minutes.
[0120] After the lithium nickel manganese composite oxide is stirred with water, solid-liquid separation is performed to obtain the lithium nickel manganese composite oxide (precipitate). The method of solid-liquid separation is not particularly limited, and a known method can be used. For example, solid-liquid separation can be performed using one or more of a suction filter selected from a Nutsche filter (Buchner funnel), a filter press, a centrifuge, and the like.
[0121] [Drying Step (S40)]
[0122] The drying step ( S40 ) is a step of drying the lithium nickel manganese composite oxide (precipitate) obtained in the water washing step ( S30 ) to obtain a powder (dried powder) of a lithium metal composite hydroxide.
[0123] The drying conditions are preferably heat treatment at a temperature of 100° C. to 250° C. in an oxidizing atmosphere or a vacuum atmosphere. When the drying temperature is 100° C. or higher, the water in the precipitate can be fully evaporated. In addition, when the drying temperature is 250° C. or lower, a compact drying device can be used, which is suitable for industrial-scale implementation.
[0124] The atmosphere during drying is preferably an atmosphere that does not contain water vapor or carbon dioxide to avoid the reaction of moisture, carbonic acid and the obtained positive electrode active material in the atmosphere, and is specifically preferably an oxidizing atmosphere or a vacuum atmosphere such as an oxygen atmosphere. In addition, from the viewpoint that the water vapor generated by drying can be quickly discharged, it is preferred to add an exhaust mechanism to the drying device.
[0125] The drying time is not particularly limited, but is preferably set to 0.5 hours or more at the highest temperature reached during drying in order to fully evaporate the water content of the raw material mixture. In addition, from the viewpoint of productivity, the upper limit of the drying time is preferably set to 48 hours or less.
[0126] 3. Lithium-ion secondary battery
[0127] The lithium-ion secondary battery of the present embodiment (hereinafter also referred to as "secondary battery") comprises a positive electrode, a negative electrode and a non-aqueous electrolyte containing the above-mentioned positive electrode active material. The secondary battery, for example, comprises a positive electrode, a negative electrode and a non-aqueous electrolyte. In addition, the secondary battery, for example, may comprise a positive electrode, a negative electrode and a solid electrolyte. In addition, any secondary battery is a secondary battery that is charged and discharged by the separation and insertion of lithium ions, for example, it may be a non-aqueous electrolyte secondary battery or an all-solid-state lithium secondary battery. It should be noted that the embodiments described below are merely illustrative, and the secondary battery of the present embodiment may be applied to various forms in which various changes and improvements are implemented based on the embodiments described in this specification.
[0128] The secondary battery of the present embodiment can achieve high thermal stability at low cost. In addition, the positive electrode active material for the secondary battery can be obtained by the above-mentioned industrial manufacturing method. In addition, the secondary battery is suitable for the power supply of small portable electronic devices (notebook personal computers, mobile phone terminals, etc.) that always require high capacity. In addition, compared with the batteries using the positive electrode active materials of lithium cobalt oxides or lithium nickel oxides in the past, the secondary battery is not only excellent in capacity, but also excellent in durability and thermal stability during overcharge. Therefore, since it can be miniaturized and high-capacity, it is suitable as a power supply for electric vehicles with restricted carrying space. In addition, the secondary battery can be used not only as a power supply for electric vehicles driven purely by electric energy, but also as a so-called hybrid vehicle power supply used in conjunction with combustion mechanisms such as gasoline engines and diesel engines.
[0129] [Example]
[0130] Hereinafter, the present invention will be further described in detail using the embodiments and comparative examples of the present invention, but the present invention is not limited to these embodiments. It should be noted that the analysis method of the metal contained in the positive electrode active material in the embodiments and comparative examples and the various evaluation methods of the positive electrode active material are as follows.
[0131] (1) Composition analysis: Measured by ICP emission analysis.
[0132] (2) Volume average particle size Mv and particle size dispersion index [(D90-D10) / average volume particle size]: The particle size distribution was measured on a volume basis using a laser diffraction scattering particle size analyzer (MICROTRAC HRA manufactured by NIKKISO CO., LTD.).
[0133] (3) Concentration of each element
[0134] The positive electrode active material was processed so that the cross-section analysis of the primary particles could be performed using S-TEM. 20 primary particles were randomly selected from the plurality of secondary particles contained in the positive electrode active material, and the composition of the internal area and the grain boundary region of each primary particle cross section was analyzed using EDX of S-TEM.
[0135] (4) Amount of dissolved lithium: 2 g of positive electrode active material was added to 125 ml of pure water at room temperature stirred by a stirrer, and titrated with a 1 mol / L HCl aqueous solution immediately after the active material was added. The titration was performed using an automatic titrator COM-1750 (manufactured by Hiranuma Sangyo Co., Ltd.) under the following conditions.
[0136] End point detection method: inflection point detection
[0137] Detection sensitivity: 2500
[0138] Dropper Model: H-1700
[0139] Dropper speed: 2
[0140] Minimum drop volume: 0.013mL
[0141] The titration result was evaluated by the Warder method, lithium hydroxide (LiOH) and lithium carbonate (Li2CO3) were calculated, and the sum of these lithium amounts was calculated as eluted lithium.
[0142] (5) Specific surface area: The specific surface area / pore size distribution measuring apparatus (manufactured by Mountech, model: Macsorb HM1200 series) was used to measure the specific surface area by the BET method using nitrogen adsorption.
[0143] (6) Initial discharge capacity:
[0144] The initial charge capacity and initial discharge capacity were prepared as follows: Figure 3 The button-type battery CBA shown in the figure is placed for about 24 hours. After the open circuit voltage OCV (open circuit voltage) stabilizes, the current density at the positive electrode is 0.1 mA / cm 2 The battery was charged to a cutoff voltage of 4.3 V and the initial charge capacity was set. After a 1-hour pause, the initial discharge capacity was set at a capacity when the battery was discharged to a cutoff voltage of 3.0 V. A multi-channel voltage / current generator (R6741A manufactured by Advantest Co., Ltd.) was used for the measurement of the discharge capacity.
[0145] (Production of button-type batteries)
[0146] 52.5 mg of the obtained positive electrode active material, 15 mg of acetylene black and 7.5 mg of polytetrafluoroethylene resin (PTFE) were mixed and press-formed at a pressure of 100 MPa into a diameter of 11 mm and a thickness of 100 μm to prepare Figure 3 The positive electrode (evaluation electrode) PE shown. After the prepared positive electrode PE was dried at 120°C in a vacuum dryer for 12 hours, the positive electrode PE was used to make a 2032 type button-type battery CBA in a glove box in an Ar atmosphere with a dew point managed at -80°C. As the negative electrode NE, lithium (Li) metal with a diameter of 17 mm and a thickness of 1 mm was used, and as the electrolyte, an equal amount of a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) with 1M LiClO4 as a supporting electrolyte (manufactured by Toyama Pharmaceutical Industry Co., Ltd.) was used. As a separator SE, a polyethylene porous membrane with a film thickness of 25 μm was used. In addition, the button-type battery CBA is a button-type battery assembled by configuring a gasket GA and a corrugated gasket WW, and using a positive electrode shell PC and a negative electrode shell NC. The measurement results of the initial charge and discharge capacity of the obtained positive electrode active material and the positive electrode resistance value are shown in Table 2.
[0147] (7) Maximum oxygen generation peak temperature
[0148] The thermal stability of the positive electrode is evaluated as follows: the positive electrode active material is made into an overcharged state and heated, and the amount of oxygen released thereby is quantified. A button-type battery is made in the same manner as (6), and CC charging (constant current-constant voltage charging) is performed at a rate of 0.05C to a cut-off voltage of 4.3V. Then, the button battery is disassembled, and only the positive electrode is carefully removed to avoid short circuit, and it is cleaned with DMC (dimethyl carbonate) and dried. About 2 mg of the dried positive electrode is measured, and a gas chromatograph-mass spectrometer (GCMS, Shimadzu Corporation, QP-2010plus) is used to heat the sample from room temperature to 450°C at a heating rate of 10°C / min. Helium is used as a carrier gas. The generation behavior of oxygen (m / z=32) generated during heating is measured to obtain the maximum oxygen generation peak temperature.
[0149] (8) Maximum oxygen release rate
[0150] The maximum oxygen release rate is calculated from the weight change caused by making the positive electrode active material overcharged and heating it. A button-type battery is made in the same manner as (6), and CC charging (constant current-constant voltage charging) is performed at a rate of 0.05C to a cut-off voltage of 4.3V. Then, the button battery is disassembled, and only the positive electrode is carefully removed to avoid short circuit, and it is cleaned with DMC (dimethyl carbonate) and dried. About 10 mg of the dried positive electrode is measured and heated from room temperature to 450°C at a heating rate of 10°C / min using a thermogravimetric analyzer (TG, manufactured by Rigaku, Thermoplus II). The measurement atmosphere is nitrogen. The weight loss during heating is differentiated, and the maximum value is set as the maximum oxygen release rate. In this embodiment, the relative value is calculated with Comparative Example 1 as 100%.
[0151] (9) Thermal runaway temperature
[0152] In order to implement the safety evaluation of the battery, a battery using a negative electrode with graphite as the negative electrode active material was prepared, and an ARC (accelerating calorimeter) measurement test was performed. The following is a method for preparing a battery for the ARC measurement test. Mix according to a ratio of 95 parts by mass of positive electrode active material, 3 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride as a binder. Use a mixer (TKHIVIS MIX, manufactured by PRIMIX Co., Ltd.) to mix the mixture and prepare a positive electrode composite slurry. Then, the positive electrode composite slurry is applied to an aluminum foil with a thickness of 15 μm, and the coating is dried to form a positive electrode active material layer on the aluminum foil. It is cut out according to a predetermined size to make a positive electrode. The prepared positive electrode and the negative electrode with graphite as the negative electrode active material are stacked in a manner facing each other through a separator to make an electrode body. Next, a non-aqueous electrolyte and an electrode body, which were mixed with ethylene carbonate (EC), ethyl methyl carbonate (MEC) and dimethyl carbonate (DMC) in a volume ratio of 3:3:4 and 1.2M lithium hexafluorophosphate (LiPF6) as a supporting salt, were inserted into an aluminum casing to make an ARC test battery. For the manufactured battery, the thermal runaway temperature was measured using ARC (accelerating calorimeter, manufactured by Thermal Hazard Technology) under the conditions shown below.
[0153] Measurement start temperature: 130°C
[0154] Keep temperature: 20min
[0155] Fever detection temperature: 0.02℃ / min
[0156] Temperature rise: 5℃
[0157] Battery voltage: 4.2V charging state
[0158] The temperature at which the heat generation rate exceeds 10° C. / min is defined as the thermal runaway temperature. In this embodiment, the thermal runaway temperature of Comparative Example 1 is used as a reference, and the difference from the thermal runaway temperature of Comparative Example 1 is calculated and shown as the thermal runaway temperature change amount.
[0159] (Reference Example 1)
[0160] [Mixing process]
[0161] Particles of nickel-manganese-cobalt composite hydroxide (mol ratio of nickel:manganese:cobalt is 85:10:5) obtained by a known method, lithium hydroxide, titanium oxide and niobic acid were weighed in such a manner that the mass ratio of lithium:(nickel+manganese+cobalt):titanium:niobium became 1.01:0.973:0.022:0.005, and then they were fully mixed using a vibration mixer device (TURBULA T2C manufactured by Willy ABachofen (WAB) Co.) to obtain a lithium mixture.
[0162] [Firing process]
[0163] The obtained lithium mixture was calcined by maintaining it at 870° C. for 10 hours in an oxygen flow, and then crushed to obtain particles of lithium nickel manganese cobalt composite oxide.
[0164] [evaluate]
[0165] Tables 1 and 3 show the production conditions and evaluation results of the obtained positive electrode active materials.
[0166] (Reference Example 2)
[0167] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, zirconium oxide, titanium oxide and niobic acid were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt): zirconium: titanium: niobium was 1.03: 0.970: 0.003: 0.022: 0.005, and in the sintering step, the sintering temperature was set to 840° C., and the positive electrode active material was obtained and evaluated in the same manner as in Reference Example 1. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 3.
[0168] (Reference Example 3)
[0169] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, zirconium oxide, titanium oxide and niobic acid were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt): zirconium: titanium: niobium was 1.03: 0.970: 0.003: 0.022: 0.005, and in the sintering step, the sintering temperature was set to 800° C., and the positive electrode active material was obtained and evaluated in the same manner as in Reference Example 1. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 3.
[0170] (Example 1)
[0171] Relative to 150 parts by mass of lithium nickel manganese cobalt titanium composite oxide obtained under the same conditions as Reference Example 1, water was mixed in a ratio of 100 parts by mass, and after stirring with water, suction filtration was performed using a Nutsche filter to obtain a precipitate (water washing process). The obtained precipitate was placed in a SUS container, heated to 100° C. using a vacuum dryer and allowed to stand for drying for 12 hours, and heated to 190° C. and allowed to stand for drying for 10 hours to obtain a positive electrode active material (drying process).
[0172] [evaluate]
[0173] The evaluation results of the obtained positive electrode active material are shown in Tables 1 to 3. In addition, in the positive electrode active material of Example 1, the ratio of the titanium concentration at the grain boundary between primary particles to the titanium concentration inside the primary particles (grain boundary / inside the particle) is 0.9, and no titanium concentration is observed at the grain boundary between primary particles. It should be noted that the maximum oxygen release rate and / or thermal runaway temperature were evaluated in some examples and comparative examples, and the evaluation results are shown in Table 2.
[0174] (Example 2)
[0175] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, titanium oxide and niobic acid were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): titanium: niobium was 1.02: 0.975: 0.022: 0.003, and the positive electrode active material was obtained and evaluated in the same manner as in Example 1. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 3.
[0176] (Example 3)
[0177] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, titanium oxide and niobic acid were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): titanium: niobium was 1.01: 0.972: 0.025: 0.003, and the positive electrode active material was obtained and evaluated in the same manner as in Example 1. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 and 3.
[0178] (Example 4)
[0179] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, zirconium oxide, titanium oxide and niobic acid were weighed so that the mass ratio of lithium: (nickel + manganese + cobalt): zirconium: titanium: niobium was 1.01: 0.970: 0.003: 0.022: 0.005, and the positive electrode active material was obtained and evaluated in the same manner as in Example 1. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 to 3.
[0180] (Example 5)
[0181] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, zirconium oxide, titanium oxide and niobic acid were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt): zirconium: titanium: niobium was 1.03: 0.970: 0.003: 0.022: 0.005, and in the sintering step, the sintering temperature was set to 860° C., and the positive electrode active material was obtained and evaluated in the same manner as in Example 1. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 to 3.
[0182] (Example 6)
[0183] In the mixing process, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, zirconium oxide, titanium oxide and niobic acid were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt): zirconium: titanium: niobium was 1.03: 0.970: 0.003: 0.022: 0.005, and in the calcining process, the calcining temperature was set to 840° C., and the positive electrode active material was obtained and evaluated in the same manner as in Example 1. It should be noted that the water washing was performed using the lithium-nickel-manganese-cobalt-titanium composite oxide obtained under the same conditions as Reference Example 2. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 to 3.
[0184] (Example 7)
[0185] In the mixing process, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, zirconium oxide, titanium oxide and niobic acid were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt): zirconium: titanium: niobium was 1.03: 0.970: 0.003: 0.022: 0.005, and in the calcining process, the calcining temperature was set to 800° C., and the positive electrode active material was obtained and evaluated in the same manner as in Example 1. It should be noted that the water washing was performed using the lithium-nickel-manganese-cobalt-titanium composite oxide obtained under the same conditions as Reference Example 3. The manufacturing conditions and evaluation results of the positive electrode active material are shown in Tables 1 to 3.
[0186] (Comparative Example 1)
[0187] In the mixing step, the particles of the nickel-manganese-cobalt composite hydroxide and lithium hydroxide were weighed in a manner such that the mass ratio of lithium: nickel: manganese: cobalt was 1.02:0.85:0.10:0.05 without preparing the titanium compound and the niobium compound, and in the sintering step, the sintering temperature was set to 800° C., and a positive electrode active material was obtained and evaluated in the same manner as in Example 1. The obtained positive electrode active material was compressed to 4.0 g / cm 3 The volume resistivity is 8.8×10 1 Tables 1 and 2 show the production conditions and evaluation results of the positive electrode active material.
[0188] (Comparative Example 2)
[0189] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide and niobic acid were weighed in a manner such that the mass ratio of lithium: (nickel + manganese + cobalt): niobium was 1.02:0.99:0.010 without preparing a titanium compound, and in the sintering step, the sintering temperature was set to 850° C., and the positive electrode active material was obtained and evaluated in the same manner as in Example 1. The obtained positive electrode active material was compressed to 4.0 g / cm 3 The volume resistivity is 3.7×10 2 Tables 1 and 2 show the production conditions and evaluation results of the positive electrode active material.
[0190] (Comparative Example 3)
[0191] In the mixing step, the obtained nickel-manganese-cobalt composite hydroxide particles, lithium hydroxide, titanium oxide and niobic acid were weighed in such a manner that the mass ratio of lithium: (nickel + manganese + cobalt): titanium: niobium was 1.01: 0.977: 0.022: 0.001. The positive electrode active material was obtained and evaluated in the same manner as in Example 1. The obtained positive electrode active material was compressed to 4.0 g / cm 3 The volume resistivity is 3.4×10 2 Table 1 shows the production conditions and evaluation results of the positive electrode active material.
[0192] [Table 1]
[0193]
[0194] [Table 2]
[0195]
[0196] [Table 3]
[0197]
[0198] (Evaluation results)
[0199] As shown in Table 1, the maximum oxygen generation peak temperature of the positive electrode active material obtained in the embodiment is above 250°C, and the amount of dissolved lithium is below 0.20% by mass, which indicates that it has high thermal stability, suppresses oxygen release during overcharging, and can suppress the gelation of the paste when making the electrode plate. In addition, in the positive electrode active material of the embodiment, the ratio of the titanium concentration at the grain boundary between the primary particles to the titanium concentration inside the primary particles (grain boundary / inside the particle) is above 0.8 and below 1.1, and no titanium concentration is observed at the grain boundary between the primary particles.
[0200] In addition, as shown in Table 2, the maximum oxygen release rate of the positive electrode active material obtained in the embodiment is less than 60% and the thermal runaway temperature is also above +8°C relative to Comparative Example 1 which does not contain titanium and niobium. This result also shows that the positive electrode active material of the embodiment suppresses oxygen release during overcharge, has a higher self-heating starting temperature, and improves thermal stability.
[0201] On the other hand, in Comparative Example 1 in which titanium and niobium were not added, the maximum oxygen generation peak temperature was less than 250°C, and the thermal stability was lower than that of the examples. In addition, in Comparative Example 2 in which only titanium was added and Comparative Example 3 in which the amount of niobium added was small, the maximum oxygen generation peak temperature was also less than 250°C, and the thermal stability was lower than that of the examples.
[0202] In addition, as shown in Table 3, compared with Reference Examples 1 to 3 in which titanium and niobium were added but the water washing process was not performed, the Example in which the water washing process was performed had a low amount of eluted alkali, and because the residual alkali component on the surface was reduced, gaps were formed near the grain boundaries on the surface of the active material, so the specific surface area was high and the discharge capacity was high. This result shows that the battery characteristics of the Example were better than those of the Reference Example in which the water washing process was not performed and the residual alkali component was not reduced.
[0203] Industrial Applicability
[0204] In this embodiment, a positive electrode active material for a lithium ion secondary battery having high thermal stability and excellent battery characteristics can be obtained by an industrial manufacturing method. The lithium ion secondary battery is suitable for power sources of small portable electronic devices (notebook personal computers, mobile terminals, etc.) that always require high capacity.
[0205] In addition, the secondary battery using the positive electrode active material of this embodiment has excellent thermal stability and capacity compared with the battery using the positive electrode active material of the conventional lithium nickel oxide, and is therefore suitable as a power source for electric vehicles with limited mounting space because it can be miniaturized.
[0206] Furthermore, the secondary battery using the positive electrode active material of this embodiment can be used not only as a power source for electric vehicles driven purely by electric energy, but also as a power source for so-called hybrid vehicles used in conjunction with a combustion mechanism such as a gasoline engine or a diesel engine, or as a stationary storage battery.
[0207] It should be noted that the technical scope of the present invention is not limited to the forms described in the above-mentioned embodiments, etc. Sometimes one or more of the elements described in the above-mentioned embodiments, etc. may be omitted. In addition, the elements described in the above-mentioned embodiments, etc. may be appropriately combined. In addition, to the extent permitted by law, the contents of all documents cited in Japanese Patent Application No. 2019-127262 and this specification are cited as part of the records of this article.
Claims
1. A positive electrode active material for a lithium ion secondary battery, comprising a lithium nickel manganese composite oxide having a hexagonal layered structure and composed of secondary particles formed by agglomeration of a plurality of primary particles, The metal elements constituting the lithium nickel manganese composite oxide include lithium (Li), nickel (Ni), manganese (Mn), cobalt (Co), titanium (Ti) and niobium (Nb) and optionally include zirconium (Zr). The amount ratio of the metal elements is represented by Li:Ni:Mn:Co:Zr:Ti:Nb=a:b:c:d:e:f:g, wherein: 0.97≤a≤1.10, 0.80≤b≤0.88, 0.04≤c≤0.12, 0.04≤d≤0.10, 0≤e≤0.004, 0.003<f≤0.030, 0.001<g≤0.006, b+c+d+e+f+g=1, In the substance amount ratio, (f+g)≤0.030 and f>g are satisfied, Niobium segregates at the grain boundaries between primary particles of the lithium nickel manganese composite oxide. When immersed in water, the amount of lithium dissolved into water is 0.20 mass % or less relative to the entire positive electrode active material. The niobium concentration at the grain boundary between primary particles of the lithium nickel manganese composite oxide determined by point analysis using STEM-EDX is 1.3 times or more the niobium concentration inside the primary particles. The titanium concentration at the grain boundaries between the primary particles of the lithium nickel manganese composite oxide, determined by point analysis using STEM-EDX, is less than 1.3 times the titanium concentration inside the primary particles.
2. The positive electrode active material for lithium ion secondary battery according to claim 1, wherein the mass ratio of the metal elements is represented by Li:Ni:Mn:Co:Zr:Ti:Nb=a:b:c:d:e:f:g, wherein: 0.97≤a≤1.10, 0.80≤b≤0.88, 0.04≤c≤0.12, 0.04≤d≤0.10, 0≤e≤0.004, 0.003<f≤0.030, 0.003≤g≤0.006, b+c+d+e+f+g=1. 3 . The positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the amount of lithium eluted into water when immersed in water is 0.10 mass % or less based on the entire positive electrode active material.
4. The positive electrode active material for a lithium ion secondary battery according to claim 1 or 2, wherein a dispersion index [(D90-D10) / Mv] indicating the particle size calculated from D90 and D10 in the particle size distribution by a laser diffraction scattering method and the volume average particle size Mv is 0.80 or more and 1.20 or less. 5 . The positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the volume average particle size Mv is 8 μm or more and 20 μm or less. 6 . A lithium ion secondary battery comprising a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode comprises the positive electrode active material for a lithium ion secondary battery according to claim 1 .